Sputtering target, method for producing sputtering target, layered film, method for producing layered film, magnetic recording medium, and method for producing magnetic recording medium
By integrating CrB into sputtering targets with Co and Pt, the challenges of controlling saturation magnetization and anisotropy in perpendicular magnetic recording media are addressed, resulting in improved magnetic separation and recording density.
Patent Information
- Application Number
- PCT/JP2024/000196
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-01-09
- Publication Date
- 2024-10-17
AI Technical Summary
Current perpendicular magnetic recording media face challenges in achieving high recording density due to difficulties in controlling saturation magnetization and magnetic anisotropy, leading to particle growth and interference between magnetic particles.
Incorporating CrB as a metal component in sputtering targets, along with Co and Pt, to enhance magnetic anisotropy (Ku) and ensure thermal stability, while maintaining saturation magnetization, thereby improving magnetic separation and reducing particle interference.
The use of CrB in sputtering targets results in higher magnetic anisotropy, improved thermal stability, and increased magnetic separation, enabling higher recording densities and reduced interference, thus enhancing the performance of magnetic recording media.
Smart Images

Figure JP2024000196_17102024_PF_FP_ABST
Abstract
Description
Sputtering target, method for manufacturing sputtering target, laminated film, method for manufacturing laminated film, magnetic recording medium, and method for manufacturing magnetic recording medium
[0001] The present invention relates to a sputtering target, a method for manufacturing a sputtering target, a laminated film, a method for manufacturing a laminated film, a magnetic recording medium, and a method for manufacturing a magnetic recording medium.
[0002] In recent years, perpendicular magnetic recording has come into practical use in the field of hard disk drives. Perpendicular magnetic recording is a method of recording magnetic data perpendicular to the recording surface. Perpendicular magnetic recording is widely adopted because it allows for higher density recording than in-plane magnetic recording. As demand for higher recording density in hard disk drives increases, development of magnetic recording media suitable for higher recording density is progressing.
[0003] A magnetic recording medium for perpendicular magnetic recording may be composed of multiple layers, including recording layers including an upper recording layer and a lower recording layer, and other layers. These layers are sequentially deposited on a substrate by sputtering using a sputtering target appropriate for each layer. In this deposition, a sputtering target may be used in which the metal phase is composed of a metal mainly containing Co and the oxide phase contains a predetermined metal oxide.
[0004] To achieve high recording densities in the recording layer of a magnetic recording medium, it is necessary to form a recording layer that exhibits the desired saturation magnetization while also providing high crystalline orientation of magnetic grains with perpendicular magnetic anisotropy and good separation between magnetic grains. One means of addressing this requirement is a sputtering target that contains 0.05 at% or more of Bi, a total metal oxide content of 10 vol% to 60 vol%, and the remainder containing at least Co and Pt (Patent Document 1). According to the invention of Patent Document 1, it is possible to suppress the growth of magnetic grains, improve the particle size dispersion of magnetic grains, and improve separation between magnetic grains while maintaining the crystalline orientation of the magnetic grains. Specific examples of the metal oxide include oxides of Co, Cr, Si, Ti, and B.
[0005] International Publication No. 2020 / 031460
[0006] The invention disclosed in Patent Document 1 makes it possible to disperse fine magnetic particles with uniform particle size distribution through oxide grain boundaries with uniform widths, but there is room for improvement in terms of controlling saturation magnetization and magnetic anisotropy.
[0007] The present invention was completed in consideration of the above problems, and aims to provide, in one embodiment, a sputtering target that achieves an increased magnetic anisotropy Ku to ensure thermal stability and high magnetic separation of magnetic particles to achieve high resolution while maintaining a saturation magnetization of a predetermined value or more, and a method for manufacturing the same. In another embodiment, the present invention aims to provide a laminated film manufactured by sputtering using such a sputtering target, a magnetic recording medium, a method for manufacturing the laminated film, and a method for manufacturing the magnetic recording medium.
[0008] As a result of extensive research, the present inventors have discovered that by incorporating CrB as a metal component, high magnetic anisotropy (Ku) and good magnetic separation between magnetic particles can be achieved. Ensuring high magnetic anisotropy ensures thermal stability. Furthermore, increasing the magnetic separation between magnetic particles makes it possible to reduce interference between magnetic particles. Consequently, when a magnetic recording medium is manufactured using the sputtering target according to the present invention, the amount of information per unit area can be increased. The present invention was completed based on the above findings, and is exemplified below.
[0009] [1] A sputtering target containing CrB as a metal component, with the remainder containing at least Co and Pt. [2] The sputtering target according to [1], in which a diffraction peak is observed at 2θ=44.94°±1° when measured using an X-ray diffraction apparatus. [3] The sputtering target according to [2], in which the analysis conditions of the X-ray diffraction apparatus are the following (1) to (15): (1) The analysis location of the sputtering target is a cut surface perpendicular to the sputtering surface. (2) Cu-Kα is used as the X-ray source. (3) The tube voltage is 40 kV. (4) The tube current is 30 mA. (5) The divergence slit is 1°. (6) The divergence vertical limiting slit is 10 mm. (7) The scattering slit is 8 mm. (8) The receiving slit is in an open state. (9) A horizontal-sample goniometer is used. (10) The scan speed is 10° / min. (11) The scan step is 0.01°. (12) The measurement range is 2θ = 20° to 80°. (13) A fitting method is used to remove background. (14) The analysis area is polished with #2000 waterproof abrasive paper and then buffed with a slurry containing dispersed alumina abrasive grains with a particle size of 0.3 μm. (15) A flat and minimally uneven surface of the analysis area is measured. [4] The sputtering target according to any one of [1] to [3], wherein, when measured using an X-ray diffractometer, the intensity ratio of the diffraction peak at 2θ = 44.94° ± 1° to the diffraction peak at 2θ = 43.06° ± 1° is 0.01 or more. [5] The sputtering target according to [4], wherein the analysis conditions of the X-ray diffraction apparatus are the following (1) to (15), and the intensity ratio of the diffraction peaks is calculated by the following (Procedure 1) and (Procedure 2): (1) The analysis portion of the sputtering target is a cut surface perpendicular to the sputtering surface. (2) Cu-Kα is used as the X-ray source. (3) The tube voltage is 40 kV. (4) The tube current is 30 mA. (5) The divergence slit is 1°. (6) The divergence vertical limiting slit is 10 mm. (7) The scattering slit is 8 mm. (8) The receiving slit is in an open state. (9) A horizontal sample goniometer is used. (10) The scan speed is 10° / min.(11) The scan step is 0.01°. (12) The measurement range is 2θ = 20° to 80°. (13) A fitting method is used for background removal. (14) The analysis area is polished with #2000 waterproof abrasive paper and then buffed using a slurry containing 0.3 μm alumina abrasive grains. (15) The flat, least uneven surface of the analysis area is measured. (Step 1) In the data obtained by removing the background, the scale markings at the highest positions of the diffraction peaks at 2θ = 44.94° ± 1° and 2θ = 43.06° ± 1° are read as peak intensities. (Step 2) The peak intensity at 2θ = 44.94° ± 1° is divided by the peak intensity at 2θ = 43.06° ± 1°. [6] The sputtering target according to any one of [1] to [5], containing 35 mol% to 60 mol% Co. [7] The sputtering target according to any one of [1] to [6], containing 5 mol% to 30 mol% Pt. [8] The sputtering target according to any one of [1] to [7], further containing one or more elements selected from the group consisting of Au, Ag, Cu, Ge, Ir, Mn, Mo, Nb, Ni, Pd, Re, Rh, Ru, Ta, W, and V in a total amount of 5 mol% or less. [9] A method for producing a sputtering target, comprising pressure sintering raw material powders containing CrB powder, Co powder, and Pt powder.
[10] The method according to [9], wherein the amount of the CrB powder is 2 wt% to 7 wt% based on the total mass of raw materials for the sputtering target.
[11] A laminated film including an underlayer and a magnetic layer formed on the underlayer, wherein the magnetic layer contains CrB as a metal component, with the remainder containing at least Co and Pt.
[12] A method for manufacturing a laminated film, comprising a step of forming a magnetic layer on the underlayer by sputtering using the sputtering target according to any one of [1] to [8].
[13] A magnetic recording medium, comprising at least an underlayer on a substrate, and a magnetic layer formed on the underlayer, wherein the magnetic layer contains CrB as a metal component, with the remainder containing at least Co and Pt.
[14] A method for manufacturing a magnetic recording medium including at least an underlayer on a substrate and a magnetic layer formed on the underlayer, the method comprising the step of forming the magnetic layer on the underlayer by sputtering using the sputtering target according to any one of [1] to [8].
[0010] According to one embodiment of the present invention, it is possible to provide a sputtering target and a method for manufacturing the same that achieves an increased magnetic anisotropy Ku to ensure thermal stability and high magnetic separation of magnetic particles to achieve high resolution while maintaining a saturation magnetization equal to or greater than a predetermined value. According to another embodiment of the present invention, it is possible to provide a laminated film manufactured by sputtering using such a sputtering target, a magnetic recording medium, a method for manufacturing the laminated film, and a method for manufacturing the magnetic recording medium.
[0011] Fig. 1 is a diagram showing the results of XRD (X-ray diffraction) analysis of the sputtering targets of the comparative example and the example. Fig. 2 is a graph showing the results of measurement of the magnetic anisotropy Ku of the magnetic films formed using the sputtering targets of the comparative example and the example. Fig. 3 is a graph showing the results of measurement of the magnetic cluster size Dn of the magnetic films formed using the sputtering targets of the comparative example and the example. Fig. 4 is a graph showing the results of measurement of the saturation magnetization Ms of the magnetic films formed using the sputtering targets of the comparative example and the example.
[0012] Next, embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate design changes and improvements may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.
[0013] The sputtering target according to this embodiment is preferably used to form a magnetic layer of a magnetic recording medium of a perpendicular magnetic recording type, and is more suitable for use in forming the lower recording layer, which is preferably the upper recording layer and lower recording layer that make up the magnetic layer and is therefore more difficult to rewrite information.
[0014] (Composition of sputtering target) The metal components of the sputtering target mainly contain Co and Pt, but it is also important to include CrB as a metal component. It is believed that the inclusion of CrB as a metal component stabilizes the hcp structure of the Co-Pt phase of the thin film formed by sputtering. Including CrB as a metal component means that a CrB alloy is present in the sputtering target. In this specification, the term "alloy" refers to a substance formed by mixing two or more metal elements, or a metal element and a nonmetal element.
[0015] In the sputtering target of this embodiment, the content of CrB as a metal component is preferably within a predetermined range relative to the total composition of the raw materials of the sputtering target. When the content of CrB as a metal component is a certain value, for example, 2 wt% or more, the magnetic anisotropy Ku is further improved. The inclusion of CrB as a metal component in a sputtering target means that B unbonded to oxygen is present. It is believed that B unbonded to oxygen easily interacts with magnetic elements during sputtering, making it easier for the magnetic elements to be oriented in a specific direction, thereby improving the magnetic anisotropy Ku of the film formed by sputtering. The improved magnetic anisotropy Ku reduces the interaction between magnetic particles. For this reason, the content of CrB as a metal component is preferably 2 wt% or more. On the other hand, when the content of CrB as a metal component is a certain value, for example, 7 wt% or less, the generation of particles during sputtering is easily suppressed. For this reason, the content of CrB as a metal component is preferably 7 wt% or less.
[0016] The presence of CrB as a metal component in a sputtering target can be confirmed, for example, by X-ray diffraction (XRD). That is, in an XRD pattern using Cu-Kα, a diffraction peak of the (111) plane of CrB is present as a main peak at approximately 2θ = 44.94° ± 1°. Furthermore, a diffraction peak of the (021) plane of CrB is present at approximately 2θ = 38.29° ± 1°, and a diffraction peak of the (110) plane of CrB is present at approximately 2θ = 32.32° ± 1°. When the main peak is observed among these peaks, it can be determined that CrB is present. Typically, these peaks are observed simultaneously.
[0017] The peak intensity ratio of the diffraction peak of the (111) plane of CrB to the diffraction peak of the (111) plane of Co—Pt in an FCC (face-centered cubic lattice) (near 2θ=43.06°±1°) is preferably 0.01 or greater. This peak intensity ratio is more preferably 0.02 or greater, even more preferably 0.03 or greater, and ideally 0.04 or greater. The peak intensity ratio can be determined by analyzing an X-ray pattern obtained by X-ray diffraction (XRD) using X-ray analysis software (PDXL2, integrated powder X-ray analysis software, manufactured by Rigaku Corporation). Specifically, it can be determined by the following steps (I) to (III). (I) The background of the X-ray pattern is removed using the above-mentioned X-ray analysis software by a fitting method (more specifically, a simple peak search is performed, the peak portion is removed, and then a polynomial is fitted to the remaining data). (II) In the data obtained by removing the background, the scale at the highest position of the diffraction peak of the (111) plane of CrB (hereinafter referred to as the CrB peak intensity) and the scale at the highest position of the diffraction peak of the (111) plane of FCC Co—Pt (hereinafter referred to as the Co—Pt peak intensity) are read. (III) The CrB peak intensity is divided by the Co—Pt peak intensity.
[0018] The sputtering target contains at least Co and Pt as metal components. The Pt content can be selected arbitrarily to achieve the desired magnetic anisotropy. It is generally known that the highest magnetic anisotropy can be obtained when the molar ratio of Pt to Co is 3:1. However, the sputtering target of this embodiment can be realized as long as the ratio of Co to Pt is in the range of 10:0 to 10:5.
[0019] The amounts of Co and Pt as metal components can be set arbitrarily as needed, but for example, Co can be contained in an amount of 35 mol % to 60 mol %, and Pt can be contained in an amount of 5 mol % to 30 mol %.
[0020] In order to optimize saturation magnetization, magnetic anisotropy, and wettability between magnetic particles and grain boundary oxides, the metal components of the sputtering target may contain, in addition to the above-mentioned Co and Pt, one or more elements selected from the group consisting of Au, Ag, Cu, Ge, Ir, Mn, Mo, Nb, Ni, Pd, Re, Rh, Ru, Ta, W, and V, in a total amount of 5 mol% or less. The contents of Co, Pt, Cr, B, Au, Ag, Cu, Ge, Ir, Mn, Mo, Nb, Ni, Pd, Re, Rh, Ru, Ta, W, and V in the sputtering target can be determined, for example, by analysis using ICP and based on the analysis results.
[0021] Furthermore, the sputtering target of this embodiment can contain at least one of TiO, SiO, CrO, BO, CoO, and CoO as the metal oxide component, which makes it possible to obtain the effects of the metal oxide TiO, SiO, CrO, BO, CoO, or CoO in addition to the effects of CrB described above.
[0022] (Method of Manufacturing Sputtering Target) The sputtering target described above can be manufactured by, for example, a powder sintering method, and a specific example of the manufacturing method will be described below.
[0023] First, as metal powders, CrB powder, Co powder, Pt powder, and, if necessary, one or more powders selected from the group consisting of Au, Ag, Cu, Ge, Ir, Mn, Mo, Nb, Ni, Pd, Re, Rh, Ru, Ta, W, and V are prepared.
[0024] The metal powder may be a powder of not only a single element but also an alloy, and preferably has a particle size in the range of 1 μm to 150 μm, since this allows for uniform mixing and prevents segregation and coarse crystallization. If the particle size of the metal powder is larger than 150 μm, the oxide particles described below may not be uniformly dispersed, and if it is smaller than 1 μm, the oxidation of the metal powder may cause the sputtering target to deviate from the desired composition.
[0025] In one embodiment of the present invention, Co—B powder can be prepared as the metal powder. The presence of Co—B allows more B as a metal component, i.e., more B not bound to oxygen, to remain in the target. Furthermore, when using Co—B powder, it is preferable to use powder with a particle size of 77 μm or more, from the viewpoint of leaving more B as a metal component in the target.
[0026] Furthermore, as needed, oxide powders such as TiO powder, SiO powder, CrO powder, and / or CoBO powder are prepared. The oxide powder preferably has a particle size in the range of 1 μm to 30 μm. This allows the oxide particles to be more uniformly dispersed in the metal phase when mixed with the metal powder and pressure sintered. If the particle size of the oxide powder is larger than 30 μm, coarse oxide particles may be generated after pressure sintering. On the other hand, if the particle size is smaller than 1 μm, the oxide powder particles may aggregate.
[0027] Next, the metal powder and oxide powder are weighed to obtain the desired composition. For example, it is preferable to weigh the CrB powder as the metal so that it accounts for 2 wt % to 7 wt % of the total mass of the raw materials for the sputtering target. Then, the materials are mixed and pulverized using a known method such as a ball mill. This allows for the production of a mixed powder in which the desired metal powder and oxide powder are uniformly mixed. However, during the pulverization, it is desirable to fill the inside of a container used for mixing and pulverization with an inert gas to minimize oxidation of the raw material powder.
[0028] The mixed powder thus obtained is then pressurized and sintered in a vacuum or inert gas atmosphere to form a desired shape such as a disk. Various pressure sintering methods can be used here, such as hot press sintering, hot isostatic sintering, and plasma discharge sintering. Among these, hot isostatic sintering is effective in terms of increasing the density of the sintered body.
[0029] The temperature to be maintained during sintering is preferably in the range of 600° C. to 1500° C., and more preferably 700° C. to 1400° C. The time for maintaining the temperature in this range is preferably 1 hour or longer.
[0030] The pressure during sintering is preferably 10 MPa or more, more preferably 20 MPa or more, which allows the oxide particles to be dispersed more uniformly in the metal phase.
[0031] The sintered body obtained by the above pressure sintering is subjected to cutting or other machining using a lathe or the like to form it into a desired shape, thereby producing a sputtering target in the shape of a disk or the like.
[0032] (Laminated Film) The laminated film has at least an underlayer and a magnetic layer formed on the underlayer. More specifically, the underlayer contains Ru, and is generally made of Ru or is a layer mainly composed of Ru.
[0033] Each layer of the laminated film can be formed by depositing the film using a magnetron sputtering device or the like, using a sputtering target of the present invention having a composition and structure appropriate for each layer.
[0034] The magnetic layer can be formed on the underlayer by sputtering using the sputtering target of one embodiment of the present invention, thereby achieving increased magnetic anisotropy Ku to ensure thermal stability and high magnetic separation of magnetic particles to achieve high resolution while maintaining a saturation magnetization above a predetermined value.
[0035] An example of a magnetic layer formed by sputtering using a sputtering target according to one embodiment of the present invention contains Cr, B, Co, and Pt. When the magnetic layer further contains at least one metal oxide selected from the group consisting of TiO2, SiO2, Cr2O3, BO3, CoO, and Co3O4 as a metal oxide component, it is preferable that Co be contained in an amount of 35 mol% to 60 mol%, Pt be contained in an amount of 5 mol% to 30 mol%, and one or more elements selected from the group consisting of Au, Ag, Cu, Ge, Ir, Mn, Mo, Nb, Ni, Pd, Re, Rh, Ru, Ta, W, and V be contained in a total amount of 5 mol% or less. However, because the distribution and texture of each metal component in the resulting magnetic layer vary depending on the sputtering conditions, it is technically difficult to unambiguously define a more specific composition.
[0036] In another aspect of the present invention, there is provided a method for manufacturing a laminated film having an underlayer and a magnetic layer on the underlayer, the method comprising forming the magnetic layer by sputtering using the sputtering target of the present invention. In yet another aspect of the present invention, there is provided a laminated film including an underlayer and a magnetic layer formed on the underlayer, the magnetic layer being formed by sputtering using the sputtering target of the present invention. Therefore, the magnetic layer of the laminated film contains CrB as a metal component, with the remainder containing at least Co and Pt.
[0037] (Magnetic Recording Medium) A magnetic recording medium comprises a laminated film having an underlayer and a magnetic layer formed on the underlayer, as described above. Magnetic recording media are typically manufactured by sequentially forming a soft magnetic layer, an underlayer, a magnetic layer, and a protective layer on a substrate such as aluminum or glass. Therefore, in yet another aspect of the present invention, a method for manufacturing a magnetic recording medium having at least an underlayer on a substrate and a magnetic layer on the underlayer is provided, the method including forming the magnetic layer by sputtering using a sputtering target of the present invention. Therefore, the magnetic layer of the magnetic recording medium contains CrB as a metal component, with the remainder containing at least Co and Pt. In yet another aspect of the present invention, a magnetic recording medium is provided, comprising at least an underlayer on a substrate and a magnetic layer formed on the underlayer, the magnetic layer being formed by sputtering using a sputtering target of the present invention. As described above, when formed by sputtering using a sputtering target of one embodiment of the present invention, the distribution and texture of each metal component vary depending on the sputtering conditions, making it difficult to unambiguously define the magnetic recording medium.
[0038] Next, the sputtering target described above was prototyped and its performance was confirmed, which will be described below. However, the description here is for illustrative purposes only and is not intended to be limiting.
[0039] As the target composition for the examples and comparative examples, sputtering targets of 50Co-5Cr-15Pt-10B-1Ru-2TiO2-2Cr2O3-15CoO (mol %) were prepared.
[0040] (Comparative Example) Co powder, Pt powder, Ru powder, Cr2O3 powder, TiBO3 powder, Co—B powder, and Co2B2O5 powder were weighed as raw material powders to match the target composition, and then placed in a 5-liter ball mill pot along with titania balls as milling media. The mixture was then mixed by rotating for 10 hours. The mixed powder removed from the ball mill was then filled into a 190 mm diameter carbon cylindrical mold and sintered by hot pressing. The hot pressing conditions were a vacuum atmosphere, a heating rate of 300°C / hour, a holding temperature of 1000°C, and a holding time of 2 hours. A pressure of 30 MPa was applied from the start of the heating period until the end of the holding period. After the holding period, the mixture was allowed to cool naturally in the chamber. The resulting sintered body was then cut to prepare a sputtering target.
[0041] (Example) As raw material powders, Co powder, Pt powder, Ru powder, TiO powder, CrO powder, CoO powder, Co—B powder, and CrB powder were weighed to match the above target composition, and a sputtering target was manufactured under the same conditions as in the comparative example. Note that the Co—B powder used had a particle size of 77 μm. The proportion of CrB powder in the entire raw material powder was 2.87 wt %.
[0042] (Evaluation by XRD) The manufactured target was subjected to XRD measurement using an XRD evaluation device (Rigaku Ultima IV). This measurement can be performed in accordance with JIS K0131:1996, and the measurement conditions can be as follows. Analysis location of sputtering target: cut surface perpendicular to sputtered surface X-ray source: Cu-Kα Tube voltage: 40 kV Tube current: 30 mA Divergence slit: 1° Divergence vertical limiting slit: 10 mm Scattering slit: 8 mm Receiving slit: open state Goniometer: sample horizontal type Scan speed: 10° / min Scan step: 0.01° Measurement range: 2θ = 20° to 80° Background removal: fitting method (more specifically, a simple peak search is performed, the peak portion is removed, and then a polynomial is fitted to the remaining data. Background removal is performed based on X-ray analysis software (PDXL2 integrated powder X-ray analysis software, manufactured by Rigaku Corporation).)
[0043] The analysis area is polished with #2000 waterproof abrasive paper, and then buffed with a slurry containing dispersed alumina abrasive grains with a particle size of 0.3 μm, and the flat and minimally uneven surface of the analysis area is measured. Note that the "flat and minimally uneven surface" is not a strict standard, and simply means that if there are any irregularities that may interfere with the analysis, those areas should be avoided.
[0044] The obtained XRD patterns were analyzed using X-ray analysis software (PDXL2, integrated powder X-ray analysis software, manufactured by Rigaku Corporation). As a result, as shown in FIG. 1, CrB was detected in the example, whereas CrB was not detected in the comparative example. Note that the X-ray patterns in FIG. 1 are data from which the background was removed using the X-ray analysis software by the above-mentioned fitting method. The XRD measurement results will be described in detail below.
[0045] As can be seen from FIG. 1 , in the example, a diffraction peak was observed near 2θ = 44.94° ± 1°. By comparing the position of this observed diffraction peak with the data on the position of the diffraction peak of the (111) plane of CrB in JCPDS card No. 01-075-1159, it was confirmed that the position of the observed peak corresponds to the position of the main peak (2θ = 44.94°) in JCPDS card No. 01-075-1159. In other words, it can be said that CrB was detected. Furthermore, a diffraction peak was observed near 2θ = 38.29° ± 1°. By comparing the position of this observed diffraction peak with the data on the position of the diffraction peak of the (021) plane of CrB in JCPDS card No. 01-075-1159, it was confirmed that the position of the observed peak corresponds to the position of the main peak (2θ = 44.94°) in JCPDS card No. 01-075-1159. It was confirmed that the position of the diffraction peak corresponded to the position of the peak (2θ = 38.29°) of JCPDS card No. 01-075-1159. Furthermore, a diffraction peak could be observed near 2θ = 32.32° ± 1°. The position of this observed diffraction peak was compared with the data on the diffraction peak position of the CrB (110) plane of JCPDS card No. 01-075-1159, and it was confirmed that the position of the observed peak corresponded to the position of the peak (2θ = 32.32°) of JCPDS card No. 01-075-1159. On the other hand, in the comparative example, a diffraction peak could not be observed near 2θ = 44.94° ± 1°. In other words, CrB could not be confirmed. Furthermore, no diffraction peak was observed near 2θ = 38.29° ± 1° or near 2θ = 32.32° ± 1°.
[0046] Furthermore, for the X-ray pattern of FIG. 1 , the highest marking on the scale of the diffraction peak of the (111) plane of CrB (near 2θ=44.94°±1°) (hereinafter referred to as the CrB peak intensity) and the highest marking on the scale of the diffraction peak of the (111) plane of FCC Co—Pt (near 2θ=43.06°±1°) (hereinafter referred to as the Co—Pt peak intensity) were read, and the peak intensity of CrB was divided by the peak intensity of Co—Pt, whereby the peak intensity ratio of the diffraction peak of the (111) plane of CrB to the diffraction peak of the (111) plane of FCC Co—Pt was found to be 0.044.
[0047] (Evaluation of magnetic anisotropy Ku) Next, a magnetron sputtering device (C-3010 manufactured by Canon Anelva Corporation) was used to form films of Cr-Ti (6 nm), Ni-W (5 nm), and Ru (20 nm) in this order on a glass substrate, and each of the sputtering targets described above was sputtered at 300 W under an Ar atmosphere of 5.0 Pa to form magnetic films with a film thickness of 11 nm. After that, a Ru (3 nm) was formed as a protective film to prevent oxidation of the magnetic film, thereby forming each layer.
[0048] The magnetic anisotropy Ku of the obtained magnetic film was measured using a Kerr measurement device manufactured by NeoArc Corp. The measurement conditions were a maximum applied magnetic field of 20 kOe and a sweep time of 20 seconds.
[0049] (Evaluation of magnetic cluster size Dn and saturation magnetization Ms) For the magnetic film obtained by the above film formation operation, the magnetic cluster size Dn and saturation magnetization Ms were measured using a vibrating sample magnetometer manufactured by Tamagawa Seisakusho. The measurement conditions were a maximum applied magnetic field of 22 kOe in all cases. Specifically, to calculate Dn, first, the demagnetizing factor Nd was calculated using the following formula: Demagnetizing factor Nd=Hd / (4πMs) Then, using the calculated Nd and the film thickness t of the magnetic film of the sample, the magnetic cluster size Dn was calculated using the following formula: Magnetic cluster size Dn=t×(1−Nd 2 ) 1 / 2 / Nd
[0050] (Discussion) The measurement results of magnetic anisotropy Ku, magnetic cluster size Dn, and saturation magnetization Ms measured in the comparative example and the example are shown in Figures 2, 3, and 4, respectively. The horizontal axes in Figures 2, 3, and 4 represent the amounts of Ar and O2 supplied to the chamber of the magnetron sputtering apparatus. The chamber refers to the container where sputtering is performed using a sputtering target. These supply amounts are set values for the magnetron sputtering apparatus, but are considered to be equivalent to the measured values. The supply amounts on the horizontal axes represent the sum of Ar and O2. A larger Ku indicates higher magnetic anisotropy. Furthermore, a smaller Dn while showing an Ms value above a certain value indicates better magnetic separation. As can be seen from Figures 2, 3, and 4, even when sputtering targets have the same composition, the presence of CrB as a metal component results in a higher Ku of the resulting magnetic film. Furthermore, the presence of CrB as a metal component results in a smaller Dn while showing an Ms value above a certain value. In other words, the separation between magnetic particles is improved.
Claims
1. A sputtering target comprising, as a metal component, CrB, with the remainder comprising at least Co and Pt.
2. The sputtering target according to claim 1, which has a diffraction peak observed at 2θ=44.94°±1° when measured using an X-ray diffraction apparatus.
3. The sputtering target according to claim 2, wherein the analysis conditions of the X-ray diffraction apparatus are as follows (1) to (15): (1) The analysis portion of the sputtering target is a cut surface perpendicular to the sputtering surface. (2) Cu-Kα is used as the X-ray source. (3) The tube voltage is 40 kV. (4) The tube current is 30 mA. (5) The divergence slit is 1°. (6) The divergence vertical limiting slit is 10 mm. (7) The scattering slit is 8 mm. (8) The receiving slit is in an open state. (9) A horizontal-sample type goniometer is used. (10) The scan speed is 10° / min. (11) The scan step is 0.01°. (12) The measurement range is 2θ = 20° to 80°. (13) A fitting method is used for background removal. (14) The analysis area is polished with #2000 waterproof abrasive paper and further buffed with a slurry in which alumina abrasive grains having a particle size of 0.3 μm are dispersed. (15) Of the analysis areas, a flat surface with minimal irregularities is measured.
4. The sputtering target according to claim 1 or 2, wherein the intensity ratio of the diffraction peak at 2θ = 44.94° ± 1° to the diffraction peak at 2θ = 43.06° ± 1° is 0.01 or more when measured using an X-ray diffraction apparatus.
5. The sputtering target according to claim 4, wherein the analysis conditions of the X-ray diffraction apparatus are the following (1) to (15), and the intensity ratio of the diffraction peaks is calculated by the following (step 1) and (step 2): (1) The analysis portion of the sputtering target is a cut surface perpendicular to the sputtering surface. (2) Cu-Kα is used as the X-ray source. (3) The tube voltage is 40 kV. (4) The tube current is 30 mA. (5) The divergence slit is 1°. (6) The divergence vertical limiting slit is 10 mm. (7) The scattering slit is 8 mm. (8) The receiving slit is in an open state. (9) A horizontal-sample type goniometer is used. (10) The scan speed is 10° / min. (11) The scan step is 0.01°. (12) The measurement range is 2θ=20° to 80°. (13) A fitting method is used for background removal. (14) The analysis area is polished with #2000 waterproof abrasive paper, and further buffed with a slurry in which alumina abrasive grains with a particle size of 0.3 μm are dispersed. (15) The flat and least uneven surface of the analysis area is measured. (Step 1) In the data obtained by removing the background, the scale at the highest position of the diffraction peak at 2θ = 44.94 ° ± 1 ° and the scale at the highest position of the diffraction peak at 2θ = 43.06 ° ± 1 ° are read as peak intensities. (Step 2) The peak intensity at 2θ = 44.94 ° ± 1 ° is divided by the peak intensity at 2θ = 43.06 ° ± 1 °.
6. The sputtering target according to claim 1 or 2, containing 35 mol % to 60 mol % Co.
7. The sputtering target according to claim 1 or 2, containing 5 mol % to 30 mol % of Pt.
8. The sputtering target according to claim 1, further comprising one or more elements selected from the group consisting of Au, Ag, Cu, Ge, Ir, Mn, Mo, Nb, Ni, Pd, Re, Rh, Ru, Ta, W, and V in a total amount of 5 mol % or less.
9. A method for producing a sputtering target, comprising pressure sintering raw material powders including CrB powder, Co powder, and Pt powder.
10. The method of claim 9, wherein the amount of the CrB powder is 2 wt % to 7 wt % based on the total mass of the sputtering target raw material.
11. A laminated film including an underlayer and a magnetic layer formed on the underlayer, the magnetic layer including, as a metal component, CrB, and the remainder including at least Co and Pt.
12. A method for producing a laminated film, comprising the step of forming a magnetic layer on an underlayer by sputtering using the sputtering target according to claim 1 or 2.
13. A magnetic recording medium comprising at least an underlayer on a substrate and a magnetic layer formed on the underlayer, the magnetic layer containing CrB as a metal component and at least Co and Pt as a balance.
14. A method for manufacturing a magnetic recording medium comprising at least an underlayer on a substrate and a magnetic layer formed on the underlayer, the method comprising the step of forming the magnetic layer on the underlayer by sputtering using a sputtering target according to claim 1 or 2.
Citation Information
Patent Citations
Cr ALLOY TARGET MATERIAL AND ITS PRODUCTION METHOD
JP2005336611A
Method for fabricating precious metal magnetic sputtering target and precious metal magnetic sputtering target fabricated by using the method
JP2006144124A
Sputtering target for forming magnetic recording medium film, and method for producing the same
JP2011174174A
Cited By
Preparation method of chromium diboride target material
CN119930297A