Coating composition for a wiper blade of a wiper frame
The coating composition with colloidal silica and cellulose fibers addresses premature wear and noise issues in windshield wiper blades by enhancing abrasion resistance and adhesion, significantly extending blade lifespan and reducing noise.
Patent Information
- Application Number
- PCT/EP2024/059791
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Windshield wiper blades experience premature wear due to incessant friction, leading to reduced wiping quality and noise, necessitating frequent replacement, and existing lubricating compositions are flammable and not suitable for non-professional use.
A coating composition comprising an aqueous phase with colloidal silica, cellulose fibers, and a solid lubricating agent, such as graphite, which improves abrasion resistance and adhesion, reducing wear by 20-25% compared to reference compositions.
The composition enhances the durability and noise reduction of windshield wiper blades by providing improved abrasion resistance and adhesion, extending the lifespan of the blades while maintaining flexibility and reducing noise.
Smart Images

Figure EP2024059791_17102024_PF_FP_ABST
Abstract
Description
Coating composition for windshield wiper blade
[0001] The invention relates to a coating composition for a wiper blade for a vehicle windshield wiper blade, the use of such a composition and a method for preparing it. It also relates to a wiper blade for a windshield wiper blade coated at least partially with the composition.
[0002] Motor vehicles are commonly equipped with windshield wiper systems to wash and / or wipe the windshield and prevent the driver's view of their surroundings from being disturbed. The wiper blades of such a system are conventionally driven by arms performing a reciprocating angular movement. These blades rub against the outer surface of the window, for example the windshield, and evacuate the water by bringing it out of the driver's field of vision. In a conventional version, the blades are made in the form of articulated levers that hold the wiper blade at several points. In a more recent version called "flat blade", the blades are made in the form of a semi-rigid assembly that holds the wiper blade along its entire length.
[0003] Generally speaking, a wiper blade is made of elastically deformable material based on an elastomer supplemented with additives, in particular to improve its mechanical properties, elasticity, wear resistance, resistance to external aggressions or to facilitate the implementation of the manufacturing process. This may, for example, be reinforcing fillers, plasticizer, vulcanizing agent, agent for protection against UV radiation, oxidation, ozone and / or wear.
[0004] In the case of wiper blades for motor vehicle windscreen wipers, these blades must have characteristics that allow effective wiping of the windscreen on which they move while providing sound comfort in use for the occupant of the vehicle, i.e. avoiding generating sound waves or noise. However, when using the windscreen wiper, the incessant friction of the blade on the windscreen causes premature wear of the blade, resulting not only in a loss of wiping quality but also in generating noise.
[0005] Blade wear requires the replacement of the entire wiper blade, although the other parts and elements of the wiper blade are still functional. In order to increase the lifespan of a wiper blade, US patent 5,447,645 describes a composition for lubricating and preserving rubber, comprising graphite, butyl titanate and isopropanol. This composition may also include other products such as anti-UV stabilizers, a binder, etc. However, such a composition has a highly flammable nature, which requires special storage conditions and is therefore not suitable for direct use by a non-professional.
[0006] FR2977258 describes compositions useful for the renovation of windshield wiper blades which are aqueous compositions comprising 5 to 25% of sliding fillers, preferably graphite powder.
[0007] There is always a need to improve the performance of windshield wiper blades, and in particular their wear resistance, allowing for a longer lifespan. It is also desirable to have coating compositions that can improve these performances, that are easy to implement and that have good adhesion to the wiper blade.
[0008] These and other objects are achieved by the compositions of the present invention.
[0009] Indeed, it has been found within the framework of the present invention that the addition of fibers and silica to coating compositions makes it possible to improve the abrasion resistance of coating compositions.
[0010] This is why the present invention relates to a coating composition for a windshield wiper blade, the composition being an aqueous phase composition comprising at least one resin and at least one solid lubricating agent in dispersion, the composition further containing
[0011] (i) from 0.1 to 10% and in particular from 1.1 to 9.3% of a colloidal silica solution comprising from 40 to 50% of dry extract, and
[0012] (ii) from 0.5 to 5% of cellulose fibres, in particular from 0.5 to 3%
[0013] the percentages being given by weight relative to the total weight of the composition.
[0014] The composition is preferably an aqueous phase composition, which generally contains from 10 to 75% aqueous solvent, in particular from 20 to 75% aqueous solvent. By aqueous solvent is meant a medium comprising water and optionally one or more hydrophilic co-solvents; such co-solvents may for example be of an alcoholic nature, in particular glycolic esters.
[0015] Advantageously, the composition contains from 12 to 50% of a solid lubricating agent in dispersion. The composition generally contains from 10 to 31%, in particular from 10 to 30.6% of a resin dispersion, comprising from 40 to 50% of dry extract. The percentages are given by weight relative to the total weight of the composition.
[0016] The solid lubricating agent content in the dispersion is adjusted to provide 3 to 15% of solid lubricating agent in the composition. The dispersion is in aqueous phase.
[0017] The composition may further contain additives. The additive content will be adapted by a person skilled in the art; if such additives are present, their concentration is generally between 0.01 and 1% by weight.
[0018] The invention also relates to a process for preparing such coating compositions. The process comprises in particular the following steps:
[0019] a) adding cellulose fibres to a dispersion of solid lubricating agent in aqueous phase, to obtain a mixture of cellulose fibres and lubricating agent in aqueous dispersion,
[0020] b) introduction of colloidal silica into the mixture of cellulose fibers and solid lubricating agent obtained in step a
[0021] c) adding at least one resin in aqueous phase to the dispersion obtained in step b.
[0022] The invention also relates to the use of such a coating composition, capable of being obtained by said method, for at least partially coating a wiper blade for a windscreen wiper.
[0023] Another object of the invention is a windshield wiper blade coated with such a composition, by using a coating composition.
[0024] For the purposes of the invention, the term "aqueous phase" is understood to mean in particular a composition which comprises an organic solvent content of less than or equal to 10% by weight of the total weight of the composition. The organic solvent content is preferably less than or equal to 5% by weight, and more preferably equal to 0% by weight of the total weight of the composition.
[0025] The concentration of colloidal silica in the compositions according to the invention may in particular be from 0.1 to 8%, in particular from 0.4 to 7% of colloidal silica by weight relative to the total weight of the composition. This means that the concentration of colloidal silica can be, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9% or 8% by weight relative to the total weight of the composition.The concentration of colloidal silica may in particular be 4 to 7% by weight, relative to the total weight of the composition.
[0026] According to variants of the invention, the concentration of amorphous silica may be approximately 0.4 to 4%, in particular 0.9 to 3.5% by weight. Good results are obtained in particular when the concentration of amorphous silica in the coating compositions is in particular approximately 2.8%.
[0027] Preferably, the silica is in the form of particles of size less than or equal to 2 nm.
[0028] According to one embodiment of the coating compositions of the invention, the silica is present in the form of a colloidal silica dispersion, in particular in the form of a colloidal silica dispersion with a solids content of 40 to 50%. Colloidal silicas are most often prepared in a multi-step process where an alkali silicate solution is partially neutralized, resulting in the formation of silica nuclei.
[0029] The coating composition may thus contain from 1 to 20% of colloidal silica dispersion with a dry extract of 40 to 50%, preferably from 1 to 10%, in particular from 1.1 to 9.5% of colloidal silica dispersion with a dry extract of 40 to 50%, in particular from 2.4 to 8% of colloidal silica dispersion with a dry extract of 40 to 50%.
[0030] The concentration of cellulose fibers in the coating compositions of the invention may in particular vary from 0.5 to 3% of cellulose fibers, in particular from 0.8 to 2.5%, in particular from 1.5 to 2% by weight, relative to the total weight of the composition. This means that the concentration of cellulose fibers may for example be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9% or 3% by weight relative to the total weight of the composition.
[0031] The cellulose fibers useful for implementing the invention preferably have a size of 6 to 12 µm.
[0032] Unexpectedly, the inventors have demonstrated that while silica or cellulose fibers used as a single additive have an effect of reducing the resistance of coating compositions, the addition of these two components to a coating composition improves the abrasion resistance.
[0033] This synergistic effect can allow a reduction of around 20 or even 25% in the rate of coating removed when using the blade, compared to a reference composition not containing it. This effect can be demonstrated in particular by an abrasion test.
[0034] The coating compositions according to the invention have good adhesion to the rubber blade.
[0035] The solid lubricating agent may be chosen from lubricants known to those skilled in the art. Examples include natural lubricants such as graphite and molybdenum disulfide, as well as synthetic lubricants such as graphite fluoride, tungsten disulfide, boron nitride, tungsten, molybdenum and niobium diselenide, or titanium iodide and disulfide, as well as their various mixtures in all proportions.
[0036] Preferably, graphite and / or molybdenum disulfide are used, and particularly powdered graphite. Preferably, the graphite has a size of less than 10 µm.
[0037] The concentration of solid lubricating agent is generally from 1 to 15% by weight relative to the total weight of the composition, in particular from 3 to 15%, in particular from 6 to 11%. The lubricating agent may be provided in the form of an aqueous dispersion, in particular a dispersion with a dry extract of 30 to 40%. The dispersion may then constitute from 10 to 55% by weight of the coating composition, in particular from 12 to 50%, in particular from 25 to 40%.
[0038] The resin may in particular be an aqueous phase resin, comprising at least one acrylic, vinyl, styrene or urethane type polymer, in aqueous phase. The polymer may be a homopolymer or a copolymer. These polymers may be used alone or mixed depending on their compatibilities or the desired final properties. Advantageously, the resin contains at least one acrylic polymer in aqueous phase.
[0039] This may include a dispersion or emulsion of polymer in aqueous phase.
[0040] The resin preferably has a glass transition temperature of less than or equal to 0°C, and more preferably less than or equal to -20°C, in order to retain the flexibility properties of the coating film at low temperatures.
[0041] The quantity of resin in the compositions will be adapted by those skilled in the art depending on the desired properties; it is generally 10 to 31% by weight relative to the total weight of the composition.
[0042] The resin may in particular be introduced in the form of a dispersion in aqueous phase, in particular with a dry extract of 40 to 50%. In this case, the dispersion may represent from 10 to 31%, in particular from 15 to 25% by weight relative to the total weight of the composition.
[0043] The composition according to the invention may further contain at least one additive chosen from thickening agents, spreading agents, dispersing agents and UV protective agents. The additive content is generally approximately 0.01 to 1% by weight, relative to the total weight of the composition.
[0044] UV protective agents include UV stabilizers and UV inhibitors.
[0045] The thickeners are preferably chosen from modified celluloses and modified urethane polymers. The content is preferably less than or equal to 0.5% by weight relative to the total weight of the composition.
[0046] The spreading agent makes it possible to reduce the surface energy of the composition. It can in particular be chosen from silicone surfactants, such as dimethylsiloxane modified polyethers.
[0047] Dispersing agents are intended to ensure better dispersion of particles, such as glass particles and solid lubricating agent. The dispersing agent is in particular a water-soluble polymeric agent; preferably, the polymeric dispersing agent comprises an ionic form of the polymer or copolymer used as resin. For example, a polyacrylate will preferably be used when the resin is a polyacrylic resin.
[0048] Coating compositions according to the invention may in particular have the following formulas (the percentages being expressed by weight relative to the total weight of the composition):
[0049] Resin(s) (dry extract 40% to 50%): 10 – 31%,
[0050] Lubricating charge in dispersion (dry extract 30% to 40%): 12 – 51%,
[0051] Cellulose fibers: 0.5 – 3%,
[0052] Colloidal silica (dry extract 40% to 50%): 1 – 10%,
[0053] Additive(s): 0.01 – 1%, and
[0054] Solvent(s): 15 – 75%.
[0055] Other compositions according to the invention have the following formulas:
[0056] Resin(s) (dry extract 40% to 50%): 15-25%,
[0057] Lubricating charge in dispersion (dry extract 30% to 40%): 25 - 40%,
[0058] Cellulose fibers: 0.80 – 2.5%,
[0059] Colloidal silica (dry extract 40% to 50%): 2.4 - 8%,
[0060] Additive(s): 0.01 – 1%, and
[0061] Solvent(s): 34 – 45%.
[0062] The invention also relates to a process for preparing a coating composition as defined above. The process advantageously comprises one or more additional steps after step c.
[0063] Any additives are added, if applicable, after step c.
[0064] The solvent(s) are also added after this step c. These are in particular water and possibly one or more co-solvents such as glycol ethers, such as 2-butoxyethanol.
[0065] The contents of the various constituents are as indicated above.
[0066] The invention also relates to the use of a coating composition as defined in the present text or capable of being obtained by the process described above, for at least partially coating a wiper blade for a windscreen wiper.
[0067] The composition can, for example, be applied directly to the wiper blade or to a profiled rubber strip, which is then re-cut into two or three parts to obtain the wiper blade. The coating composition is applied by dipping the wiper blade or profiled rubber strip into the composition, by spraying the composition onto the wiper blade or profiled rubber strip, or by coating the wiper blade or profiled rubber strip with the composition. The wiper blade or profiled rubber strip is then dried. In the case of the rubber strip, this is finally re-cut into two or three parts to obtain the wiper blades.
[0068] The application step may be preceded by a preheating step and baking of the coating, particularly in an infrared oven or a convection oven.
[0069] The thickness of the coating layer is between 1 and 10 µm, preferably between 3 and 7 µm, and more preferably between 4 and 6 µm.
[0070] The invention also relates to a windshield wiper blade to which the coating composition has been applied. The blade is coated with a composition comprising at least solid lubricants, graphene and resin, as defined above, but in which the solvent has been evaporated.
[0071] The silica content in the coating, in the form of a dry film, on the surface of the blade thus coated is generally 0.4 to 4% by weight relative to the total weight of the coating, for example 0.4 to 3.8% by weight relative to the weight of the dry film. The cellulose fiber content in this coating is generally 0.5 to 3% by weight, relative to the weight of the coating in the form of a dry film.
[0072] The coating composition for a windscreen wiper blade according to the invention may in particular be an aqueous phase composition comprising at least one resin and at least one solid lubricating agent, the composition further containing (i) from 0.4 to 4% of amorphous silica, (ii) from 0.5 to 3% of cellulose fibers, the percentages being given by weight relative to the total weight of the composition.
[0073] The invention also relates to the coating composition as it results from its application to a support. The invention thus relates to a coating composition in the form of a dry film which comprises from 0.4 to 4% of silica, in particular from 0.4 to 3.8% and from 0.5 to 3%, in particular from 0.5 to 2.5% by weight of cellulose fibers, the percentages being given by weight relative to the weight of the dry film. Brief description of the figures
[0074] The invention will be better understood on reading the following description, given solely by way of example and with reference to the appended drawings in which:
[0075] represents a wiping blade of a windshield wiper blade according to the invention.
[0076] represents the dust resistance histogram for a reference composition and for compositions containing increasing contents of cellulose fibers. The quantity of fibers is indicated in % on the right-hand y-axis.
[0077] represents the dust resistance histogram for a reference composition and for compositions containing increasing colloidal silica contents. The amount of colloidal silica is indicated in % on the right-hand y-axis.
[0078] represents the dust resistance histogram for a reference composition and for compositions containing a fixed cellulose fiber content (1.7%) and increasing colloidal silica contents. The amount of colloidal silica is indicated in % on the right-hand y-axis Examples
[0079] Example 1: Dust resistance tests of compositions containing cellulose fibers alone
[0080] The compositions corresponding to the following formulas are prepared:ReferenceMNOResin(s)23232323Lubricating filler(s)46.740.428.29.7Cellulose fibers-1.7510Additive(s)0.10.10.10.1Solvent(s)30.234.843.757.2
[0081] Adhesion tests are compliant for all compositions
[0082] Dust resistance tests are carried out. The test consists of sliding the rubber blades coated with the composition over a dry, abrasive flat surface under a certain load (here 15N / m) and for a certain number of cycles (here 10) to determine their dust resistance.
[0083] After determining the height of the coating removed by abrasion, it is compared to that observed for the reference composition.
[0084] The dust resistance test results are shown in Figure 2 and in the following tableReferenceMNOCellulose fibers01.7510Resistance (wear rate between reference and test formulas (%)066.766.751.6
[0085] Resistance is expressed as a percentage of coating removed compared to the reference.
[0086] The presence of cellulose fibers alone weakens the coating. Indeed, as soon as 1.7% of fibers are added, the resistance of the coating decreases significantly and becomes nearly 67% wear compared to the reference. The addition of cellulose fibers alone does not provide additional resistance.
[0087] Example 2: Dust resistance tests of compositions containing colloidal silicas alone
[0088] Compositions corresponding to the following formulas are preparedReferencePQRResin(s)23232323Lubricating filler(s)46.743.338.920.8Colloidal silica-257Additive(s)0.10.10.10.1Solvent(s)30.231.63349.1
[0089] The silica rate is a wet rate
[0090] The results are presented in figure number 3 and in the following tableReferencePQRColloidal silica content0257Resistance (wear rate between the reference and the test formulas (%)053.818.366.7
[0091] The presence of colloidal silica leads to a reduction in the resistance of the coating. Indeed, from the addition of 2% of silica, an increase in wear of almost 54% is observed compared to the reference.
[0092] Example 3: Dust resistance test of compositions according to the invention
[0093] The dust resistance of a composition containing 1.7% cellulose fibers and a colloidal silica content ranging from 2.4 to 7% is measured.
[0094] The test consists of sliding the rubber blades coated with the composition on a dry and abrasive flat surface, under a certain load (here 15N / m) and for a certain number of cycles (here 10) to determine their resistance.
[0095] After determining the height of the coating removed by abrasion, it is compared to that observed for the reference composition.
[0096] The tested compositions are shown in the following tableReferenceDEFResin(s)23232323Lubricating filler(s)46.734.136.830Cellulose fibers-1.71.71.7Colloidal silica4.32.47Additive(s)0.10.10.10.1Solvent(s)30.238.33638.2
[0097] The results of the dust resistance tests are shown in Figure 4 and in the following table: ReferenceEDFColloidal silica content02.44.37Resistance (wear rate between the reference and the test formulas (%))0-1.1%-7.5%-19.4%
[0098] It is observed that for a given cellulose fiber rate, the higher the silica rate, the lower the proportion of coating removed (i.e. the less the coating is damaged). This reflects an improvement in the dust resistance of the coating.
Claims
Coating composition for a windshield wiper blade, the composition being an aqueous phase composition comprising at least one resin and at least one solid lubricating agent, the composition further containing (i) from 0.1 to 10% of a colloidal silica solution comprising from 40 to 50% of dry extract (ii) from 0.5 to 3% of cellulose fibers, the percentages being given by weight relative to the total weight of the composition. Composition according to claim 1, characterized in that the silica is in the form of particles of a size less than or equal to 2 nm. Composition according to at least one of claims 1 or 2, characterized in that it contains (i) from 0.1 to 8% of colloidal silica, in particular from 0.4 to 7% of colloidal silica and (ii) from 0.5 to 3% of cellulose fibers, in particular from 0.8 to 2.5%. Composition according to at least one of the preceding claims, characterized in that the silica is in the form of a dispersion of colloidal silica. Composition according to at least one of the preceding claims, characterized in that it contains from 3 to 15% of a solid lubricating agent. Composition according to at least one of the preceding claims, characterized in that it also contains at least one additive chosen from thickening agents, spreading agents, dispersing agents and UV protective agents. Composition according to at least one of the preceding claims, characterized in that it comprises from 10 to 31% by weight of a resin dispersion comprising from 40 to 50% of dry extract. Process for preparing a composition according to at least one of the preceding claims, characterized in that it comprises the following steps: a) Addition of cellulose fibers to a dispersion of solid lubricating agent in aqueous phase, to obtain a mixture of cellulose fibers and lubricating agent in aqueous dispersion, b) introduction of colloidal silica to the mixture of cellulose fibers and solid lubricating agent obtained in step a) c) addition of at least one resin in aqueous phase to the dispersion obtained in step b). Use of a composition according to at least one of claims 1 to 7, or of a composition obtainable by the process according to claim 8, for at least partially coating a wiper blade for a windscreen wiper. Wiper blade for windscreen wiper blade coated at least in part with a composition according to one of claims 1 to 7 or capable of being obtained by the use according to claim 9. Wiper blade for windscreen wiper according to the preceding claim, characterized in that it is coated at least in part with a composition which is in the form of a dry film comprising from 0.4 to 4% of silica and from 0.5 to 3% by weight of cellulose fibers, the percentages being given by weight relative to the weight of the dry film. Coating composition in the form of a dry film as defined in the preceding claim, characterized in that it comprises from 0.4 to 4% of silica and from 0.5 to 3% by weight of cellulose fibers, the percentages being given by weight relative to the weight of the dry film.
Citation Information
Patent Citations
Aqueous composition, useful for renovation of a wiper of windshield wiper brush, comprises black filler, preferably graphite powder, binder comprising polyurethane acrylic resin, dispersing agent, spreading agent and thickening agent
FR2977258A1
Composition and method for lubricating and preserving rubber
US5447645A
Coating solution for rubber materials, preferably for wiper rubber of windscreen wiper, comprises a binder having a resin component, which is hydrophilic in nature
DE102008002249A1
Coating composition for lubrication
EP0372559A1
Surface coating member
EP0562191A2