Water-absorbent resin particles and production method therefor, absorbent body, and absorbent article

The regeneration of water-absorbing resin particles through chemical decomposition and crosslinking addresses the challenge of maintaining performance and reducing polymer dissolution, resulting in high-efficiency and sustainable water-absorbing materials for recycling.

WO2024214558A1PCT designated stage expired Publication Date: 2024-10-17SUMITOMO SEIKA CHEM CO LTD

Patent Information

Application Number
PCT/JP2024/012891
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-03-28
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing methods for recycling water-absorbing resin particles from used sanitary products often compromise between maintaining high water-absorbing performance and suppressing the dissolution of polymer components, as the cross-linked structure is typically destroyed during treatment, leading to increased dissolved polymer content.

Method used

A method for producing water-absorbing resin particles involves chemically decomposing used water-absorbing resins to regenerate particles with high water-absorbing performance and low dissolved content, involving a preparation step with a polymer solution, crosslinking via covalent bonds, and subsequent processing to achieve desired molecular weight and particle characteristics.

Benefits of technology

The method effectively regenerates water-absorbing resin particles with high performance and low dissolved content, enhancing the recycling efficiency and sustainability of water-absorbing materials while maintaining their absorbency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012891_17102024_PF_FP_ABST
    Figure JP2024012891_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a production method for water-absorbent resin particles containing a crosslinked polymer, said method comprising a preparation step for preparing a polymer solution which contains a polymer and a solvent, and a crosslinking step for forming a crosslinked polymer by crosslinking the polymer via a covalent bond in the polymer solution. The water-absorbent resin particles have a soluble component index, which is represented by the following formula, of 2×10-3 to 6×10-3. Soluble component index=soluble content(g / g) / CRC (g / g)
Need to check novelty before this filing date? Find Prior Art

Description

Water-absorbent resin particles and their manufacturing method, absorbent body, and absorbent article

[0001] The present invention relates to water-absorbent resin particles, a method for producing the same, an absorbent body, and an absorbent article.

[0002]

[0003] Generally, disposable sanitary products are constructed by enclosing pulp fibers and a water-absorbent resin between a water-impermeable cover sheet and a water-permeable nonwoven fabric, and the water-absorbent resin absorbs water and swells to absorb bodily waste. After use, such sanitary products are disposed of by incineration or landfilling, but recently, research has been conducted into the recovery and reuse of components from used sanitary products. For example, Patent Document 1 discloses a water-absorbent resin decomposition technology that focuses on cleavage of crosslinks within the water-absorbent resin, and a technology for recovering the water-soluble recycled polymer obtained by decomposing the water-absorbent resin as an aggregate by crosslinking with multivalent metal ions.

[0003] Japanese Patent Application Laid-Open No. 2020-49398

[0004] In many of the techniques disclosed as methods for regenerating water-absorbent resins recovered from used sanitary products, the water-absorbent capacity of the water-absorbent resin is compared before and after a predetermined treatment, and if the water-absorbent capacity is at least the same as before the treatment, it is considered to have been regenerated. However, since the crosslinked structure of the water-absorbent resin is destroyed by the predetermined treatment, making the polymer components more likely to leach out, it is necessary to suppress not only the water-absorbent capacity but also the increase in the soluble polymer. However, it is difficult to say that Patent Document 1 achieves both maintaining the water-absorbent capacity and suppressing the dissolution of the polymer.

[0005] One aspect of the present invention relates to a method for producing water-absorbent resin particles having high water absorption capacity and low soluble content, which can be applied to regenerate water-absorbent resin particles from a polymer formed by chemically decomposing a water-absorbent resin.

[0006] One aspect of the present disclosure includes, for example, the following means. [1] A method for producing water-absorbent resin particles containing a crosslinked polymer, comprising: a preparation step of preparing a polymer solution containing a polymer and a solvent; and a crosslinking step of forming the crosslinked polymer by crosslinking the polymer via a covalent bond. [2] The production method according to [1], wherein the preparation step includes cleaving a crosslinked structure of the crosslinked polymer of a recycled water-absorbent resin containing a crosslinked polymer to obtain the polymer. [3] The production method according to [2], wherein the preparation step further includes recovering the recycled water-absorbent resin from an absorbent article. [4] The production method according to any one of [1] to [3], wherein the weight-average molecular weight of the polymer is 100,000 or more. [5] The production method according to any one of [1] to [4], wherein the crosslinking step involves gelling the polymer solution. [6] The production method according to any one of [1] to [5], wherein the polymer has carboxyl groups, and the polymer is crosslinked by a reaction between the carboxyl groups and a crosslinking agent and / or a reaction between the carboxyl groups. [7] The method according to any one of [1] to [6], wherein the polymer is crosslinked via at least one group selected from the group consisting of a carboxylic acid ester group, a thioester group, an amide group, an acid anhydride group, an oxyalkylene group, and an oxyarylene group. [8] A soluble component index represented by the following formula is 2×10 -3 ~6 x 10 -3 Water-absorbent resin particles, wherein the soluble component index is soluble component (g / g) / CRC (g / g). [9] An absorbent body comprising the water-absorbent resin particles according to [8].

[10] An absorbent article comprising the absorbent body according to [9].

[0007] According to one aspect of the present invention, it is possible to provide a method for producing water-absorbent resin particles having high water absorption performance and a small amount of dissolved content, which can be applied to regenerate water-absorbent resin particles from a polymer formed by chemically decomposing a water-absorbent resin.

[0008] Fig. 1 is a cross-sectional view showing an example of an absorbent article having an absorbent body. Fig. 2 is a schematic view showing a nonwoven fabric bag produced when measuring a centrifuge retention capacity.

[0009] The present invention is not limited to the following examples.

[0010] In this specification, "(meth)acrylic" refers to both acrylic and methacrylic. "Acrylate" and "methacrylate" are also written as "(meth)acrylate." The same applies to other similar terms. "(Poly)" refers to both cases with and without the prefix "poly." In the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. In the numerical ranges described in this specification, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. The materials exemplified in this specification may be used alone or in combination of two or more. "Physiological saline" refers to a 0.9% by mass aqueous sodium chloride solution. "Standard sieve" refers to a test sieve (metal mesh sieve) specified in JIS Z 8801-1:2019. Unless otherwise specified, the examples and comparative examples were carried out in an environment of 1 atmosphere, normal temperature and normal humidity, and the various parameters disclosed in this specification were also values ​​measured in the same environment, with the temperature of the various samples being normal temperature. "1 atmosphere" is 101,325 Pa, "normal temperature" is 25°C, and "normal humidity" is 50% RH.

[0011] One example of a method for producing water-absorbent resin particles includes a preparation step of preparing a polymer solution containing a polymer and a solvent, and a crosslinking step of forming a crosslinked polymer by crosslinking the polymer in the polymer solution via a covalent bond. The water-absorbent resin particles contain a crosslinked polymer. This method allows water-absorbent resin particles to be regenerated from a polymer formed by chemically decomposing the water-absorbent resin (specifically, by cleaving the crosslinked structure of the water-absorbent resin), and also allows water-absorbent resin particles having high water absorption performance and a low dissolved content to be produced. The water-absorbent resin subjected to chemical decomposition (hereinafter, sometimes referred to as "recycled water-absorbent resin") is preferably a used water-absorbent resin (i.e., a water-absorbent resin that has become gelatinous due to absorption), but may also be an unused water-absorbent resin (e.g., waste water-absorbent resin generated during the production process of the water-absorbent resin), or a mixture of both.

[0012] In the preparation step, the polymer in the polymer solution can be obtained, for example, by cleaving the crosslinked structure of the crosslinked polymer of the water-absorbent resin containing the crosslinked polymer. The solvent in the polymer solution may be any solvent that can dissolve the polymer, and examples thereof include water and organic solvents.

[0013] The water absorbent resin may be, for example, a recycled water absorbent resin obtained by crushing absorbent articles. That is, the preparation step may include cleaving a crosslinked structure of a crosslinked polymer of a recycled water absorbent resin containing a crosslinked polymer to obtain a polymer, and may further include recovering the recycled water absorbent resin from the absorbent articles.

[0014] Examples of absorbent articles include diapers (e.g., disposable diapers), toilet training pants, incontinence pads, sanitary materials (sanitary napkins, tampons, etc.), sweat pads, pet sheets, portable toilet components, and animal waste disposal materials. The absorbent article may be a used one. The recycled water-absorbent resin recovered from a used water-absorbent article may form a gel by absorbing liquid during use.

[0015] The recycled water absorbent resin contains, for example, a polymer (crosslinked polymer) of an ethylenically unsaturated monomer. Examples of the ethylenically unsaturated monomer include (meth)acrylic acid and its salts, 2-(meth)acrylamido-2-methylpropanesulfonic acid and its salts, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-methylol(meth)acrylamide, polyethylene glycol mono(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide. The ethylenically unsaturated monomer may contain at least one compound selected from the group consisting of acrylic acid and its salts, methacrylic acid and its salts, acrylamide, methacrylamide, and N,N-dimethylacrylamide.

[0016] The crosslinked polymer may contain a monomer other than the ethylenically unsaturated monomer. The proportion of the ethylenically unsaturated monomer units (particularly, (meth)acrylic acid and salts thereof) in the polymer may be 70 to 100 mol % based on the total amount of monomer units. The proportion of (meth)acrylic acid and salts thereof in the ethylenically unsaturated monomers may be 70 to 100 mol %.

[0017] The recycled water absorbent resin contains, for example, a crosslinked polymer having a poly(meth)acrylic acid structure. Examples of such crosslinked polymers include: a polymer obtained by polymerizing a monomer composition containing (meth)acrylic acid and a crosslinking agent capable of reacting with the carboxyl group of (meth)acrylic acid to form a covalent bond; a polymer obtained by polymerizing a monomer composition containing (meth)acrylic acid to obtain a polymer, and then treating the surface of the polymer with a crosslinking agent capable of reacting with the carboxyl group of the polymer to form a covalent bond; a polymer obtained by polymerizing a monomer composition containing (meth)acrylic acid and a crosslinking agent capable of reacting with the carboxyl group of (meth)acrylic acid to form a covalent bond, and then treating the surface of the polymer with a crosslinking agent capable of reacting with the carboxyl group of the polymer to form a covalent bond.

[0018] The shape of the recycled water-absorbent resin is not particularly limited, and may be in the form of irregularly crushed pieces, flakes, granules, or the like.

[0019] The crosslinked structure of the crosslinked polymer of the water absorbent resin for recycling can be cleaved by contacting the water absorbent resin for recycling with an acidic component (e.g., sulfuric acid), an alkaline component (e.g., sodium hydroxide), an oxidizing agent, a reducing agent, etc. That is, in the preparation step, the crosslinked structure of the crosslinked polymer may be cleaved by contacting the water absorbent resin for recycling with at least one selected from the group consisting of an acidic component, an alkaline component, an oxidizing agent, and a reducing agent, to obtain a polymer.

[0020] The acidic component may be an inorganic acidic component, for example, at least one inorganic acidic component selected from the group consisting of acetic acid, nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, and boric acid, or at least one inorganic acidic component selected from sulfuric acid and hydrochloric acid.

[0021] The alkaline component may be an inorganic alkaline component, for example, at least one inorganic alkaline component selected from the group consisting of sodium hydroxide, ammonia, potassium hydroxide, and calcium hydroxide, or at least one inorganic alkaline component selected from the group consisting of sodium hydroxide, potassium hydroxide, and calcium hydroxide.

[0022] When the recycled water absorbent resin is brought into contact with an acidic component, the temperature of the solution containing the recycled water absorbent resin and the acidic component may be 80° C. to 140° C. When the recycled water absorbent resin is brought into contact with an alkaline component, the temperature of the solution containing the recycled water absorbent resin and the alkaline component may be 50° C. to 150° C., or 50° C. to 120° C.

[0023] Specifically, when the crosslinked structure of the crosslinked polymer is cleaved by an alkaline component, for example, the crosslinked structure can be cleaved by stirring a solution containing a water absorbent resin for recycling and an alkaline component at a temperature of 50°C to 150°C and in an environment of pH 10 or more for 1 hour to 50 hours.

[0024] When the recycled water absorbent resin contains a crosslinked polymer having a poly(meth)acrylic acid structure, the polymer obtained by cleaving the crosslinked polymer has a poly(meth)acrylic acid structure. When the recycled water absorbent resin contains a crosslinked polymer having a poly(meth)acrylic acid structure, the crosslinked polymer may be cleaved by contacting the recycled water absorbent resin with an alkaline component, from the viewpoint of easily producing water absorbent resin particles having high water absorption performance and low soluble content by avoiding cleavage of the poly(meth)acrylic acid structure.

[0025] The weight average molecular weight of the polymer obtained in the preparation step may be 100,000 or more, 300,000 or more, 500,000 or more, 700,000 or more, 1,000,000 or more, 1,300,000 or more, 1,500,000 or more, 1,700,000 or more, or 1,900,000 or more. The weight average molecular weight of the polymer may be 10,000,000 or less, 8,000,000 or less, 6,000,000 or less, 4,000,000 or less, 3,000,000 or less, or 2,000,000 or less. The weight average molecular weight of the polymer may be 100,000 to 10,000,000, 500,000 to 6,000,000, or 1,000,000 to 3,000,000. The weight average molecular weight of the polymer can be measured by GPC (gel permeation chromatography) under the following conditions. Apparatus: HLC-8320GPC (manufactured by Tosoh Corporation) Column: TSKgel Guard Column PWXL, G6000PWXL, GMPWXL, G3000PWXL (all manufactured by Tosoh Corporation) connected in this order for measurement Detector: differential refractometer (RI detector) Eluent: 0.2 M NaNO 3 Aqueous solution Flow rate: 1.0 mL / min Column temperature: 60°C Sample injection volume: 100 μL Calibration curve: sodium polyacrylate standard (Agilent Technologies) Sample preparation procedure and measurement procedure A sample solution adjusted to contain 0.01 g of polymer was placed in a 300 mL beaker, and 0.2 M NaNO as the eluent was added to make the total volume 100 mL. 3 The aqueous solution is added and stirred at 250 rpm for 1 hour. If the pH of the sample solution is not neutral, adjust it to pH 7 using hydrochloric acid (e.g., Nacalai Tesque, 1 mol / L hydrochloric acid). After stirring, the sample solution is filtered through a 0.8 μm filter syringe and the filtrate is measured by GPC.

[0026] After the crosslinked structure of the crosslinked polymer is cleaved to obtain a polymer, solid-liquid separation may be performed to remove impurities from the polymer solution before the crosslinking step is performed. For example, the polymer solution may be subjected to filtration or ultrafiltration. Before the filtration of the polymer solution, the pH of the polymer solution may be adjusted to approximately neutral.

[0027] After the crosslinked structure of the crosslinked polymer is cleaved to obtain a polymer, and before the crosslinking step is performed, dilution, heating, addition of a salt (a salt containing a monovalent cation), or the like may be performed in order to reduce the viscosity of the polymer solution.

[0028] After the crosslinked structure of the crosslinked polymer is cleaved to obtain the polymer, the polymer solution may be subjected to a sterilization treatment before the crosslinking step is carried out.

[0029] After obtaining a polymer by cleaving the crosslinked structure of the crosslinked polymer, and before carrying out the crosslinking step, the polymer may be recovered from the polymer solution by contacting the polymer solution with a poor solvent to precipitate the polymer dissolved in the polymer solution, thereby obtaining a polymer dispersion. By carrying out such an operation, the purity of the polymer can be increased. The poor solvent means a solvent in which the solubility of the polymer in 100 g of the solvent at 25°C is less than 0.1 g. The poor solvent may be a water-soluble organic solvent.

[0030] Examples of methods for contacting a polymer solution with a poor solvent for the polymer include adding the poor solvent to the polymer solution and adding the polymer solution to the poor solvent. When adding a poor solvent to a polymer solution, the entire amount of poor solvent to be used may be added to the polymer solution at once, or may be added to the polymer solution over time. Similarly, when adding a poor polymer solution to a poor solvent, the entire polymer solution may be added to the poor solvent at once, or may be added to the poor solvent over time. Note that "addition over time" means adding the poor solvent (or polymer solution) to the polymer solution (or poor solvent) continuously or intermittently over a predetermined time. From the viewpoint of reducing the amount of poor solvent used, a method of adding the poor solvent to the polymer solution over time may be adopted.

[0031] Examples of the poor solvent include alcohols, phenols, ketones, ethers, nitriles, etc., each having 1 to 10 carbon atoms. From the viewpoint of facilitating the production of a polymer with higher purity, the poor solvent may be at least one selected from the group consisting of alcohols, phenols, and ketones having 1 to 10 carbon atoms.

[0032] Examples of alcohols having 1 to 10 carbon atoms include methanol, ethanol, propanol, butanol, pentanol, ethylene glycol, and glycerin. Examples of phenols include phenol, cresol, dibutylhydroxytoluene, and eugenol. Examples of ketones include acetone, methyl ethyl ketone, and diethyl ketone. Examples of ethers include dimethyl ether, ethyl methyl ether, diethyl ether, furan, and tetrahydrofuran. Examples of nitriles include acrylonitrile. The poor solvent may be at least one selected from the group consisting of methanol, ethanol, and acetone.

[0033] When the contact between the polymer solution and the poor solvent is performed by adding the poor solvent to the polymer solution over time, the concentration of the poor solvent in the finally obtained polymer dispersion may be 60% by mass or less, 50% by mass or less, 40% by mass or less, 30% by mass or less, or 20% by mass or less, from the viewpoint of easily obtaining a polymer in a shorter time. The concentration of the poor solvent in the polymer dispersion may be 10% by mass or more, or 20% by mass or more. The content of the poor solvent in the polymer dispersion may be 10% by mass to 60% by mass, or 20% by mass to 50% by mass.

[0034] Furthermore, when the contact between the polymer solution and the poor solvent is performed by adding the poor solvent to the polymer solution over time, the rate of addition of the poor solvent may be 20% by mass / min or less, or 10% by mass / min or less, relative to the polymer solution, from the viewpoint that the polymer is more likely to precipitate in the form of small particles, thereby making it difficult for impurities to remain inside the precipitated polymer (i.e., increasing the purity of the polymer), and may be 0.1% by mass / min or more, or 1% by mass / min or more, from the viewpoint of reducing the time required for dropwise addition. The dropwise addition rate of the poor solvent may be 0.1% by mass / min to 20% by mass / min, or 1% by mass / min to 10% by mass / min.

[0035] The polymer yield in the dispersion step may be 75% by weight or more, 80% by weight or more, 85% by weight or more, or 90% by weight or more.

[0036] The polymer dispersed in the polymer dispersion may be in the form of particles or lumps.

[0037] The polymer dispersion has a transmittance of 0.85% or less for light with a wavelength of 425 nm over a 1 cm optical path length, and from the viewpoint of sufficiently precipitating a polymer that easily forms spherical particles in a dispersion medium in a reversed-phase suspension system, the transmittance may be 0.80% or less, 0.70% or less, or less than 0.70%. The polymer dispersion has a transmittance of 0.01% or more, 0.10% or more, 0.20% or more, or 0.30% or more for light with a wavelength of 425 nm over a 1 cm optical path length, from the viewpoint of suppressing aggregation of the precipitated polymer and thereby facilitating the formation of spherical particles in a dispersion medium in a reversed-phase suspension system. From these viewpoints, the transmittance of the polymer dispersion may be 0.01% to 0.80%, 0.01% to 0.70%, or 0.01% or more but less than 0.70%.

[0038] The viscosity of the polymer dispersion at 25°C may be 5000 mPa·s or less, 3000 mPa·s or less, or 2000 mPa·s or less, from the viewpoint of making it easier to disperse the polymer in the dispersion medium in a reversed-phase suspension system, thereby suppressing aggregation of the polymer in the dispersion medium, and facilitating the formation of spherical particles. The viscosity of the polymer dispersion at 25°C may be 50 mPa·s or more, 100 mPa·s or more, 1000 mPa·s or more, 1500 mPa·s or more, 3000 mPa·s or more, 5000 mPa·s or more, or 10000 mPa·s or more. From these viewpoints, the viscosity of the polymer dispersion at 25°C may be 50 mPa·s to 5000 mPa·s, 50 mPa·s to 3000 mPa·s, or 50 mPa·s to 2000 mPa·s, 100 mPa·s to 5000 mPa·s, 100 mPa·s to 3000 mPa·s, or 100 mPa·s to 2000 mPa·s.

[0039] The weight average molecular weight of the polymer in the polymer dispersion may be 1.7 million or more, 1.8 million or more, or 1.9 million or more, and may be 2.5 million or less, or 2.4 million or less. The weight average molecular weight of the polymer in the polymer dispersion may be 1.7 million to 2.5 million, or 1.8 million to 2.4 million.

[0040] After the polymer dispersion medium is added to the dispersion medium in the reverse phase suspension system, the median particle size of the dried polymer may be 100 μm or more, 150 μm or more, or 200 μm or more, or may be less than 300 μm or 290 μm or less, or may be 100 μm or more and less than 300 μm.

[0041] In the crosslinking step, for example, a solution containing a polymer and a crosslinking agent capable of forming a covalent bond with a functional group of the polymer is prepared, and the polymer is crosslinked. In the crosslinking step, the polymer solution may be gelled. In this case, the entire polymer solution loses fluidity, and a gel containing a crosslinked polymer and water is formed. When crosslinking progresses to the extent that a gel is formed, it is particularly easy to obtain water-absorbent resin particles having high water absorption performance and a small amount of dissolved matter.

[0042] Examples of functional groups possessed by the polymer include carboxyl groups. When the polymer has carboxyl groups, the polymer is crosslinked by a reaction between the carboxyl groups and a crosslinking agent and / or a reaction between the carboxyl groups themselves. The covalent bond may be at least one selected from the group consisting of an ester bond, a thioester bond, an amide bond, an ether bond, and a carbon-carbon bond. The polymer may be crosslinked, for example, via at least one group selected from the group consisting of a carboxylic acid ester group, a thioester group, an amide group, an acid anhydride group, an oxyalkylene group, and an oxyarylene group.

[0043] Examples of the crosslinking agent include aliphatic polyhydric alcohols such as (poly)ethylene glycol, (poly)propylene glycol, (poly)glycerin, and pentaerythritol; glycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerin diglycidyl ether; bisacrylamide compounds such as N,N'-methylenebis(meth)acrylamide; allylated starch; diallyl phthalate; N,N',N"-triallyl isocyanurate; divinylbenzene; ethylenediamine, polyethyleneimine, and glycidyl (meth)acrylate.

[0044] The amount of the crosslinking agent may be 0.0001 parts by mass or more, 0.001 parts by mass or more, or 0.005 parts by mass or more, and may be 15 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less, relative to 100 parts by mass of the polymer, from the viewpoint of sufficiently crosslinking the polymer. The amount of the crosslinking agent may be 0.0001 parts by mass to 15 parts by mass, 0.001 parts by mass to 10 parts by mass, or 0.005 parts by mass to 5 parts by mass, relative to 100 parts by mass of the polymer.

[0045] The reaction temperature when crosslinking the polymer is appropriately set depending on the type, amount, etc. of the crosslinking agent used, but from the viewpoint of sufficiently crosslinking the polymer, it may be 50° C. or higher, 80° C. or higher, or 100° C. or higher, and may be 220° C. or lower, 200° C. or lower, or 180° C. or lower. The reaction temperature when crosslinking the polymer may be 50° C. to 220° C., 80° C. to 200° C., or 100° C. to 180° C.

[0046] The reaction time for crosslinking the polymer is appropriately set depending on the type and amount of the crosslinking agent used, the reaction temperature, etc., but may be 1 to 200 minutes, or 5 to 150 minutes, from the viewpoint of sufficiently crosslinking the polymer.

[0047] After obtaining the crosslinked polymer, a surface crosslinking step of performing surface crosslinking on the crosslinked polymer may be provided. The surface crosslinking can be performed, for example, by adding a crosslinking agent for performing surface crosslinking (surface crosslinking agent) to the crosslinked polymer and allowing it to react.

[0048] The surface crosslinking agent may be a compound having two or more reactive functional groups reactive with the functional group (e.g., carboxyl group) of the crosslinked polymer. The surface crosslinking agent may be the same as or different from the crosslinking agent in the crosslinking step.

[0049] The reactive functional groups of the surface cross-linking agent may be carbonate groups, alcoholic hydroxyl groups, epoxy groups, halogeno groups in haloepoxy compounds, isocyanate groups, oxetanyl groups, oxazoline groups, or combinations thereof. Carbonate groups are considered two reactive functional groups because they can react with two other molecules.

[0050] Examples of surface cross-linking agents having a carbonate group include alkylene carbonates (ethylene carbonate, etc.). Examples of surface cross-linking agents having an alcoholic hydroxyl group include polyol compounds such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin, and hydroxyalkylamide compounds (bis[N,N-di(β-hydroxyethyl)]adipamide, etc.). Examples of surface cross-linking agents having two or more epoxy groups include (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether. Examples of haloepoxy compounds having an epoxy group and a halogeno group include epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin. Examples of surface crosslinking agents having an isocyanate group include 2,4-tolylene diisocyanate and hexamethylene diisocyanate. Examples of surface crosslinking agents having an oxetanyl group include 3-methyl-3-oxetanemethanol, 3-ethyl-3-oxetanemethanol, 3-butyl-3-oxetanemethanol, 3-methyl-3-oxetaneethanol, 3-ethyl-3-oxetaneethanol, and 3-butyl-3-oxetaneethanol.

[0051] The amount of the surface crosslinking agent may be 0.001 parts by mass or more, 0.005 parts by mass or more, or 0.01 parts by mass or more, and may be 5 parts by mass or less, 3 parts by mass or less, or 1 part by mass or less, relative to 100 parts by mass of the crosslinked polymer, from the viewpoint of sufficiently achieving surface crosslinking of the crosslinked polymer. The amount of the crosslinking agent may be 0.001 parts by mass to 5 parts by mass, 0.005 parts by mass to 3 parts by mass, or 0.01 parts by mass to 1 part by mass, relative to 100 parts by mass of the polymer.

[0052] Water-absorbent resin particles (regenerated water-absorbent resin particles) containing the crosslinked polymer are formed by a method including removing water from the obtained crosslinked polymer. When the reaction liquid is an aqueous solution, the water-absorbent resin particles are formed by a method including a drying step of removing water from a block of crosslinked polymer formed by gelling the reaction liquid itself, drying the crosslinked polymer to form a dried product, and a pulverizing step of pulverizing the dried product.

[0053] The method for drying the crosslinked polymer may be a common method such as a squeezing method such as centrifugation, dehydration using an organic solvent, natural drying, heat drying, air drying, freeze drying, or a combination thereof. The heating temperature for drying may be 80°C to 220°C, 90°C to 200°C, or 100°C to 180°C from the viewpoint of efficiently removing water.

[0054] The moisture content of the dried product may be, for example, 20% by mass or less, 10% by mass or less, or 5% by mass or less. The moisture content of the dried product is based on the total amount of the dried product. In other words, it means the proportion of moisture in the dried product. When a crosslinked polymer containing water is heated at 200°C for 2 hours, the difference in mass of the crosslinked polymer before and after heating can be considered to be the moisture content of the dried product.

[0055] Before drying the crosslinked polymer, the crosslinked polymer may be crushed to form a crushed product containing structures of a certain size. By forming a crushed product, water can be efficiently removed. The structures constituting the crushed product can be, for example, elongated structures, granular structures (particles), or a combination thereof. The crushed product may include a plurality of structures having a shape that can pass through a circular hole with a diameter of 10 mm or 7 mm. The elongated structures may be curved, and as long as their maximum width is 10 mm or less, they can be said to have a shape that can pass through a circular hole with a diameter of 10 mm. The granular structures (particles) may be irregular in shape and may have a shape that can pass through a circular hole with a diameter of 10 mm while changing direction. Examples of crushing devices for crushing the crosslinked polymer include kneaders (e.g., pressure kneaders, double-arm kneaders), meat choppers, cutter mills, and farm mills.

[0056] The dried product is pulverized to form water-absorbent resin particles. The pulverization method is not particularly limited. For example, the dried product can be pulverized using a pulverizer such as a centrifugal pulverizer, a roller mill, a stamp mill, a jet mill, a high-speed rotary pulverizer, or a container-driven mill.

[0057] The water-absorbent resin particles obtained by pulverization may be classified. Classification refers to an operation of dividing a particle group (powder) into two or more particle groups having different particle size distributions. A part of the water-absorbent resin particles after classification may be pulverized and classified again.

[0058] The classification method is not particularly limited, and may be, for example, screen classification or air classification. Screen classification is a method of classifying particles on a screen into particles that pass through the meshes of the screen and particles that do not pass through by vibrating the screen. Screen classification can be performed using, for example, a vibrating sieve, a rotary sifter, a cylindrical stirring sieve, a blower sifter, or a rotary shaker. Air classification is a method of classifying particles by utilizing an air flow.

[0059] The median particle size of the crosslinked polymer powder obtained through pulverization and, if necessary, classification may be, for example, 200 μm to 500 μm, or 300 μm to 500 μm. The particle size distribution may be adjusted by mixing two or more powders obtained by classification and having different median particle sizes.

[0060] The centrifuge retention capacity (CRC) of the water-absorbent resin particles may be 15 g / g or more, 20 g / g or more, 25 g / g or more, 30 g / g or more, 35 g / g or more, 40 g / g or more, 45 g / g or more, or 50 g / g or more. The larger the CRC of the water-absorbent resin particles, the better the water retention capacity, and a CRC of 15 g / g or more can be said to have sufficient water absorption capacity. The upper limit of the CRC of the water-absorbent resin particles is not particularly limited, but may be, for example, 70 g / g or less, 60 g / g or less, or 55 g / g or less. The CRC of the water-absorbent resin particles may be 15 g / g to 70 g / g, 15 g / g to 60 g / g, or 15 g / g to 55 g / g. The CRC of the water-absorbent resin particles is a value measured by the method described in the Examples below.

[0061] The soluble content of the water-absorbent resin particles may be 0.2 g / g or less, 0.15 g / g or less, 0.12 g / g or less, 0.1 g / g or less, 0.09 g / g or less, or 0.08 g / g or less. The smaller the soluble content of the water-absorbent resin particles, the more the dissolution of the polymer can be suppressed, and if the soluble content is 0.2 g / g or less, it can be said that the dissolution of the polymer is sufficiently suppressed. The lower limit of the soluble content of the water-absorbent resin particles is not particularly limited, but may be, for example, 0.01 g / g or more, 0.02 g / g or more, or 0.03 g / g or more. The soluble content of the water-absorbent resin particles may be 0.01 g / g to 0.2 g / g, 0.02 g / g to 0.2 g / g, or 0.03 g / g to 0.2 g / g. The soluble content of the water-absorbent resin particles is a value measured by the method described in the Examples below.

[0062] The soluble component index of the water-absorbent resin particles calculated according to the following formula is 9×10 -3 Below, 8 x 10 -3 Below, 7 x 10 -3 Below, 6 x 10 -3 Below, 5.5 x 10 -3 Below, 5 x 10 -3 Below, 4.5 x 10 -3 Below, 4 x 10 -3 Below, 3.9 x 10 -3 Below, 3.8 x 10 -3 Below, 3.7 x 10 -3 Below, 3.6 x 10 -3 or less, or 3.5 x 10 -3 The smaller the soluble component index of the water-absorbent resin particles, the more sufficient the water absorption capacity is, and the more effectively the dissolution of the polymer is suppressed. The soluble component index of the water-absorbent resin particles may be 1×10 or less. -3 That's it, 1.5 x 10 -3 That's it, 2 x 10 -3 That's it, 2.5 x 10 -3 That's it, 3 x 10 -3 That's it, 3.1 x 10 -3 That's it, 3.2 x 10 -3 That's it, 3.3 x 10 -3 That's it, 3.4 x 10 -3 or more, or 3.5 x 10 -3 The soluble component index of the water-absorbent resin particles may be 1×10 or more. -3 ~9 x 10 -3 , 2 × 10-3 ~6 x 10 -3 , or 3 x 10 -3 ~5 x 10 -3 The soluble content index can be expressed by the following formula: soluble content index = soluble content [g / g] / CRC [g / g]

[0063] Fig. 1 is a cross-sectional view showing an example of an absorbent article having an absorbent body containing water-absorbent resin particles. The absorbent article 100 shown in Fig. 1 comprises a water-absorbent sheet 50 having a film-like absorbent body 10, a liquid-permeable sheet 30, and a liquid-impermeable sheet 40.

[0064] The water-absorbent sheet 50 includes an absorbent body 10 containing a powder of water-absorbent resin particles 1, and two core wrap sheets 20a and 20b. The absorbent body 10 is disposed inside the core wrap sheets 20a and 20b. The absorbent body 10 maintains its shape by being sandwiched between the two core wrap sheets 20a and 20b. The core wrap sheets 20a and 20b may consist of two sheets, a single folded sheet, or a single bag. A sheet member that does not have any other components on the outside of the core wrap sheets 20a and 20b that wrap the absorbent body 10 is sometimes referred to as a water-absorbent sheet.

[0065] The absorbent body 10 is a component that mainly contains a powder of water-absorbent resin particles 1 and is retained to have a certain shape. The absorbent body 10 may contain fibrous material 3 in addition to the powder of water-absorbent resin particles 1, or may not contain fibrous material 3. The content of the water-absorbent resin particles 1 in the absorbent body 10 may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, or 90% by mass or more and 100% by mass or less, based on the mass of the absorbent body 10.

[0066] The thickness of the absorbent body 10 may be, for example, 20 mm or less, 15 mm or less, 10 mm or less, 5 mm or less, 4 mm or less, or 3 mm or less, or may be 0.1 mm or more, or 0.3 mm or more. The thickness of the absorbent body 10 may be 0.1 mm or more and 20 mm or less. The mass per unit area of ​​the absorbent body 10 is 1000 g / m 2 Below, 800g / m 2or less than 600 g / m 2 or less, and 2 It may be more than that.

[0067] The fibrous material 3 can be, for example, a cellulosic fiber, a synthetic fiber, or a combination thereof. Examples of cellulosic fibers include comminuted wood pulp, cotton, cotton linters, rayon, and cellulose acetate. Examples of synthetic fibers include polyamide fibers, polyester fibers, and polyolefin fibers. The fibrous material may also be a hydrophilic fiber (e.g., pulp).

[0068] The absorbent 10 may further contain inorganic powder (e.g., amorphous silica), a deodorant, an antibacterial agent, a fragrance, etc. When the water-absorbent resin particles 1 contain inorganic particles, the absorbent 10 may contain inorganic powder in addition to the inorganic particles in the water-absorbent resin particles 1.

[0069] The water-absorbent sheet 50 may further have an adhesive 21 interposed between the core wrap sheet 20a and the absorbent body 10. An adhesive layer may be interposed between the core wrap sheets 20a, 20b on both sides and the absorbent body 10. The adhesive 21 is not particularly limited, and may be, for example, a hot-melt adhesive.

[0070] The core wrap sheets 20a, 20b may be, for example, nonwoven fabrics. The two core wrap sheets 20a, 20b may be the same or different nonwoven fabrics. The nonwoven fabric may be a nonwoven fabric made of short fibers (i.e., staple) (short fiber nonwoven fabric) or a nonwoven fabric made of long fibers (i.e., filaments) (long fiber nonwoven fabric). The staple may have a fiber length of, but is not limited to, typically several hundred millimeters or less.

[0071] The core wrap sheets 20a, 20b may be a thermal bonded nonwoven fabric, an air-through nonwoven fabric, a resin bonded nonwoven fabric, a spunbonded nonwoven fabric, a meltblown nonwoven fabric, an airlaid nonwoven fabric, a spunlace nonwoven fabric, a point bonded nonwoven fabric, or a laminate containing two or more types of nonwoven fabric selected from these.

[0072] The nonwoven fabric used as the core wrap sheets 20a, 20b can be made of synthetic fibers, natural fibers, or a combination thereof. Examples of synthetic fibers include fibers containing synthetic resins selected from polyolefins such as polyethylene (PE) and polypropylene (PP), polyesters such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT) and polyethylene naphthalate (PEN), polyamides such as nylon, and rayon. Examples of natural fibers include fibers containing cotton, silk, hemp, or pulp (cellulose). The fibers forming the nonwoven fabric may be polyolefin fibers, polyester fibers, or a combination thereof. The core wrap sheets 20a, 20b may also be tissue paper.

[0073] The water-absorbent sheet 50 may be used to manufacture various other absorbent articles. Examples of absorbent articles include diapers (e.g., disposable diapers), toilet training pants, incontinence pads, sanitary materials (sanitary napkins, tampons, etc.), sweat pads, pet sheets, portable toilet components, and animal waste disposal materials. The absorbent bodies that make up these absorbent articles often move or deform due to the movements of the user of the absorbent article, etc.

[0074] The liquid-permeable sheet 30 is positioned as the outermost layer on the side into which the liquid to be absorbed penetrates. The liquid-permeable sheet 30 is positioned outside the core wrap sheet 20b while in contact with the core wrap sheet 20b. The liquid-impermeable sheet 40 is positioned as the outermost layer on the opposite side of the absorbent article 100 from the liquid-permeable sheet 30. The liquid-impermeable sheet 40 is positioned outside the core wrap sheet 20a while in contact with the core wrap sheet 20a. The liquid-permeable sheet 30 and the liquid-impermeable sheet 40 have main surfaces that are wider than the main surface of the water-absorbent sheet 50, and the outer edges of the liquid-permeable sheet 30 and the liquid-impermeable sheet 40 extend around the absorbent body 10 and the core wrap sheets 20a, 20b. However, the size relationships among the absorbent body 10, the core wrap sheets 20a, 20b, the liquid-permeable sheet 30, and the liquid-impermeable sheet 40 are not particularly limited and may be appropriately adjusted depending on the intended use of the absorbent article, etc.

[0075] The liquid-permeable sheet 30 may be a nonwoven fabric. The nonwoven fabric used as the liquid-permeable sheet 30 may have appropriate hydrophilicity from the viewpoint of the liquid absorption performance of the absorbent article. From that viewpoint, the liquid-permeable sheet 30 may be a nonwoven fabric having a hydrophilicity of 5 to 200 as measured in accordance with the Pulp and Paper Testing Method No. 68 (2000) of the Paper and Pulp Technology Association. The hydrophilicity of the nonwoven fabric may also be 10 to 150. For details of Pulp and Paper Testing Method No. 68, see, for example, WO2011 / 086843.

[0076] Hydrophilic nonwoven fabrics may be made from fibers with moderate hydrophilicity, such as rayon, or from fibers obtained by hydrophilizing hydrophobic chemical fibers, such as polyolefin and polyester fibers. Methods for obtaining nonwoven fabrics containing hydrophilized hydrophobic chemical fibers include spunbonding a mixture of hydrophobic chemical fibers and a hydrophilizing agent, adding a hydrophilizing agent to the hydrophobic chemical fibers, and impregnating a spunbond nonwoven fabric obtained from hydrophobic chemical fibers with a hydrophilizing agent. Examples of hydrophilizing agents include anionic surfactants such as aliphatic sulfonates and higher alcohol sulfates, cationic surfactants such as quaternary ammonium salts, nonionic surfactants such as polyethylene glycol fatty acid esters, polyglycerin fatty acid esters, and sorbitan fatty acid esters, silicone surfactants such as polyoxyalkylene-modified silicones, and stain release agents made from polyester, polyamide, acrylic, or urethane resins.

[0077] The basis weight (mass per unit area) of the nonwoven fabric used as the liquid-permeable sheet 30 is set to 5 g / m from the viewpoint of imparting good liquid permeability, flexibility, strength, and cushioning properties to the absorbent article, and from the viewpoint of increasing the liquid permeation rate of the absorbent article. 2 ~200g / m 2 , 8 g / m 2 ~150g / m 2 , or 10 g / m 2~100g / m 2 The thickness of the liquid-permeable sheet 30 may be 20 μm to 1400 μm, 50 μm to 1200 μm, or 80 μm to 1000 μm.

[0078] The liquid-impermeable sheet 40 prevents liquid absorbed by the absorbent body 10 from leaking out through the liquid-impermeable sheet 40. The liquid-impermeable sheet 40 may be a resin sheet or a nonwoven fabric. The resin sheet may be a sheet made of a synthetic resin such as polyethylene, polypropylene, or polyvinyl chloride. The nonwoven fabric may be a spunbond / meltblown / spunbond (SMS) nonwoven fabric in which a water-resistant meltblown nonwoven fabric is sandwiched between high-strength spunbond nonwoven fabrics. The liquid-impermeable sheet 40 may be a composite sheet of a resin sheet and a nonwoven fabric (e.g., a spunbond nonwoven fabric or a spunlace nonwoven fabric). The liquid-impermeable sheet 40 may be breathable to reduce stuffiness during wear and to alleviate discomfort to the wearer. For example, a low-density polyethylene (LDPE) resin sheet can be used as the breathable liquid-impermeable sheet 40.

[0079] In order to ensure flexibility and not impair the wearing comfort of the absorbent article, the basis weight (mass per unit area) of the liquid impermeable sheet 40 is 10 g / m 2 ~50g / m 2 may be.

[0080] The present invention will be described in more detail below with reference to examples.

[0081] (Example 1) A commercially available disposable diaper (Merrys Pants, Suhada Sarasa Air Through, L size, manufactured by Kao Corporation) was prepared, and water-absorbent resin particles containing a crosslinked polymer containing acrylic acid and an acrylate salt as monomer units were collected from inside the disposable diaper.

[0082] A reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirrer (a 4L round-bottom cylindrical separable flask equipped with a stirring blade having two stages of four inclined paddle blades with a blade diameter of 50 mm, manufactured by DURAN Co., Ltd.) were prepared. 45 g of water-absorbent resin particles collected from disposable diapers were weighed into the separable flask, and 855 g of ion-exchanged water was added and allowed to stand for 5 minutes to swell the water-absorbent resin particles. Next, 1200 g of a 1.5 mol / kg aqueous sodium hydroxide solution was added to the separable flask, and the internal temperature was maintained at 80 ° C. for 24 hours while stirring at 160 rpm with a stirring blade to cleave the crosslinked structure of the crosslinked polymer of the water-absorbent resin particles. A decomposition liquid (aqueous solution of water-soluble recycled polymer, pH 13) containing a polymer that is a water-absorbent resin solubilized by cleavage of the crosslinked structure was obtained. The weight average molecular weight of the water-soluble recycled polymer was measured using the above-mentioned method, and was found to be Mw = 1,950,000.

[0083] The obtained decomposition liquid was filtered using a filter (UHP-150K, manufactured by ADVANTEC) and an ultrafiltration membrane (molecular weight cutoff: 500,000, manufactured by Nitto Denko Corporation). The residue on the filtration membrane was then dried to obtain 39 g of a water-soluble recycled polymer from the decomposition liquid. Before filtration, the pH of the decomposition liquid was adjusted to 7 using sulfuric acid (special grade, manufactured by Hayashi Pure Chemical Industries, Ltd.) in order to minimize damage to the ultrafiltration membrane.

[0084] 285 g of ion-exchanged water was weighed out into a 500 mL plastic beaker, and the ion-exchanged water in the plastic beaker was stirred at 400 rpm using two paddles (blade diameter 75 mm) attached to a jar tester (MJS-10-700, manufactured by Daido Kogyosho Co., Ltd.). Next, 15 g of a water-soluble recycled polymer was added to the ion-exchanged water, and the mixture was stirred for 60 minutes to prepare a polymer solution, which was a 5% by mass aqueous solution of the water-soluble recycled polymer.

[0085] The prepared polymer solution was stirred at 650 rpm for 20 minutes using a high-speed stirrer (MK-H4 manufactured by Panasonic), and 0.75 g (0.043 mmol) of an aqueous solution containing 1% by mass of ethylene glycol diglycidyl ether as a crosslinking agent was added thereto while stirring for 5 minutes.

[0086] After stirring with a high-speed stirrer, the polymer solution was transferred to a Teflon (registered trademark)-coated tray (20 cm x 16 cm) and heated at 115°C for 60 minutes in an air dryer (FV-320, manufactured by ADVANTEC) to crosslink the water-soluble recycled polymer with the crosslinking agent. As the crosslinking of the water-soluble recycled polymer progressed, the entire polymer solution gelled. A massive gel containing the crosslinked polymer and water was removed from the tray, and the gel was roughly cut into 3 cm squares for efficient drying. The cut gel was transferred back to the tray and dried by heating at 115°C for 120 minutes in an air dryer to obtain a water-soluble recycled polymer crosslinked product.

[0087] The obtained water-soluble recycled polymer crosslinked product was pulverized at 6000 rpm using a centrifugal pulverizer (ZM-2000 manufactured by Retsch) with a 1 mm screen to obtain 11.5 g of recycled water-absorbent resin particles having a median particle size of 384 μm.

[0088] Example 2 The same procedure as in Example 1 was carried out except that 1.2 g (0.069 mmol) of a 1% by mass aqueous solution of ethylene glycol diglycidyl ether was added as a crosslinking agent, to obtain 11.0 g of recycled water-absorbent resin particles having a median particle size of 388 μm.

[0089] Example 3 The same procedure as in Example 1 was carried out except that 7.6 g (2.19 mmol) of a 5 wt % aqueous solution of ethylene glycol diglycidyl ether was added as a crosslinking agent, to obtain 10.8 g of recycled water-absorbent resin particles having a median particle diameter of 396 μm.

[0090] Example 4: A 1-liter beaker equipped with a liquid feed pump and a stirrer (with a fluororesin-coated surface) was prepared. 50.00 g of a 6.0% by weight aqueous solution of sodium polyacrylate (neutralization degree 70 mol%) was added as a polymer solution to the beaker, and the stirrer rotation speed was set to 1000 r / min. 50.00 g of a 70.0% by weight aqueous solution of ethanol was added dropwise to the beaker using a liquid feed pump at a rate of 7.9% by weight / min (10 ml / min) relative to the polymer solution, resulting in a cloudy colloidal solution (polymer dispersion). 1.50 g (0.0086 mmol) of a 0.1% by weight aqueous solution of ethylene glycol diglycidyl ether was added as a crosslinking agent to the beaker.

[0091] A round-bottomed cylindrical separable flask with an inner diameter of 100 mm was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirring blade (with a fluororesin surface coated) having three stages of four inclined paddle blades with a blade diameter of 50 mm as a stirrer. 0.50 g of sucrose stearate ester with an HLB of 3 (HLB: 3, Mitsubishi Chemical Foods Co., Ltd., Ryoto Sugar Ester S-370) was added to this flask as a surfactant, and 0.50 g of maleic anhydride-modified ethylene-propylene copolymer (Mitsui Chemicals, Inc., Hiwax 1105A) was added as a polymer dispersant, and the stirrer rotation speed was set to 500 r / min. 500.00 g of n-heptane was added to this separable flask, the temperature was raised to 85 ° C., and the surfactant and dispersant were dissolved, and the internal temperature was set to 75 ° C. The rotation speed of the stirrer was set to 1000 r / min, and the colloidal solution after the addition of the crosslinking agent was added to this separable flask, and a crosslinking reaction was carried out for 60 minutes. Thereafter, the flask was immersed in an oil bath set to 125°C, and n-heptane and water were evaporated to dryness, and the resulting mixture was passed through a standard sieve with an opening of 300 µm, thereby obtaining 1.14 g of water-absorbent resin particles having a median particle size of 197 µm.

[0092] Example 5 The same procedure as in Example 4 was carried out except that 4.3 g (0.024 mmol) of a 0.1% by mass aqueous solution of ethylene glycol diglycidyl ether was added as a crosslinking agent, to obtain 1.88 g of recycled water-absorbent resin particles having a median particle size of 176 μm.

[0093] Example 6 The same procedure as in Example 4 was carried out except that 0.55 g (0.063 mmol) of a 2.0 mass % aqueous solution of ethylene glycol diglycidyl ether was added as a crosslinking agent, to obtain 1.40 g of recycled water-absorbent resin particles having a median particle size of 150 μm.

[0094] Comparative Example 1 The same procedure as in Example 1 was carried out, except that the aqueous solution containing 1% by mass of ethylene glycol diglycidyl ether was replaced with 7.2 g (2.45 mmol) of a 5% by mass aqueous solution containing calcium chloride dihydrate (special grade, manufactured by Kanto Chemical Co., Ltd.) as a crosslinking agent. The water-soluble recycled polymer was crosslinked via ionic bonds formed by calcium ions. As the crosslinking progressed, the polymer solution became more viscous, but fluidity was maintained and gelation did not occur. No aggregate formation was observed in the polymer solution. The viscous polymer solution was dried in a tray by heating at 115°C for 120 minutes using a blower dryer to obtain a water-soluble recycled polymer crosslinked product. The obtained water-soluble recycled polymer crosslinked product was pulverized using a centrifugal crusher (manufactured by Retsch, ZM-2000) with a 1 mm screen at 6000 rpm to obtain 10.5 g of recycled water-absorbent resin particles having a median particle size of 398 μm.

[0095] (Comparative Example 2) The same operation as in Comparative Example 1 was carried out except that 30 g (10.2 mmol) of a 5 mass % aqueous solution of calcium chloride dihydrate (special grade, manufactured by Kanto Chemical Co., Ltd.) was used as a crosslinking agent, to obtain 10.6 g of recycled water-absorbent resin particles having a median particle size of 378 μm. As the crosslinking proceeded, the formation of aggregates was observed in the polymer solution.

[0096] (Comparative Example 3) The same operation as in Example 1 was carried out, except that the crosslinking agent was changed to 15 g (2.19 mmol) of a 5 mass% aqueous solution of aluminum sulfate (manufactured by Kanto Chemical Co., Ltd., special grade aluminum sulfate), to obtain 11.1 g of recycled water-absorbent resin particles having a median particle diameter of 377 μm.

[0097] (Comparative Example 4) The same operation as in Comparative Example 1 was carried out, except that 30 g (4.38 mmol) of a 5 mass % aqueous solution of aluminum sulfate (Kanto Chemical Co., Ltd., special grade) was used as the crosslinking agent, to obtain 11.2 g of recycled water-absorbent resin particles having a median particle size of 399 μm. As the crosslinking proceeded, the formation of aggregates was observed in the polymer solution.

[0098] Reference Example 1 Water-absorbent resin particles were collected from the disposable diaper used in the Examples (Merry's Pants, Smooth Air Through, L size, manufactured by Kao Corporation).

[0099] <Evaluation Method> The centrifuge retention capacity (CRC), soluble content, soluble content index, and median particle diameter (particle size distribution) of the obtained water-absorbent resin particles were measured according to the following evaluation method. The measurement results of the centrifuge retention capacity (CRC), soluble content, and soluble content index of the water-absorbent resin particles are shown in Table 1. In Table 1, the amount of bonds (mmol) is calculated as the product of the amount (mmol) of the crosslinking agent and the number of functional groups that serve as crosslinking points of the crosslinking agent.

[0100] [Centrifuge Retention Capacity (CRC)] The centrifuge retention capacity (CRC) was measured according to the EDANA method (NWSP 241.0.R2(19)) using the following procedure. The measurement was carried out under an environment of a temperature of 25±2°C and a relative humidity of 50±10%.

[0101] Two 60 mm x 85 mm pieces of nonwoven fabric were heat-sealed together at 5 mm-wide edges along each of three sides to produce a 60 mm x 85 mm nonwoven fabric bag. Approximately 0.2 g of precisely weighed recycled water-absorbent resin particles was placed in the nonwoven fabric bag. The nonwoven fabrics were then heat-sealed together at the open edge to close the nonwoven fabric bag shown in Figure 2.

[0102] A plurality of nonwoven fabric bags containing recycled water-absorbent resin particles were floated on 500 g of physiological saline solution contained in a stainless steel tray (240 mm x 320 mm x 45 mm) without overlapping each other, thereby completely wetting the entire nonwoven fabric bag. One minute after floating the nonwoven fabric bags on the physiological saline solution, the entire nonwoven fabric bag was immersed in the physiological saline solution using a spatula.

[0103] After 30 minutes had passed since the nonwoven fabric bag began to float in the saline solution, i.e., the total time of 1 minute of floating time and 29 minutes of immersion time, the nonwoven fabric bag was removed from the saline solution. The removed nonwoven fabric bag was dehydrated for 3 minutes at a centrifugal force of 250 G using a centrifuge (manufactured by Kokusan Co., Ltd., model number: H-122). After dehydration, the mass Wc [g] of the nonwoven fabric bag, including the mass of the gel, was weighed. The above-mentioned operation was performed on a nonwoven fabric bag that did not contain the recycled water-absorbent resin particles to be measured, and the mass B [g] of the nonwoven fabric bag after dehydration was measured. The CRC [g / g] was calculated according to the following formula. Sc [g] is the precisely weighed value of 0.2 g of the recycled water-absorbent resin particles to be measured. CRC [g / g] = {(Wc - B) - Sc} / Sc

[0104] [Soluble Content, Soluble Content Index] The soluble content of the recycled water-absorbent resin was measured under an environment of 25°C ± 2°C and 50% ± 10% humidity. 500 g of saline solution in a 500 mL beaker was stirred with a stirring bar (cylindrical, 8 mm diameter x 30 mm length, no ring) rotating at 600 rpm. The temperature of the saline solution was 25°C. 2.000 g of recycled water-absorbent resin particles were added, and the dispersion containing the recycled water-absorbent resin particles was stirred for 3 hours. The dispersion was filtered through a 75 μm standard sieve, and the filtrate was recovered. 80 g of the resulting filtrate was weighed into a weighed 100 mL beaker that had been pre-weighed at 140°C. The filtrate in the beaker was heated in a 140°C air-blowing dryer (FV-320, manufactured by ADVANTEC) for 15 hours to remove moisture, and the mass Wa (g) of the remaining solid component was measured. A blank test was carried out in the same manner as above, without adding the recycled water-absorbent resin particles to physiological saline, and the mass Wb (g) of the solid component remaining in the beaker was measured. The soluble component was calculated according to the following formula. Furthermore, the soluble component index was calculated from the above-mentioned CRC and soluble component according to the following formula: soluble component [g / g] = ((Wa - Wb) / 80) x 500 / 2 soluble component index = soluble component [g / g] / CRC [g / g]

[0105] [Median Particle Diameter (Particle Size Distribution)] The median particle diameter of recycled water-absorbent resin particles was measured under normal temperature and humidity conditions using the following procedure. Using a continuous, fully automatic ultrasonic vibration sieving measuring instrument (Robot Sifter RPS-205, manufactured by Seishin Enterprise Co., Ltd.), the particle size distribution of 2 g of recycled water-absorbent resin particles was measured using standard sieves with JIS mesh sizes of 850 μm, 600 μm, 500 μm, 425 μm, 300 μm, 250 μm, and 180 μm, as well as a tray. The recycled water-absorbent resin particles were placed on the top standard sieve and classified by shaking for 5 minutes. By integrating the particle masses on the standard sieves in descending order of particle size, the relationship between the mesh size of the standard sieves and the integrated value of the mass percentage of the particles remaining on the standard sieves was plotted on logarithmic probability paper. The plots on the probability paper were connected with a straight line to obtain the particle size corresponding to a cumulative mass percentage of 50 mass % as the median particle size.

[0106]

[0107] It was shown that the absorbent articles using the recycled water-absorbent resin particles obtained in the examples had high water absorption performance and could suppress the dissolution of the polymer.

[0108] 1...water-absorbent resin particles, 10...absorbent body, 20a, 20b...core wrap sheet, 30...liquid-permeable sheet, 40...liquid-impermeable sheet, 50...water-absorbent sheet, 100...absorbent article, 150...heat-sealed portion, 200...nonwoven fabric bag.

Claims

1. A method for producing water-absorbent resin particles containing a crosslinked polymer, comprising: a preparation step of preparing a polymer solution containing a polymer and a solvent; and a crosslinking step of forming the crosslinked polymer by crosslinking the polymer via a covalent bond.

2. The method according to claim 1, wherein the preparation step includes cleaving a crosslinked structure of a crosslinked polymer contained in a recycled water absorbent resin containing a crosslinked polymer to obtain the polymer.

3. The method according to claim 2, wherein the preparation step further comprises recovering the recycled water-absorbent resin from an absorbent article.

4. The method according to any one of claims 1 to 3, wherein the weight average molecular weight of the polymer is 100,000 or more.

5. The method according to any one of claims 1 to 3, wherein the polymer solution is gelled in the crosslinking step.

6. The method according to any one of claims 1 to 3, wherein the polymer has a carboxyl group, and the polymer is crosslinked by a reaction between the carboxyl group and a crosslinking agent and / or a reaction between the carboxyl groups themselves.

7. The method according to any one of claims 1 to 3, wherein the polymer is crosslinked via at least one group selected from the group consisting of a carboxylate group, a thioester group, an amide group, an acid anhydride group, an oxyalkylene group, and an oxyarylene group.

8. The soluble component index expressed by the following formula is 2 x 10 -3 ~6×10 -3 Water absorbent resin particles, where the soluble component index is the soluble component (g / g) / the CRC (g / g).

9. An absorbent comprising the water-absorbent resin particles according to claim 8.

10. An absorbent article comprising the absorbent body according to claim 9.

Citation Information

Patent Citations

  • New polymer obtained from water absorbent polymer and use thereof

    JP2012219172A

  • Processing method of used sanitary articles

    JP2020049398A

  • Method for recycling water absorbent resin

    WO2021162082A1

Cited By

  • Method for producing solid polymer and method for producing water-absorbent resin particles

    WO2025205319A1

  • Method for producing polymer dispersion and method for producing water-absorbing resin particle

    WO2025205320A1