Thick product made of aluminium copper lithium alloys with improved toughness, and method for obtaining same

The described process for aluminum-copper-lithium alloy sheets, involving casting, homogenization, hot rolling, and tempering, addresses the need for improved elastic limit and toughness, enhancing mechanical properties and thermal stability for aerospace applications.

WO2024213843A1PCT designated stage expired Publication Date: 2024-10-17CONSTELLIUM ISSOIRE +1

Patent Information

Application Number
PCT/FR2024/050449
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-05
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

There is a need for aluminum-copper-lithium alloy sheets with a thickness greater than 25 mm that offer an improved compromise between elastic limit and toughness, while maintaining thermal stability, corrosion resistance, and fatigue endurance, which is not adequately met by existing products.

Method used

A process involving casting, homogenization at 515°C to 540°C for 5 to 50 hours, hot rolling to achieve a thickness of 25 mm to 50 mm, followed by solution treatment, quenching, and tempering to achieve a rolled product with specific grain texture distributions and mechanical properties, including an elastic limit of at least 505 MPa and toughness of at least 45.5 MPa.Vm.

Benefits of technology

The process enhances the elastic limit and toughness of aluminum-copper-lithium alloy sheets, achieving improved mechanical properties and thermal stability, while maintaining corrosion resistance and fatigue endurance, specifically targeting aerospace applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FR2024050449_17102024_PF_FP_ABST
    Figure FR2024050449_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a rolled product which has an improved Rp0.2 (L) – K1c (L-T) compromise, the thickness of which is between 25 mm and 50 mm, and which is made of aluminium alloy with the following composition by weight: - Cu 2.2-3.9 - Li 0.7-1.2 - Mg 0.1-0.8 - Mn 0.1-0.6 - Zr 0.07-0.15 - Ti 0.01-0.15 - Fe <0.1 - Si <0.1% - Ag ≤ 0.40 - Zn ≤ 0.70, other elements <0.05 each and <0.15 in total, the remainder being aluminium, such that, at mid-thickness, the volume fraction of the grains having a brass texture is less than 21%. This product is obtained by a method comprising a step of casting, homogenising, hot rolling, solution heat treating, quenching, and tempering such that, during the hot rolling step, the outlet temperature is between 395 and 445°C.
Need to check novelty before this filing date? Find Prior Art

Description

DESCRIPTION Title: Thick product made of aluminum copper lithium alloys with improved toughness and method for obtaining the same TECHNICAL FIELD

[0001] The invention relates to thick products made of aluminum-copper-lithium alloys, more particularly, such products with a thickness of between 25 mm and 50 mm, their manufacturing and use methods, intended in particular for aeronautical and space construction. PREVIOUS ART

[0002] Most structural applications in the aerospace industry require a high level of strength, as well as a high level of toughness. Therefore, products with the best static-toughness compromise are sought.

[0003] Products intended for aircraft wing structures are mainly made from thick sheets according to the definition given in EN 12258-1. For products intended for aircraft wing structures, it is advantageous to focus on the yield strength compromise in the longitudinal direction (R p o.2(L)) and tenacity in the LT direction (Ki c (LT)). This is particularly the case for wing skins, central box panels or spars. In this case, where the main stress is along the largest dimension of the sheet, the tensile properties in the L direction (rolling direction) are of prime importance, as well as the toughness in the LT direction, this term meaning that the stress is applied in the L direction and the crack propagates in the T direction (long cross-section).

[0004] Lithium aluminum alloys are considered in the metallic design of aircraft structural elements, and in particular aircraft wing structures because they offer an excellent compromise between density, mechanical characteristics, toughness, fatigue and corrosion resistance.

[0005] Among the aluminum-lithium based alloys, aluminum copper lithium alloys are well known in the prior art for their interesting properties. Specifically, US patent 7,229,509 describes an alloy comprising (% by weight): 2.5-5.5 Cu; 0.1-2.5 Li; 0.2-1.0 Mg; 0.2-0.8 Ag; 0.2-0.8 Mn; 0.4 max Zr or other grain refining agents such as Cr, Ti, Hf, Sc, V, having in particular a toughness Kic(LT)>37.4 MPa.Vm for a yield strength R P o,2( L) > 448.2 MPa (products with a thickness greater than 76.2 mm) and in particular a toughness K1C(L)>38.5 MPaVm for an elastic limit RpO,2(L) > 489.5 MPa (products with a thickness less than 76.2 mm).

[0006] EP2235224 discloses a substantially non-recrystallized rolled product obtained from a sheet having a thickness of at least 30 mm, comprising: 2.2 to 3.9 wt% Cu, 0.7 to 2.1 wt% Li; 0.2 to 0.8 wt% Mg; 0.2 to 0.5 wt% Mn; 0.04 to 0.18 wt% Zr; less than 0.05 wt% Zn and, optionally, 0.1 to 0.5 wt% Ag, the remainder being aluminum and unavoidable impurities, having a low propensity for crack bifurcation in a fatigue test along the LS direction. The product according to EP2235224, also published according to WO 2009 / 103899, has a crack deflection angle T of at least 20° under an equivalent stress intensity factor K eff max 10 MPa.Vm for a cracked SL specimen subjected to mixed mode I and II stress, in which the angle between a plane perpendicular to the crack direction and the stress direction is 75°.

[0007] EP3384061, also published according to WO 2017 / 093680, discloses a rolled and / or forged product of an aluminum-based alloy comprising, in wt%, Cu: 3.2 - 4.0; Li: 0.80 - 0.95; Zn: 0.45 - 0.70; Mg: 0.15 - 0.7; Zr: 0.07 - 0.15; Mn: 0.1 - 0.6; Ag: < 0.15; Fe + Si < 0.20; at least one of Ti: 0.01 - 0.15; Sc: 0.02 - 0.1; Cr: 0.02 - 0.1; Hf: 0.02 - 0.5; V: 0.02 - 0.1 other elements < 0.05 each and < 0.15 in total, remainder aluminum.The products according to EP3384061 are obtained from a process in which a bath of liquid metal based on aluminum alloy according to the invention is prepared, a raw form is cast from said bath of liquid metal; said raw form is homogenized at a temperature between 450°C and 550°; said raw form is hot deformed and optionally cold deformed, preferably to a thickness of at least 15 mm: said product is dissolved between 490 and 530°C for 15 min to 8 h and is quenched; said product is fractionated in a controlled manner with a permanent deformation of 1 to 7% and said product is tempered. The product is advantageous for the manufacture of aircraft structural elements.

[0008] EP2675933 discloses wrought products of lithium aluminum alloy having a thickness of at least 12.7 mm and containing from 3.00 to 3.80 wt% Cu, from 0.05 to 0.35 wt% Mg, from 0.975 to 1.385 wt% Li, where -0.3*Mg-0.15Cu +1.65 = Li = -0.3*Mg- 0.15Cu +1.85, from 0.05 to 0.50 wt% of at least one element for controlling grain structure selected from the group consisting of Zr, Sc, Cr, V, Hf, other rare earth elements, and combinations thereof, up to 1.0 wt% Zn, up to 1.0 wt% Mn, up to 0.12 wt% Si, up to 0.15 wt% Fe, up to 0.15 wt% Ti, up to 0.10 % by weight of any other element, the total of such other elements not exceeding 0.35% by weight, the remainder being aluminum.

[0009] There is a need for sheets thicker than 25 mm of lithium copper aluminum alloy with an improved R compromise P o.2(L))- Ki c(LT) compared to existing products while maintaining thermal stability, corrosion resistance and fatigue endurance properties. STATEMENT OF THE INVENTION

[0010] The subject matter of the patent relates to a method for manufacturing a rolled product in which an aluminum alloy plate is cast, the composition of which, in weight %, is: Cu 2. -3.9; Li 0.7- 1.2; Mg 0.1-0.8; Mn 0.1-0.6; Zr 0.07-0.15; Ti 0.01-0.15; Fe <0.1; Si <0.1%; Ag <0.40; Zn <0.70; other elements <0.05 each and <0.15 in total, remainder aluminum.

[0011] Preferably, the Zn content is from 0.05 to 0.25% by weight and the Ag content is from 0.20 to 0.40% by weight.

[0012] In another preferred embodiment, the Zn content is from 0.45 to 0.70% by weight and the Ag content is less than or equal to 0.15% by weight.

[0013] The cast plate is then homogenized at a temperature of 515°C to 540°C for 5 to 50 hours.

[0014] Said homogenized plate is hot-formed by rolling, so as to obtain a rolled product, such that the final hot-forming temperature is between 395°C and 445°C to obtain a rolled product whose thickness is between 25 mm and 50 mm. Preferably, the final thickness of the product is between 30 mm and 40 mm. Preferably, the rolling exit temperature is between 410°C and 445°C.

[0015] Said rolled product having a thickness of 25 mm to 50 mm is solution-treated at a temperature of 490°C to 530°C for 15 minutes to 8 hours. Said solution-treated product is quenched with water. Preferably, the quenching water is at room temperature. Said quenched product is then pulled in a controlled manner with a permanent deformation of 1 to 6%. Said product is then tempered by heating at a temperature of 120°C to 170°C for 5 to 100 hours.

[0016] The invention also relates to a rolled product whose thickness is from 25 mm to 50 mm, preferably from 30 mm to 40 mm, made of aluminum alloy of composition in % by weight, Cu 2.2-3.9; Li 0.7-1.2; Mg 0.1-0.8; Mn 0.1-0.6; Zr 0.07-0.15; Ti 0.01-0.15; Fe <0.1; Si <0.1%; Ag <0.40; Zn <0.70; other elements <0.05 each and <0.15 in total, remainder aluminum and such that at mid-thickness, the volume fraction of grains having a brass texture is less than 21%, preferably less than 20%, even more preferably less than 19%.

[0017] Preferably, the mid-thickness rolled product is such that at mid-thickness the sum of the volume fractions of the grains having a copper, brass and S texture is less than or equal to 60%, preferably less than or equal to 55%.

[0018] Preferably, the composition of the product comprises a Zn content of 0.05 to 0.25% by weight and an Ag content of 0.20 to 0.40% by weight.

[0019] In another preferred embodiment, the composition of the product comprises a Zn content of 0.45 to 0.70% by weight and an Ag content of 0.05 to 0.15% by weight.

[0020] Preferably, the rolled product has an elastic limit at mid-thickness in the long direction R p o.2(L) at least equal to 505 MPa and a toughness Ki c (LT) of at least 45.5 MPa.Vm. FIGURES

[0021] Figure 1 shows the evolution of the stress intensity factor Ki c (TL) as a function of the final hot rolling temperature of the products of Example 1.

[0022] Figure 2 shows the yield strength trade-off R p o.2 - direction L - stress intensity factor Ki c (LT) (LT) of the products of Example 1.

[0023] Figure 3 shows the evolution of the stress intensity factor Ki c (LT) as a function of the final hot rolling temperature of the products of Example 2. DETAILED DESCRIPTION OF THE INVENTION

[0024] Unless otherwise stated, all information regarding the chemical composition of alloys is expressed as a percentage by weight based on the total weight of the alloy. Alloy designations are made in accordance with the regulations of The Aluminium Association, known to those skilled in the art. Density depends on the composition and is determined by calculation rather than by a weight measurement method. Values ​​are calculated in accordance with the procedure of The Aluminium Association, which is described on pages 2-12 and 2-13 of "Aluminum Standards and Data". Definitions of metallurgical tempers are given in European Standard EN 515.

[0025] Unless otherwise stated, the static mechanical characteristics, in other words the breaking strength R m , the elastic limit in tension R po,2 and the elongation at break A, are determined by a tensile test according to standard EN 10002-1 or NF EN ISO 6892-1, the location at which the parts are taken and their direction being defined by standard EN 485-1.

[0026] The stress intensity factor (KO.) is determined according to ASTM E 399. Thus, the proportion of specimens defined in paragraph 7.2.1 of this standard is always verified as well as the general procedure defined in paragraph 8. ASTM E 399 gives in paragraphs 9.1.3 and 9.1.4 criteria for determining whether KO. is a valid value of Kic. Thus, a Kic value is always a KO. value, the converse not being true.

[0027] Unless otherwise stated, the definitions of EN 12258 apply. The crystallographic texture can be described by a 3-dimensional mathematical function. This function is known in the art as the Orientation Density Function (ODF). It is defined as the volume fraction of the material dV / V having an orientation g to within dg: where (4>1, d>, 4>2) are the Euler angles describing the orientation g.

[0028] The present inventors calculated the FDO of each sheet by the spherical harmonics method from four pole figures measured by X-ray diffraction on a traditional texture goniometer. In the context of the invention, the measurements of the pole figures were carried out on samples cut at mid-thickness of the sheets. Similarly, in order to obtain statistically representative measurements, the size of the samples was adapted to the grain size. Preferably, the size of the samples is chosen so as to be able to analyze at least 3000 grains, preferably 5000.

[0029] It is possible to simplify the information contained in the FDO. This is commonly done in the art to describe selected aspects of the distribution of orientations in the material. An example of this practice is the calculation of the volume fraction of crystallites that have a specific orientation. To do this, the reference orientation is arbitrarily defined, along with an angle of maximum misorientation around this orientation. The FDO is then integrated into the domain thus defined, which allows the relative volume of orientations contained in this domain to be deduced compared to the total volume.

[0030] The present inventors used a tolerance of 15° around the orientations “copper”, “brass”, “S” in order to describe the texture obtained. The crystallographic orientations “copper”, “brass”, “S” are known to those skilled in the art and described for example in the reference document by UF Kocks, CN Tomé, and H. -R. Wenk, “Texture and anisotropy: preferred orientations in polycrystals and their effect on materials properties”. Cambridge University Press, 2000.

[0031] The “copper”, “brass”, “S” orientations are reproduced in the table below.

[0032] The inventors found that it is possible to improve the R compromise p o.2 (L) - Ki c(L- T), on rolled products with a thickness of 25 mm to 50 mm, preferably at least 30 mm, and at most 45 mm or 40 mm if a mid-thickness texture is maintained such that the volume fraction of grains having a brass texture is less than 21%, preferably less than 20%, or 19%. Preferably, it is possible to improve the compromise R p o.2 (L) - Kic (LT), on rolled products with a thickness of 25 mm to 50 mm, if the sum of the volume fractions of the grains having a compression texture, i.e. the sum of the volume fractions of the grains with copper, brass, and S texture, is less than or equal to 60%, preferably less than or equal to 55%.

[0033] Preferably, the rolled products with a thickness of 25 mm to 50 mm, preferably at least 30 mm, and at most 40 mm or 45 mm according to the invention have a yield strength at mid-thickness in the long direction R po.2( L) of at least 505 MPa and a toughness Ki c (LT) of at least 45.5 MPa.Vm.

[0034] Preferably, the rolled products for which the composition is such that the Zn content is less than or equal to 0.25% by weight, preferably between 0.05% and 0.25% and the Ag content is between 0.20 and 0.40% by weight have an elastic limit in the long direction R p o.2( L) of at least 510 MPa and a toughness Ki c (LT) of at least 46 MPa.Vm.

[0035] The rolled products according to the invention are obtained by a process comprising the steps of casting, homogenization, hot rolling, solution treatment, stress relief, and tempering.

[0036] An aluminum alloy plate is cast according to the invention.

[0037] The aluminum alloy according to the invention comprises in % by weight Cu 2.2-3.9, Li 0.7-1.2, Mg 0.1-0.8, Mn 0.1-0.6, Zr 0.07-0.15, Ti 0.01-0.15, Fe <0.1, Si <0.1%, Ag <0.40, Zn <0.70, other impurities <0.05, total 0.15, remainder aluminum.

[0038] The copper content is from 2.2% to 3.9% by weight. In an advantageous embodiment, the copper content is at least 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%. In another advantageous embodiment, the copper content is at most 3.8%, 3.7%. Any combination of the previously described Cu values ​​constitutes an advantageous embodiment of the invention.

[0039] The lithium content is from 0.7% to 1.2% by weight. In an advantageous embodiment, the lithium content is at least 0.80%, 0.85%, 0.90%. In another advantageous embodiment, the lithium content is at most 1.15%, 1.10%, 1.05%, 1.0%. Any combination of the previously described Li values ​​constitutes an advantageous embodiment of the invention.

[0040] The magnesium content is from 0.1 to 0.8% by weight. In an advantageous embodiment, the magnesium content is at least 0.2%, 0.3%, 0.35%, 0.40%. In another advantageous embodiment, the magnesium content is at most 0.6%, 0.5%. Any combination of the Mg values ​​previously described constitutes an advantageous embodiment of the invention.

[0041] The silver content is less than or equal to 0.40% by weight. In an advantageous embodiment, the silver content is at least 0.05%, 0.10%, 0.15%, 0.20%. In another advantageous embodiment, the silver content is at most 0.35%, 0.30%, 0.25%, 0.20%, 0.15%. Any combination of the previously described Mg values ​​constitutes an advantageous embodiment of the invention.

[0042] The zinc content is less than or equal to 0.70% by weight. In an advantageous embodiment, the zinc content is at least 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%. In another advantageous embodiment, the zinc content is at most 0.65%, 0.60%, 0.55%, 0.50%, 0.45%, 0.40%, 0.35%, 0.30%, 0.25%, 0.20%, 0.15%.

[0043] Advantageously, the Zn content is less than or equal to 0.25% by weight, preferably between 0.05% and 0.25% and the Ag content is between 0.20 and 0.40% by weight. In another advantageous embodiment, the Zn content is between 0.45% and 0.70% by weight. and the Ag content is less than or equal to 0.15%, preferably from 0.05% to 0.15% by weight.

[0044] The zirconium content is between 0.07 and 0.15% and preferably between 0.09 and 0.12%.

[0045] The manganese content is between 0.1 and 0.6% by weight. Advantageously, the manganese content is between 0.2 and 0.4% in order to improve toughness without compromising mechanical strength. In the absence of manganese addition, the desired compromise is not achieved.

[0046] The titanium content is between 0.01 and 0.15% by weight. Preferably, between 0.02 and 0.10% by weight of titanium is chosen.

[0047] It is preferable to limit the content of impurities in the alloy. These elements include iron and silicon and any other unavoidable impurities. The iron content and the silicon content are each at most 0.1% by weight. Preferably, the iron and silicon contents are each at most 0.08% by weight. In an advantageous embodiment of the invention, the iron and silicon contents are at most 0.06% and 0.04% by weight, respectively. The other impurities have a content of less than 0.05% by weight each and 0.15% by weight in total. The remainder corresponds to aluminum.

[0048] The cast plate is then homogenized. The homogenization temperature is preferably between 510°C and 540°C for 5 to 50 hours. Preferably, the temperature is at least 515°C. Preferably, the temperature is at most 530°C, or 525°C. In another preferred embodiment, the homogenization is carried out in two stages, with at least one of the two stages at a temperature between 510°C and 540°C or between 510°C and 525°C or between 515°C and 525°C.

[0049] After homogenization, the plate is usually cooled to room temperature before being reheated in order to be hot rolled. The purpose of reheating is to allow the hot deformation of the product. However, it is possible to avoid this reheating if the homogenized plate can be rolled without being cooled. Preferably, the initial hot rolling temperature is between 420°C and 520°C, preferably, the initial rolling temperature is at most 510°C, 500°C, or 490°C.

[0050] The plate is then hot rolled to obtain a rolled product with a thickness of 25 mm to 50 mm, preferably at least 30 mm, and at most 40 mm or 45 mm.

[0051] The inventors found that by controlling the end-of-rolling temperature from 395°C to 445°C for this final thickness range of 25 to 50 mm, preferably at least 30 mm, and at most 40 mm or 45 mm, it was possible to increase the toughness Klc (LT), also called critical stress intensity factor, and to improve the compromise between the yield strength at mid-thickness in the long direction R p o.2( L) and tenacity Ki c (LT).

[0052] The end of rolling temperature is between 395°C and 445°C. The end of rolling temperature is preferably at least 400°C, or 405°C or 410°C or 415°C or 420°C or 425°C or 435°C. Preferably, the end of rolling temperature is at most 440°C. There are several ways to control the final rolling temperature. For example, one can act on the rolling speed or the reduction rate per pass, or the waiting time between passes or the cooling / reheating means such as the temperature of the working rolls of the rolling mill or the quantity of emulsion supplied, or even by sprinkling. The measurement of the rolling temperature can be done by infrared pyrometers. It is also possible to use a rolling model.Rolling forces and torques are linked to the temperature of the rolled product, so that by knowing the deformations and deformation rates imposed during a rolling pass, the forces measured on the rolling mill make it possible to deduce the temperature of the metal, using a model implemented in the rolling mill control software.

[0053] The product thus obtained is then put into solution, preferably by heat treatment at 490 to 530°C for 15 min to 8 h, then typically quenched with water.

[0054] The inventors have found that the total equivalent time for homogenization and dissolution t(eq) can exceed 40h, preferably 50h, where T (in Kelvin) is the instantaneous treatment temperature, which changes with time t (in hours), and Tref is a reference temperature set at 773 K. The equivalent time at 500°C (773K) is defined by the formula in which T is the instantaneous temperature expressed in Kelvin which changes with time t (in hours) and T re f is a reference temperature of 500 °C (773 K). t(eq) is expressed in hours. The constant Q / R = 26100 K is derived from the activation energy for Mn diffusion, Q = 217000 J / mol.

[0055] The dissolved product then undergoes a controlled traction of 1 to 6% and preferably at least 2%, or 3%, typically around 4%.

[0056] An income is carried out on the pulled product at a temperature of 120 to 170°C for 5 to 100 hours, preferably 140 to 160°C for 10 to 60 hours. EXAMPLES Example 1

[0057] Five AI-Cu-LI alloy plates referenced A, B, C, D, E were cast. Their composition is given in Table 1

[0058] [Table 1] - Composition (% by weight) of the different plates.

[0059] The plates were homogenized for 12 hours at 508°C + 15 hours at 518°C. They were then hot rolled after being reheated to a temperature of 525°C for approximately 20 hours to achieve a final thickness of approximately 31 mm. The initial and final rolling thickness, initial and final hot rolling temperature of each plate are shown in Table 2.

[0060] [Table 2] - Rolling conditions

[0061] The sheets thus obtained were then solution-treated for 2 hours at 515°C and quenched with cold water. The solution-treated and quenched sheets were tensile in a controlled manner, with a permanent elongation of 3.75% and were tempered for 18 hours at 155°C. Thick sheets A, B, C are produced according to the invention. Thick sheets D and E correspond to reference examples.

[0062] The thick plates were mechanically tested to determine their static mechanical properties in the long rolling direction (L) and their stress intensity factor (Kic) in the LT direction according to standard E 399 (see Table 3).

[0063] [Table 3] - Static mechanical properties and stress intensity factor (Kic) measured at mid-thickness (T / 2)

[0064] Figure 1 shows the evolution of the stress intensity factor as a function of the final hot rolling temperature. Figure 2 shows the compromise between yield strength (L direction) and stress intensity factor (LT stress), i.e. the compromise (R po.2-L) - KIC (LT). These tests show that the stress intensity factor KIC (LT) increases if the end-of-rolling temperature is between 395°C and 445°C, preferably between 410°C and 445°C. This increase in the stress intensity factor is obtained without degradation of the yield strength of the product. The products according to the invention A, B, C have a limit elasticity greater than 505 MPa in the longitudinal direction and a toughness Ki c (LT) greater than 45.5 MPa.Vm. Example 2

[0065] Two plates made of the same H alloy were cast. The H composition is shown in Table 4. The plates were homogenized in two stages of 12h 508°C then 15h30525°C. They were then hot rolled after being reheated to a temperature of 525°C for a period of approximately 20h to reach a final thickness of approximately 40 mm. The thick H1 plate was hot rolled to reach a final temperature of 480°C. The H-2 plate was hot rolled to reach a final rolling temperature of 403°C.

[0066] [Table 4] - Composition (% by weight) of the different plates.

[0067] The resulting sheets were solution-treated for 2 hours at 515°C and quenched with cold water. The solution-treated and quenched sheets were tensile-treated in a controlled manner, with a permanent elongation of 3.75%, and were tempered for 18 hours at 155°C.

[0068] The thick plates were mechanically tested to determine their static mechanical properties in the long rolling direction (L) and their stress intensity factor (Kic) in the LT direction according to standard E 399 (see Table 5).

[0069] [Table 5] - Static mechanical properties and stress intensity factor (Kic) measured at mid-thickness (T / 2)

[0070] These tests show that the stress intensity factor KIC (LT) increases if the end-of-rolling temperature is between 395°C and 445°C (Figure 3). The product according to the invention H-2 has a yield strength greater than 505 MPa in the longitudinal direction and a toughness Ki c (LT) greater than 45.5 MPa.Vm.

[0071] Texture measurement by X-ray diffractometry was carried out on the H1 and H-2 sheets at mid-thickness. The analyzed surface is approximately 50 x 50 mm 2The volume fraction in % of the orientations, brass, copper and S, for each of the samples is given in Table 6.

[0072] [Table 6] - Volume fraction of the components Copper, Brass and S measured at mid-thickness

[0073] It is observed that the product H-2 according to the invention has a brass texture of less than 21%, precisely less than or equal to 18%. The sum of the copper, brass and S textures is less than or equal to 60%, precisely less than or equal to 51%.

Claims

CLAIMS 1. Process for manufacturing a rolled product in which: a) an aluminum alloy plate of composition in % by weight is cast, Cu 2.2-3.9 Li 0.7-1.2 Mg 0.1-0.8 Mn 0.1-0.6 Zr 0.07-0.15 Ti 0.01-0.15 Fe <0.1 If <0.1% Ag <0.40 Zn <0.70 Other elements <0.05 each and <0.15 in total, remainder aluminum, b) said plate is homogenized at a temperature of 515°C to 540°C for 5 to 50 hours, c) said homogenized plate is hot-formed by rolling such that the final hot-forming temperature is 395°C to 445°C to obtain a rolled product with a thickness of 25 mm to 50 mm, d) said product is solution-molded at a temperature of 490°C to 530°C for 15 minutes to 8 hours, e) quenching with water, f) said product is pulled in a controlled manner with a permanent deformation of 1 to 6%, g) said product is tempered by heating at a temperature of 120°C to 170°C for 5 to 100 hours.

2. A method of manufacturing a rolled product according to claim 1 wherein the Zn content is from 0.05 to 0.25% by weight and the Ag content is from 0.20 to 0.40% by weight.

3. Method of manufacturing a rolled product according to claim 1 in which the Zn content is from 0.45 to 0.70% by weight and the Ag content is less than or equal to 0.15% by weight.

4. Method of manufacturing a rolled product according to any one of claims 1 to 3 in which during step c) the rolling outlet temperature is between 410°C and 445°C.

5. Method of manufacturing a rolled product according to any one of claims 1 to 4 in which during step c) the final thickness of the product is between 30 mm and 40 mm.

6. Rolled product with a thickness of 25 mm to 50 mm made of aluminium alloy with a composition in % by weight, Cu 2. -3.9 Li 0.7-1.2 Mg 0.1-0.8 Mn 0.1-0.6 Zr 0.07-0.15 Ti 0.01-0.15 Fe <0.1 If <0.1% Ag < 0.40 Zn < 0.70 Other elements <0.05 each and <0.15 in total, remainder aluminum, characterized in that at mid-thickness, the volume fraction of grains having a brass texture is less than 21%.

7. Rolled product according to claim 6 characterized in that at mid-thickness the sum of the volume fractions of the grains having a copper, brass and S texture is less than or equal to 60%.

8. Rolled product according to claim 6 or 7 characterized in that the Zn content is from 0.05 to 0.25% by weight and the Ag content is from 0.20 to 0.40% by weight.

9. Rolled product according to claim 6 or 7 characterized in that the Zn content is from 0.45 to 0.70% by weight and the Ag content is from 0.05 to 0.15% by weight.

10. Rolled product according to any one of claims 6 to 9 characterized in that the elastic limit at mid-thickness in the long direction RpO.2(L) is at least equal to 505 MPa and in that the toughness Klc (LT) is at least 45.5 MPa.Vm, said elastic limit RpO.2(L) being measured according to standard EN10002-1 and said toughness Klc (LT) being measured according to standard ASTM E399.

Citation Information

Patent Citations

  • Rolled product made of aluminum-lithium alloy for aeronautical applications

    EP2235224A1

  • 2xxx series aluminum lithium alloys

    EP2675933A2

  • Aluminium-copper-lithium alloy having improved mechanical strength and improved toughness

    EP3384061A1

  • Al-Cu-Li-Mg-Ag-Mn-Zr alloy for use as structural members requiring high strength and high fracture toughness

    US7229509B2

  • Rolled product made of aluminum-lithium alloy for aeronautical applications

    WO2009103899A1

Cited By

  • High-strength aluminum alloy with excellent fatigue damage resistance and preparation method thereof

    CN119640114A