Transmission circuit board and laminated film
The transmission circuit board design with a laminated film structure and specific tetrafluoroethylene polymer-based resin and polyimide layer thickness ratios addresses the challenge of high-frequency transmission loss, achieving improved electrical and mechanical properties for advanced mobile communication devices.
Patent Information
- Application Number
- PCT/JP2024/014066
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-04-05
- Publication Date
- 2024-10-17
AI Technical Summary
Current printed circuit board materials face challenges in achieving low transmission loss and excellent electrical properties at high frequencies due to limitations in thermal conductivity, linear expansion coefficient, and dielectric properties.
A transmission circuit board design incorporating a laminated film structure with specific thickness ratios of tetrafluoroethylene polymer-based resin layers and polyimide layers, optimized to enhance mechanical and electrical properties while minimizing transmission loss in high frequency ranges.
The proposed solution effectively reduces transmission loss and maintains excellent electrical properties in high frequency ranges, making it suitable for advanced mobile communication devices.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Transmission circuit board and laminated film
[0001] The present invention relates to a transmission circuit board and a laminate film. More specifically, the present invention relates to a transmission circuit board having low transmission loss even in the high frequency range, and a laminate film constituting such a transmission circuit board and having a resin layer containing a tetrafluoroethylene-based polymer.
[0002] In recent years, in order to cope with the increasing speed and frequency of mobile communication devices such as mobile phones, materials with high thermal conductivity, low linear expansion coefficient, low dielectric constant and low dielectric loss tangent are required for printed circuit boards of communication devices, and tetrafluoroethylene-based polymers with low dielectric constant and low dielectric loss tangent have attracted attention. For example, Patent Document 1 discloses a three-layer film in which a polyimide film is used as a base film and a tetrafluoroethylene-based polymer layer is provided on each side of the base film.
[0003] International Publication No. 2015 / 080260
[0004] The three-layer film proposed in Patent Document 1 possesses the mechanical properties of polyimide and the electrical properties and heat resistance of tetrafluoroethylene-based polymers, making it useful as a material applicable to electrical and electronic fields such as printed circuit boards and wire coatings. The inventors conducted research to expand the application fields of such films and discovered that, in a film having a polyimide base film and a resin layer containing a tetrafluoroethylene-based polymer, transmission loss in the high-frequency range is improved when both layers are within a specific thickness range and the thickness of the resin layer containing the tetrafluoroethylene-based polymer is set to a specific ratio. They then found that this film can be effectively applied to the production of transmission circuit boards, leading to the present invention. The object of the present invention is to provide a transmission circuit board that exhibits low transmission loss and excellent electrical properties even in the high-frequency range, and a laminate film comprising such a transmission circuit board and having a resin layer containing a tetrafluoroethylene-based polymer.
[0005] The present invention has the following aspects: [1] A transmission circuit board comprising a first laminate film, a metal pattern layer, and a second laminate film laminated in this order, the first laminate film comprising a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer laminated in this order, and the second laminate film comprising a third resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a fourth resin layer containing a tetrafluoroethylene-based polymer laminated in this order, the total thickness of the first laminate film, the metal pattern layer, and the second laminate film being greater than 150 μm and not greater than 400 μm, where S is the total thickness and F is the proportion of the total thickness of the third resin layer and the fourth resin layer to S, and the thickness S and the proportion F satisfy the following formula (1): proportion F ≧ 43872 × (thickness S). -2.14...(1) [2] The transmission circuit board of [1], wherein the tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether). [3] The transmission circuit board of [1] or [2], further comprising a metal layer on one or both outermost layers. [4] A transmission circuit board in which a first laminate film, a metal pattern layer, and a second laminate film are laminated in this order, the first laminate film having a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer laminated in this order, and the second laminate film has a third resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a fourth resin layer containing a tetrafluoroethylene-based polymer laminated in this order, the ratio of the total thickness of the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer to the total thickness of the first laminate film, the metal pattern layer, and the second laminate film is more than 50% and not more than 75%, and the total thickness is more than 150 μm and not more than 400 μm. [5] The transmission circuit board of [4], wherein the tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether). [6] The transmission circuit board of [4] or [5], further comprising a metal layer on one or both outermost layers. [7] A laminated film comprising a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer laminated in this order, wherein the total thickness of the first resin layer, the polyimide layer, and the second resin layer is more than 50 μm and 200 μm or less, and wherein, where Sa is the total thickness and Fa is the ratio of the total thickness of the first resin layer and the second resin layer to the thickness Sa, the thickness Sa and the ratio Fa satisfy the following formula (11): Ratio Fa ≧ 43872 × (thickness Sa) -2.14...(11) [8] The laminate film of [7], wherein the thicknesses of the first resin layer and the second resin layer are each more than 20 μm and not more than 100 μm, and the thickness of the polyimide layer is not more than 50 μm. [9] The laminate film of [7] or [8], wherein the tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether).
[10] The laminate film of any of [7] to [9], wherein the tetrafluoroethylene-based polymer is a heat-fusible tetrafluoroethylene-based polymer having a carbonyl group-containing group.
[11] A laminate film comprising a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer laminated in this order, wherein the total thickness of the first resin layer, the polyimide layer, and the second resin layer is more than 50 μm and not more than 200 μm, and wherein the proportion of the combined thickness of the first resin layer and the second resin layer to the total thickness is more than 50% and not more than 75%.
[12] The laminate film of
[11] , wherein the thickness of the first resin layer and the second resin layer is each more than 20 μm and not more than 100 μm, and the thickness of the polyimide layer is not more than 50 μm.
[13] The laminate film of
[11] or
[12] , wherein the tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether).
[14] The laminate film of any of
[11] to
[13] , wherein the tetrafluoroethylene-based polymer is a heat-meltable tetrafluoroethylene-based polymer having a carbonyl group-containing group.
[0006] According to the present invention, there are provided a transmission circuit board which has small transmission loss even in the high frequency range and excellent electrical properties, and a laminate film which constitutes such a transmission circuit board and has a resin layer containing a tetrafluoroethylene-based polymer.
[0007] The following terms have the following meanings. "Average particle size (D50)" is the volume-based cumulative 50% diameter of particles determined by laser diffraction / scattering. That is, particle size distribution is measured by laser diffraction / scattering, and a cumulative curve is calculated assuming the total volume of the particle population to be 100%. The particle size is the particle size at the point on the cumulative curve where the cumulative volume is 50%. The D50 of particles is determined by dispersing the particles in water and analyzing them by laser diffraction / scattering using a laser diffraction / scattering particle size distribution analyzer (LA-920, manufactured by Horiba, Ltd.). "Melting temperature" is the temperature corresponding to the maximum value of the melting peak of the polymer measured by differential scanning calorimetry (DSC). "Glass transition temperature (Tg)" is a value measured by analyzing the polymer by dynamic mechanical analysis (DMA). "Viscosity" is determined by measuring the composition using a Brookfield viscometer at 25°C and a rotation speed of 30 rpm. The measurement is repeated three times, and the average value of the three measurements is used. "Thixotropy ratio" refers to the viscosity η of a composition measured at a rotation speed of 30 rpm. 1 The viscosity η measured at a rotation speed of 60 rpm 2 The viscosity is calculated by dividing the viscosity by the average value of the three measurements. Each viscosity measurement is repeated three times, and the average of the three measurements is used. The "unit" in a polymer means an atomic group based on a monomer formed by polymerization of the monomer. The unit may be a unit formed directly by the polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by treating the polymer. Hereinafter, a unit based on monomer a will also be simply referred to as a "monomer a unit."
[0008] The first transmission circuit board of the present invention (hereinafter also referred to as "the present transmission circuit board 1") comprises a first laminate film, a metal pattern layer, and a second laminate film laminated in this order, the first laminate film comprising a first resin layer containing a tetrafluoroethylene-based polymer (hereinafter also referred to as "F polymer"), a polyimide layer, and a second resin layer containing the F polymer laminated in this order, and the second laminate film comprising a third resin layer containing the F polymer, a polyimide layer, and a fourth resin layer containing the F polymer laminated in this order, the total thickness of the first laminate film, the metal pattern layer, and the second laminate film is greater than 150 μm and not more than 400 μm, and where the total thickness is thickness S and the proportion of the total thickness of the third resin layer and the fourth resin layer to thickness S is proportion F, thickness S and proportion F satisfy the following formula (1): proportion F ≧ 43872 × (thickness S) -2.14 ...(1)
[0009] The second transmission circuit board (hereinafter also referred to as "the present transmission circuit board 2") of the present invention is a transmission circuit board in which a first laminate film, a metal pattern layer, and a second laminate film are laminated in this order, the first laminate film having a first resin layer containing an F polymer, a polyimide layer, and a second resin layer containing an F polymer laminated in this order, the second laminate film having a third resin layer containing an F polymer, a polyimide layer, and a fourth resin layer containing an F polymer laminated in this order, the ratio of the total thickness of the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer to the total thickness of the first laminate film, the metal pattern layer, and the second laminate film is more than 50% and not more than 75%, and the total thickness is more than 150 μm and not more than 400 μm. Note that, hereinafter, the present transmission circuit board 1 and the present transmission circuit board 2 may be collectively referred to as "the present transmission circuit board."
[0010] The first laminate film of the present invention (hereinafter also referred to as "the present laminate film 1") is a laminate film in which a first resin layer containing an F polymer, a polyimide layer, and a second resin layer containing an F polymer are laminated in this order, the total thickness of the first resin layer, the polyimide layer, and the second resin layer is more than 50 μm and 200 μm or less, and where the total thickness is Sa and the proportion of the total thickness of the first resin layer and the second resin layer to the thickness Sa is Fa, the thickness Sa and the proportion Fa satisfy the following formula (11): proportion Fa ≧ 43872 × (thickness Sa) -2.14 ...(11)
[0011] The second laminate film of the present invention (hereinafter also referred to as "the present laminate film 2") comprises a first resin layer containing an F polymer, a polyimide layer, and a second resin layer containing an F polymer laminated in this order, the total thickness of the first resin layer, the polyimide layer, and the second resin layer is more than 50 μm and not more than 200 μm, and the ratio of the total thickness of the first resin layer and the second resin layer to the total thickness is more than 50% and not more than 75%. Note that, hereinafter, the present laminate film 1 and the present laminate film 2 may be collectively referred to as the "present laminate film."
[0012] The present transmission circuit board preferably comprises the present laminate film, a metal pattern layer, and another present laminate film laminated in this order, and has excellent physical properties such as mechanical properties, heat resistance, and electrical properties (low linear expansion coefficient, low dielectric constant, and low dielectric loss tangent) based on the polyimide layer and the resin layer containing F polymer possessed by each laminate film layer, and has small transmission loss, particularly in the high frequency range.
[0013] In a three-layer laminate film having a first resin layer containing an F polymer, a polyimide layer, and a second resin layer containing an F polymer laminated in that order, the following considerations have been made regarding the thickness of each layer. Specifically, the polyimide layer is made to have a certain thickness in order to ensure mechanical properties such as the foldability of the laminate film. Meanwhile, the thicknesses of the first and second resin layers are made equal to each other in order to suppress warpage and ensure dimensional stability, due to the high linear expansion coefficient of the F polymer. Furthermore, the thicknesses of the first and second resin layers are made as thin as possible within a range that ensures heat resistance and electrical properties in order to reduce the overall thickness of the printed circuit board. However, the inventors' studies have found that, in a laminate film having such a layered structure, even if the overall thickness of the laminate film is within a predetermined range and the sum of the thicknesses of the first and second resin layers is equal to or greater than a predetermined power of the overall thickness of the laminate film, in other words, even if the thickness of the F polymer-containing layer accounts for a large proportion of the overall thickness of the laminate film, a laminate film, i.e., laminate film 1, can be obtained that not only has the required mechanical properties but also exhibits more advanced electrical properties.
[0014] Furthermore, the inventors unexpectedly discovered that the ratio of the total thickness of the first resin layer and the second resin layer to the total thickness of the first resin layer, the polyimide layer, and the second resin layer (i.e., the thickness of the entire laminate film) is important from the viewpoint of improving the transmission loss of the laminate film in the high frequency range. The inventors also discovered that by setting the total thickness and the ratio of the total thickness of the first resin layer and the second resin layer to the total thickness within a specific range, a laminate film can be obtained that not only suppresses warping and has excellent mechanical properties such as heat resistance and bendability, and electrical properties, but also reduces transmission loss, i.e., laminate film 2. Furthermore, the inventors also discovered that this effect is significantly exhibited when the first resin layer and the second resin layer contain a specific F polymer, as described below.
[0015] The F polymer constituting the present laminated film is a polymer containing units (hereinafter also referred to as "TFE units") based on tetrafluoroethylene (hereinafter also referred to as "TFE"). The F polymer is preferably heat-meltable. Here, a heat-meltable polymer means a polymer that has a temperature at which the melt flow rate is 1 to 1000 g / 10 min under a load of 49 N. The melting temperature of the F polymer is preferably 200°C or higher, more preferably 260°C or higher. The melting temperature of the F polymer is preferably 325°C or lower, more preferably 320°C or lower.
[0016] The glass transition temperature of the F polymer is preferably 60°C or higher, more preferably 75°C or higher. The glass transition temperature of the F polymer is preferably 120°C or lower, more preferably 100°C or lower. The fluorine content of the F polymer is preferably 70% by mass or higher, more preferably 72 to 76% by mass. The surface tension of the F polymer is preferably 16 to 26 mN / m. The surface tension of the F polymer can be measured by placing a droplet of a mixture for wetting tension testing specified in JIS K 6768 (manufactured by Wako Pure Chemical Industries, Ltd.) on a flat plate made of the F polymer.
[0017] F polymer is preferably the polymer (ETFE) that comprises TFE unit and ethylene-based unit, the polymer that comprises TFE unit and propylene-based unit, the polymer (PFA) that comprises TFE unit and perfluoro(alkyl vinyl ether) (PAVE)-based unit (PAVE unit), the polymer (FEP) that comprises TFE unit and hexafluoropropylene-based unit, more preferably PFA and FEP, and even more preferably PFA.These polymers may further comprise units that are based on other comonomers.PAVE is preferably CF 2 = CFOCF 3 , C.F. 2 = CFOCF 2 CF 3 and CF 2 = CFOCF 2 CF 2 CF 3 (hereinafter also referred to as "PPVE") is preferred, and PPVE is more preferred.
[0018] The F polymer preferably has an oxygen-containing polar group, more preferably a hydroxyl group-containing group or a carbonyl group-containing group, and even more preferably a carbonyl group-containing group. In this case, the adhesion of the first resin layer and the second resin layer in the present laminate film to the polyimide layer is likely to be enhanced, and the adhesion of the outermost surface of the present laminate film is also likely to be improved. Furthermore, the present laminate film is likely to have excellent physical properties such as heat resistance and electrical properties (low linear expansion coefficient, low dielectric constant, and low dielectric loss tangent), and the transmission loss in the high-frequency range of a transmission circuit board formed therefrom is likely to be reduced. The hydroxyl group-containing group is preferably a group containing an alcoholic hydroxyl group, such as -CF 2 CH 2 OH and -C(CF 3 ) 2 OH is more preferred. The carbonyl group-containing group is a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (—OC(O)NH 2 ), acid anhydride residue (-C(O)OC(O)-), imide residue (-C(O)NHC(O)-, etc.), formyl group, halogenoformyl group, urethane group (-NHC(O)O-), carbamoyl group (-C(O)-NH 2 ), ureido group (-NH-C(O)-NH 2 ), an oxamoyl group (—NH—C(O)—C(O)—NH 2 ) and carbonate group (—OC(O)O—), and acid anhydride residues are more preferred. When the F polymer has an oxygen-containing polar group, the number of oxygen-containing polar groups in the F polymer is 1×10 6 The number per unit is preferably 10 to 5000, more preferably 100 to 3000. The number of oxygen-containing polar groups in the F polymer can be quantified by the composition of the polymer or the method described in WO 2020 / 145133.
[0019] The oxygen-containing polar group may be contained in a unit derived from a monomer in the F polymer, or may be contained in a terminal group of the main chain of the F polymer, the former being preferred. Examples of the latter include an F polymer having an oxygen-containing polar group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., and an F polymer obtained by subjecting an F polymer to plasma treatment or ionizing radiation treatment.
[0020] The F polymer is preferably a polymer (1) containing TFE units and PAVE units, with 2.0 to 5.0 mol% of PAVE units relative to the total units, and having no oxygen-containing polar group, or a polymer (2) containing TFE units and PAVE units and having an oxygen-containing polar group. The use of such an F polymer facilitates the formation of spherulites with a relatively small radius. Therefore, the first resin layer and the second resin layer in the laminate film have high surface smoothness and further improved adhesion to the polyimide layer.
[0021] The polymer (1) is preferably composed of only TFE units and PAVE units, and more preferably contains more than 2.5 mol% and not more than 5.0 mol% of PAVE units based on the total units. The term "polymer (1) having no oxygen-containing polar group" means that the number of carbon atoms constituting the polymer main chain is 1 × 10 6 This means that the number of oxygen-containing polar groups possessed by the polymer is less than 500 per unit. The number of the oxygen-containing polar groups is preferably 100 or less, more preferably less than 50. The lower limit of the number of the oxygen-containing polar groups is 1. The polymer (1) may be produced using a polymerization initiator or chain transfer agent that does not generate an oxygen-containing polar group as the terminal group of the polymer chain, or may be produced by fluorinating an F polymer having an oxygen-containing polar group (such as an F polymer having an oxygen-containing polar group derived from a polymerization initiator at the terminal group of the polymer main chain). Examples of fluorination treatment methods include methods using fluorine gas (see JP 2019-194314 A, etc.).
[0022] Polymer (2) is preferably a heat-fusible F polymer having a carbonyl group-containing group containing TFE units and PAVE units, and more preferably a polymer containing TFE units, PAVE units, and units based on a monomer having a carbonyl group-containing group, and containing these units in the following order, 90 to 99 mol%, 0.99 to 9.97 mol%, and 0.01 to 3 mol%, based on the total units. Specific examples of such F polymers include the polymers described in WO 2018 / 16644. Preferred monomers having a carbonyl group-containing group are itaconic anhydride, citraconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH"), with NAH being more preferred.
[0023] The polyimide layer constituting the present laminate film is preferably formed from a polyimide base film (hereinafter also referred to as "polyimide film"). The polyimide film preferably has high yield strength, specifically, a stress at 5% strain of 180 MPa or more and 500 MPa or less. The polyimide film is also preferably resistant to plastic deformation, specifically, a stress at 15% strain of 225 MPa or more and 580 MPa or less. When the polyimide layer constituting the present laminate film is a polyimide film having the above-mentioned properties, the absolute value of the linear expansion coefficient of the present laminate film is easily sufficiently reduced, and warping can be suppressed. The tensile modulus of the polyimide film at 320°C is preferably 0.2 GPa or more and 10 GPa or less, from the viewpoint of the processability and flexibility of the present laminate film.
[0024] In this laminate film, a first resin layer, a polyimide layer, and a second resin layer containing an F polymer are laminated in this order. It is preferable that the first resin layer and the polyimide layer, and the polyimide layer and the second resin layer, are in direct contact with each other. That is, it is preferable that the resin layers are directly formed (laminated) on both surfaces of the polyimide film without surface treatment using a silane coupling agent, adhesive, or the like. In this case, the physical properties of the F polymer and polyimide layer of this laminate film are more likely to be exhibited. Furthermore, in this laminate film, due to the above-mentioned configuration, high adhesion between the polyimide layer and the resin layer is easily exhibited even when the polyimide layer and the resin layer are in direct contact with each other.
[0025] The total thickness of the first resin layer, polyimide layer, and second resin layer of the present laminate film is more than 50 μm and not more than 200 μm. The total thickness is preferably 65 μm or more, more preferably 80 μm or more. The total thickness is preferably 180 μm or less, more preferably 160 μm or less. The thicknesses of the first resin layer and the second resin layer are each preferably more than 20 μm and not more than 100 μm. The thicknesses of the first resin layer and the second resin layer are each more preferably 25 μm or more, even more preferably more than 25 μm, and particularly preferably 30 μm or more. The thicknesses are each more preferably 75 μm or less, even more preferably 65 μm or less, and particularly preferably 60 μm or less. The thicknesses of the first resin layer and the second resin layer may be different, but are preferably equal. In this case, the linear expansion coefficients of the two resin layers become closer, making the present laminate film less prone to warping.
[0026] The thickness of the polyimide layer is preferably 15 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. The thickness of the polyimide layer is preferably 50 μm or less, more preferably 40 μm or less. The thicknesses of the present laminate film, the polyimide film constituting the polyimide layer, the first resin layer, and the second resin layer are measured using a contact thickness gauge DG-525H (manufactured by Ono Sokki Co., Ltd.) with a probe AA-026 (Φ10 mm, SR7).
[0027] In the present laminate film, the ratio of the combined thickness of the first resin layer and the second resin layer to the total thickness is more than 50% and not more than 75%. This ratio is preferably 55% or more, more preferably 60% or more. This ratio is preferably 72% or less, more preferably 70% or less. The ratio of the combined thickness of the first resin layer and the second resin layer to the thickness of the polyimide layer in the present laminate film is preferably more than 1 and not more than 2. In this case, the physical properties of the polyimide film and the electrical properties of the F polymer, such as low dielectric constant and low dielectric loss tangent, and low water absorption, are easily balanced. Furthermore, warping and peeling of the present laminate film are easily suppressed, and transmission loss in the high-frequency range is easily improved.
[0028] The content of the F polymer in each of the first and second resin layers is preferably 80% by mass or more, more preferably 90% by mass or more. The respective contents may be 100% by mass or less. Oxygen-containing polar groups are preferably present on the surfaces of the first and second resin layers (the surfaces opposite the polyimide film). The presence of oxygen-containing polar groups on the surface of the layer increases adhesion, improving the adhesive strength between the film and metal foil or other components bonded to the surface. Such oxygen-containing polar groups are preferably hydroxyl- or carbonyl-containing groups. Examples of methods for introducing oxygen-containing polar groups into the surfaces of the first and second resin layers include using an F polymer having oxygen-containing polar groups, or performing surface treatments such as corona discharge treatment, plasma treatment, UV ozone treatment, excimer treatment, chemical etching, and silane coupling treatment on the surfaces of the first and second resin layers to introduce oxygen-containing polar groups.
[0029] The dielectric constant (relative permittivity) of the present laminate film is preferably 2.0 to 3.0. The dielectric loss tangent of the present laminate film is preferably 0.0001 to 0.003. The dielectric loss tangent of the present laminate film is preferably less than 0.003, more preferably 0.0025 or less, and even more preferably 0.002 or less.
[0030] The absolute value of the linear expansion coefficient of the present laminate film is preferably 30 ppm / °C or less, more preferably 15 ppm / °C or less. In this case, warping of the present laminate film is effectively prevented regardless of the temperature of the atmosphere in which the present laminate film is placed. The lower limit of the absolute value of the linear expansion coefficient of the present laminate film is 0 ppm / °C. The peel strength of the present laminate film is preferably 10 N / cm or more, more preferably 15 N / cm or more. In this case, the present laminate film is suitable for use as a printed circuit board material or a coating material for metal conductors (coating materials for electric wires, etc.). The upper limit of the peel strength of the present laminate film is 100 N / cm. The water absorption of the present laminate film is preferably 0.1% or less. In this case, the present laminate film is more resistant to water vapor permeation and exhibits excellent insulation properties over a long period of time, making it particularly suitable for use as a coating material for metal conductors. The water absorption is determined in accordance with ASTM D570.
[0031] The first and second resin layers in the present laminate film are preferably formed from a resin film containing an F polymer. Specifically, the present laminate film can be produced by disposing the resin films containing an F polymer that will become the first and second resin layers on both surfaces of a polyimide base film and laminating them preferably by hot pressing to form the first resin layer, the polyimide layer, and the second resin layer.
[0032] The first and second resin layers in the present laminate film are preferably formed from a liquid composition containing F polymer particles (hereinafter also referred to as "F particles") and a dispersion medium. Specifically, the present laminate film can be produced by applying a liquid composition containing F particles and a dispersion medium (hereinafter also referred to as "the present liquid composition") to both surfaces of a polyimide base film (hereinafter also referred to as "polyimide film") and heating the applied composition to form the first and second resin layers.
[0033] The F particles preferably have an average particle diameter (D50) of 0.3 μm or more and less than 10 μm. The D50 of the F particles is preferably 0.5 μm or more, more preferably 1.0 μm or more. The D50 of the F particles is preferably less than 10 μm, more preferably 8 μm or less. In this case, the liquid composition is likely to have excellent dispersibility and processability, and the resin layer formed from the liquid composition is likely to have excellent physical properties such as heat resistance and electrical properties (low linear expansion coefficient, low dielectric constant, and low dielectric dissipation factor), as well as excellent surface appearance. The F particles are preferably particles containing an F polymer and are made of an F polymer. One type of F particle may be used, or two or more types may be used.
[0034] The dispersion medium contained in the liquid composition is preferably at least one selected from the group consisting of water, amides, ketones, and esters. Examples of amides include N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylpropanamide, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-diethylformamide, hexamethylphosphoric triamide, and 1,3-dimethyl-2-imidazolidinone. Examples of ketones include acetone, methyl ethyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl n-pentyl ketone, methyl isopentyl ketone, 2-heptanone, cyclopentanone, cyclohexanone, and cycloheptanone. Examples of the ester include methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, ethyl 3-ethoxypropionate, γ-butyrolactone, and γ-valerolactone.
[0035] The liquid composition may further contain a surfactant. The surfactant is preferably a nonionic surfactant. Examples of nonionic surfactants include glycol-based surfactants, acetylene-based surfactants, silicone-based surfactants, and fluorine-based surfactants.
[0036] The liquid composition may further contain inorganic particles. Examples of inorganic particles include silicon compounds such as quartz powder, silica, wollastonite, talc, silicon nitride, silicon carbide, and mica; nitrogen compounds such as boron nitride and aluminum nitride; metal oxides such as aluminum oxide, zinc oxide, titanium oxide, cerium oxide, beryllium oxide, magnesium oxide, nickel oxide, vanadium oxide, copper oxide, iron oxide, and silver oxide; carbon fibers; carbon allotropes such as graphite, graphene, and carbon nanotubes; and metals such as silver and copper. One type of inorganic particle may be used, or two or more types may be used in combination.
[0037] The liquid composition may further contain another resin different from the F polymer. Such another resin may be contained in the liquid composition as non-hollow particles, or may be dissolved or dispersed in a liquid dispersion medium (hereinafter also referred to as "liquid dispersion medium"), such as a liquid compound constituting the liquid composition. Examples of the other resin include polyester resins such as liquid crystalline aromatic polyesters, polyimide resins, polyamideimide resins, epoxy resins, maleimide resins, urethane resins, polyphenylene ether resins, polyphenylene oxide resins, and polyphenylene sulfide resins. The other resin is preferably a polyimide or a precursor thereof, and more preferably at least one polyimide or precursor thereof selected from the group consisting of aromatic polyimides, aromatic polyamic acids, aromatic polyamideimides, and aromatic polyamideimide precursors. The polyimide or precursor thereof is preferably contained in the liquid composition as a varnish dissolved in the liquid dispersion medium. When the liquid composition further contains a polyimide or a precursor thereof, the content of the polyimide or precursor thereof relative to the F particles is preferably 1 to 25% by mass.
[0038] The present liquid composition may further contain additives such as a thixotropic agent, a viscosity modifier, an antifoaming agent, a dehydrating agent, a plasticizer, a weathering agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a whitening agent, a colorant, a conductive agent, a mold release agent, and a flame retardant.
[0039] The content of F particles in the present liquid composition is preferably 25% by mass or more, more preferably 30% by mass or more. The content of F particles is preferably 75% by mass or less, more preferably 60% by mass or less. The viscosity of the present liquid composition is preferably 10 mPa·s or more, more preferably 100 mPa·s or more. The viscosity of the present liquid composition is preferably 10,000 mPa·s or less, more preferably 3,000 mPa·s or less. In this case, the present liquid composition has excellent coatability and is easy to form a resin layer of any desired thickness. Furthermore, the present liquid composition having a viscosity within this range is easy to highly express the physical properties of the F polymer in the resin layer formed therefrom.
[0040] In preparing the present laminated film, the present liquid composition is preferably applied to both surfaces of a polyimide film to form coating layers of the present liquid composition on both surfaces of the polyimide film. Examples of methods for applying the present liquid composition include coating, droplet discharging, and immersion, with roll coating, knife coating, bar coating, die coating, and spraying being preferred.
[0041] Next, the polyimide film having the coating layer is heated to remove the liquid compound that constitutes the liquid composition. Heating to remove the liquid compound is preferably performed at 100 to 200°C for 0.1 to 30 minutes. In this heating, the liquid compound does not need to be completely removed; it is sufficient to remove it to the extent that the layer formed by the packing of the F particles can maintain a self-supporting film. Furthermore, during heating, air may be blown onto the film to promote removal of the liquid compound by air drying. Heating to bake the F polymer is preferably performed at a temperature above the melting temperature of the F polymer, specifically at 340 to 400°C for 0.1 to 30 minutes.
[0042] Examples of heating devices for each heating method include an oven and a ventilated drying furnace. The heat source in the device may be a contact heat source (hot air, hot plate, etc.) or a non-contact heat source (infrared, etc.). Each heating method may be performed under normal pressure (atmospheric pressure) or under reduced pressure. The atmosphere for each heating method may be either an air atmosphere or an inert gas atmosphere (helium gas, neon gas, argon gas, nitrogen gas, etc.).
[0043] The first and second resin layers are formed by applying the liquid composition to a polyimide film and heating the film. These steps may be performed once or twice or more times. For example, the liquid composition may be applied to the surface of a polyimide film to form a coating layer, a resin layer may be formed by heating, and a second resin layer may be formed by heating. Alternatively, the liquid composition may be applied to the surface of a polyimide film to form a coating layer, and after the liquid compound is removed by heating, the liquid composition may be applied to the surface of the coating layer and a resin layer may be formed by heating. In this manner, the present laminate film is obtained, having resin layers containing an F polymer on both surfaces of the polyimide film.
[0044] When the liquid composition contains a polyimide or a precursor thereof as a resin other than the F polymer, it is preferred that the polyimide component derived from the polyimide or the precursor thereof be concentrated on the polyimide layer side of each of the first and second resin layers, thereby improving the adhesion between the first and second resin layers and the polyimide layer, thereby improving the physical properties of both layers and reducing transmission loss in the high-frequency range.
[0045] The dielectric constant of the first resin layer and the second resin layer is preferably 2.4 or less, more preferably 2.0 or less. The dielectric constant is preferably greater than 1.0. The dielectric dissipation factor of the first resin layer and the second resin layer is preferably 0.0022 or less, more preferably 0.0020 or less. The dielectric dissipation factor is preferably greater than 0.0010. The thermal conductivity of the first resin layer and the second resin layer is preferably 1 W / m·K or more, more preferably 3 W / m·K or more. The thermal conductivity of the resin layer refers to the thermal conductivity in the in-plane direction of the resin layer. The linear expansion coefficient of the first resin layer and the second resin layer is preferably 100 ppm / °C or less, more preferably 80 ppm / °C or less. The lower limit of the linear expansion coefficient of the first resin layer and the second resin layer is 10 ppm / °C. The linear expansion coefficient refers to the value measured for a test piece at a temperature range of 25°C to 260°C according to the measurement method specified in JIS C 6471:1995. The peel strength between the first resin layer and the second resin layer and the polyimide film (polyimide layer) is preferably 10 N / cm or more, more preferably 15 N / cm or more. The peel strength is preferably 100 N / cm or less.
[0046] The present transmission circuit board comprises a first present laminate film having a first resin layer containing an F polymer, a polyimide layer, and a second resin layer containing an F polymer laminated in this order; and a second present laminate film having a metal pattern layer, a third resin layer containing an F polymer, a polyimide layer, and a fourth resin layer containing an F polymer laminated in this order, wherein the ratio of the total thickness of the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer to the total thickness of the first laminate film, the metal pattern layer, and the second laminate film is more than 50% and not more than 75%, and the total thickness is more than 150 μm and not more than 400 μm. The details of the F polymer and polyimide layer contained in the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer in the first present laminate film and the second present laminate film are as described above. The preferred ranges of the thicknesses of the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer, as well as the polyimide layer, are also as described above.
[0047] The total thickness of the transmission circuit board is greater than 150 μm and less than 400 μm, preferably greater than 160 μm, and more preferably greater than 180 μm. The total thickness is preferably less than 360 μm, and more preferably less than 330 μm. Furthermore, the ratio of the total thickness of the first resin layer, second resin layer, third resin layer, and fourth resin layer to the total thickness of the first laminate film, metal pattern layer, and second laminate film is greater than 50% and less than 75%. This ratio is preferably greater than 55%, and more preferably greater than 55%. This ratio is preferably less than 72%, and more preferably less than 70%. Within this range, the transmission circuit board exhibits low transmission loss in the high-frequency range and excellent electrical characteristics.
[0048] The metal pattern layer constituting the present transmission circuit board is preferably encapsulated in an adhesive resin. Examples of adhesive resins include commercially available thermosetting resins such as epoxy resins. The metal pattern layer can be encapsulated using an adhesive resin commercially available as a bonding sheet.
[0049] This transmission circuit board can be preferably produced by forming a metal pattern layer from a metal foil layer formed on one surface of the second present laminate film described above, encapsulating the metal pattern layer using an adhesive resin commercially available as a bonding sheet, and then further stacking and pressing the first laminate film onto the surface of the encapsulated metal pattern layer.
[0050] Examples of metals for the metal foil layer include metal foils such as copper, nickel, aluminum, titanium, and alloys thereof. Copper is particularly preferred. The ten-point average roughness of the surface of the metal foil layer is preferably 0.01 to 4 μm. In this case, adhesion to the resin layer is improved, making it easier to obtain a printed circuit board with excellent transmission characteristics. The thickness of the metal foil is preferably 2 to 30 μm, more preferably 3 to 25 μm. The outermost layers of this transmission circuit board on both sides are resin layers containing an F polymer, which provides excellent adhesion and therefore prevents the metal layer from peeling off. This transmission circuit board may further have a metal layer or a metal pattern layer on the outermost layer on one or both sides. A method for laminating a metal layer on the surface of this transmission circuit board includes heat pressing the transmission circuit board and metal foil.
[0051] The present transmission circuit board is useful as an antenna component, a printed circuit board, an aircraft component, an automobile component, etc., and is particularly useful as a printed circuit board material for flexible printed wiring boards, rigid printed wiring boards, etc. The printed circuit board can be manufactured, for example, by processing the metal layer of the present transmission circuit board, which has a metal layer on one or both sides of the outermost layer, into a conductor circuit (pattern circuit) of a predetermined pattern by etching or the like, or by processing the present transmission circuit board into a pattern circuit by electroplating (semi-additive process (SAP process), modified semi-additive process (MSAP process), etc.). In manufacturing the printed circuit board, after forming the pattern circuit, an interlayer insulating film may be formed on the pattern circuit, and a conductor circuit may further be formed on the interlayer insulating film. Alternatively, a solder resist may be laminated on the pattern circuit, or a coverlay film may be laminated on the pattern circuit.
[0052] Although the present transmission circuit board and the present laminate film have been described above, the present invention is not limited to the configurations of the above-described embodiments. For example, the present transmission circuit board and the present laminate film may have any other configuration added to the configurations of the above-described embodiments, or may be replaced with any configuration that produces a similar effect.
[0053] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. 1. Preparation of each component [F polymer] F particle 1: A polymer containing 97.9 mol % of TFE units, 0.1 mol % of NAH units, and 2.0 mol % of PPVE units, in this order, and having a carbonyl group-containing group with a main chain carbon number of 1×10 6 Tetrafluoroethylene polymer particles (melting temperature: 300°C) with 1000 particles per particle (D50: 2.4 μm, Tg: 85°C, specific surface area: 9 m) 2 / g)
[0054] 2. Liquid Composition Production Examples [Production Example 1] F particles 1 and water were mixed using a planetary centrifugal mixer to produce liquid composition 1 containing 33% by mass of F particles 1.
[0055] 3. Production Examples of Laminated Films [Example 1] By a roll-to-roll process, the liquid composition 1 obtained according to Production Example 1 was applied to one surface of a polyimide film (thickness 25 μm) by a small-diameter gravure reverse method to form a coating layer, and the film was passed through a ventilation drying oven (oven temperature 150 ° C) for 3 minutes to remove water and form a dry film. In addition, the liquid composition 1 was similarly applied to the other surface of the polyimide film to form a coating layer, and then dried to form a dry film. Next, the substrate with the dry film formed on both sides was passed through a far-infrared oven at an oven temperature of 350 ° C for 5 minutes to melt and bake the F particles 1, and a laminated film 1 was obtained in which a first resin layer (thickness 12.5 μm) containing an F polymer, a polyimide layer, and a second resin layer (thickness 12.5 μm) containing an F polymer were laminated in this order.
[0056] [Examples 2 to 5] The same procedure as in Example 1 was carried out, except that the thickness of the polyimide layer and the thickness of the coating layer of Liquid Composition 1 applied to the polyimide layer were changed as shown in Table 1, to obtain laminate films 2 to 5 in which a first resin layer containing an F polymer, a polyimide layer, and a second resin layer containing an F polymer were laminated in this order.
[0057]
[0058] 4. Transmission Circuit Board Production Examples [Example 6] A laminate film 1 and an electrolytic copper foil (manufactured by Fukuda Metal Foil & Powder Co., Ltd., "CF-T49A-DS-HD2", thickness: 12 μm) were placed opposite each other and thermocompression bonded under conditions of a temperature of 270°C, a pressure of 1 MPa, and an atmospheric pressure of 10 kPa, to obtain a copper foil with a laminate film 1. The copper foil of the copper foil with the laminate film 1 was etched to form a metal pattern layer on the surface of the laminate film 1. Furthermore, a thermosetting adhesive as a bonding agent was placed on the metal pattern layer side of this laminate film 1, and then a laminate film 2 was placed thereon, followed by similar thermocompression bonding to obtain a transmission circuit board 1 having, in this order, the laminate film 1, the metal pattern layer encapsulated in the bonding agent, and the laminate film 2.
[0059] Examples 7 and 8 Transmission circuit boards 2 and 3 were obtained in the same manner as in Example 5, except that the type of laminated film was changed as shown in Table 2.
[0060] 5. Evaluation 5-1. Transmission Loss Electrolytic copper foil (manufactured by Fukuda Metal Foil & Powder Co., Ltd., "CF-T49A-DS-HD2", thickness: 12 μm) was placed on both sides of the transmission circuit board obtained in each example, and pressed under vacuum at 340°C for 20 minutes to produce printed circuit boards as double-sided copper-clad laminates, and the signal transmission loss was measured using the following method. Signals up to 40 GHz were processed using a vector network analyzer (manufactured by Keysight Technologies, Inc., E8361A) and measured using a solderless connector. A microstrip line (MSL) was used as the transmission line formed on the printed circuit board, and the characteristic impedance of the line was 50 Ω. The surface of the copper conductor of the printed circuit board was subjected to an anti-rust treatment. TRL calibration (Thru-Reflect-Line calibration) was used as the calibration method. The line length was 50 mm, and the transmission loss per unit length was measured. As a measure of transmission loss, an "S-parameter" (hereinafter also referred to as the S value), which is one of the circuit network parameters used to represent the characteristics of high-frequency electronic circuits and high-frequency electronic components, was used. The S21 value, which is one of the S values, indicates that the closer the value is to 0, the smaller the transmission loss. It was confirmed that the absolute value of S21 for transmission circuit boards 2 and 3 at a frequency of 10 GHz was 2.0 [dB / 100 mm] or more, which was 20% or more smaller than the value for transmission circuit board 1. It was confirmed that transmission circuit boards 2 and 3 have significantly smaller transmission loss in the high-frequency region than transmission circuit board 1. In Table 2, if the configuration of the transmission circuit board satisfies the formula (1), it is marked as conforming to formula (1) ("Yes" is written in the formula (1) conformance evaluation column), and if it does not satisfy the formula (1), it is marked as not conforming to formula (1) ("No" is written in the formula (1) conformance evaluation column).
[0061] 5-2. Mechanical Properties (Bending Properties) The transmission circuit board obtained in each example was cut into a 5 mm square, bent 180° with a curvature radius of 300 μm, and evaluated based on the appearance after applying a load (50 mN, 1 minute) from above and then returning to its original shape. Transmission circuit boards 1 to 3 had the same bending properties, and all transmission circuit boards had excellent mechanical properties.
[0062]
[0063] Example 9 The same procedure as in Example 1 was carried out, except that the thickness of the polyimide layer and the thickness of the coating layer of Liquid Composition 1 applied to the polyimide layer were changed as shown in Table 3, to obtain laminate films 6 to 9 in which a first resin layer containing an F polymer, a polyimide layer, and a second resin layer containing an F polymer were laminated in this order. Note that laminate films 6 and 8 satisfy the formula (11), while laminate films 7 and 9 do not satisfy the formula (11) below.
[0064]
[0065] When the transmission circuit boards obtained from the laminate film 6 and the laminate film 8 are subjected to the evaluation of the above-mentioned "5-1. Transmission loss", the absolute value of S21 is 2.0 [dB / 100 mm] or more, and the transmission loss in the high frequency range is significantly smaller than that of the transmission circuit boards obtained from the laminate film 7 and the laminate film 9.
[0066] The transmission circuit board of the present invention has excellent heat resistance, mechanical properties, electrical properties, etc. due to the physical properties of the F polymer, and further has small transmission loss in the high frequency range, so it can be effectively used for printed circuit boards, etc. in various mobile communication devices such as mobile phones that are compatible with higher speeds and higher frequencies.
[0067] The entire contents of the specification, claims, and abstract of Japanese Patent Application No. 2023-063254, filed on April 10, 2023, are incorporated herein by reference as the disclosure of the present invention.
Claims
1. A transmission circuit board in which a first laminated film, a metal pattern layer, and a second laminated film are laminated in this order, the first laminated film is laminated in this order with a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer, the second laminated film is laminated in this order with a third resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a fourth resin layer containing a tetrafluoroethylene-based polymer, the first laminated film, the metal pattern layer, and the second laminated film have a total thickness of more than 150 μm and 400 μm or less, the total thickness is thickness S, and the ratio of the total thickness of the third resin layer and the fourth resin layer to thickness S is ratio F, the thickness S and ratio F satisfy the formula represented by the following formula (1). Ratio F ≧ 43872 × (thickness S) -2.14 ...(1) 2. The transmission circuit board of claim 1, wherein said tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether).
3. The transmission circuit board according to claim 1, further comprising a metal layer on one or both outermost layers.
4. A transmission circuit board comprising a first laminate film, a metal pattern layer, and a second laminate film laminated in this order, the first laminate film comprising a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer laminated in this order, the second laminate film comprising a third resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a fourth resin layer containing a tetrafluoroethylene-based polymer laminated in this order, the ratio of the total thickness of the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer to the total thickness of the first laminate film, the metal pattern layer, and the second laminate film is more than 50% and not more than 75%, and the total thickness is more than 150 μm and not more than 400 μm.
5. The transmission circuit board of claim 4, wherein said tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether).
6. The transmission circuit board according to claim 4, further comprising a metal layer on one or both outermost layers.
7. A laminated film in which a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer are laminated in this order, the total thickness of the first resin layer, the polyimide layer, and the second resin layer is more than 50 μm and 200 μm or less, the total thickness is Sa, and the ratio of the total thickness of the first resin layer and the second resin layer to the thickness Sa is Fa, the thickness Sa and the ratio Fa satisfy the formula represented by the following formula (11): ratio Fa ≧ 43872 × (thickness Sa) -2.14 ...(11) 8. The laminate film according to claim 7, wherein the thickness of the first resin layer and the second resin layer is each more than 20 μm and not more than 100 μm, and the thickness of the polyimide layer is not more than 50 μm.
9. The laminate film of claim 7, wherein the tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether).
10. The laminate film according to claim 7, wherein the tetrafluoroethylene polymer is a heat-fusible tetrafluoroethylene polymer having a carbonyl group-containing group.
11. A laminated film comprising a first resin layer containing a tetrafluoroethylene-based polymer, a polyimide layer, and a second resin layer containing a tetrafluoroethylene-based polymer laminated in this order, the total thickness of the first resin layer, the polyimide layer, and the second resin layer being more than 50 μm and not more than 200 μm, and the ratio of the total thickness of the first resin layer and the second resin layer to the total thickness being more than 50% and not more than 75%.
12. The laminate film according to claim 11, wherein the thickness of the first resin layer and the second resin layer is each more than 20 μm and not more than 100 μm, and the thickness of the polyimide layer is not more than 50 μm.
13. The laminate film of claim 11, wherein the tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether).
14. The laminate film according to claim 11, wherein the tetrafluoroethylene polymer is a heat-fusible tetrafluoroethylene polymer having a carbonyl group-containing group.
Citation Information
Patent Citations
Adhesive film and flexible metal laminated plate
WO2015080260A1
Film, method for producing film, metal-clad laminate, and coated metal conductor
WO2021039735A1