Resin foam body and foam member

The resin foam addresses the need for reduced carbon emissions and enhanced shock absorption by using a cellular structure with limited petroleum-derived resin and plant-derived polyolefin, ensuring effective cushioning for thinner electronic devices.

WO2024214480A1PCT designated stage expired Publication Date: 2024-10-17NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010217
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-13
Filing Date
2024-03-15
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The challenge is to develop a resin foam that reduces carbon dioxide emissions while maintaining excellent shock absorption properties, particularly for use in thinner electronic devices with smaller components, where traditional cushioning materials fall short in both environmental sustainability and performance.

Method used

A resin foam with a cellular structure, where the content ratio of petroleum-derived resin is 50% or less, and optimized parameters such as apparent density, cell diameter, and plant-derived polyolefin resin composition, including a plant-derived polypropylene polymer, are used to achieve reduced carbon emissions and enhanced shock absorption.

Benefits of technology

The solution effectively reduces carbon dioxide emissions and provides superior shock absorption and flexibility, making it suitable for thinner electronic devices with improved environmental sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010217_17102024_PF_FP_ABST
    Figure JP2024010217_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a resin foam body capable of contributing to reduction in carbon dioxide emission and having excellent impact absorption property. [1] A resin foam body according to one embodiment of the present invention has a foam structure, has a content a of a petroleum-derived resin of 50 wt% or less, and satisfies formula (1). (1): [apparent density (g / cm3)] < -0.0025×[content a (%) of petroleum-derived resin]+0.48 [2] In the resin foam body described in [1], the aspect ratio of the foam may be 4 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Resin foam and foamed material

[0001] The present invention relates to a resin foam and a foam member.

[0002] Foam materials are often used as cushioning materials for protecting the screens, circuit boards, electronic components, and the like of electronic devices. In recent years, with the trend toward thinner electronic devices, there has been a demand for narrower clearances in the areas where cushioning materials are placed. Furthermore, as electronic devices become smaller and more multifunctional, the electronic components used also tend to become smaller, which may require thinner cushioning materials (foam materials) that have excellent shock absorption properties. Furthermore, with the recent increasing demand for environmental consideration, there is also a demand for reduced carbon dioxide emissions from the above-mentioned cushioning materials (foam materials).

[0003] JP 2017-186504 A JP 2015-034299 A

[0004] An object of the present invention is to provide a resin foam that can contribute to reducing carbon dioxide emissions and has excellent impact absorption properties.

[0005] [1] A resin foam according to an embodiment of the present invention is a resin foam having a cellular structure, in which the content ratio a of a petroleum-derived resin is 50% by weight or less, and the following formula (1) is satisfied: [apparent density (g / cm 3 )】<−0.0025×[content ratio a (%) of petroleum-derived resin]+0.48 (1) [2] In the resin foam according to the above [1], the aspect ratio of the cells of the resin foam may be 4 or less. [3] In the resin foam according to the above [1] or [2], the 50% compressive load of the resin foam may be 40 N / cm 2 [4] The resin foam according to any one of [1] to [3] above, wherein a 25% compressive load of the resin foam is 25 N / cm or less. 2 [5] In the resin foam according to any one of [1] to [4] above, the resin foam may have an average cell diameter of 200 μm or less. [6] In the resin foam according to any one of [1] to [5] above, the resin foam may have an apparent density of 0.4 g / cm or less. 3[7] In the resin foam according to any one of [1] to [6] above, the coefficient of variation of cell diameter of the resin foam may be 0.6 or less. [8] In the resin foam according to any one of [1] to [7] above, the resin foam may contain a plant-derived polyolefin resin. [9] In the resin foam according to [8] above, the plant-derived polyolefin may contain a plant-derived polyolefin, and the melt flow rate of the plant-derived polyolefin at a temperature of 230°C may be less than 20 g / 10 min.

[10] In the resin foam according to any one of [1] to [9] above, the melt tension of the plant-derived polyolefin may be 10 cN or more.

[11] In the resin foam according to [8] above, the die swelling ratio at a melting point + 20°C of the plant-derived polyolefin may be 1.5 or less.

[12] In the resin foam according to any one of [1] to

[11] above, the die swelling ratio of the resin composition forming the resin foam at a melting point + 20°C of the plant-derived polyolefin may be 1.5 or less.

[13] The resin foam according to any one of [8] to

[12] above may contain a plant-derived polypropylene polymer as the plant-derived polyolefin resin.

[14] In the resin foam according to any one of [8] to

[13] above, the plant-derived polyolefin resin may be a mixture of a polyolefin other than a polyolefin elastomer and a polyolefin elastomer, the polyolefin being a plant-derived polyolefin, and the polyolefin elastomer being a plant-derived polyolefin elastomer or a petroleum-derived polyolefin elastomer.

[15] The resin foam according to any one of [1] to

[14] above may have a heat-melting layer on one or both sides.

[16] A foam member according to one embodiment of the present invention comprises a resin foam layer composed of the resin foam according to any one of [1] to

[15] above, and a pressure-sensitive adhesive layer disposed on at least one side of the resin foam layer.

[0006] According to the present invention, it is possible to provide a resin foam that can contribute to reducing carbon dioxide emissions and has excellent impact absorption properties.

[0007] 1 is a schematic cross-sectional view of a foam member according to one embodiment of the present invention.

[0008] A. Resin Foam A-1. Overview of Resin Foam A resin foam according to an embodiment of the present invention has a petroleum-derived resin content ratio a of 50% by weight or less and satisfies the following formula (1): [Apparent Density (g / cm 3 ) )] < -0.0025 × [petroleum-derived resin content a (%)] + 0.48 (1) The petroleum-derived resin content a is a content based on the total amount of resin constituting the resin foam.

[0009] The resin foam has a cell structure. Examples of the cell structure include a closed cell structure, an open cell structure, and a semi-open, semi-closed cell structure (a cell structure in which a closed cell structure and an open cell structure are mixed). Preferably, the cell structure of the resin foam is a semi-open, semi-closed cell structure. Typically, the resin foam of the present invention is obtained by foaming a resin composition. The resin composition is a composition containing at least the resin that constitutes the resin foam.

[0010] According to an embodiment of the present invention, the content ratio a of the petroleum-derived resin is set to the above range, and the apparent density (g / cm 3 ) and the content ratio a (%) of the petroleum-derived resin satisfy the above relationship, a resin foam with reduced carbon dioxide emissions can be provided. Furthermore, according to the present invention, by focusing on the apparent density and the content ratio a of the petroleum-derived resin and optimizing the relationship between them, it is possible to achieve both reduced carbon dioxide emissions and impact absorption. The resin foam is also advantageous in that it is thin yet has excellent impact absorption and flexibility. In other words, one of the major achievements of the present invention is that it has achieved improved impact absorption while simultaneously reducing carbon dioxide emissions.

[0011] The content ratio a of the petroleum-derived resin in the resin foam is preferably less than 45% by weight, more preferably less than 40% by weight. Within such a range, the above-mentioned effects become significant.

[0012] Preferably, the resin foam contains a plant-derived resin. More preferably, it contains a plant-derived polyolefin-based resin. Even more preferably, it contains a plant-derived polypropylene-based resin. When a plant-derived polypropylene-based resin is used, the above effects become more pronounced, and further, a resin foam having excellent heat resistance can be obtained.

[0013] In addition, petroleum-derived resins and plant-derived resins differ in biomass content (the ratio of sample carbon to standard modern carbon). 14 Petroleum-derived resins can be distinguished by their C concentration. 14 It does not contain radioactive carbon-14 (half-life 5730 years). On the other hand, plant-derived resins 14 C (radioactive carbon 14, half-life 5730 years). The biomass ratio of the plant-derived resin is preferably 50% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more. 14 The concentration of C can be measured by accelerator mass spectrometry.

[0014] The content b of the plant-derived resin in the resin foam is preferably more than 50% by weight, more preferably 45% by weight or more, and even more preferably 40% by weight or more. Within such a range, the above-mentioned effects become significant.

[0015] In one embodiment, the value calculated by "-0.0025 x [petroleum-derived resin content a (%)] + 0.48" may preferably be 0.01 or more, 0.03 or more, or 0.05 or more. Also, the value calculated by "-0.0025 x [petroleum-derived resin content a (%)] + 0.48" may be 0.5 or less, 0.4 or less, or 0.3 or less.

[0016] A-2. Properties of resin foam The apparent density of the resin foam is preferably 0.4 g / cm 3 More preferably, it is 0.3 g / cm or less. 3 More preferably, it is 0.2 g / cm or less. 3 or less, and more preferably 0.1 g / cm 3 More preferably, it is 0.08 g / cm or less. 3More preferably, it is 0.05 g / cm or less. 3 or less, and more preferably 0.04 g / cm 3 More preferably, it is 0.03 g / cm or less. 3 The apparent density of the resin foam is preferably 0.01 g / cm or less. 3 More preferably, 0.02 g / cm 3 More preferably, it is 0.03 g / cm 3 That's all. The foamability can be judged by the apparent density. In the present invention, by setting the apparent density within the above range, a resin foam that is thin yet has excellent flexibility and impact absorption properties can be obtained. It is also possible to reduce carbon dioxide emissions. The method for measuring the apparent density will be described later.

[0017] The resin foam has a cell content (cell ratio) of preferably 97% or less, more preferably 96% or less. The resin foam has a cell content (cell ratio) of preferably 30% or more, more preferably 50% or more, and even more preferably 60% or more. Within these ranges, a resin foam having appropriate flexibility can be obtained.

[0018] The cell density of the resin foam is preferably 30 cells / mm 2 More preferably, 50 pieces / mm 2 More preferably, 70 pieces / mm 2 More preferably, 80 pieces / mm 2 More preferably, 90 pieces / mm 2 More preferably, 100 pieces / mm 2 More preferably, it is 110 pieces / mm 2 or more, and most preferably 120 / mm 2 Within this range, a resin foam having favorable flexibility and excellent punching processability can be obtained. Furthermore, the higher the cell number density, the easier it is to store energy when compressed, and a resin foam having excellent compression recovery force can be obtained. The upper limit of the cell number density of the resin foam is preferably 400 cells / mm 2 and more preferably 350 pieces / mm2 and more preferably 300 pieces / mm 2 and more preferably 250 pieces / mm 2 and particularly preferably 200 pieces / mm 2 The cell number density of a resin foam is the number density of cells in a cross section observed in a randomly selected cross section of the resin foam, and can be determined by image analysis of the cross section of the resin foam.

[0019] The resin foam has an average cell diameter (average cell diameter) of preferably 200 μm or less, more preferably 155 μm or less, even more preferably 145 μm or less, even more preferably 130 μm or less, even more preferably 110 μm or less, even more preferably 90 μm or less, even more preferably 80 μm or less, and even more preferably 70 μm or less. Within these ranges, a resin foam with excellent impact absorption properties can be obtained. In one embodiment, the resin foam has an average cell diameter (average cell diameter) of 90 μm or less. Furthermore, the resin foam has an average cell diameter (average cell diameter) of preferably 10 μm or more, even more preferably 20 μm or more, and even more preferably 40 μm or more. When the average cell diameter (average cell diameter) is within the above range, a resin foam with excellent flexibility and stress dispersibility and favorable impact absorption properties can be obtained. Furthermore, a resin foam with excellent compression recovery, punching processability, and resistance to repeated impacts can be obtained. The method for measuring the average cell diameter will be described later.

[0020] The resin foam has a maximum cell diameter of preferably 400 μm or less, more preferably 300 μm or less, even more preferably 250 μm or less, even more preferably 220 μm or less, even more preferably 170 μm or less, even more preferably 150 μm or less, even more preferably 130 μm or less, even more preferably 120 μm or less, even more preferably 110 μm or less, and even more preferably 100 μm or less. The resin foam also has a maximum cell diameter of preferably 40 μm or more, more preferably 60 μm or more, even more preferably 70 μm or more, and particularly preferably 80 μm or more. Within these ranges, a resin foam with particularly excellent impact absorption properties can be obtained. In one embodiment, the resin foam has a maximum cell diameter of 170 μm or less.

[0021] The coefficient of variation of the cell diameter of the resin foam is preferably 0.6 or less, more preferably 0.55 or less, even more preferably 0.5 or less, even more preferably 0.45 or less, and even more preferably 0.40 or less. Within such a range, deformation due to impact becomes uniform, local stress load is prevented, and a resin foam having excellent stress dispersion and particularly excellent impact absorption properties can be obtained. The smaller the coefficient of variation, the more preferable it is, and the lower limit thereof is, for example, 0.15 (preferably 0.1, more preferably 0.01). A method for measuring the coefficient of variation of the cell diameter will be described later.

[0022] When the resin foam has a semi-open, semi-closed cell structure, the proportion of closed cell structures therein is preferably 40% or less, more preferably 30% or less. In this specification, the proportion of closed cell structures in a resin foam is determined, for example, by submerging a measurement target in water at a temperature of 23°C and a humidity of 50%, measuring the mass thereafter, and then thoroughly drying the target in an oven at 80°C and measuring the mass again. Furthermore, since open cells can retain moisture, the mass of the open cells is measured and determined.

[0023] The aspect ratio of the cells in the resin foam is preferably 4 or less, more preferably 3 or less, even more preferably 2 or less, still more preferably 1.5 or less, and particularly preferably 1.3 or less. Within such a range, a resin foam having excellent impact absorption properties can be provided. The aspect ratio of the cells in the resin foam is, for example, 1 or more, preferably greater than 1.1. A method for measuring the aspect ratio of the cells in a resin foam will be described later.

[0024] The thickness of the cell walls of the resin foam is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, particularly preferably 0.7 μm or more, and most preferably 1 μm or more. The thickness of the cell walls of the resin foam is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 5 μm or less, particularly preferably 4 μm or less, and most preferably 3 μm or less. Resin foams with a thickness within this range can have appropriate strength. Such resin foams have excellent punching processability and are prevented from tearing, dust generation, or remaining cuts during punching. Furthermore, a cell wall thickness within the above range can result in a resin foam with superior flexibility and stress dispersibility. The cell wall thickness can be measured by capturing an enlarged image of the cell portion of the resin foam and analyzing the image using the instrument's analysis software.

[0025] The 50% compression load of the resin foam is preferably 40 N / cm 2 More preferably, it is 20 N / cm or less. 2 or less, and more preferably 10 N / cm 2 More preferably, it is 5 N / cm or less. 2 More preferably, it is 4 N / cm or less. 2 More preferably, it is 3 N / cm or less. 2 More preferably, it is 2 N / cm or less. 2 Within this range, a resin foam having preferable flexibility and impact absorption properties can be obtained. The lower limit of the 50% compression load of the resin foam is, for example, 0.5 N / cm2 The 50% compression load of a resin foam is the stress (N) when compressed to a compression rate of 50% per unit area (1 cm 2 ) converted into

[0026] The 25% compression load of the resin foam is preferably 25 N / cm 2 More preferably, it is 15 N / cm or less. 2 or less, and more preferably 10 N / cm 2 More preferably, it is 6 N / cm or less. 2 More preferably, it is 5 N / cm or less. 2 More preferably, it is 3 N / cm or less. 2 More preferably, it is 2 N / cm or less. 2 and more preferably 1.5 N / cm or less. 2 Within this range, a resin foam having preferable flexibility and impact absorption properties can be obtained. The lower limit of the 25% compression load of the resin foam is, for example, 0.5 N / cm 2 The 25% compression load of a resin foam is the stress (N) when compressed to a compression rate of 50% per unit area (1 cm 2 ) converted into

[0027] The thickness of the resin foam is preferably 8000 μm or less, more preferably 5000 μm or less, even more preferably 4000 μm or less, and particularly preferably 2000 μm or less. The thickness of the resin foam is preferably 100 μm or more, more preferably 200 μm or more, even more preferably 300 μm or more, and particularly preferably 400 μm or more. A thickness in this range is advantageous in that a fine and uniform cell structure can be formed, and excellent impact absorption properties can be achieved.

[0028] The thickness change rate of the resin foam upon compression bonding is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, particularly preferably 2% or less, and most preferably 1% or less. Within such ranges, a resin foam having good recovery properties and excellent punching processability can be obtained. In this specification, the "thickness change rate of a resin foam upon compression bonding" refers to the thickness change rate when a resin foam and an adhesive are laminated together, pressed back and forth with a 5 kg roller three times, and then left for 30 minutes, and is a change rate calculated by the following formula: Thickness change rate upon compression bonding [%] = (thickness before compression bonding - thickness after compression bonding) / thickness before compression bonding) × 100

[0029] The impact absorption of the resin foam is preferably 40% or more, more preferably 55% or more, even more preferably 60% or more, particularly preferably 70% or more, and most preferably 80% or more. Impact absorption is measured as follows: A test specimen is formed by placing the resin foam, double-sided tape (product number: No. 5603W, manufactured by Nitto Denko), and PET film (product number: Diafoil MRF75, manufactured by Mitsubishi Plastics) in this order on an impact force sensor. A 66 g iron ball is dropped onto the test specimen from a height of 50 cm above the PET film to measure the impact force F1. Furthermore, the iron ball is dropped directly onto the impact force sensor as described above to measure the impact force F0 of the blank. Impact absorption (%) is calculated from F1 and F0 using the formula (F0 - F1) / F0 x 100.

[0030] The stress retention of the resin foam is preferably 60% or more, more preferably 63% or more. Furthermore, the stress retention of the resin foam is preferably 100% or less, more preferably 95% or less. Within these ranges, a resin foam can be obtained that has excellent stress dispersion properties and exhibits excellent impact absorption even when thin. In this specification, the stress retention is defined as the ratio of the tensile strength immediately after stretching to the tensile strength after 120 seconds of holding after stretching (tensile strength after 120 seconds of holding / stress retention immediately after stretching × 100) when a resin foam (width 10 mm × length 100 mm) is stretched 20% in the longitudinal direction at a speed of 300 m / min.

[0031] In one embodiment, a resin having a die swell ratio of 1.5 or less at a melting point (the melting point of the resin constituting the resin foam) + 20°C is used as the resin constituting the resin foam. That is, in one embodiment, the die swell ratio of the resin forming the resin foam at a melting point + 20°C before foaming is 1.5 or less. By using a resin having a die swell ratio within the above range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The die swell ratio of the resin forming the resin foam at a melting point + 20°C before foaming is preferably 1.5 or less, more preferably 1.25 or less. The lower limit of the die swell ratio of the resin (before foaming) is, for example, 1.05 (preferably 1.02, more preferably 1.01). Furthermore, the die swell ratio at the melting point + 20°C of the resin constituting the resin foam (i.e., the resin after foaming) is preferably 1.5 or less, more preferably 1.25 or less, and even more preferably 1.1 or less. The lower limit of the die swell ratio of the resin (after foaming) is, for example, 1.05 (preferably 1.02, more preferably 1.01). In this specification, the die swell ratio refers to the value obtained by dividing the diameter of the resin extruded when a molten sample (resin, resin composition) to be measured is extruded from a die by the diameter of the die. The die swell ratio is calculated by measuring the diameter of the resulting string-like molded product by the formula: diameter of the molded product (mm) / die diameter (mm). The melting point of the resin is measured by the peak top temperature of the endothermic peak obtained by differential scanning calorimetry (DSC) measurement. Differential scanning calorimetry (DSC) is measured using a differential scanning calorimeter (for example, product name "Q-2000" manufactured by TA Instruments) under the conditions of a sample weight of 3 mg and a heating rate of 10°C / min. When two or more peaks are present, the peak top temperature on the higher side is taken as the melting point.

[0032] The melt tension of the resin constituting the resin foam is preferably 10 cN or more, more preferably 15 cN or more, even more preferably 20 cN or more, and particularly preferably 25 cN or more. The melt tension of the resin constituting the resin foam is preferably 50 cN or less, more preferably 45 cN or less. Within this range, a resin foam containing small-sized bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The melt tension is the melt tension at the melting point of the compound to be measured + 20°C. The melt tension is measured as follows.

[0033] -Method for measuring melt tension of resin Using a twin capillary rheometer "RH7-2 Model" (manufactured by Rosand Precision), a sample to be measured (resin, resin composition) is extruded into a molten strand at an extrusion speed of 8.8 mm / min under conditions of a temperature 20°C higher than the melting point of the resin and an orifice diameter of 1 mmφ, and the strand is taken up at a take-up speed of 0.5 m / min. The take-up speed is increased in increments of 0.1 m / min. The melt tension at which the strand of resin breaks is taken as the "melt tension."

[0034] The resin foam may have any suitable shape depending on the purpose. A typical example of such a shape is a sheet, in which case the resin foam of the present invention can be treated as a resin foam layer.

[0035] When the resin foam is in the form of a sheet (i.e., a resin foam layer), its thickness is preferably 5000 μm or less, more preferably 4000 μm or less, even more preferably 3000 μm or less, and particularly preferably 2500 μm or less. The thickness of the resin foam is preferably 30 μm or more, more preferably 35 μm or more, even more preferably 40 μm or more, and even more preferably 45 μm or more. The resin foam of the present invention can exhibit excellent impact absorption even when thin. Such a resin foam can be suitably used as a protective material applied to small clearances.

[0036] The resin foam of the present invention may have a heat-meltable layer on one or both sides thereof. A resin foam having a heat-meltable layer can be obtained, for example, by rolling a resin foam (or a precursor of a resin foam) using a pair of heated rolls heated to a temperature equal to or higher than the melting temperature of the resin composition constituting the resin foam.

[0037] The cellular content (cell content) of the thermally fused layer is preferably 30% or less, more preferably 20% or less, even more preferably 10% or less, particularly preferably 5% or less, and most preferably 0%. The thickness of the thermally fused layer is preferably 0.60 mm or less, more preferably 0.40 mm or less, and even more preferably 0.20 mm or less. The thickness of the thermally fused layer is preferably 0.05 mm or more, more preferably 0.07 mm or more, and even more preferably 0.09 mm or more.

[0038] A-3. Method for Forming Resin Foam The resin foam can be formed by any appropriate method as long as the effects of the present invention are not impaired. A representative example of such a method is a method of foaming a resin composition containing a resin material (polymer). The resin composition contains any appropriate resin material (polymer).

[0039] In one embodiment, a resin composition is used having a die swell ratio of 1.5 or less (preferably 1.25 or less) at the melting point of the resin composition + 20°C. Within this range, a resin foam containing small-sized bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The lower limit of the die swell ratio of the resin composition is, for example, 1.05 (preferably 1.02, more preferably 1.01). The melting point of the resin composition refers to the melting point of the compound having the highest melting point among the compounds in the resin composition.

[0040] The melt tension of the resin composition is preferably 10 cN or more, more preferably 15 cN or more, even more preferably 20 cN or more, and particularly preferably 25 cN or more. The melt tension of the resin composition is preferably 50 cN or less, more preferably 45 cN or less. Within this range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. As described above, the melt tension is the melt tension at a temperature 20°C above the melting point of the compound to be measured (i.e., the resin composition), and the melting point of the resin composition is the melting point of the compound with the highest melting point among the compounds in the resin composition.

[0041] Examples of the polymer include acrylic resins, silicone resins, urethane resins, polyolefin resins, ester resins, rubber resins, etc. The polymers may be used alone or in combination of two or more.

[0042] The polymer content is preferably 30 parts by weight or more, more preferably 35 parts by weight or more, and even more preferably 40 parts by weight or more, based on 100 parts by weight of the resin composition. The polymer content is preferably 95 parts by weight or less, more preferably 90 parts by weight or less, even more preferably 80 parts by weight or less, and particularly preferably 60 parts by weight or less, based on 100 parts by weight of the resin composition. Within these ranges, a resin foam having superior flexibility and stress dispersibility can be obtained.

[0043] In one embodiment, a polyolefin resin is used as the polymer.

[0044] Preferably, the polyolefin resin is a plant-derived polyolefin resin, more preferably a plant-derived polypropylene resin. A plant-derived polyolefin resin (preferably a propylene resin) and a petroleum-derived polyolefin resin may be used in combination.

[0045] The content of the polyolefin resin is preferably 50 to 100 parts by weight, more preferably 70 to 100 parts by weight, even more preferably 90 to 100 parts by weight, particularly preferably 95 to 100 parts by weight, and most preferably 100 parts by weight, relative to 100 parts by weight of the polymer.

[0046] The polyolefin resin is preferably at least one selected from the group consisting of polyolefins and polyolefin elastomers, and more preferably a combination of polyolefins and polyolefin elastomers. The polyolefins and polyolefin elastomers may each be used alone or in combination of two or more. In this specification, the term "polyolefin" does not include "polyolefin elastomers."

[0047] When a polyolefin and a polyolefin elastomer are used in combination as the polyolefin resin, the weight ratio of the polyolefin to the polyolefin elastomer (polyolefin / polyolefin elastomer) is preferably 1 / 99 to 99 / 1, more preferably 10 / 90 to 90 / 10, even more preferably 20 / 80 to 80 / 20, and particularly preferably 30 / 70 to 70 / 30. In one embodiment, the weight ratio of the polyolefin to the polyolefin elastomer (polyolefin / polyolefin elastomer) is preferably 25 / 75 to 75 / 25, more preferably 35 / 65 to 65 / 35. Within this range, a resin foam can be obtained that has excellent compression recovery, is suppressed in shape change (particularly thickness change) before and after punching, has appropriate strength, and is excellent in punching processability.

[0048] In one embodiment, a plant-derived polyolefin (preferably a polypropylene-based polymer) is used as the polyolefin, and a plant-derived or petroleum-derived polyolefin elastomer is used as the polyolefin-based elastomer. In this case, the weight ratio of the polyolefin (i.e., plant-derived polyolefin) is preferably 50 wt% or more, more preferably 53 wt% or more, even more preferably 60 wt% or more, and even more preferably 70 wt% or more, based on the total weight of the polyolefin and the polyolefin-based elastomer. Within such a range, the effects of the present invention are remarkable. The upper limit of the weight ratio of the polyolefin (i.e., plant-derived polyolefin) is, for example, 99% (preferably 100%) based on the total weight of the polyolefin and the polyolefin-based elastomer.

[0049] Any appropriate polyolefin may be used as the polyolefin as long as it does not impair the effects of the present invention. Examples of such polyolefins include linear polyolefins and branched (branched) polyolefins. In one embodiment, a branched polyolefin is used as the polyolefin-based resin. In this embodiment, only a branched polyolefin may be used as the polyolefin, or a branched polyolefin and a linear polyolefin may be used in combination. By using a branched polyolefin, a resin foam having a small average cell diameter and excellent impact absorption can be obtained. The content of the branched polyolefin is preferably 30 parts by weight or more, more preferably 50 parts by weight or more, per 100 parts by weight of the polyolefin. Furthermore, the content of the branched polyolefin is preferably 100 parts by weight or less, more preferably 80 parts by weight or less, per 100 parts by weight of the polyolefin.

[0050] One type of polyolefin may be used alone, or two or more types may be used in combination. When one type of polyolefin is used, a plant-derived polyolefin may be used as the polyolefin. When two or more types of polyolefins are used, at least one of them may be a plant-derived polyolefin. The content of the plant-derived polyolefin is preferably 50 parts by weight or more, more preferably 80 parts by weight or more, and even more preferably 90 parts by weight or more, relative to 100 parts by weight of the polyolefin blend amount. Particularly preferably, all of the polyolefins used are plant-derived polyolefins. As described above, plant-derived polyolefins are 14 C (radioactive carbon-14, half-life 5730 years)-containing polyolefin.

[0051] Examples of the polyolefin include polymers containing structural units derived from α-olefins. The polyolefin may be composed solely of structural units derived from α-olefins, or may be composed of structural units derived from α-olefins and structural units derived from monomers other than α-olefins. When the polyolefin is a copolymer, any appropriate copolymerization form may be adopted. Examples include random copolymers and block copolymers.

[0052] Examples of α-olefins that can constitute polyolefins include α-olefins having 2 to 8 carbon atoms (preferably 2 to 6, more preferably 2 to 4) (e.g., ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, etc.). Only one type of α-olefin may be used, or two or more types may be used.

[0053] Examples of the monomer other than α-olefin constituting the polyolefin include ethylenically unsaturated monomers such as vinyl acetate, acrylic acid, acrylic acid esters, methacrylic acid, methacrylic acid esters, vinyl alcohol, etc. The monomer other than α-olefin may be one type only, or two or more types may be used.

[0054] Specific examples of polyolefins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene (propylene homopolymer), copolymers of ethylene and propylene, copolymers of ethylene and an α-olefin other than ethylene, copolymers of propylene and an α-olefin other than propylene, copolymers of ethylene, propylene and an α-olefin other than ethylene and propylene, and copolymers of propylene and an ethylenically unsaturated monomer.

[0055] In one embodiment, a polypropylene-based polymer having a structural unit derived from propylene is used as the polyolefin. Examples of the polypropylene-based polymer include polypropylene (propylene homopolymer), a copolymer of ethylene and propylene, and a copolymer of propylene and an α-olefin other than propylene, and polypropylene (propylene homopolymer) is preferred. One type of polypropylene-based polymer may be used alone, or two or more types may be used in combination.

[0056] The plant-derived polyolefin is preferably a plant-derived polypropylene-based polymer. The plant-derived polypropylene-based polymer may be a homopolymer of plant-derived propylene or a copolymer of plant-derived propylene and another monomer. When the copolymer is used, the content of structural units based on plant-derived propylene in the copolymer is preferably 50 parts by weight or more, more preferably 70 parts by weight or more, per 100 parts by weight of the plant-derived polypropylene-based polymer.

[0057] The plant-derived polypropylene-based polymer may be polypropylene produced using biomass as a raw material. For example, it may be a polypropylene-based polymer produced using biopropylene produced by dehydrating propanol produced by fermentation. It may also be a polypropylene-based polymer produced using biopropylene produced during a bioethylene synthesis reaction. It may also be a polypropylene-based polymer produced using biopropylene synthesized from bioethanol.

[0058] The melt flow rate (MFR) of the polyolefin at 230°C is preferably 0.25 g / 10 min or more, more preferably 0.3 g / 10 min or more, and even more preferably 0.35 g / 10 min or more. The melt flow rate (MFR) of the polyolefin at 230°C is preferably 20 g / 10 min or less, more preferably 10 g / 10 min or less, even more preferably 6 g / 10 min or less, still more preferably 5 g / 10 min, particularly preferably 1 g / 10 min or less, and most preferably 0.6 g / 10 min or less. In this specification, the melt flow rate (MFR) refers to the MFR measured at 230°C and a load of 2.16 kgf (21.2 N) in accordance with ISO 1133 (JIS-K-7210). In one embodiment, the die swell ratio and shear viscosity of the resin are controlled by the melt flow rate of the polyolefin constituting the resin foam.

[0059] The melt flow rate (MFR) of the plant-derived polyolefin at 230°C is preferably less than 20 g / 10 min, more preferably less than 10 g / 10 min, even more preferably less than 6 g / 10 min, even more preferably less than 5 g / 10 min, particularly preferably less than 1 g / 10 min, and most preferably 0.6 g / 10 min or less. Furthermore, the melt flow rate (MFR) of the plant-derived polyolefin at 230°C is preferably 0.25 g / 10 min or more, more preferably 0.3 g / 10 min or more, and even more preferably 0.35 g / 10 min or more. Within these ranges, the effects of the present invention are remarkable. This is particularly advantageous in that a resin foam with excellent impact absorption properties can be obtained.

[0060] In one embodiment, the die swell ratio of the plant-derived polyolefin at a melting point +20°C is 1.5 or less (preferably 1.25 or less). Within this range, a resin foam containing small-sized bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The lower limit of the die swell ratio of the plant-derived polyolefin is, for example, 1.05 (preferably 1.02, more preferably 1.01).

[0061] The melt tension of the plant-derived polyolefin is preferably 10 cN or more, more preferably 15 cN or more, even more preferably 20 cN or more, and particularly preferably 25 cN or more. The melt tension of the plant-derived polyolefin is preferably 50 cN or less, more preferably 45 cN or less. Within this range, a resin foam containing small-sized bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide.

[0062] The weight-average molecular weight of the polyolefin is preferably 50,000 or more, more preferably 55,000 or more, and even more preferably 60,000 or more. The weight-average molecular weight of the polyolefin is 120,000 or less, more preferably 110,000 or less, and even more preferably 100,000 or less. Within these ranges, the die swell ratio and shear viscosity of the resin can be preferably adjusted. The molecular weight distribution (weight-average molecular weight / number-average molecular weight) of the polyolefin is preferably 7 to 10, more preferably 6 to 9. Within these ranges, the die swell ratio and shear viscosity of the resin can be preferably adjusted. The weight-average molecular weight and number-average molecular weight can be determined by gel permeation chromatography (solvent: tetrahydrofuran, polystyrene equivalent).

[0063] Any appropriate polyolefin elastomer may be used as the polyolefin elastomer as long as it does not impair the effects of the present invention. Examples of such polyolefin elastomers include so-called non-crosslinked thermoplastic olefin elastomers (TPOs) such as ethylene-propylene copolymers, ethylene-propylene-diene copolymers, ethylene-vinyl acetate copolymers, polybutene, polyisobutylene, chlorinated polyethylene, elastomers in which a polyolefin component and a rubber component are physically dispersed, and elastomers in which a polyolefin component and a rubber component are microphase-separated; and dynamically crosslinked thermoplastic olefin elastomers (TPVs) which are multiphase polymers obtained by dynamically heat-treating a mixture containing a resin component A (olefin resin component A) that forms a matrix and a rubber component B that forms domains in the presence of a crosslinking agent, and which have a sea-island structure in which crosslinked rubber particles are finely dispersed as domains (island phases) in the resin component A that forms a matrix (sea phase).

[0064] The polyolefin-based elastomer preferably contains a rubber component. Examples of such rubber components include those described in JP-A-08-302111, JP-A-2010-241934, JP-A-2008-024882, JP-A-2000-007858, JP-A-2006-052277, JP-A-2012-072306, JP-A-2012-057068, JP-A-2010-241897, JP-A-2009-067969, and JP-A-03 / 002654.

[0065] Specific examples of elastomers having a microphase-separated structure of a polyolefin component and an olefinic rubber component include elastomers made of polypropylene resin (PP) and ethylene-propylene rubber (EPM), elastomers made of polypropylene resin (PP) and ethylene-propylene-diene rubber (EPDM), etc. The weight ratio of the polyolefin component to the olefinic rubber component (polyolefin component / olefinic rubber) is preferably 90 / 10 to 10 / 90, and more preferably 80 / 20 to 20 / 80.

[0066] Dynamically crosslinked thermoplastic olefin elastomers (TPVs) generally have a higher elastic modulus and a smaller compression set than non-crosslinked thermoplastic olefin elastomers (TPOs), which results in good recovery properties and allows the formation of resin foams with excellent recovery properties.

[0067] As described above, a dynamically crosslinked thermoplastic olefin-based elastomer (TPV) is obtained by dynamically heat-treating a mixture containing a resin component A (olefin-based resin component A) that forms a matrix and a rubber component B that forms domains in the presence of a crosslinking agent, and is a multiphase polymer having a sea-island structure in which crosslinked rubber particles are finely dispersed as domains (island phases) in the resin component A that forms the matrix (sea phase).

[0068] Examples of dynamically crosslinked thermoplastic olefin-based elastomers (TPVs) include those described in JP-A-2000-007858, JP-A-2006-052277, JP-A-2012-072306, JP-A-2012-057068, JP-A-2010-241897, JP-A-2009-067969, and JP-A-03 / 002654.

[0069] As the dynamically crosslinked thermoplastic olefin-based elastomer (TPV), commercially available products may be used, such as "Zeotherm" (manufactured by Zeon Corporation), "Thermorun" (manufactured by Mitsubishi Chemical Corporation), and "Sarlink 3245D" (manufactured by Toyobo Co., Ltd.).

[0070] The polyolefin elastomer preferably has a melt flow rate (MFR) of 1.5 g / 10 min or more, more preferably 2 g / 10 min or more, at 230° C. The polyolefin elastomer preferably has a melt flow rate (MFR) of 25 g / 10 min or less, more preferably 20 g / 10 min or less, and even more preferably 15 g / 10 min at 230° C. In this way, the melt tension of the polyolefin elastomer is preferably adjusted, and as a result, the effects of the present invention become more pronounced.

[0071] In one embodiment, two or more polyolefin elastomers having different melt flow rates (MFR) at 230°C within the above range are used in combination. In this case, a polyolefin elastomer (low MFR polyolefin elastomer) having a melt flow rate (MFR) at 230°C of preferably 1.5 g / 10 min or more and less than 8 g / 10 min (more preferably 2 g / 10 min to 5 g / 10 min) can be used in combination with a polyolefin elastomer (high MFR polyolefin elastomer) having a melt flow rate (MFR) at 230°C of preferably 8 g / 10 min to 25 g / 10 min (more preferably 9 g / 10 min to 20 g / 10 min, and even more preferably 10 g / 10 min to 20 g / 10 min). In this way, the melt tension of the polyolefin elastomer can be preferably adjusted, resulting in remarkable effects of the present invention.

[0072] The blending ratio of the low MFR polyolefin elastomer to the high MFR polyolefin elastomer (low MFR polyolefin elastomer / high MFR polyolefin elastomer; weight ratio) is preferably 1.5 to 5, more preferably 1.8 to 3.5, and particularly preferably 2 to 3. Within such a range, the melt tension of the polyolefin elastomer can be suitably adjusted, resulting in remarkable effects of the present invention.

[0073] The melt tension of the polyolefin elastomer is preferably 5 cN or more, more preferably 10 cN or more. The melt tension of the polyolefin elastomer is preferably 50 cN or less. In one embodiment, the die swelling ratio and shear viscosity of the resin constituting the resin foam are controlled by the melt tension of the polyolefin elastomer.

[0074] The JIS A hardness of the polyolefin elastomer is preferably 30° or more, more preferably 40° or more, even more preferably 45° or more, and most preferably 50° or more. The JIS A hardness of the polyolefin elastomer is preferably 95° or less, more preferably 90° or less, even more preferably 88° or less, particularly preferably 85° or less, and most preferably 83°. The JIS A hardness is measured based on ISO 7619 (JIS K6253).

[0075] In one embodiment, the resin foam (i.e., the resin composition) may further contain a filler. By incorporating a filler, a resin foam can be formed that requires a large amount of energy to deform the cell walls, and the resin foam exhibits excellent impact absorption properties. Furthermore, by incorporating a filler, a fine and uniform cell structure can be formed, which is advantageous in that excellent impact absorption properties can be exhibited. Only one type of filler may be used alone, or two or more types may be used in combination.

[0076] The content of the filler is preferably 10 parts by weight or more, more preferably 30 parts by weight or more, and even more preferably 50 parts by weight or more, based on 100 parts by weight of the polymer constituting the resin foam. The content of the filler is preferably 150 parts by weight or less, more preferably 130 parts by weight or less, and even more preferably 100 parts by weight or less, based on 100 parts by weight of the polymer constituting the resin foam. Within this range, the above-mentioned effects become significant.

[0077] In one embodiment, the filler is an inorganic substance. Examples of materials constituting the inorganic filler include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whiskers, silicon nitride, boron nitride, crystalline silica, amorphous silica, metals (e.g., gold, silver, copper, aluminum, nickel), carbon, and graphite.

[0078] In one embodiment, the filler is an organic substance. Examples of materials constituting the organic filler include polymethyl methacrylate (PMMA), polyimide, polyamide-imide, polyether ether ketone, polyether-imide, and polyester-imide.

[0079] A flame retardant may be used as the filler. Examples of the flame retardant include bromine-based flame retardants, chlorine-based flame retardants, phosphorus-based flame retardants, and antimony-based flame retardants. From the viewpoint of safety, a non-halogen, non-antimony-based flame retardant is preferably used.

[0080] Examples of non-halogen-non-antimony flame retardants include compounds containing aluminum, magnesium, calcium, nickel, cobalt, tin, zinc, copper, iron, titanium, boron, etc. Examples of such compounds (inorganic compounds) include hydrated metal compounds such as aluminum hydroxide, magnesium hydroxide, magnesium oxide-nickel oxide hydrate, and magnesium oxide-zinc oxide hydrate.

[0081] The filler may be subjected to any suitable surface treatment, such as silane coupling treatment or stearic acid treatment.

[0082] The bulk density of the filler is preferably 0.8 g / cm 3 or less, more preferably 0.6 g / cm 3 More preferably, it is 0.4 g / cm or less. 3 or less, and particularly preferably 0.3 g / cm 3 Within this range, the filler can be incorporated with good dispersibility, and the effect of adding the filler can be fully exhibited even with a low filler content. A resin foam with a low filler content is advantageous in that it is highly foamed, flexible, and has excellent stress dispersibility and appearance. The lower limit of the bulk density of the filler is, for example, 0.01 g / cm 3 and preferably 0.05 g / cm 3 and more preferably 0.1 g / cm 3 is.

[0083] The number average particle diameter (primary particle diameter) of the filler is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. Within this range, the filler can be incorporated with good dispersibility and a uniform cell structure can be formed. As a result, a resin foam with excellent stress dispersion and appearance can be obtained. The lower limit of the number average particle diameter of the filler is, for example, 0.1 μm. The number average particle diameter of the filler can be measured using a particle size distribution analyzer (Micrtrac II, Microtrac Bell Co., Ltd.) using a suspension prepared by mixing 1 g of filler with 100 g of water as a sample.

[0084] The specific surface area of ​​the filler is preferably 2 m 2 / g or more, more preferably 4m 2 / g or more, and more preferably 6m 2 / g or more. Within this range, the filler can be incorporated with good dispersibility and a uniform cell structure can be formed. As a result, a resin foam with excellent stress dispersion and appearance can be obtained. The upper limit of the specific surface area of ​​the filler is, for example, 20 m 2 The specific surface area of ​​the filler can be measured by the BET method, that is, by adsorbing molecules with known adsorption areas onto the surface of the filler at low temperatures using liquid nitrogen, and measuring the amount of adsorption.

[0085] The resin composition may contain any appropriate other component as long as the effects of the present invention are not impaired. Such other components may be present in a single type or in two or more types. Examples of such other components include rubber, resins other than the polymers blended as the resin material, softeners, aliphatic compounds, antioxidants, antioxidants, light stabilizers, weathering agents, UV absorbers, dispersants, plasticizers, carbon, antistatic agents, surfactants, crosslinking agents, thickeners, rust inhibitors, silicone compounds, tension modifiers, shrinkage inhibitors, flow modifiers, gelling agents, curing agents, reinforcing agents, foaming agents, foam nucleating agents, colorants (pigments, dyes, etc.), pH adjusters, solvents (organic solvents), thermal polymerization initiators, photopolymerization initiators, lubricants, crystal nucleating agents, crystallization accelerators, vulcanizing agents, surface treatment agents, and dispersing aids.

[0086] As described above, resin foams are typically obtained by foaming a resin composition. The foaming method (cell formation method) can be a method typically used in foam molding, such as a physical method or a chemical method. That is, the resin foam may typically be a foam formed by foaming using a physical method (physical foam) or a foam formed by foaming using a chemical method (chemical foam). Physical methods generally involve dispersing a gas component such as air or nitrogen into a polymer solution and mechanically mixing the resulting mixture to form cells (mechanical foam). Chemical methods generally involve forming cells using gas generated by thermal decomposition of a blowing agent added to a polymer base, thereby obtaining a foam.

[0087] The resin composition to be subjected to foam molding may be prepared, for example, by mixing the constituent components using any suitable melt-kneading device, such as an open-type mixing roll, a non-open-type Banbury mixer, a single-screw extruder, a twin-screw extruder, a continuous kneader, or a pressure kneader.

[0088] Embodiment 1 for Forming Resin Foam In one embodiment 1 for forming a resin foam, for example, a resin foam is formed through a step (Step A) of mechanically foaming an emulsion resin composition (an emulsion containing a resin material (polymer), etc.). Examples of foaming devices include high-speed shear devices, vibration devices, and pressurized gas discharge devices. Among these foaming devices, high-speed shear devices are preferred from the viewpoints of miniaturizing the bubble diameter and large-volume production. This embodiment 1 for forming a resin foam can be applied to formation from any resin composition.

[0089] From the viewpoint of film-forming properties, the solids concentration of the emulsion is preferably high, and the solids concentration of the emulsion is preferably 30% by weight or more, more preferably 40% by weight or more, and even more preferably 50% by weight or more.

[0090] The bubbles generated by mechanical stirring are gases trapped in the emulsion. Any suitable gas can be used as long as it is inert to the emulsion and does not impair the effects of the present invention. Examples of such gases include air, nitrogen, and carbon dioxide.

[0091] The resin foam of the present invention can be obtained by applying the foamed emulsion resin composition (bubble-containing emulsion resin composition) to a substrate and drying it (Step B). Examples of the substrate include a release-treated plastic film (e.g., a release-treated polyethylene terephthalate film) and a plastic film (e.g., a polyethylene terephthalate film).

[0092] Any appropriate method can be used as the coating method and drying method in step B as long as the effects of the present invention are not impaired. Step B preferably includes a preliminary drying step B1 in which the bubble-containing emulsion resin composition applied to the substrate is dried at 50°C or higher and lower than 125°C, and a main drying step B2 in which the bubble-containing emulsion resin composition is further dried at 125°C or higher and 200°C or lower.

[0093] By providing the preliminary drying step B1 and the main drying step B2, it is possible to prevent bubble coalescence and bubble burst due to a sudden rise in temperature. The preliminary drying step B1 is particularly significant in a foamed sheet with a small thickness, since a sudden rise in temperature can cause bubbles to coalesce and burst. The temperature in the preliminary drying step B1 is preferably 50°C to 100°C. The duration of the preliminary drying step B1 is preferably 0.5 to 30 minutes, more preferably 1 to 15 minutes. The temperature in the main drying step B2 is preferably 130°C to 180°C or less, more preferably 130°C to 160°C. The duration of the main drying step B2 is preferably 0.5 to 30 minutes, more preferably 1 to 15 minutes.

[0094] In one embodiment, a resin foam is formed by foaming a resin composition with a foaming agent. The foaming agent may be one typically used in foam molding. From the viewpoints of environmental protection and low contamination of the foamed object, it is preferable to use a high-pressure inert gas.

[0095] Any suitable inert gas can be used as the inert gas as long as it is inert to the resin composition and can be impregnated. Examples of such inert gases include carbon dioxide, nitrogen gas, and air. These gases may be used in combination. Among these, carbon dioxide is preferred from the viewpoints of a large amount of impregnation into the resin material (polymer) and a fast impregnation rate.

[0096] The inert gas is preferably in a supercritical state. That is, it is particularly preferable to use carbon dioxide in a supercritical state. In a supercritical state, the solubility of the inert gas in the resin composition is further increased, allowing for high concentrations of the inert gas to be mixed in. In addition, the inert gas becomes highly concentrated during a sudden pressure drop, resulting in increased generation of bubble nuclei. The density of the bubbles formed by the growth of the bubble nuclei is greater than in other states even if the porosity is the same, so that fine bubbles can be obtained. The critical temperature of carbon dioxide is 31°C and the critical pressure is 7.4 MPa.

[0097] Examples of methods for forming a foam by impregnating a resin composition with a high-pressure inert gas include a gas impregnation step in which a resin composition containing a resin material (polymer) is impregnated with an inert gas under high pressure, a decompression step in which the pressure is reduced to foam the resin material (polymer), and a heating step in which bubbles are grown by heating, if necessary. In this case, a pre-formed unfoamed molded body may be impregnated with the inert gas, or a molten resin composition may be impregnated with the inert gas under pressure and then molded under reduced pressure. These steps may be performed using either a batch process or a continuous process. That is, a batch process may be used in which the resin composition is pre-formed into an appropriate shape, such as a sheet, to form an unfoamed resin molded body, and then the unfoamed resin molded body is impregnated with a high-pressure gas and foamed by releasing the pressure. Alternatively, a continuous process may be used in which the resin composition is kneaded with a high-pressure gas under pressure, molded, and then the pressure is released simultaneously, thereby simultaneously molding and foaming.

[0098] An example of producing a foam using the batch method is shown below. For example, a resin sheet for foam molding is produced by extruding a resin composition using an extruder such as a single-screw extruder or a twin-screw extruder. Alternatively, the resin composition is uniformly kneaded using a kneader equipped with blades such as a roller, cam, kneader, or Banbury type, and then pressed to a predetermined thickness using a hot plate press or the like to produce an unfoamed resin molded body. The unfoamed resin molded body thus obtained is placed in a high-pressure container and a high-pressure inert gas (such as carbon dioxide in a supercritical state) is injected to impregnate the unfoamed resin molded body with the inert gas. Once the inert gas has sufficiently impregnated the unfoamed resin molded body, the pressure is released (usually to atmospheric pressure) to generate bubble nuclei in the resin. The bubble nuclei may be allowed to grow at room temperature or, in some cases, may be grown by heating. Heating methods that can be used include known and conventional methods such as a water bath, oil bath, heated roll, hot air oven, far infrared rays, near infrared rays, and microwaves. After the bubbles have grown in this way, the product is rapidly cooled with cold water or the like to fix the shape, thereby obtaining a foam. The unfoamed resin molded product to be foamed is not limited to a sheet-like product, and various shapes can be used depending on the application. The unfoamed resin molded product to be foamed can also be produced by other molding methods such as extrusion molding, press molding, and injection molding.

[0099] An example of continuous foam production is shown below. For example, a resin composition is kneaded using an extruder such as a single-screw extruder or a twin-screw extruder while injecting (introducing) a high-pressure gas (particularly an inert gas, or even carbon dioxide) to sufficiently impregnate the resin composition with the high-pressure gas in a kneading / impregnation step. The resin composition is then extruded through a die or the like at the tip of the extruder to release the pressure (usually to atmospheric pressure), and foaming and foaming are simultaneously performed in a molding / decompression step. Furthermore, continuous foam molding may optionally include a heating step in which cells are grown by heating. After the cells have grown in this manner, the cells may be rapidly cooled with cold water or the like to fix the shape, if necessary. The high-pressure gas may be introduced continuously or discontinuously. Furthermore, the kneading / impregnation step and the molding / decompression step may be performed using, for example, an extruder or an injection molding machine. Heating methods for growing cell nuclei include any appropriate method, such as a water bath, an oil bath, a heated roll, a hot air oven, far infrared rays, near infrared rays, or microwaves. The foam may have any suitable shape, such as a sheet, a prism, a cylinder, or an irregular shape.

[0100] The amount of gas mixed when foam-molding the resin composition is preferably 2 to 10% by weight, more preferably 2.5 to 8% by weight, and even more preferably 3 to 6% by weight, relative to the total amount of the resin composition, in order to obtain a highly foamed resin foam.

[0101] The pressure when impregnating the resin composition with an inert gas can be appropriately selected taking into consideration operability, etc. Such a pressure is, for example, preferably 6 MPa or more (e.g., 6 MPa to 100 MPa), more preferably 8 MPa or more (e.g., 8 MPa to 50 MPa). When using carbon dioxide in a supercritical state, the pressure is preferably 7.4 MPa or more from the viewpoint of maintaining the supercritical state of carbon dioxide. If the pressure is lower than 6 MPa, bubble growth during foaming is significant, the bubble diameter becomes too large, and a desirable average cell diameter (average cell diameter) may not be obtained. This is because, at low pressures, the amount of gas impregnated is relatively small compared to high pressures, the rate of bubble nucleation decreases, and the number of bubble nuclei formed decreases. Consequently, the amount of gas per bubble increases, resulting in an extremely large bubble diameter. Furthermore, in pressure regions lower than 6 MPa, even a small change in impregnation pressure significantly changes the bubble diameter and cell density, making it difficult to control the bubble diameter and cell density.

[0102] The temperature in the gas impregnation step varies depending on the type of inert gas used and the types of components in the resin composition, and can be selected from a wide range. When operability and other factors are taken into consideration, the temperature is preferably 10°C to 350°C. When an unfoamed molded body is impregnated with an inert gas, the impregnation temperature is preferably 10°C to 250°C, and more preferably 40°C to 230°C, in a batch process. When the gas-impregnated molten polymer is extruded to simultaneously foam and mold, the impregnation temperature is preferably 60°C to 350°C in a continuous process. When carbon dioxide is used as the inert gas, the temperature during impregnation is preferably 32°C or higher, and more preferably 40°C or higher, in order to maintain a supercritical state.

[0103] In the depressurizing step, the depressurizing speed is preferably 5 MPa / sec to 300 MPa / sec in order to obtain uniform fine bubbles.

[0104] The heating temperature in the heating step is preferably 40°C to 250°C, more preferably 60°C to 250°C.

[0105] In one embodiment, after obtaining a foam structure through a predetermined process (e.g., after obtaining a resin foam by the method of <Embodiment 1> or <Embodiment 2>), the foam structure is thinned and then rolled to obtain a resin foam. Through these processes, a resin foam with an appropriately adjusted aspect ratio can be obtained. Furthermore, a resin foam with a small thickness (e.g., 0.2 mm or less) can be obtained.

[0106] The foam structure can be thinned using any appropriate slicer. The thickness of the foam structure after thinning is preferably 0.01 mm or more, more preferably 0.05 mm or more, even more preferably 0.1 mm or more, and particularly preferably 0.15 mm or more. The upper limit of the thickness of the foam structure after thinning is preferably 3 mm or less, more preferably 2 mm or less, even more preferably 1.5 mm or less, even more preferably 1 mm or less, even more preferably 0.8 mm or less, and particularly preferably 0.5 mm or less. Within such a range, the number of cells in the resin foam is particularly preferably adjusted, making it difficult for crushing to occur due to punching, and therefore, a resin foam with particularly excellent punching processability can be obtained.

[0107] Preferably, the rolls used for the rolling are heated rolls, and the temperature of the rolls is preferably 150°C to 250°C, more preferably 160°C to 230°C.

[0108] The rolling ratio of the foamed structure (thickness after rolling / thickness before rolling × 100) is preferably 80% or less, more preferably 10% to 80%, even more preferably 20% to 75%, and particularly preferably 30% to 75%. Within such ranges, a resin foam with an appropriately adjusted aspect ratio can be obtained.

[0109] B. Foam Member Fig. 1 is a schematic cross-sectional view of a foam member according to one embodiment. The foam member 100 has a resin foam layer 10 and a pressure-sensitive adhesive layer 20 disposed on at least one side of the resin foam layer 10. The resin foam layer 10 is composed of the above-described resin foam.

[0110] The thickness of the resin foam layer of the foam material is preferably 30 μm or more, more preferably 35 μm or more, even more preferably 40 μm or more, and particularly preferably 45 μm or more. The thickness of the resin foam layer of the foam material is preferably 5000 μm or less, more preferably 4000 μm or less, even more preferably 3000 μm or less, and more preferably 2500 μm or less. When the thickness of the resin foam layer is within the above range, the resin foam layer can easily conform to even minute clearances. Furthermore, when the thickness of the resin foam layer is within the above range, bubbles can be uniformly contained, resulting in excellent impact absorption properties.

[0111] The thickness of the pressure-sensitive adhesive layer is preferably 5 μm or more, more preferably 6 μm or more, even more preferably 7 μm or more, and particularly preferably 8 μm or more. The thickness of the pressure-sensitive adhesive layer is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and most preferably 50 μm or less. When the thickness of the pressure-sensitive adhesive layer is within the above range, the foam material of the present invention can exhibit excellent impact absorption properties.

[0112] The pressure-sensitive adhesive layer may be a layer made of any appropriate pressure-sensitive adhesive. Examples of pressure-sensitive adhesives constituting the pressure-sensitive adhesive layer include rubber-based pressure-sensitive adhesives (synthetic rubber-based pressure-sensitive adhesives, natural rubber-based pressure-sensitive adhesives, etc.), urethane-based pressure-sensitive adhesives, acrylic urethane-based pressure-sensitive adhesives, acrylic-based pressure-sensitive adhesives, silicone-based pressure-sensitive adhesives, polyester-based pressure-sensitive adhesives, polyamide-based pressure-sensitive adhesives, epoxy-based pressure-sensitive adhesives, vinyl alkyl ether-based pressure-sensitive adhesives, fluorine-based pressure-sensitive adhesives, and rubber-based pressure-sensitive adhesives. The pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is preferably at least one selected from acrylic-based pressure-sensitive adhesives, silicone-based pressure-sensitive adhesives, and rubber-based pressure-sensitive adhesives. Only one type of such pressure-sensitive adhesive may be used, or two or more types may be used. The pressure-sensitive adhesive layer may be a single layer, or two or more layers.

[0113] Pressure-sensitive adhesives can be classified by adhesive form, for example, emulsion-type pressure-sensitive adhesives, solvent-type pressure-sensitive adhesives, ultraviolet-crosslinking (UV-crosslinking) pressure-sensitive adhesives, electron-beam-crosslinking (EB-crosslinking) pressure-sensitive adhesives, hot-melt pressure-sensitive adhesives, etc. Only one type of such pressure-sensitive adhesive may be used, or two or more types may be used.

[0114] The water vapor permeability of the pressure-sensitive adhesive layer is preferably 50 (g / (m 2 24 hours)) or less, and more preferably 30 (g / (m 2 24 hours)) or less, and more preferably 20 (g / (m 2 24 hours)) or less, and particularly preferably 10 (g / (m 2 When the water vapor permeability of the pressure-sensitive adhesive layer is within the above range, the foam sheet of the present invention can stabilize the impact absorption properties without being affected by moisture.

[0115] The adhesive constituting the adhesive layer may contain any other appropriate component within a range that does not impair the effects of the present invention.

[0116] Examples of other components include other polymer components, softeners, antioxidants, curing agents, plasticizers, fillers, antioxidants, thermal polymerization initiators, photopolymerization initiators, UV absorbers, light stabilizers, colorants (pigments, dyes, etc.), solvents (organic solvents), surfactants (e.g., ionic surfactants, silicone surfactants, fluorine-based surfactants, etc.), crosslinking agents (e.g., polyisocyanate-based crosslinking agents, silicone-based crosslinking agents, epoxy-based crosslinking agents, alkyl-etherified melamine-based crosslinking agents, etc.), etc. The thermal polymerization initiator and the photopolymerization initiator can be included in the material for forming the polymer component.

[0117] The foam material of the present invention can be produced by any appropriate method, such as a method of laminating a resin foam layer and a pressure-sensitive adhesive layer, or a method of laminating a pressure-sensitive adhesive layer-forming material and a resin foam layer, and then forming a pressure-sensitive adhesive layer by a curing reaction or the like.

[0118] The present invention will be specifically described below using examples, but the present invention is not limited to these examples. The test and evaluation methods used in the examples are as follows. The term "parts" means "parts by weight" unless otherwise specified, and the term "%" means "% by weight" unless otherwise specified.

[0119] <Evaluation Method> (1) Apparent Density The density (apparent density) of the resin foam was calculated as follows. The resin foam obtained in each of the Examples and Comparative Examples was punched out to a size of 20 mm x 20 mm to prepare a test piece, and the dimensions of the test piece were measured with a vernier caliper. Next, the weight of the test piece was measured with an electronic balance. Then, the apparent density (g / cm) was calculated using the following formula. 3 ) = weight of test piece / volume of test piece (2) 25% Compression Load This was measured in accordance with the method for measuring the compression hardness of resin foams described in JIS K 6767. Specifically, the resin foams obtained in the examples and comparative examples were cut into test pieces of 30 mm x 30 mm in size, and the stress (N) when compressed at a compression rate of 10 mm / min until the compression ratio reached 25% was measured per unit area (1 cm 2 ) and converted to a 25% compression load (N / cm 2 (3) 50% Compression Load This was measured in accordance with the method for measuring the compression hardness of resin foams described in JIS K 6767. Specifically, the resin foams obtained in the examples and comparative examples were cut into test pieces of 30 mm x 30 mm in size, and the stress (N) when compressed at a compression rate of 10 mm / min until the compression ratio reached 50% was measured per unit area (1 cm 2 ) and converted to a 50% compression load (N / cm 2) were used. (4) Average bubble diameter (average cell diameter), maximum bubble diameter (maximum cell diameter), and coefficient of variation of bubble diameter (cell diameter) The resin foam was cut using a razor blade in the direction perpendicular to the main surface of the resin foam (thickness direction), and a digital microscope (product name "VHX-500", manufactured by Keyence Corporation) was used as a measuring instrument to capture an image of the cross section of the resin foam. The image was analyzed using the instrument's analysis software to determine the number-average bubble diameter (average cell diameter) and maximum bubble diameter (maximum cell diameter). The number of bubbles in the captured enlarged image was approximately 400. The standard deviation was calculated from all the cell diameter data, and the coefficient of variation was calculated using the following formula. Coefficient of variation = standard deviation / average cell diameter (average cell diameter) (5) Cell diameter aspect ratio Using a digital microscope (trade name "VHX-2000" manufactured by Keyence Corporation) as a measuring instrument, the aspect ratio of the cells in the resin foams obtained in the Examples and Comparative Examples was measured by the following method. The resin foam was cut with a razor blade in the direction perpendicular to the main surface of the resin foam (thickness direction), and the cut surface was measured with a microscope (for example, "VHX-2000" manufactured by Keyence) to obtain a predetermined area (3 mm 2The area was observed at 100x magnification, and the length of each bubble in the thickness direction and the direction perpendicular to the thickness direction were measured. Similar measurements were performed on all bubbles present within a given area. The aspect ratio of a bubble was calculated by dividing the length perpendicular to the thickness direction by the length in the thickness direction. The same calculation was performed for all bubbles, and the average value was used as the "aspect ratio of the bubbles in the resin foam." (6) Melt Tension Using a twin capillary rheometer "RH7-2" (manufactured by Rosand Precision), the resin (plant-derived polypropylene polymer) contained in the resin foam was extruded into a molten strand at an extrusion rate of 8.8 mm / min at a temperature 20°C higher than the melting point of the plant-derived polypropylene polymer and an orifice diameter of 1 mmφ. The strand was then taken up at a take-up rate of 0.5 m / min. The take-up rate was increased in increments of 0.1 m / min, and the melt tension at which the strand-shaped resin broke was defined as the "melt tension." (7) Die swell ratio Using an extensional viscometer (trade name "RH-7", Malvern Instruments) as a measuring instrument, a sample (size: 5 mm square) was placed in a cylinder at a temperature 20 ° C higher than the melting point of the resin constituting the resin foam, and allowed to melt for 7 minutes. The molten material was then extruded at a shear rate of 20 mm / s into a die having a length of 10 mm and a diameter of 1 mmφ, and the diameter of the resulting string-like molded product was measured using a digital caliper (trade name "CD67-s PM", Mitutoyo Corporation), and the die swell ratio was calculated using the following formula. Die swell ratio = diameter of molded product (mm) / die diameter (mm) As the sample, a plant-derived polypropylene polymer contained in the resin foam and a resin composition forming the resin foam were used, and the die swell ratio of these samples was measured. (8) Impact Absorption A test specimen was formed by placing a resin foam, double-sided tape (product number: No. 5603W, manufactured by Nitto Denko), and a PET film (product number: Diafoil MRF75, manufactured by Mitsubishi Plastics) in this order on an impact force sensor. A 66 g iron ball was dropped on the test specimen from a height of 50 cm above the PET film to measure the impact force F1. In addition, an iron ball was dropped directly onto the impact force sensor as described above to measure the blank impact force F0. Impact absorption (%) was calculated from F1 and F0 using the formula (F0-F1) / F0×100.(9) CO derived from raw materials. 2 Amount generated [kg / m 2 ] CO required for producing petroleum-derived resin 2 The amount of CO generated is 1.8 kg / kg-resin, and the amount of CO required to produce plant-derived resin 2 The generated amount is 1.0 kg / kg-resin, and the foam is 1 m 2 When the weight of the petroleum-derived resin contained in the foam is wp and the weight of the plant-derived resin is wb, the CO2 derived from the raw materials of the foam is 2 The amount of generated dust can be calculated by 1.8×wp+1.0×wb.

[0120] Example 1: 56 parts by weight of a plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF", MFR: 0.85 g / 10 min), 49 parts by weight of polyolefin elastomer A (melt flow rate (MFR): 15 g / 10 min), 10 parts by weight of magnesium hydroxide, 1 part by weight of stearic acid monoglyceride, and 10 parts by weight of carbon black were kneaded at 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into strands, cooled with water, and formed into pellets. The pellets were placed in a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 MPa (12 MPa after injection) in an atmosphere of 220°C. The carbon dioxide gas was injected at a ratio of 5.2 parts by weight per 100 parts by weight of resin. After being fully saturated with carbon dioxide gas, the mixture was cooled to a temperature suitable for foaming, extruded through a die, and sliced ​​to a thickness of 1.0 mm to obtain a sheet-like resin foam. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0121] Example 2 A resin foam was obtained in the same manner as in Example 1, except that the blending amount of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was 65 parts by weight, the blending amount of polyolefin elastomer A was 35 parts by weight, and the injected amount of carbon dioxide gas was 5.5 parts by weight per 100 parts by weight of the resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0122] [Example 3] A resin foam was obtained in the same manner as in Example 1, except that the blending amount of the plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was 65 parts by weight and the blending amount of the polyolefin elastomer A was 35 parts by weight. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0123] [Example 4] A resin foam was obtained in the same manner as in Example 2, except that the amount of carbon dioxide gas injected was 5.8 parts by weight per 100 parts by weight of the resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0124] Example 5: 65 parts by weight of a plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF", MFR: 0.85 g / 10 min), 35 parts by weight of polyolefin elastomer A (melt flow rate (MFR): 15 g / 10 min), 10 parts by weight of magnesium hydroxide, 1 part by weight of stearic acid monoglyceride, and 10 parts by weight of carbon black were kneaded at 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into strands, cooled with water, and formed into pellets. The pellets were placed in a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 MPa (12 MPa after injection) in an atmosphere of 220°C. The carbon dioxide gas was injected at a ratio of 5.8 parts by weight per 100 parts by weight of resin. After being fully saturated with carbon dioxide gas, the mixture was cooled to a temperature suitable for foaming, extruded through a die, and sliced ​​to a thickness of 2.0 mm to obtain a sheet-like resin foam. Furthermore, the foamed structure was passed through the gap between a pair of rolls, one of which was heated to 200°C (the gap between the rolls), to obtain a resin foam B having a thickness of 1.0 mm. The gap between the rolls was set so that a resin foam B having a thickness of 1.0 mm was obtained.

[0125] Example 6 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of plant-derived polypropylene polymer (manufactured by SABIC, trade name "Rely 61EK61PS", MFR: 0.3 g / 10 min) was used, and the amount of carbon dioxide gas injected was changed to 5.5 parts by weight per 100 parts by weight of the resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0126] Example 7 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of plant-derived polypropylene polymer (manufactured by SABIC, trade name "Rely 71EK71PS", MFR: 0.3 g / 10 min) was used, and the amount of carbon dioxide gas injected was changed to 5.5 parts by weight per 100 parts by weight of the resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0127] Example 8 A resin foam was obtained in the same manner as in Example 1, except that the blending amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 75 parts by weight, the blending amount of polyolefin elastomer A was 25 parts by weight, and the injected amount of carbon dioxide gas was 5.2 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0128] Example 9 A resin foam was obtained in the same manner as in Example 1, except that the blending amount of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was 75 parts by weight, the blending amount of polyolefin elastomer A was 25 parts by weight, and the injected amount of carbon dioxide gas was 5.4 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0129] Example 10 A resin foam was obtained in the same manner as in Example 1, except that the blending amount of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was 65 parts by weight, the blending amount of polyolefin elastomer A was 35 parts by weight, and the injected amount of carbon dioxide gas was 6.2 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0130] Example 11 A resin foam was obtained in the same manner as in Example 1, except that the blending amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 65 parts by weight, the blending amount of polyolefin elastomer A was 35 parts by weight, and the injected amount of carbon dioxide gas was 6.4 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0131] Comparative Example 1 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BC250MO", MFR: 4 g / 10 min) was used, and the amount of carbon dioxide gas injected was changed to 5.5 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0132] Comparative Example 2 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of plant-derived polypropylene polymer (manufactured by Borealis, trade name "BB125MO", MFR: 1.3 g / 10 min) was used, and the amount of carbon dioxide gas injected was changed to 5.5 parts by weight per 100 parts by weight of the resin. The obtained resin foam was subjected to the above-mentioned evaluations. The results are shown in Table 1.

[0133]

[0134] The resin foam of the present invention can be suitably used, for example, as a cushioning material for electronic devices.

[0135] 100 Foam member 10 Resin foam layer (resin foam) 20 Pressure-sensitive adhesive layer

Claims

1. A resin foam having a cell structure, wherein the content ratio a of a petroleum-derived resin is 50% by weight or less and the following formula (1) is satisfied. [Apparent density (g / cm 3 ) ]<−0.0025×[content a (%) of petroleum-derived resin] + 0.48 ... (1) 2. The resin foam according to claim 1, wherein the aspect ratio of the bubbles contained in the resin foam is 4 or less.

3. The 50% compression load of the resin foam is 40 N / cm 2 The resin foam according to claim 1 , wherein:

4. The 25% compression load of the resin foam is 25 N / cm 2 The resin foam according to claim 1 , wherein:

5. The resin foam according to claim 1, wherein the resin foam has an average cell diameter of 200 μm or less.

6. The apparent density of the resin foam is 0.4 g / cm 3 The resin foam according to claim 1 , wherein:

7. The resin foam according to claim 1, wherein the resin foam has a coefficient of variation of cell diameter of 0.6 or less.

8. The resin foam according to claim 1, comprising a plant-derived polyolefin resin.

9. The resin foam according to claim 8, wherein the plant-derived polyolefin resin comprises a plant-derived polyolefin, and the plant-derived polyolefin has a melt flow rate at a temperature of 230°C of less than 20 g / 10 min.

10. The resin foam according to claim 1, wherein the plant-derived polyolefin has a melt tension of 10 cN or more.

11. The resin foam according to claim 8, wherein the die swell ratio at the melting point of the plant-derived polyolefin + 20°C is 1.5 or less.

12. The resin foam according to claim 1, wherein the die swell ratio at the melting point of the resin composition forming the resin foam + 20°C is 1.5 or less.

13. The resin foam according to claim 8, wherein the plant-derived polyolefin resin comprises a plant-derived polypropylene polymer.

14. The resin foam according to claim 8, wherein the plant-derived polyolefin resin is a mixture of a polyolefin other than a polyolefin-based elastomer and a polyolefin-based elastomer, the polyolefin being a plant-derived polyolefin, and the polyolefin-based elastomer being a plant-derived polyolefin-based elastomer or a petroleum-derived polyolefin-based elastomer.

15. The resin foam according to claim 1, having a heat-fusible layer on one or both sides.

16. A foam member comprising a resin foam layer formed from the resin foam according to claim 1 and an adhesive layer disposed on at least one side of the resin foam layer.

Citation Information

Patent Citations

  • Foam sheet, and adhesive tape

    JP2021031608A

  • Polyethylene-based resin foam sheet

    JP2021130796A

  • Foam sheet, composite article and interior material for vehicle

    JP2021147423A

  • Resin foam body

    WO2022209767A1

  • Propylene-based resin composition and use thereof

    WO2023042701A1