Poly(ethylene terephthalate) film for vapor deposition and transparent gas-barrier film
By modifying the PET film surface to enhance the Lewis acid/base component and vapor-depositing aluminum oxide and silicon oxide, the PET film achieves improved gas barrier performance, addressing the insufficiency of existing PET films in barrier properties and maintaining transparency and cost-effectiveness.
Patent Information
- Application Number
- PCT/JP2024/014659
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
The existing polyethylene terephthalate (PET) films for transparent gas barrier applications do not achieve sufficient barrier performance even with an inorganic layer deposition due to inadequate surface modification, leading to insufficient gas barrier properties.
A PET film with a modified surface having a Lewis acid/base component of 6.5 mN/m or more, achieved through corona treatment, is used as a base for vapor-depositing an inorganic layer, specifically aluminum oxide and silicon oxide, to enhance the gas barrier properties without an additional overcoat.
This approach results in a transparent gas barrier film with improved barrier performance, maintaining excellent transparency and allowing for long-term storage of contents, while being cost-effective and maintaining barrier properties.
Smart Images

Figure JP2024014659_17102024_PF_FP_ABST
Abstract
Description
Polyethylene terephthalate film for vapor deposition and transparent gas barrier film
[0001] The present invention relates to a polyethylene terephthalate film (PET film) that is excellent in transparency, gas barrier properties, printability, and flexibility and is used as a packaging material for foods, medicines, electronic components, etc., which require airtightness, or as a base material for a transparent gas barrier film that has excellent properties as a gas blocking material, and to a transparent gas barrier film using the same.
[0002] Transparent gas barrier films are made by laminating an inorganic material onto a plastic film. Metal oxides are often used as the inorganic material from the viewpoint of transparency. In particular, films made by laminating silicon oxide, aluminum oxide, or mixtures of these metal oxides by vapor deposition or CVD are mainly commercially available (see, for example, Patent Document 1).
[0003] The surface of the PET film on which the inorganic material barrier layer is laminated is subjected to anchor coating to improve the adhesive strength between the barrier layer and the PET film or the barrier properties, or the surface of the PET film is modified with plasma or the like.
[0004] There is a laminate in which a polyamide resin film is subjected to corona treatment or the like to reduce the contact angle of water to 70° or less, and the contact angle of diiodomethane to 35° or less, preferably 10 to 20°, and an inorganic layer is laminated on the film, and a sealant film is laminated on the film, thereby improving the barrier stability against retort treatment (see, for example, Patent Document 2).
[0005] It also states that by forming a smooth layer on the surface of a PET film and increasing the surface free energy according to the Kitazaki-Hata theory (an extension of the Foulkes equation) to 30 mN / m to 40 mN / m, good adhesion and barrier properties can be achieved by special CVD (see, for example, Patent Document 3).
[0006] Furthermore, with regard to PET films for battery exteriors other than transparent gas barrier films, a polyester film for battery exteriors is known in which the static contact angle of diiodomethane is increased to 22° or more by subjecting the film surface to corona treatment or the like (see, for example, Patent Document 4).
[0007] Patent No. 2638797 JP 10-52879 WO 2015-025783 JP 2012-238491
[0008] However, according to the investigations of the present inventors, it has been found that the degree of corona treatment in the polyester film for battery exteriors described in Patent Document 4 is insufficient, and even if an inorganic layer is vapor-deposited, sufficient barrier performance cannot be obtained.
[0009] Therefore, an object of the present invention is to provide a PET film, which is a vapor-deposited raw sheet of a transparent gas barrier film, having an improved surface condition that improves barrier performance, without using an anchor coat in which another resin is laminated on the substrate or an overcoat in which a resin is laminated on the inorganic layer that serves as a barrier layer, in order to improve the gas barrier performance of the transparent gas barrier film having an inorganic substance formed on the PET film.An object of the present invention is also to provide a transparent gas barrier film using the PET film as a substrate, with improved barrier performance.
[0010] The present inventors have conducted extensive research into the optimal surface condition of the PET film used as the raw material in order to improve the barrier properties of a transparent gas barrier film having an inorganic layer laminated thereon, and have discovered a PET film with a surface condition that densifies the inorganic layer, leading to the present invention.
[0011] That is, the present invention includes the following: [1] A polyethylene terephthalate film for vapor deposition used in applications in which an inorganic layer is vapor-deposited, the polyethylene terephthalate film for vapor deposition having a modified surface on the side where the inorganic layer is vapor-deposited, the modified surface having a Lewis acid-base (AB) component of surface free energy of 6.5 mN / m or more. [2] The polyethylene terephthalate film for vapor deposition according to [1], wherein the modified surface is formed by corona treatment. [3] A transparent gas barrier film comprising a polyethylene terephthalate film having a modified surface having a Lewis acid-base (AB) component of surface free energy of 6.5 mN / m or more, and an inorganic layer vapor-deposited on the modified surface. [4] The transparent gas barrier film according to [3], wherein the modified surface is formed by corona treatment. [5] The transparent gas barrier film according to [3] or [4], wherein the inorganic layer contains aluminum oxide and silicon oxide.
[0012] The present invention provides a PET film for producing a transparent gas barrier film that is inexpensive, has excellent transparency, and can maintain its barrier properties, allowing contents to be stored for a long period of time. It also provides a transparent gas barrier film that uses the PET film as a substrate and has improved barrier properties.
[0013] 1 is a cross-sectional view for explaining a dynamic contact angle; FIG. 2 is a cross-sectional view for explaining a corona treatment; FIG. 3 is a schematic diagram of an electron beam heating type vapor deposition apparatus;
[0014] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits.
[0015] The polyethylene terephthalate film for deposition of the present invention is a polyethylene terephthalate film for deposition used in applications in which an inorganic layer is vapor-deposited, characterized in that it has a modified surface on the side on which the inorganic layer is vapor-deposited, and the surface free energy Lewis acid-base (AB) component of the modified surface is 6.5 mN / m or more.
[0016] The inorganic layer in the present invention may be made of a metal such as Al, Si, Ti, Zn, Zr, Mg, Sn, Cu, or Fe, or an oxide, nitride, fluoride, or sulfide of these metals. Specific examples include SiOx (x=1.0 to 2.0), alumina, magnesia, zinc sulfide, titania, zirconia, cerium oxide, or a mixture thereof.
[0017] In particular, aluminum oxide, silicon oxide and mixtures thereof are suitable for use as transparent gas barrier films, and the modified surface of the present invention is particularly effective for the binary vapor deposition of aluminum oxide and silicon oxide.
[0018] The PET film referred to in the present invention refers to a film obtained by melt-extruding a PET resin whose main raw material is polyethylene terephthalate obtained by polymerizing ethylene glycol and terephthalic acid, to which other polymers may be mixed to adjust the film properties, or to which known additives such as ultraviolet absorbers, antistatic agents, plasticizers, lubricants, and colorants may be added, and then, as necessary, stretching in the machine direction (MD) and / or the transverse direction (TD), cooling, and heat setting.
[0019] The thickness of the PET film is not particularly limited, but the thickness of the PET film of the present invention is preferably in the range of 5 to 1000 μm, and more preferably in the range of 7 to 25 μm for roll-to-roll vacuum deposition.
[0020] The Lewis acid-base (AB) component of surface free energy referred to in the present invention refers to the Lewis acid-base component of the method proposed by C. J. van Oss, R. J. Good, and R. J. Busscher, which is a method for determining the surface free energy of a solid from the contact angle between the solid and a probe liquid.
[0021] The Lewis acid / base (AB) component referred to in the present invention refers to a value determined from the contact angle of water, diiodomethane, and formamide, which are probe liquids.
[0022] Table 1 shows the Lifshitz-van der Waals (LW) components of the probe solution used in the present invention: γ LW , Lewis acid-base (AB) component: γ AB, acidic component (+): γ + , base component (-): γ - and total: γ total shows the surface free energy.
[0023]
[0024] The Lewis acid-base (AB) components in the present invention are calculated by solving the three equations given for the three probe liquids using the values in Table 1 as three simultaneous equations. AB S In Equation 1, the subscript S represents the solid PET film, L represents the liquid probe liquid, and θ is the contact angle between the probe liquid and the solid PET film.
[0025]
[0026] In the present invention, purified water with a resistivity of 18 MΩcm or more is used as the probe liquid. Diiodomethane is used as a special-grade reagent with a purity of 99% or more. Formamide is used as a special-grade reagent with a purity of 98.5% or more.
[0027] As shown in Figure 1, the dynamic contact angle referred to in the present invention is the internal angle (θ) formed between the tangent 3 to the surface of a droplet 2 and the surface of the PET film 1 one second after the droplet 2 is placed on the PET film 1. The contact angle measured one second after the droplet is a dynamic contact angle, and is a value measured under extremely short conditions among dynamic contact angles. On the other hand, the static contact angle described in paragraph 0052 of JP 2012-238491 is a contact angle generally measured after 30 to 60 seconds, and is a measurement value different from the dynamic contact angle.
[0028] The diiodomethane referred to in the present invention is a special grade diiodomethane having a purity of 99% or more. The dynamic contact angle referred to in the present invention is a value measured in an environment at room temperature of 23°C and humidity of 50%.
[0029] The Lewis acid-base (AB) component has a viscosity of 6.5 mN / m or more, preferably 7.0 mN / m or more. A viscosity of 6.5 mN / m or more tends to improve the water vapor transmission rate (WVTR). Even when forming an inorganic layer by vapor deposition, deterioration of the WVTR is minimized even in poor conditions of the vapor deposition apparatus and relatively high pressure. Furthermore, the Lewis acid-base (AB) component is preferably 8.5 mN / m or less. A viscosity of 8.5 mN / m or less reduces the occurrence of corona strike-through (the phenomenon in which the back side of the treated surface is treated), and reduces the occurrence of blocking when the film is wound into a roll.
[0030] In the present invention, as a preferred condition of the PET film, a method for increasing the Lewis acid-base (AB) component to 6.5 mN / m or more is preferably corona treatment.
[0031] Higher values of Lewis acid-base (AB) components are preferable, but since the PET film may be processed on surfaces other than the intended surface or may be damaged by heat during the processing process, the value should be set as high as possible within the allowable range of other physical properties.
[0032] Corona treatment is a method of treating the surface of PET with plasma by generating a discharge in the atmosphere. For example, the corona treatment method shown in Figure 2 can be used to corona treat a long PET film. A high AC voltage of 10 to 60 kHz is applied to an electrode 4 in the atmosphere to cause a discharge. The PET film 6 to be treated runs over a dielectric-coated roll 5 covered with silicone rubber or the like, and is treated with plasma generated between the dielectric-coated roll 5 and the electrode 4.
[0033] The degree of treatment associated with the Lewis acid-base (AB) component can be adjusted by adjusting the distance between the electrode 4 and the dielectric-coated roll 5, the power applied to the electrode 4 and the dielectric-coated roll 5, and the running speed of the PET film 6.
[0034] Generally, the gap between the electrode 4 and the dielectric-coated roll 5 is set to 5 mm or less. If the gap is too large, discharge becomes difficult. If the gap is narrowed, the treatment degree increases and the value of the Lewis acid-base (AB) component rises. A narrow gap is preferable, but if it is too narrow, the electrode will deform and the film will flap, causing contact between the film and the electrode and scratches.
[0035] Increasing the power applied to the electrode 4 and the dielectric-coated roll 5 increases the degree of treatment and the value of the Lewis acid-base (AB) component. Simply increasing the power can cause abnormal discharge or the electrodes to overheat and deform, so the number and shape of the electrodes must be selected appropriately.
[0036] Furthermore, when the processing is performed with the same power, if the traveling speed of the PET film 6 is slowed down, the processing degree increases and the value of the Lewis acid-base (AB) component increases.
[0037] Although it is possible to supply gas such as nitrogen or helium between the discharge electrodes to generate a discharge, it is preferable to use normal atmospheric air containing 78% nitrogen and 21% oxygen. To ensure stable processing, a fixed amount of atmospheric air with a stable temperature and humidity is blown through a filter.
[0038] Corona discharge converts some of the oxygen in the air into ozone, which changes the surface of the PET film. Free release of ozone can have an adverse effect on the human body and also on the degree of surface treatment, so it is preferable to surround the corona treatment area and exhaust the air uniformly.
[0039] The corona treatment can be carried out on a PET film that has already been formed using a rewinder equipped with a corona treatment device or a slitter that changes the width of the film, but it is preferable to carry out the corona treatment on the PET film during film formation.
[0040] That is, it is preferable to melt the PET resin, extrude it through a T-die, stretch it in the MD (film running direction), stretch it in the TD (film width direction), and then treat it through a corona treatment machine.
[0041] By carrying out the treatment in the same step, not only can the treatment be carried out easily, but also the corona treatment can be carried out in a fresher state on the surface of the PET film, which is preferable.
[0042] Furthermore, the transparent gas barrier film of the present invention is a transparent gas barrier film characterized by laminating an inorganic layer on the above-mentioned PET film, that is, a transparent gas barrier film comprising a polyethylene terephthalate film having a modified surface in which the Lewis acid-base (AB) component of the surface free energy is 6.5 mN / m or more, and an inorganic layer vapor-deposited on the modified surface.
[0043] As a method for laminating an inorganic layer on the PET film of the present invention, a dry process using a vacuum is suitable. Among them, a vapor deposition method is suitable. The vapor deposition method allows for laminating an inorganic layer over a large area at high speed.
[0044] The deposition method can be any of the following: a resistance heating method in which the deposition material is evaporated using a resistance heating boat; an induction heating method in which the deposition material is placed in a carbon crucible and heated by applying a high-frequency electromagnetic field; and an electron beam heating method in which the deposition material is heated using an electron gun.
[0045] A schematic diagram of an electron beam heating type vapor deposition apparatus is shown in Fig. 3. A process for laminating an inorganic layer will be described, but the present invention is not limited to this.
[0046] A PET film (hereinafter referred to as the PET film of the present invention) having a modified surface with a Lewis acid-base (AB) component value of 6.5 mN / m or more is prepared on the unwinding roll 7 of the vapor deposition device.
[0047] The present PET film 8 is unwound from the unwinding roll 7 and its surface is treated by a plasma treatment device 9. The plasma treatment device 9 has electrodes and is designed to allow gas to be introduced between the electrodes and the present PET film 8. A direct current or alternating current voltage is applied to the electrodes to cause a discharge and generate plasma. The modified surface is treated by this plasma. The purpose of the plasma treatment is to remove moisture and other substances that adhere to the present PET film when it is stored in the atmosphere. For this purpose, a rare gas such as argon is preferably introduced.
[0048] After passing through the plasma treatment device 9, the present PET film 8 is transferred to a coating roll 10 cooled to −20° C. An electron beam 12 emitted from an electron gun 11 heats a deposition material 13 placed in a crucible, evaporating the material, and an inorganic layer is laminated on the modified surface of the present PET film 8.
[0049] A transparent gas barrier film (hereinafter referred to as the transparent gas barrier film of the present invention) having an inorganic layer laminated on the modified surface of the PET film 8 of the present invention has electrons charged on the surface of the transparent gas barrier film of the present invention removed by a static eliminator 14 before leaving the coating roll 10. The transparent gas barrier film of the present invention is detached from the coating roll 10 and taken up onto a take-up roll 17, but before that the film thickness or film thickness and composition of the laminated inorganic layer are measured using an optical film thickness meter 15, a fluorescent X-ray film thickness meter 16, or both. In order to achieve the target film thickness or film thickness and composition, the measured values are fed back to the electron gun 11, and the intensity and scanning of the electron beam 12 are adjusted to the target values.
[0050] The inorganic layer of the transparent gas barrier film of the present invention preferably has a thickness of 5 nm to 30 nm. If it is too thin, the film will not be uniform and the barrier properties will not be maintained. If it is too thick, the inorganic layer will crack when the transparent gas barrier film of the present invention is deformed, resulting in a decrease in the barrier properties.
[0051] As described above, aluminum oxide, silicon oxide, and mixtures thereof are suitable for the inorganic layer of the transparent gas barrier film of the present invention. A mixture of aluminum oxide and silicon oxide is particularly suitable. In particular, in the mixture of aluminum oxide and silicon oxide, the aluminum oxide content is preferably 20 to 60 mass %. When the aluminum oxide content is 20 mass % or more, the barrier properties are improved. When the content is 60 mass % or less, the inorganic layer does not become too hard, and it is possible to prevent the inorganic layer from cracking and the barrier properties from decreasing when the transparent gas barrier film is deformed.
[0052] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The physical properties and characteristics in the examples were measured or evaluated by the following methods.
[0053] (1) Dynamic Contact Angle The dynamic contact angle was measured in a room adjusted to a room temperature of 23°C and a humidity of 50%. The measuring device used was a DROP SHAPE ANALYER-DSA100 manufactured by KRUESS. Purified water from Trusco Nakayama Corporation was used. Special-grade diiodomethane from Nacalai Tesque Inc. was used. JIS special-grade formamide from Nacalai Tesque Inc. was used.
[0054] For the measurements, droplets were made with the amounts of liquid shown in Table 2. Water was dropped onto the surface of a PET film using a 0.5 mm diameter stainless steel needle, and diiodomethane formamide was dropped onto the surface of a PET film using a 0.5 mm diameter PTFE needle. After 1 second, the droplets were photographed and the contact angles were calculated using the θ / 2 method (width-height method). Measurements were taken at 10 points, and the average value was used as the contact angle of the sample.
[0055]
[0056] The measured contact angles of water, diiodomethane, and formamide and the values shown in Table 1 were applied to Equation 1 to calculate the surface free energy.
[0057] (2) Water Vapor Transmission Rate (WVTR) Water vapor transmission rate (WVTR) was measured in accordance with JIS K7129 Method B using a water vapor transmission rate measuring device (MOCON Corporation, USA, PRMATRAN-W3 / 34G) under measurement conditions of a temperature of 40°C and a humidity of 90% RH. (Example 1) PET resin was melted, extruded through a T-die, stretched in the MD direction, and then stretched in the TD direction. The PET film surface was treated with a corona treatment device. The contact angles of water, diiodomethane, and formamide on the surface of the formed PET film were measured, and the surface free energy Lewis acid-base (AB) component was calculated and confirmed. Corona treatment conditions were found under which the surface free energy Lewis acid-base (AB) component was 6.5 mN / m, and a PET film was formed under these confirmed conditions. After corona treatment, the film was wound up as a roll film on a take-up roll. The PET film had a thickness of 12 μm.
[0058] The wound PET film was slit to a width suitable for processing in an electron beam deposition apparatus, and the PET film was placed in an electron beam deposition apparatus as shown in Figure 3. Alumina and silica with a purity of 99% or higher were placed in a crucible. After evacuating the deposition apparatus, the placed PET film was withdrawn from the unwinding roll and passed through an argon gas plasma. A mixed film of alumina and silica was laminated as an inorganic layer on a coating roll cooled to -20°C. After laminating the alumina-silica film, the film was neutralized and peeled from the coating roll. The film thickness and composition were measured using a fluorescent X-ray film thickness meter. The electron gun was controlled to achieve a film thickness of 13 nm and an aluminum oxide content of 45% by mass. After winding the transparent gas barrier film on the winding roll and opening it to the atmosphere, a sample was taken of the film and its WVTR was measured. The results are shown in Table 3. The remaining PET film remaining on the unwinding roll was sampled, and the contact angles of water, diiodomethane, and formamide on the PET film surface were measured, and the surface free energy (Lewis acid-base (AB) component) was calculated. Table 3 shows the results.
[0059] (Examples 2 to 10) PET films were produced in the same manner as in Example 1. The treatment conditions of the corona treatment device were changed to obtain PET films with the surface free energy Lewis acid-base (AB) components shown in Table 3. An alumina-silica inorganic layer was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 3.
[0060] (Example 11) A PET film was produced in the same manner as in Example 4. The treatment conditions of the corona treatment device were changed to obtain a PET film with the surface free energy Lewis acid-base (AB) components shown in Table 3. Furthermore, a transparent gas barrier film was produced under the same conditions as in Example 4, except that instead of laminating an inorganic layer of alumina-silica, only alumina with a purity of 99% or more was laminated, and the WVTR was measured. The results are shown in Table 3.
[0061] Comparative Examples 1 to 4 PET films were produced in the same manner as in Example 1. The treatment conditions of the corona treatment device were changed to obtain PET films with the surface free energy Lewis acid-base (AB) components shown in Table 3. An alumina-silica inorganic layer was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 3.
[0062] Comparative Example 5 A PET film was formed in the same manner as in Example 1. However, the corona treatment was stopped during the formation of the PET film. An inorganic layer of alumina-silica was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 3.
[0063] (Comparative Example 6) A transparent gas barrier film was produced under the same conditions as in Example 1 of the present application using a PET film that had been subjected to a corona treatment under the same conditions as in Example 1 of JP 2012-238491 A, and the WVTR was measured. That is, a PET film was produced in the same manner as in Example 1 of the present application, and then a corona discharge treatment was applied to the upper surface of the film with an E value of 30, and the film was taken up to obtain a polyester film. The results are shown in Table 3. The E value is the corona discharge treatment intensity, and is a function of the applied voltage (Vp), applied current (Ip), treatment speed (S), and treatment width (Wt), where E = (Vp × Ip) / (S × Wt).
[0064] Comparative Example 7 A transparent gas barrier film was produced under the same conditions as in Example 1 of the present application using a PET film that had been subjected to a corona treatment under the same conditions as in Example 3 of JP 2012-238491 A, and the WVTR was measured. That is, a PET film was produced in the same manner as in Example 1 of the present application, and then the upper surface of the film was subjected to a corona discharge treatment with an E value of 60 and taken up to obtain a polyester film. The results are shown in Table 3.
[0065]
[0066] As the results in Table 1 show, in Examples 1 to 11, the surface free energy Lewis acid-base (AB) component was 6.5 mN / m or more, and therefore the WVTR of the transparent gas barrier films using those PET films was low. This is thought to be because a dense inorganic layer could be formed, and as can be seen from a comparison between Examples 4 and 11, this effect was particularly remarkable when an alumina-silica inorganic layer was formed. In contrast, in Comparative Examples 1 to 7, the surface free energy Lewis acid-base (AB) component was less than 6.5 mN / m, and therefore the WVTR of the transparent gas barrier films using those PET films was high.
[0067] The present invention can provide a PET film that is a substrate for producing a transparent gas barrier film that has excellent properties as a gas barrier material, and can also provide a transparent gas barrier film that uses the substrate and has excellent properties as a gas barrier material.
[0068] 1: Substrate (PET film) 2: Droplet (diiodomethane, etc.) 3: Tangent line 4: Electrode 5: Dielectric-coated roll 6: PET film 7: Unwinding roll 8: PET film of the present invention 9: Plasma treatment device 10: Coating roll 11: Electron gun 12: Electron beam 13: Vapor deposition material 14: Static neutralizer 15: Optical film thickness gauge 16: Fluorescent X-ray film thickness gauge 17: Winding roll
Claims
1. A polyethylene terephthalate film for deposition used in applications in which an inorganic layer is deposited, the polyethylene terephthalate film having a modified surface on the side on which the inorganic layer is deposited, the modified surface having a Lewis acid-base (AB) component of the surface free energy of 6.5 mN / m or more.
2. The polyethylene terephthalate film for deposition according to claim 1, wherein the modified surface is formed by corona treatment.
3. A transparent gas barrier film comprising: a polyethylene terephthalate film having a modified surface in which the Lewis acid-base (AB) component of the surface free energy is 6.5 mN / m or more; and an inorganic layer vapor-deposited on the modified surface.
4. The transparent gas barrier film according to claim 3, wherein the modified surface is formed by corona treatment.
5. The transparent gas barrier film according to claim 3 or 4, wherein the inorganic layer contains aluminum oxide and silicon oxide.
Citation Information
Patent Citations
Vapor deposited film
JP1987077453A
Polyester-based film for vapor deposition
JP1991126860A
Gas barrier laminated film and its manufacturing method
JP2007210208A
Vapor-deposited polyester film
JP2017065264A