Polyimide resin and adhesive film

A solvent-soluble polyimide resin with a cyclic imide structure and specific diamine residues addresses the challenges of adhesive residue and warpage in semiconductor packaging by providing excellent adhesion and removability, ensuring effective heat resistance and low decomposition.

WO2024214735A1PCT designated stage expired Publication Date: 2024-10-17PI R & D +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014521
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing polyimide resins for semiconductor packaging face challenges such as adhesive residue, warpage, and mold flash during high-temperature processes, with a lack of a resin that effectively balances heat resistance, low decomposition, and re-peelability without leaving residue.

Method used

A solvent-soluble polyimide resin with a cyclic imide structure, containing tetracarboxylic dianhydride and diamine residues, including polysiloxane diamine and aromatic diamines, which provides excellent adhesion and removability, reducing volatile matter generation and warpage, and preventing mold flash.

Benefits of technology

The polyimide resin achieves good adhesion at low temperatures, allows lamination at room temperature, and can be easily peeled without residue after high-temperature treatment, while maintaining heat resistance and preventing warpage, thus addressing the limitations of previous polyimide resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a polyimide resin which, if used in an adhesive film for the production of a semiconductor or an electronic component, is less likely to generate a volatile component even at high temperatures, has good adhesiveness at low temperatures, can be laminated at normal temperature, has proper adhesive force after passing through a high-temperature heat treatment process, can be easily peeled off at normal temperature without leaving an adhesive residue, has little warping in each process, and is capable of preventing a mold flash. The present invention provides a solvent-soluble polyimide resin which has a cyclic imide structure, and which also has a repeating unit that contains a diamine residue of a polysiloxane-based diamine, and a diamine residue having an anilide group and / or a diamine residue having a carboxyl group. The present invention also provides an adhesive film which is obtained by superposing a resin composition that contains the polyimide resin on at least one surface of a heat-resistant film.
Need to check novelty before this filing date? Find Prior Art

Description

Polyimide resin and adhesive film

[0001] The present invention relates to a polyimide resin suitable for use as a heat-resistant adhesive for semiconductor or electronic component manufacturing. More specifically, the present invention relates to a polyimide resin for semiconductor or electronic component manufacturing that is attached to a semiconductor element mounting substrate when manufacturing a semiconductor package, a resin composition containing the same, an adhesive, and an adhesive film.

[0002] In recent years, with the increasing demand for smaller and lighter electronic devices, the electronic components built into them must also be smaller and more densely packed. To address this, various semiconductor package configurations have been developed. For example, the area array packaging type CSP (Chip Size Package) is a significantly smaller version of the BGA (Ball Grid Array) package. Among these CSPs, the QFN (Quad Flat Non-leaded Package) was developed to reduce the size and height of the QFP (Quad Flat Package) that uses leads. It uses electrode pads instead of leads as connection terminals. Because QFNs have outer leads in the encapsulation area, mold flash, a problem in which the encapsulation resin wraps around the lead frame, has been a problem. Protecting the outer leads of the lead frame with an adhesive film during resin encapsulation is an effective solution. From this perspective, various adhesive films have been proposed for use in semiconductor packages such as QFNs.

[0003] Such adhesive films are generally produced by providing various adhesive layers on a heat-resistant film. Examples of heat-resistant films that have been proposed include polyimide, polyamide, polyamideimide, polyetherimide, polyester, polyphenylene sulfide, polysulfone, and polyethersulfone, while examples of resins for the adhesive layer include acrylic, silicone, polyamide, and polyimide resins. Since the adhesive layer is heated to high temperatures during heating processes such as die attach, wire bonding, and resin encapsulation, and then peeled off from the lead frame, it is necessary to address not only mold flash issues but also compatibility with each process, adhesive residue, and warpage. Therefore, various adhesive layers have been proposed for this purpose.

[0004] For example, Patent Document 1 discloses that a polyimide resin whose main amine components are a diaminosiloxane compound and 2,2-bis(4-(4-aminophenoxy)phenyl)propane or 1,3-bis(3-aminophenoxy)benzene, which is soluble in organic solvents and has a glass transition temperature of 100 to 150°C, can be used as a film-like adhesive for semiconductor packaging materials.

[0005] Furthermore, Patent Document 2 discloses that a resin composition containing a polyimide resin and a methylol compound, in which the diamine residues of the polyimide resin are residues of a polysiloxane diamine and residues of an aromatic diamine having a hydroxyl group, serves as a heat-resistant adhesive that can be used in the manufacture of electronic devices. Patent Document 2 also discloses that, in the absence of either the residue of an aromatic diamine having a hydroxyl group in the polyimide resin or the methylol compound in the resin composition, the adhesive strength with the polyimide film substrate increases significantly after treatment at 300°C, and peeling is not possible at room temperature (paragraph 0098).

[0006] Furthermore, Patent Document 3 discloses that an adhesive film having a heat-resistant film and an adhesive layer, in which the adhesive layer contains a polyimide copolymer containing 30 to 100 mol% of polysiloxane-based diamine residues based on all diamine residues, can be used as an adhesive film for manufacturing semiconductors or electronic components.

[0007] In Patent Documents 2 and 3, polyamic acid is synthesized, and a resin composition containing the polyamic acid is applied to a substrate such as a glass substrate or a polyimide film, and then completely imidized by heating at 250° C. However, the pressure-sensitive adhesive films using the polyimide resins described in Patent Documents 1 to 3 have a problem in that adhesive residue occurs depending on the conditions when the pressure-sensitive adhesive layer is peeled off from the lead frame after the high-temperature heating process.

[0008] Japanese Patent Application Laid-Open No. 2004-277619 International Publication No. 2014 / 050878 Japanese Patent Application Laid-Open No. 2020-136600

[0009] As mentioned above, the properties required for a highly heat-resistant adhesive resin or adhesive film for semiconductor manufacturing include heat resistance at high temperatures, low decomposition, lamination at room temperature, removability at room temperature after high-temperature heat treatment, and low warpage during each process. Various polyimide resins, such as those mentioned above, have been investigated as resins that meet these requirements, but no polyimide resins have yet been found that fully possess all of these properties. In particular, it has been difficult to find a polyimide resin that can solve the problem of adhesive residue when the adhesive layer is peeled off after a high-temperature heating process. Furthermore, when a resin composition containing polyamic acid is applied to a substrate such as a glass substrate or a polyimide film and then heated to a high temperature, such as 250°C, to perform complete imidization, a dehydration shrinkage reaction occurs, causing the adhesive film to curl.

[0010] In light of these circumstances, the object of the present invention is to provide a polyimide resin having a cyclic imide structure, which generates little volatile matter due to decomposition or the like even at high temperatures of 250°C or higher, has good adhesive properties at low temperatures, can be laminated at room temperature, has appropriate adhesive strength after passing through a high-temperature heat treatment process, can be easily re-peeled at room temperature without leaving any adhesive residue, shows little warping in each process, and is capable of preventing mold flash, as well as a resin composition and adhesive film using the same, and a method for producing the same.

[0011] As a result of intensive research to solve the above problems, the present inventors have found that by using a copolymer having a tetracarboxylic dianhydride residue, a diamine residue of a polysiloxane-based diamine, and a diamine residue having an anilide group and / or a diamine residue having a carboxyl group as a polyimide resin having a cyclic imide structure, a solvent-soluble polyimide resin having a cyclic imide structure that provides appropriate adhesiveness and removability can be obtained.The present inventors have also found that by using a resin composition containing such a resin, the above problems can be solved, and that a pressure-sensitive adhesive for semiconductor or electronic component production, which has all of the following properties, can be provided: heat resistance at high temperatures, low decomposition, lamination properties at room temperature, removability at room temperature after high-temperature heat treatment, and low warpage in each process, and a pressure-sensitive adhesive film using the same, and have completed the present invention.

[0012] That is, the present invention provides a solvent-soluble polyimide resin having a cyclic imide structure, characterized in that the polyimide resin has a repeating unit represented by the following general formula (1):

[0013]

[0014] (In the formula, Z is a tetracarboxylic dianhydride residue, and A is a diamine residue of a polysiloxane-based diamine, and a diamine residue having an anilide group and / or a diamine residue having a carboxyl group.)

[0015] The present invention also provides a resin composition containing the polyimide resin of the present invention and an organic solvent. The present invention also provides a pressure-sensitive adhesive for semiconductor or electronic component production, which contains the polyimide resin of the present invention. The present invention also provides a pressure-sensitive adhesive film for semiconductor or electronic component production, which comprises a heat-resistant film and the resin composition of the present invention laminated on at least one side of the heat-resistant film.

[0016] The present invention provides a polyimide resin that generates little volatile matter due to decomposition or the like even at high temperatures of 250°C or higher, has good adhesive properties at low temperatures, can be laminated at room temperature, has appropriate adhesive strength after a high-temperature heat treatment process, can be easily removed at room temperature without leaving any adhesive residue, shows little warping in each process, and is capable of preventing mold flash, as well as a resin composition, adhesive, and adhesive film containing the polyimide resin.Furthermore, because a solvent-soluble polyimide resin having a cyclic imide structure is used, a heating step for imidization is not required in the production process of the adhesive film, and a highly productive production process can be provided.

[0017] [Polyimide Resin] The polyimide resin of the present invention is a solvent-soluble polyimide resin having a repeating unit represented by the following general formula (1) and a cyclic imide structure. In the present invention, the term "cyclic imide structure" refers to a structure in which imide groups form a ring. Furthermore, the term "solvent-soluble" in the present invention is a term used for the organic polar solvent used in synthesizing the polyimide and the organic solvent used to dilute the polyimide resin in the resin composition described below, and refers to a polyimide resin that dissolves 5 g or more in 100 g of solvent.

[0018]

[0019] (In the formula, Z is a tetracarboxylic dianhydride residue, and A is a diamine residue of a polysiloxane-based diamine, and a diamine residue having an anilide group and / or a diamine residue having a carboxyl group.)

[0020] The repeating unit represented by the general formula (1) has at least a tetracarboxylic dianhydride residue (Z) and a diamine residue (A), and the diamine residue (A) is a diamine residue (A) of a polysiloxane-based diamine. 1 ), and a diamine residue having an anilide group (A 2 ) and / or a diamine residue having a carboxyl group (A 3 That is, in the polyimide resin of the present invention, the diamine residue (A) is a diamine residue of a polysiloxane-based diamine (A 1), and the diamine residue (A) is a diamine residue having an anilide group (A 2 ) or the following repeating unit (1-2) in which the diamine residue (A) is a diamine residue having a carboxyl group (A 3 ) is a polymer containing the following repeating unit (1-3):

[0021]

[0022] (wherein Z is a tetracarboxylic dianhydride residue, A 1 is the diamine residue of polysiloxane-based diamine)

[0023]

[0024] (wherein Z is a tetracarboxylic dianhydride residue, A 2 is a diamine residue having an anilide group)

[0025]

[0026] (wherein Z is a tetracarboxylic dianhydride residue, A 3 is a diamine residue having a carboxyl group)

[0027] The polyimide resin of the present invention may be a random copolymer containing the repeating unit (1-1) and the repeating unit (1-2) and / or the repeating unit (1-3) arranged randomly, or may be a block polymer containing a structure in which only a portion of the repeating units (1-1) to (1-3) are polymerized first.

[0028] As will be described in detail later, resin compositions containing the polyimide resin of the present invention can be suitably used as heat-resistant adhesives for the production of semiconductors or electronic components. By making the diamine residue (A) constituting the polyimide resin of the present invention have the specific structure described above, the adhesive layer laminated on a heat-resistant film can achieve both appropriate adhesive strength and adhesive residue upon peeling (no adhesive residue). When a diamine residue having a functional group other than a carboxyl group or an anilide group is used, it is difficult to achieve both appropriate adhesive strength and adhesive residue upon peeling.

[0029] (Tetracarboxylic acid dianhydride residue) The tetracarboxylic acid dianhydride residue (Z) preferably contains a residue of an aromatic tetracarboxylic acid dianhydride. Specific examples of the aromatic tetracarboxylic acid dianhydride include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 2,2'dimethyl-3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 5,5'dimethyl-3,3',4,4'-biphenyltetracarboxylic acid dianhydride, and the like. phenyltetracarboxylic acid dianhydride, 2,3,3',4'-biphenyltetracarboxylic acid dianhydride, 2,2',3,3'-biphenyltetracarboxylic acid dianhydride, 3,3',4,4'-diphenylethertetracarboxylic acid dianhydride, 2,3,3',4'-diphenylethertetracarboxylic acid dianhydride, 2,2',3,3'-diphenylethertetracarboxylic acid dianhydride, 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride, 2,2',3,3'-benzophenonetetracarboxylic acid dianhydride, 2,3,3',4'-benzophenonetetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic acid dianhydride, 2,3,3',4'-diphenylsulfonetetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfoxidetetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfidetetracarboxylic dianhydride, 3,3',4,4'-diphenylmethylenetetracarboxylic dianhydride, 4,4'-isopropylidenediphthalic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,3",4,4"-para-terphenyltetracarboxylic dianhydride, 3,3",4,4"-meta-terphenyltetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 1,2,7,8-phenanthrenetetracarboxylic dianhydride, and the like. The aromatic tetracarboxylic dianhydrides may be used alone or in combination of two or more.Among these, monocyclic acid dianhydrides such as pyromellitic acid dianhydride are preferred in that they can improve heat resistance by increasing the heat reduction temperature.

[0030] (Diamine Residue) The diamine residue (A) in general formula (1) is a diamine residue of a polysiloxane-based diamine, and a diamine residue having an anilide group and / or a diamine residue having a carboxyl group. The polysiloxane-based diamine constituting the diamine residue of the polysiloxane-based diamine is not particularly limited, but is preferably a polysiloxane-based diamine represented by the following general formula (2):

[0031]

[0032] In formula (2), n is a natural number and is an integer of 1 to 150. n is preferably 5 to 50, and more preferably 7 to 15. R 1 and R 2 are the same or different and represent an alkylene group or a phenylene group having 1 to 40 carbon atoms. 1 and R 2 is preferably an alkylene group or a phenylene group having 1 to 10 carbon atoms, and more preferably an alkylene group having 2 to 5 carbon atoms. 3 ~R 6 are the same or different and represent an alkyl group having 1 to 40 carbon atoms, a phenyl group, or a phenoxy group. 3 ~R 6 is preferably an alkyl group having 1 to 10 carbon atoms or a phenoxy group, more preferably an alkyl group having 1 to 5 carbon atoms.

[0033] Specific examples of the polysiloxane-based diamine represented by the general formula (2) include α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydiethylsiloxane, α,ω-bis(3-aminopropyl)polydipropylsiloxane, α,ω-bis(3-aminopropyl)polydibutylsiloxane, α,ω-bis(3-aminopropyl)polydiphenoxysiloxane, α,ω-bis(2-aminoethyl)polydimethylsiloxane, α,ω-bis(2-aminoethyl)polydiphenoxysiloxane, α Examples of suitable diamines include α,ω-bis(4-aminobutyl)polydimethylsiloxane, α,ω-bis(4-aminobutyl)polydiphenoxysiloxane, α,ω-bis(5-aminopentyl)polydimethylsiloxane, α,ω-bis(5-aminopentyl)polydiphenoxysiloxane, α,ω-bis(4-aminophenyl)polydimethylsiloxane, and α,ω-bis(4-aminophenyl)polydiphenoxysiloxane. Of these, α,ω-bis(3-aminopropyl)polydimethylsiloxane is preferred because of its excellent balance of adhesiveness, reactivity, and solubility in reactive solvents. The polysiloxane-based diamines represented by the general formula (2) above may be used alone or in combination of two or more.

[0034] From the viewpoint of achieving both appropriate adhesive strength and adhesive residue upon peeling (no adhesive residue), the content of diamine residues in the polysiloxane diamine is preferably 60 mol% or more, 65 mol% or more, further 68 mol% or more, and particularly 70 mol% or more of the total diamine residues, and is preferably 97 mol% or less, 95 mol% or less, further 93 mol% or less, and particularly 90 mol% or less. If the diamine residues in the polysiloxane diamine exceed 97 mol% of the total diamine residues, the adhesive strength tends to increase and adhesive residue may occur.

[0035] The diamine residue having a carboxyl group is preferably a residue of a carboxyl group-containing aromatic diamine represented by the following general formula (3).

[0036]

[0037] In formula (3), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, or an ether group, p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4. However, when p is 0, m1 is an integer of 1 to 4. Of these, X is preferably a single bond, p is preferably 0 to 1, and m1 is preferably 1 to 2.

[0038] Specific examples of the carboxyl group-containing aromatic diamine represented by the above general formula (3) include 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, 5,5'-methylenebis(2-aminobenzoic acid), 3,5-bis(4-aminophenoxy)benzoic acid, 4,4'-diaminobiphenyl-3,3'-dicarboxylic acid, etc. Among these, monocyclic carboxyl group-containing aromatic diamines such as 3,5-diaminobenzoic acid and 3,4-diaminobenzoic acid are preferred in that the adhesive strength of the adhesive film is maintained at an appropriate value after the adhesive film has passed through a high-temperature heat treatment process, and no adhesive residue is left when the adhesive film is peeled off at room temperature.

[0039] Furthermore, as the diamine residue having a carboxyl group, a residue of a carboxyl group-containing aromatic diamine of the following formula (4) or (5) may be used.

[0040]

[0041]

[0042] In the present invention, from the viewpoint of achieving both appropriate adhesive strength and adhesive residue upon peeling (no adhesive residue), the number of carboxyl groups possessed by the carboxyl group-containing aromatic diamine is preferably 1 to 5, more preferably 1 to 3, even more preferably 1 or 2, and particularly preferably 1. The above-mentioned carboxyl group-containing aromatic diamines may be used alone or in combination of two or more kinds.

[0043] The diamine residue having an anilide group is preferably at least one of the anilide group-containing aromatic diamines represented by the following general formulas (6-1) to (6-3).

[0044]

[0045] In the formula, R 1 ~R8 are the same or different and represent an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and among these, an alkyl group having 1 to 3 carbon atoms or an alkoxy group having 1 to 3 carbon atoms is preferred. Furthermore, n1 to n8 each represent an integer of 0 to 4, and among these, 0 or 1 is preferred.

[0046] Specific examples of the anilide group-containing aromatic diamines represented by the above general formulae (6-1) to (6-3) include 4,4'-diaminobenzanilide, 3,4'-diaminobenzanilide, 4,3'-diaminobenzanilide, 4,4'-diaminoterephthalanilide, 4,4'-diaminoisophthalanilide, 3,3'-diaminoterephthalanilide, 3,3'-diaminoisophthalanilide, 3,4'-diaminoterephthalanilide, 3,4'-diaminoisophthalanilide, 2-methoxy-4,4'-diaminobenzanilide, 2,2'-dimethoxy-4,4'-diaminobenzanilide, 2,6-dimethoxy-4,4'-diaminobenzanilide, and 2,6'-dimethoxy-4,4'-diaminobenzanilide. Among these, those having a benzanilide structure are preferred, and anilide group-containing aromatic diamines represented by the above general formula (6-1) are preferred, in that they maintain an appropriate adhesive strength after the PSA film has passed through a high-temperature heat treatment process and leave no adhesive residue when the PSA film is peeled off at room temperature. The above anilide group-containing aromatic diamines may be used alone, or two or more types may be used. In the present invention, the number of anilide groups possessed by the anilide group-containing aromatic diamine is preferably 1 to 3, more preferably 1 to 2, and even more preferably 1, from the viewpoint of achieving both appropriate adhesive strength and adhesive residue (no adhesive residue) upon peeling. The above carboxyl group-containing aromatic diamines and anilide group-containing aromatic diamines may be used in combination, or either one may be used alone.

[0047] From the viewpoint of achieving both appropriate adhesive strength and adhesive residue upon peeling, the total content of diamine residues having carboxyl groups and diamine residues having anilide groups is preferably 3 mol% or more, 5 mol% or more, or even 7 mol% or more, and particularly 10 mol% or more of the total diamine residues, and is preferably 40 mol% or less, 35 mol% or less, or even 32 mol% or less, and particularly 30 mol% or less. If the total content of diamine residues having carboxyl groups and diamine residues having anilide groups is less than 3 mol%, adhesive residue may occur, while if it exceeds 40 mol%, adhesive strength may decrease. When the above-mentioned carboxyl group-containing aromatic diamine and anilide group-containing aromatic diamine are used in combination, the molar ratio of diamine residues having carboxyl groups to diamine residues having anilide groups contained in the polyimide resin is preferably 9-5:1-5, and more preferably 8-6:2-4.

[0048] (Method of Synthesizing Polyimide Resin) The solvent-soluble polyimide may be synthesized by any known method without particular limitation. For example, a solvent-soluble polyimide can be synthesized by reacting approximately equal amounts of the aromatic tetracarboxylic dianhydride and diamine described above in an organic polar solvent in the presence of a catalyst and a dehydrating agent at 160 to 200°C for several hours. The solvent-soluble polyimide resin of the present invention is a copolymer. When the polyimide is synthesized by a one-stage polymerization reaction, a random copolymer is obtained. However, if necessary, the polyimide resin can also be synthesized as a block copolymer by a block copolymerization reaction. For example, the polyimide can be produced by a two-stage sequential addition reaction. In the first stage, a polyimide oligomer is synthesized from the aromatic tetracarboxylic dianhydride and diamine described above. Then, in the second stage, an aromatic tetracarboxylic dianhydride and / or diamine is further added and polycondensed to form a block copolymerized polyimide.

[0049] The dehydration imidization reaction can be accelerated by using a two-component acid-base catalyst that utilizes the lactone equilibrium reaction as a catalyst for these reactions. Specifically, a two-component catalyst (lactone catalyst) consisting of γ-valerolactone and pyridine or N-methylmorpholine is used. As shown in the following formula, water is generated as the imidization proceeds, and the generated water participates in the lactone equilibrium, acting as an acid-base catalyst and exhibiting catalytic action.

[0050]

[0051] The water produced by the imidization reaction is removed from the system by azeotropy with a dehydrating agent, such as toluene or xylene, that coexists in the polar solvent. When the reaction is complete, the water in the solution is removed, and the acid-base catalyst is converted into γ-valerolactone and pyridine or N-methylmorpholine, which are then removed from the system. In this way, a high-purity polyimide solution can be obtained.

[0052] The polyimide obtained by the direct imidization reaction using the lactone catalyst system consisting of the lactone and a base can be obtained in the form of a solution dissolved in a polar solvent, and the polyimide concentration can be set within a preferred range of 10 to 50 wt % in terms of the solid content of the polyimide resin. Therefore, the produced polyimide solution can be preferably used as it is.

[0053] Other two-component catalysts that can be used include oxalic acid or malonic acid and pyridine or N-methylmorpholine. In a reaction solution at 160 to 200°C, oxalates or malonates act as acid catalysts to promote the imidization reaction. A catalytic amount of oxalic acid or malonic acid remains in the resulting polyimide solvent. This polyimide solution is applied to a substrate and then heated to 200°C or higher to remove the solvent and form a film. When this film is formed, the oxalic acid or malonic acid remaining in the polyimide undergoes thermal decomposition as shown in the following formula and is removed from the system as a gas. Oxalic acid-pyridine catalysts are more active than valerolactone-pyridine catalysts and can produce high-molecular-weight polyimides in a short period of time.

[0054]

[0055] As the organic polar solvent used in the synthesis of the solvent-soluble polyimide, glycol ether-based solvents, amide-based polar solvents, and ketone-based solvents are preferred from the viewpoint of the solubility and storage stability of the polyimide copolymer or polyimide resin.

[0056] Specific examples of glycol ether solvents include propylene glycol mono-t-butyl ether, ethylene glycol mono-t-butyl ether, propylene glycol mono-n-butyl ether, propylene glycol monopropyl ether, propylene glycol monoethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol monopropyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, dipropylene glycol dipropyl ether, dipropylene glycol di-n-butyl ether, dipropylene glycol di-t-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monopropyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tripropylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0057] Specific examples of amide-based polar solvents include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and 1,3-dimethyl-2-imidazoline. Specific examples of ketone-based solvents include cyclohexanone. These organic polar solvents can be used alone or in combination of two or more. Among these, glycol ether-based solvents are preferred because they can enhance the storage stability of the synthesized polyimide resin solution.

[0058] The above method allows for the synthesis of highly pure solvent-soluble polyimide resins having a cyclic imide structure. Because the resulting polyimide resin has a cyclic imide structure, unlike polyamic acid, it is not necessary to apply the resin to a substrate and then heat it to a high temperature, such as 250°C, to achieve complete imidization. This avoids the problem of adhesive film deformation and allows for the elimination of the high-temperature heating step, thereby providing a highly productive process. The molecular weight of the resulting solvent-soluble polyimide resin is 10,000 to 200,000, as a weight-average molecular weight converted to polystyrene. Polyimide resins within this weight-average molecular weight range can achieve good solvent solubility, film properties, and insulating properties.

[0059] [Resin Composition] The resin composition containing the solvent-soluble polyimide resin and organic solvent produced as described above can be suitably used as a heat-resistant adhesive for the production of semiconductors or electronic components. The resin composition of the present invention is a resin composition in a solution state in which a polyimide resin is dissolved in an organic solvent to a solids content of, for example, 10 to 50 wt %. The organic polar solvent used in the synthesis of the solvent-soluble polyimide resin described above can be used as the organic solvent contained in the resin composition. By using the organic solvent used in the synthesis method of the solvent-soluble polyimide resin as the organic solvent for the resin composition, a resin composition in a solution state in which a polyimide resin is dissolved in the organic polar solvent to a solids content of 10 to 50 wt % can be easily obtained.

[0060] Among the organic solvents contained in the resin composition, cyclohexanone, either alone or mixed with other organic solvents, is preferred because it allows for a lower drying temperature during coating and reduces the amount of residual solvent during the drying process at a relatively low temperature (160-180°C). When cyclohexanone is used as the organic solvent, the proportion of cyclohexanone in the organic solvent contained in the resin composition is typically 20-60% by volume, preferably 30-50% by volume, and more preferably 35-45% by volume. When cyclohexanone is combined with other organic solvents in the resin composition, glycol ether-based solvents such as triethylene glycol dimethyl ether are preferred as the other organic solvent. For example, the combined use of a glycol ether-based solvent such as triethylene glycol dimethyl ether and a ketone-based solvent such as cyclohexanone (volume ratio) in a ratio of 8:2 to 4:6, preferably 7:3 to 5:5, offers the advantages of improved monomer solubility, reduced drying temperature, and stability. The organic solvents contained in the resin composition are not limited to those listed above, and other organic solvents can also be used.

[0061] (Epoxy Compound) The resin composition of the present invention preferably contains an epoxy compound from the viewpoint of adjusting adhesive strength. The epoxy compound is not particularly limited and can be selected based on its compatibility with the polyimide resin composition. Examples of epoxy compounds that can be used include phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, triazine skeleton-containing epoxy resins, fluorene skeleton-containing epoxy resins, naphthalene epoxy resins, biphenyl epoxy resins, crystalline epoxy resins, and bisphenol A epoxy resins, and polymeric epoxy resins thereof can also be used. Among these, polyfunctional epoxy compounds are preferred from the viewpoint of reactivity, and a monocyclic tetrafunctional epoxy compound (N,N,N',N'-tetraglycidyl-1,3-benzenedi(methanamine)) represented by the following general formula (7) is particularly suitable.

[0062]

[0063] The content of the epoxy compound in the resin composition is preferably 1 part by weight (solid content) or more, more preferably 2 parts by weight or more, even more preferably 3 parts by weight or more, and particularly preferably 4 parts by weight or more, relative to 100 parts by weight (solid content) of the solvent-soluble polyimide, and is preferably 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, even more preferably 7 parts by weight or less, and particularly preferably 6 parts by weight or less.

[0064] (Other Additives) Surfactants, silane coupling agents, leveling agents, etc. may be added to the resin composition of the present invention to improve properties such as adhesion, heat resistance, and coatability. A leveling agent can be added if there is concern that the resin composition may exhibit a slight tendency to repel paint during application, but leveling agents are not essential components for achieving the effects of the present invention. The resin composition of the present invention can also contain inorganic fine particles. The inclusion of inorganic fine particles improves the heat resistance and dimensional stability of the resin composition and adjusts its adhesion. Specific examples of inorganic fine particles include silica, alumina, titanium oxide, quartz powder, magnesium carbonate, potassium carbonate, barium sulfate, mica, and talc, with silica being preferred. The content of inorganic particles in the resin composition is preferably 2 to 70 parts by weight, more preferably 5 to 40 parts by weight, and most preferably 7 to 20 parts by weight, per 100 parts by weight (solids content) of polyimide resin.

[0065] [Adhesive Film] The resin composition is laminated as a polyimide-based adhesive on at least one side of a heat-resistant film to form an adhesive layer on the surface of the heat-resistant film, thereby forming an adhesive film having a heat-resistant film and an adhesive layer. (Heat-Resistant Film) The heat-resistant film is an insulating plastic film that can be used in high-temperature processes such as die attach, wire bonding, resin sealing, reflow, and other heating processes. Specific examples include plastic films such as polyimide, polyamide, polyamideimide, polyetherimide, polyester, polyphenylene sulfide, polysulfone, and polyethersulfone, with polyimide films being preferred from the perspective of heat resistance. In order to improve the adhesion of the resin composition to the heat-resistant film, it is preferable to subject the heat-resistant film to a surface treatment (roughening treatment) such as plasma treatment or corona treatment. Examples of plasma gases that can be used in the plasma treatment include oxygen, nitrogen, water, carbon dioxide, argon, and mixtures thereof.

[0066] (Adhesive Layer) The adhesive film of the present invention can be produced by applying a resin composition directly or via a primer layer to a heat-resistant film to form an adhesive layer. Examples of methods for applying the resin composition of the present invention to a heat-resistant film include a spin coater, a roll coater, a comma coater, gravure printing, screen printing, and a slit die coater. An adhesive layer with excellent adhesiveness and heat resistance can be obtained by applying the resin composition, drying it at 100 to 150°C, and then continuously or intermittently heat-treating it at 160 to 240°C for 2 minutes to 1 hour. In the present invention, the adhesive layer may be formed by directly applying and drying the resin composition to a glass substrate or the like. Examples of methods for applying the resin composition to a glass substrate or the like include a spin coater, screen printing, gravure coater, slit die coater, and bar coater.

[0067] The adhesive layer preferably exhibits a weight loss rate of 0.8% or less, more preferably 0.5% or less, and even more preferably 0.3% or less, when heated from 30°C to 300°C. A weight loss rate greater than 0.8% may result in contamination of the semiconductor element mounting substrate or poor wire bonding during the semiconductor manufacturing process. The thickness of the adhesive layer is preferably 2 to 30 μm, more preferably 3 to 20 μm, and even more preferably 4 to 10 μm. If the adhesive layer is less than 2 μm thick, it may be difficult to conform to the irregularities on the surface of the semiconductor element mounting substrate. As a result, filling between the adhesive and, for example, the lead frame serving as the semiconductor element mounting substrate may be impossible, resulting in mold flash. If the adhesive layer is thicker than 30 μm, this may cause poor wire bonding during wire bonding, and the adhesive strength to the lead frame and encapsulating resin may increase, potentially reducing workability during the peeling process.

[0068] The pressure-sensitive adhesive layer of the present invention typically has a glass transition temperature of -10°C or higher, -8°C or higher, -5°C or higher, or -3°C or higher, and preferably 40°C or lower, further preferably 30°C or lower, and particularly preferably 25°C or lower. If the glass transition temperature exceeds 40°C, good adhesion may not be obtained when a substrate to be adhered is laminated to the pressure-sensitive adhesive layer formed using the resin composition of the present invention. Although the lower limit of the glass transition temperature does not affect the effects of the present invention, if the temperature is too low, the adhesion may become excessively high. In the present invention, "good adhesion" refers to an adhesive strength at least sufficient to prevent spontaneous peeling of the substrate when the pressure-sensitive adhesive layer film is laminated to the substrate at room temperature. Specifically, this refers to an adhesive strength of 5 g / cm or higher when the substrate to be adhered is peeled at a peel angle of 90° and a rate of 10 mm / min. This initial peel strength to the substrate can also be increased by increasing the lamination temperature.

[0069] Generally, adhesive layers containing polyimide-based adhesives increase in adhesive strength after high-temperature heat treatment. However, adhesives containing the polyimide resin of the present invention increase in adhesive strength after the initial heat treatment at approximately 150°C, but show little change in adhesive strength after subsequent high-temperature heat treatments (150°C to 250°C). Specifically, the polyimide resin of the present invention contains a diamine residue with a specific structure as a repeating unit, thereby imparting and maintaining an appropriate adhesive strength to the adhesive layer. The appropriate adhesive strength is typically 5 to 400 g / cm, preferably 8 to 300 g / cm, and more preferably 10 to 200 g / cm. Furthermore, if desired, this adhesive strength can be adjusted by adding an epoxy compound or inorganic fine particles (filler).

[0070] (Adhesive Film) The adhesive film of the present invention is suitable as an adhesive film for semiconductor manufacturing. Specifically, the adhesive film of the present invention has an adhesive layer containing the polyimide resin having the specific diamine residue described above, and therefore can be attached to a semiconductor element mounting substrate at room temperature (5 to 35°C). Furthermore, by using the specific polyimide resin of the present invention, the adhesive film exhibits stable adhesive strength with little change such as decomposition or deterioration due to thermal history during the die attach process, wire bonding process, flip chip process, rewiring layer formation process, resin encapsulation process, and other processes in the semiconductor manufacturing process. Furthermore, by using the specific polyimide resin of the present invention, adhesive residue is less likely to occur on the semiconductor element mounting substrate when peeled from the semiconductor element mounting substrate after encapsulation.

[0071] Furthermore, since the adhesive film of the present invention is less susceptible to changes such as decomposition and deterioration due to thermal history, it is also suitable as an adhesive film for manufacturing electronic components, and can be suitably used in manufacturing processes for electronic components that use high-temperature processes such as reflow.

[0072] The pressure-sensitive adhesive film of the present invention may have a peelable protective film (insulating film) laminated on the surface of the pressure-sensitive adhesive layer to protect the pressure-sensitive adhesive layer and prevent blocking. In this case, any protective film may be used, such as a plastic film such as polyethylene, polypropylene, or polyethylene terephthalate, a metal foil such as aluminum foil or copper foil, or a laminate film of a plastic film and a metal foil. In addition, to facilitate peeling of the protective film, the surface of the protective film may be subjected to a release treatment with a silicone-based or fluorine-based release agent.

[0073] When the pressure-sensitive adhesive film of the present invention is used as a pressure-sensitive adhesive transfer film, one or both sides of the heat-resistant film may be subjected to a release treatment depending on the purpose. As the release treatment, a treatment of coating with a silicone resin, a fluorine-based resin, or the like is preferred.

[0074] The pressure-sensitive adhesive film of the present invention can be used to attach semiconductor element-mounting substrates that carry semiconductors or electronic components. Examples of semiconductor element-mounting substrates include lead frames, printed circuit boards, wafers, and sealing resin substrates for fan-out wafer-level packages (FOWLPs). Semiconductor elements refer to semiconductors and electronic components. For example, semiconductor elements can be mounted on lead frames via die attach films, or on printed circuit boards by flip-chip connection and subsequent reflow processes. Furthermore, semiconductor elements can be mounted on sealing resin wafer substrates by attaching chips to the pressure-sensitive adhesive film of the present invention, as in fan-out packages, and then encapsulating the attached chips in a single resin. Furthermore, semiconductor elements also include wafers on which semiconductor elements and electrical circuits such as comb-shaped electrodes are formed.

[0075] By using the polyimide resin of the present invention, for example, in a fan-out packaging process, since there is no adhesive residue on the exposed surface after peeling the adhesive film from the sealing resin wafer substrate, it is possible to perform the process of forming a rewiring layer and the process of dicing the rewiring layer on the exposed surface.

[0076] The present invention will be described in detail below based on examples, but the present invention is not limited to the following examples.

[0077] 1. Synthesis of Solvent-Soluble Polyimide Resin and Resin Composition (Example 1) A separable three-necked glass flask was equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark apparatus. 304.08 g (0.358 mol) of polysiloxane diamine KF-8010 (functional group equivalent (g / mol) = 425, manufactured by Shin-Etsu Chemical Co., Ltd., polysiloxane diamine of the present invention represented by general formula (2)), 86.70 g (0.397 mol) of pyromellitic dianhydride (hereinafter referred to as PMDA), 6.05 g (0.040 mol) of 3,5-diaminobenzoic acid (hereinafter referred to as 3,5-DABA), 1.99 g (0.020 mol) of γ-valerolactone, 3.14 g (0.040 mol) of pyridine, 285 g of triethylene glycol dimethyl ether, 190 g of cyclohexanone, and 70 g of toluene were charged and stirred at room temperature under a nitrogen atmosphere at 180 rpm for 30 minutes, and then heated to 180°C. During the reaction, water was removed by azeotropy with toluene. After the distillation of water was confirmed, the mixture was heated and stirred for 6 hours, cooled, and 1.94 parts by weight of KL-700 (a 100% by weight leveling agent manufactured by Kyoeisha Chemical Co., Ltd.) was added. The mixture was then further cooled to room temperature to obtain an adhesive resin composition with a solid content of 45 wt %.

[0078] (Example 2) In Example 1, the amount of KF-8010 used was 236.13 g (0.278 mol), and the amount of 3,5-DABA used was 18.11 g (0.119 mol), and an adhesive resin composition having a solid content of 40 wt% was obtained in the same manner as in Example 1.

[0079] Example 3 A pressure-sensitive adhesive resin composition having a solid content of 45 wt % was obtained in the same manner as in Example 1, except that 8.86 g (0.039 mol) of 4,4'-diaminobenzanilide was used instead of 3,5-DABA.

[0080] (Example 4) To the resin composition of Example 1, 5 parts by weight of N,N,N',N'-tetraglycidyl-1,3-benzenedi(methanamine) was added per 100 parts by weight of the solid content of the polyimide resin, and the mixture was diluted with cyclohexanone to obtain an adhesive resin composition with a solid content of 48 wt %.

[0081] (Example 5) To the resin composition of Example 1, 10 parts by weight of a solid content of spherical silica slurry (manufactured by Admatechs Co., Ltd., SO-C1 (particle size 0.2 to 0.4 μm) N-methyl-2-pyrrolidone (hereinafter referred to as NMP) slurry, 50 wt % solid content product) was added relative to 100 parts by weight of a solid content of polyimide resin, and the mixture was diluted with NMP to obtain an adhesive resin composition with a solid content of 45 wt %.

[0082] Comparative Example 1 A pressure-sensitive adhesive resin composition having a solid content of 45 wt % was obtained in the same manner as in Example 1, except that 11.23 g (0.040 mol) of 4,4'-methylenebis(2-ethyl-6-methylaniline) was used instead of 3,5-DABA.

[0083] Comparative Example 2 A separable three-neck glass flask was equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark apparatus. 245.01 g (0.288 mol) of KF-8010, 62.87 g (0.288 mol) of PMDA, 1.44 g (0.014 mol) of valerolactone, 2.28 g (0.029 mol) of pyridine, 553 g of NMP, and 70 g of toluene were charged and stirred at 180 rpm for 30 minutes under a nitrogen atmosphere at room temperature, and then heated to 180°C. During the reaction, water was removed by azeotropy with toluene. After confirming the distillation of water, the mixture was heated and stirred for 6 hours, cooled, and 1.94 parts by weight of KL-700 (a 100 wt% leveling agent manufactured by Kyoeisha Chemical Co., Ltd.) was added. The mixture was then further cooled to room temperature to obtain a pressure-sensitive adhesive resin composition with a solids content of 35 wt%.

[0084] Comparative Example 3 A pressure-sensitive adhesive resin composition having a solid content of 45 wt % was obtained in the same manner as in Example 1, except that 11.62 g (0.040 mol) of 1,3-bis(3-aminophenoxy)benzene was used instead of 3,5-DABA.

[0085] Comparative Example 4 A pressure-sensitive adhesive resin composition having a solid content of 45 wt % was obtained in the same manner as in Example 1, except that 7.96 g (0.040 mol) of 4,4'-diaminodiphenyl ether was used instead of 3,5-DABA.

[0086] Comparative Example 5 An adhesive resin composition having a solid content of 45 wt % was obtained in the same manner as in Example 1, except that 8.44 g (0.040 mol) of 3,3'-diaminobenzophenone was used instead of 3,5-DABA.

[0087] 2. Evaluation of properties of polyimide resin composition and adhesive film The adhesive resin compositions synthesized in Examples 1 to 5 and Comparative Examples 1 to 5 were applied to a SUS plate with a spin coater so that the adhesive layer thickness was 8 μm. Then, for the resins of Examples 1 to 4 and Comparative Examples 1, 3 to 5, the resins were dried at 120 ° C. for 10 minutes and then at 180 ° C. for 20 minutes, and for the resins of Example 5 and Comparative Example 2, the resins were dried at 120 ° C. for 10 minutes and then at 220 ° C. for 20 minutes. The drying conditions were changed in this way to make the amount of residual solvent uniform even when solvents with different boiling points were used in the examples and comparative examples, but such changes in drying conditions do not affect the properties of the adhesive film.

[0088] (1) Glass transition temperature Tg (°C) After drying, the resin of the adhesive layer obtained was scraped off with a cutter or the like, and about 10 mg was placed in an aluminum standard container. The resin was measured using a differential scanning calorimeter (DSC), and the glass transition temperature (°C) was determined from the inflection point of the obtained DSC curve. After pre-drying at 80°C for 30 minutes, the measurement was performed at a heating rate of 10°C / min.

[0089] (2) Thermal weight loss rate (%) After drying, the resin of the adhesive layer obtained was scraped off with a cutter or the like, and about 15 mg of the resin was placed in a standard aluminum container and measured using a thermogravimetric analyzer TG-DTA. The measurement conditions were to raise the temperature to 400°C at a rate of 5°C / min, and measure the weight loss rate (%) from 30 to 300°C.

[0090] Next, on a 50 μm thick polyimide film, the resin compositions synthesized in Examples 1 to 5 and Comparative Examples 1 to 5 were applied with a spin coater so that the adhesive layer thickness was 8 μm, and then, for the resins of Examples 1 to 4 and Comparative Examples 1, 3 to 5, it was dried at 120 ° C. for 10 minutes and then at 180 ° C. for 20 minutes, and for the resins of Example 5 and Comparative Example 2, it was dried at 120 ° C. for 10 minutes and then at 220 ° C. for 20 minutes to obtain an adhesive film. For Examples 1 to 4, it was dried at 120 ° C. for 10 minutes and then at 180 ° C. for 20 minutes, and for Example 5 and Comparative Examples 1 and 2, it was dried at 120 ° C. for 10 minutes and then at 220 ° C. for 20 minutes to obtain an adhesive film.

[0091] (3) Adhesive strength Next, the obtained adhesive film was laminated to a 125 μm thick copper plate (C-7025) at 25 ° C using a laminator. The initial value was measured by peeling the adhesive film from the copper plate in a 90 ° direction at room temperature. After that, after heat treatment at 175 ° C for 2 hours, 220 ° C for 0.5 hours, and then at 175 ° C for 1 hour, the adhesive film was peeled from the copper plate in a 90 ° direction at room temperature and the adhesive strength was measured. Since there is some variation in adhesive strength, the average value (rounded off) of the values ​​measured five times was taken. In addition, the transfer of adhesive from the adhesive film to the copper plate (glue residue) after the adhesive strength measurement was confirmed.

[0092] (4) Sealing resin leakage and warpage of substrates laminated with adhesive film: This adhesive film was attached to a copper lead frame (C-7025, 125 μm thick, size: 65 mm x 250 mm, linear expansion coefficient 17.6 ppm / °C) at 25°C, heat treated at 175°C for 2.0 hours and at 220°C for 0.5 hours, and then transfer molded with an epoxy-based sealing material (linear expansion coefficient 12 ppm / °C) at 175°C, 8 MPa pressure, and 5 minutes. After molding, leakage of the molding resin from the outer lead portion to which the adhesive film was attached was visually confirmed. The amount of warpage was also measured. The evaluation results are shown in Tables 1 and 2 below. The weight-average molecular weight of the polyimide resin obtained in each example and comparative example was approximately 25,000.

[0093]

[0094]

[0095] The resin composition containing the polyimide resin of the present invention has adhesiveness at room temperature, excellent heat resistance, and excellent removability, and therefore can be suitably used in the fields of heat-resistant adhesive films used in the process of encapsulating semiconductors or electronic components with encapsulating resin in semiconductor element mounting substrates such as lead frames, printed circuit boards, wafers, and encapsulating resin substrates for fan-out wafer-level packages, or in the field of heat-resistant adhesive films used in reflow processes, etc.

Claims

1. A solvent-soluble polyimide resin having a cyclic imide structure, characterized in that it has a repeating unit represented by the following general formula (1): (In the formula, Z is a tetracarboxylic dianhydride residue, and A is a diamine residue of a polysiloxane-based diamine, and a diamine residue having an anilide group and / or a diamine residue having a carboxyl group.) 2. The polyimide resin according to claim 1, wherein the polysiloxane diamine is represented by the following general formula (2), and the diamine residues of the polysiloxane diamine represented by the following general formula (2) account for 60 to 97 mol % of all diamine residues. (In the formula, n is a natural number and is an integer from 1 to 150. 1 and R 2 R are the same or different and each represents an alkylene group or a phenylene group having 1 to 40 carbon atoms. 3 ~R 6 are the same or different and represent an alkyl group having 1 to 40 carbon atoms, a phenyl group, or a phenoxy group.

3. The polyimide resin according to claim 1, wherein the combined content of said diamine residues having an anilide group and said diamine residues having a carboxyl group is 3 to 40 mol % of the total diamine residues.

4. The polyimide resin according to claim 1, wherein the diamine residue having a carboxyl group is a diamine residue of at least one diamine represented by the following general formulas (3) to (5): (In the formula, X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, or an ether group, p is an integer from 0 to 2, m1 is an integer from 0 to 4, and m2 is an integer from 0 to 4. However, when p is 0, m1 is an integer from 1 to 4.) 5. The polyimide resin according to claim 1, wherein the diamine residue having an anilide group is a diamine residue of at least one diamine represented by the following general formulas (6-1) to (6-3): (In the formula, R 1 ~R 8 are the same or different and represent an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and n1 to n8 each represent an integer of 0 to 4.

6. A resin composition comprising the polyimide resin according to claim 1 and an organic solvent.

7. The resin composition according to claim 6, wherein said resin composition contains an epoxy compound.

8. The resin composition according to claim 7, wherein the epoxy compound is a compound represented by the following formula (7):

9. The resin composition according to claim 6, wherein said organic solvent comprises cyclohexanone.

10. The resin composition according to claim 6, which has a glass transition temperature of -10 to 40°C after drying.

11. A pressure sensitive adhesive for use in the manufacture of semiconductors or electronic parts, comprising the polyimide resin according to claim 1.

12. An adhesive film for use in the production of semiconductors or electronic parts, comprising a heat-resistant film and the resin composition according to claim 6 laminated on at least one side thereof.

13. The adhesive film according to claim 12, wherein the surface of the heat-resistant film on which the resin composition is laminated has been subjected to a roughening treatment.

14. The pressure-sensitive adhesive film according to claim 12, further comprising a release-treated heat-resistant insulating film laminated on the surface of said resin composition laminated on at least one side of said heat-resistant film.

15. The adhesive film according to claim 12, which is an adhesive film used for attaching to a semiconductor element mounting substrate, and the semiconductor element mounting substrate is a lead frame, a printed circuit board, a wafer, and a sealing resin substrate for a fan-out wafer level package.

16. A method for manufacturing a semiconductor or electronic component, comprising the steps of: attaching the adhesive film according to claim 12 to a semiconductor element mounting substrate; and peeling off the adhesive film after heat treatment.

17. A method for producing the polyimide resin according to claim 1, comprising reacting a tetracarboxylic dianhydride, a polysiloxane-based diamine, a diamine having an anilide group and / or a diamine having a carboxyl group in the presence of a lactone-based catalyst.

Citation Information

Patent Citations

  • Heat-resistant adhesive composition

    JP1993156231A

  • Resin composition, heat resistant resin laminate film using the same, and metal-clad laminate film

    JP2007137933A

  • Photosensitive resin composition and flexible printed wiring board using the same

    JP2009276526A

  • Polyimide-based adhesive composition, cured product, adhesive sheet, laminate, and flexible printed board