Method for producing sio2 hardened body

A method using SiO2 raw materials, alcohol, and catalysts to produce a cement-free concrete substitute with high compressive strength and durability, addressing the carbon footprint and material scarcity issues in traditional concrete production.

WO2024214833A1PCT designated stage expired Publication Date: 2024-10-17THE UNIV OF TOKYO
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015013
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-15
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The production of concrete emits significant carbon dioxide due to cement usage, and there is a shortage of high-quality sand and gravel, necessitating alternative materials that can be efficiently produced without these limitations.

Method used

A method involving a mixture of SiO2 raw materials, an alcohol compound, and a catalyst compound, heat-treated at low temperatures, followed by hot pressing and optional heating and baking, to create a cured product with high compressive strength, which can serve as a cement-free concrete substitute.

Benefits of technology

The method produces a durable, low-cost concrete substitute with minimal volume change, resistance to water and acid deterioration, and rapid strength development, maintaining compressive strength even after water immersion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015013_17102024_PF_FP_ABST
    Figure JP2024015013_17102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide a novel method for producing an SiO2 hardened body that can be a concrete substitute without using a cement in the manufacturing process of which a large amount of carbon dioxide is emitted. [Solution] It was newly found that a large-sized SiO2 hardened body can be obtained using a general-purpose facility compared with a conventional method, by adding an alcohol compound and a catalyst compound to an SiO2-containing material, heat-treating the resultant mixture at a relatively low temperature, and then hot-pressing and heat-firing. Thus, the SiO2 hardened body having a high compressive strength can be efficiently obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method of SiO2 hardened body

[0001] The present invention is directed to the production of SiO2 such as sand and gravel. 2 The present invention relates to a method for efficiently obtaining a hardened body from an inclusion.

[0002] Concrete is the most widely used construction material in the world. Cement is used as the main ingredient in concrete, but cement has the problem of emitting a large amount of carbon dioxide during its production. In addition, there is a global shortage of high-quality sand and gravel, the main raw materials for cement, so the development of cement-free alternative materials for concrete has become an urgent issue (see, for example, Patent Document 1).

[0003] Requirements for alternative materials include the availability of almost unlimited raw materials and the ability to be reused. In this regard, sand and gravel, primarily composed of silicon, are the most abundant materials on Earth. If construction materials could be directly produced from these materials, they would be considered viable alternatives to concrete. However, practical concrete alternatives have yet to be fully realized. Meanwhile, the present inventors have previously developed a method for producing a hardened product by placing sand or gravel in alcohol and an alkali metal and treating it at high temperatures in a sealed container to chemically bond the sand and gravel together (Patent Document 2). However, high-temperature treatment in a sealed container generates high pressures, which necessitates expensive, pressure-resistant equipment.

[0004] JP 2019-6610 A JP 2021-127264 A JP 2019-119736 A

[0005] Therefore, the present invention provides a concrete substitute that does not use cement, which emits a large amount of carbon dioxide during the manufacturing process. 2 The object of the present invention is to provide a novel method for producing a cured product.

[0006] As a result of extensive research into solving the above problems, the present inventors have found that SiO 2 A raw material containing SiO 2The mixture of the alcohol compound and the catalyst compound is heated at a relatively low temperature, and then hot pressed (and optionally heated and fired) to produce a large SiO2 powder using general-purpose equipment, which is easier than conventional methods. 2 SiO that can obtain a hardened body and has high compressive strength 2 The present inventors have newly discovered that a cured product can be efficiently obtained, and have completed the present invention.

[0007] That is, in one aspect, the present invention provides SiO 2 Regarding the method for producing a cured body, more specifically, 2 A method for producing a cured body, comprising: a) forming a SiO 2 a) preparing a mixture by mixing a raw material containing the compound, an alcohol compound, and a catalyst compound, wherein the catalyst compound is an alkali metal salt or an alkaline earth metal salt; b) heat-treating the mixture obtained in the step a); c) hot-pressing the treated product obtained in the step b); and d) optionally heating and calcining the treated product obtained in the step c); 2 The hardened body is SiO 2 SiO present on the surface of the raw material containing 2 The SiO 2<2> The manufacturing method according to the above <1>, wherein at least a part of the processed product obtained in the step c) is in a gelled state; <3> The manufacturing method according to the above <1>, wherein the hot pressing in the step c) is carried out under conditions of a temperature in the range of 20 to 200°C and a pressure in the range of 1 to 100 MPa; <4> The manufacturing method according to the above <1>, wherein the hot pressing time in the step c) is 10 seconds to 1 hour; <5> The manufacturing method according to the above <1>, wherein at least a part of the processed product obtained in the step b) is in a liquefied or gelled state; <6> The manufacturing method according to the above <1>, wherein the heating temperature in the step b) is in the range of 90 to 200°C; <7> The manufacturing method according to the above <1>, wherein the heating time in the step b) is 1 hour to 10 days; <8> The manufacturing method according to the above <1>, further comprising a step of drying the processed product obtained in the step c) at 200°C or less before the step d); <9> The manufacturing method according to the above <1>, wherein the heating and firing in the step d) is carried out at a temperature in the range of 300 to 800°C; <10> The manufacturing method according to the above <1>, wherein the heating and firing time in the step d) is 1 to 24 hours; <11> The SiO 2 <12> The method according to the above <1>, wherein the raw material containing SiO includes silica stone, silica sand, diatomaceous earth, quartz, or silica; 2 <13> The manufacturing method according to the above <1>, wherein the raw material containing SiO is an inorganic material selected from sand, gravel, coal ash, biomass combustion ash, and combinations thereof; 2 The raw material containing 10% by weight or more of SiO 2 <14> The manufacturing method according to the above <1>, comprising: 2<15> The manufacturing method according to the above <1>, wherein the raw material containing the above has a particle shape with a particle size in the range of 1 nm to 10 cm; <16> The manufacturing method according to the above <1>, wherein the alcohol compound is ethanol; <17> The manufacturing method according to the above <1>, wherein the catalyst compound is at least one selected from the group consisting of hydroxides, halides, sulfates, carbonates, and hydrogencarbonates of alkali metals or alkaline earth metals; <18> The manufacturing method according to the above <1>, wherein the catalyst compound is potassium hydroxide (KOH), sodium hydroxide (NaOH), calcium hydroxide (Ca(OH) 2 <19> The manufacturing method according to the above <18>, wherein the catalyst compound is a combination of potassium hydroxide and calcium hydroxide; <20> The manufacturing method according to the above <19>, wherein the ratio of potassium hydroxide to calcium hydroxide is in the range of 1:1 to 2:1 by weight; <21> The manufacturing method according to the above <1>, wherein the amount of catalyst compound added to the mixture is 10 to 60% by weight.

[0008] In another aspect, the present invention provides a SiO 2 The present invention also relates to a cured product and a gel composition containing the same, more specifically, <22> SiO 2 The inclusions are bonded to each other by chemical bonds. 2 A hardened body, the compressive strength of which after immersion in water is maintained at 50% or more of that before immersion. 2 <23> A cured product according to the above <22>, having a compressive strength of 20 MPa or more after immersion in water. 2 Cured body; <24>SiO 2 The inclusions are bonded to each other by chemical bonds. 2 A cured body component and a tetraalkoxysilane component (Si(OR) 4 and (ii) a gel composition comprising:

[0009] According to the present invention, it is possible to produce a SiO 2It is possible to obtain a hardened body in which the raw materials are directly bonded to each other, and it is possible to provide a new concrete substitute or the like at low cost and efficiently. In addition, according to the manufacturing method of the present invention, it is possible to produce a large SiO 2 SiO that can obtain a hardened body and has high compressive strength 2 A cured product can be obtained efficiently.

[0010] In addition, SiO obtained by the manufacturing method of the present invention 2 The hardened body is hardened without using conventional cement paste, and therefore has the following advantages, for example: - Small volume change due to drying and wetting; - Small creep change; - Deterioration caused by calcium elution due to water or acid can be suppressed; - Deterioration due to alkali-aggregate reaction (the phenomenon of aggregate expansion in an alkaline environment) can be suppressed; - The time required for strength development can be shortened (while it takes about one month for ordinary concrete, this can be done in about 24 hours with the present invention); - The alkali metal compound used in the manufacturing process is a catalyst, so it can be reused. - The alcohol compound used in the manufacturing process also returns to its original state after high-temperature treatment, so it can be reused.

[0011] Figure 1 is a graph showing the particle size distribution of the raw silica sand used in the examples. 2 3 is an image of a cured product. 2 The SiO obtained when the concentration of ethanol added to the raw material was changed 2 4 is a graph showing the compressive strength and porosity of the hardened body. 2 SiO obtained when the concentration of KOH added to the raw material was changed 2 5 is a graph showing the compressive strength and porosity of the hardened body. 2 1 is a graph showing the compressive strength and porosity of the hardened body.

[0012] The following describes embodiments of the present invention. The scope of the present invention is not limited to these descriptions, and other than the following examples, the present invention can be implemented with appropriate modifications within the scope that does not depart from the spirit of the present invention.

[0013] 1. Method for producing a cured product of the present invention The method for producing a cured product of the present invention is 2 The method for producing a cured body is characterized by comprising the following steps a) to d): a) SiO 2 a) preparing a mixture by mixing a raw material containing the above, an alcohol compound, and a catalyst compound; b) heat-treating the mixture obtained in step a); c) hot-pressing the treated product obtained in step b); and d) optionally, heating and calcining the treated product obtained in step c).

[0014] The SiO obtained here 2 The hardened body is SiO 2 Raw material containing (SiO 2 SiO present on the surface of the raw material 2 At least some of the components are bonded to each other by chemical bonds (Si—O—Si), and multiple SiO 2 It is an aggregate (hardened body) in which the raw materials are directly bonded together. 2 is known to produce porous silica by sol-gel reaction, but the present invention is 2 Only the surface of the raw material is sol-formed, and SiO 2 The embodiment of a hardened body in which raw materials are bonded together is also included. 2 The bonding between the raw materials can involve not only the above-mentioned chemical bonding but also mechanical bonding (adhesion) and physical bonding (van der Waals force, etc.). 2 In the cured body, not only such mechanical or physical bonding but also SiO 2 At least some of the components are characterized by forming chemical bonds with each other.

[0015] Without necessarily being bound by theory, in the manufacturing method of the present invention, SiO 2 The mechanism by which a hardened body is obtained is presumed to be as follows. 2They reported that the organosilicon compound tetraalkoxysilane can be obtained by decomposing and dehydrating the raw material (Chemistry Letters 2016 45:7, 828-830). This reaction is represented by the following reaction formula (1).

[0016] In the paper by Fukaya et al., the reaction product water (H 2 By removing O, the equilibrium of the reaction equation shifts to the right, and tetraalkoxysilane (Si(OR) 4 ) is efficiently produced. Since the reaction in equation (1) is a reversible equilibrium reaction, SiO 2 This can be interpreted as the repeated breaking and regeneration of chemical bonds.

[0017] Conventionally, this reaction has been applied to the synthesis of tetraalkoxysilane (Si(OR) 4 Attempts have been made to efficiently produce H on the right side of formula (1) using molecular sieves, dehydrating agents, etc. (for example, JP 2019-119736 A). 2 Tetraalkoxysilane can be obtained by removing O and promoting the equilibrium reaction to the right side. In this case, the product is tetraalkoxysilane, not SiO on the left side. 2 is not produced, and a hardened product thereof is not obtained.

[0018] Furthermore, Patent Document 2 (JP 2021-127264 A) focuses on such an equilibrium reaction and 2 The above reaction formula (1) is applied to the raw material, and once tetraalkoxysilane is produced, SiO 2 By regenerating SiO 2 SiO present on the surface of the raw material 2 The components bond to each other and SiO 2 It is disclosed that an aggregate (hardened body) in which raw materials are directly bonded to each other is obtained. However, the method disclosed in Patent Document 2 requires a dehydration operation by adding dimethoxypropane (DMP) or the like in the process of producing the hardened body, and the degree of hardness and strength of the obtained hardened body are not sufficient.

[0019] In contrast, the present invention uses SiO 2 SiO in raw materials 2 The component is converted into SiO by the above reaction formula (1). 2 However, unlike the conventional method, the method does not add a dehydrating agent in the production process, but instead involves hot pressing the mixture and then heating and firing it, making it easier to produce large SiO2 particles using general-purpose equipment than conventional methods. 2 SiO that can obtain a hardened body and has high compressive strength 2 It can be said that the feature of this invention is that it has been newly discovered that a hardened body can be obtained efficiently.

[0020] In the present invention, "SiO 2 Raw material containing SiO 2 The "raw material" is SiO 2 There are no particular limitations on the material as long as it contains a certain amount of SiO , and it may be a natural mineral, an artificial object, a material of biological origin, or the like. Examples of natural minerals include silica stone, silica sand, diatomaceous earth, quartz, and opal. Examples of artificial objects include ordinary glass, silica gel, fumed silica, silica alumina, zeolite, glass beads, glass fiber, and glass wool. Examples of biological materials include diatom shells, radiolarian skeletons, plant combustion ash, and plant silica bodies contained in plants (so-called plant opals). Preferably, SiO 2 The raw material may include silica stone, silica sand, diatomaceous earth, quartz, silica, or a combination of one or more thereof, and may also include, for example, granite, rhyolite, etc. From the viewpoint of availability, typically, SiO 2 The raw material may be an inorganic material selected from sand, gravel, coal ash, biomass combustion ash, and combinations thereof. Such gravel or sand may be used as aggregate in the production of concrete or mortar. The sand may be gravel from extraterrestrial celestial bodies (such as the Moon) called regolith, or simulated sand that imitates regolith.

[0021] SiO used in the present invention 2The raw material contains 10% by weight or more of SiO 2 Preferably, the content of SiO is 45% by weight or more, and particularly preferably 60% by weight or more. 2 A raw material containing the following can be used.

[0022] In addition, SiO 2 From the viewpoint of efficiency during the curing reaction, it is preferable that the raw material has a particulate or approximately particulate shape. In this case, the particle size (average particle size) can be in the range of 1 nm to 10 cm, typically 1 μm to 10 cm, preferably 10 μm to 5 cm, and more preferably 100 μm to 3 cm. However, as mentioned above, SiO 2 The raw material does not need to be in a perfect particle shape, and may be in an uneven shape like sand or gravel, so the "particle size" here should be understood to represent an approximate size. By the manufacturing method of the present invention, SiO particles having such a particle shape or an approximately particle shape can be bonded together and integrated. 2 A hardened body is obtained.

[0023] <Step a)> As described above, step a) in the production method of the present invention comprises the steps of: 2 This is a process for preparing a mixture of the raw material, 2) an alcohol compound, and 3) a catalyst compound, which allows the chemical equilibrium state shown in the above reaction formula (1) to be achieved.

[0024] The alcohol compound used in step a) can be an alcohol having a linear or branched alkyl, and the alkyl moiety may be substituted with an optional substituent. The alcohol compound is preferably an alcohol having 1 to 10 carbon atoms, more preferably an alcohol having 1 to 5 carbon atoms. Typically, the alcohol compound is methanol or ethanol, and preferably ethanol. The alcohol compound can be a raw material for obtaining the tetraalkoxysilane on the right side of the above reaction formula (1), but can also return to the alcohol on the left side in the overall equilibrium reaction.

[0025] The alcohol compound is typically added to the mixture in the form of an alcohol solution containing water. The concentration of the alcohol solution is preferably 20% by volume (v / v%) or more, more preferably 50% by volume or more, and even more preferably 80% by volume or more. In a preferred embodiment, the volume of the alcohol solution is in the range of 50 to 95% by volume, particularly preferably 80 to 99% by volume.

[0026] The amount of the alcohol solution containing the alcohol compound added in step a) can be appropriately set, but is preferably 1 to 50 parts by weight, more preferably 1 to 15 parts by weight, per 100 parts by weight of the raw material mixture.

[0027] The catalyst compound used in step a) is an alkali metal salt or alkaline earth metal salt, and is SiO 2 This component promotes the cleavage of the silicon-oxygen bond in the reaction mixture, and functions as a catalyst for the production of alkoxysilane on the right side of the above reaction formula (1).

[0028] Examples of the alkali metals and alkaline earth metals in such alkali metal salts and alkaline earth metal salts include lithium (Li), sodium (Na), magnesium (Mg), potassium (K), calcium (Ca), and cesium (Cs). Examples of the counter anions include hydroxides, halides, oxides, carbonates, bicarbonates, alkoxides, silicates, aluminates, phosphates, organic acid salts, sulfates, and nitrates. Among these, hydroxides, halides, carbonates, and bicarbonates are preferred, with alkali metal hydroxides, alkali metal halides, alkali metal carbonates, and alkali metal bicarbonates being more preferred.

[0029] Specific examples of the catalyst compound include lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide, cesium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, sodium fluoride, potassium fluoride, and cesium fluoride. The catalyst compound may be used alone or in combination of two or more. The alkali metal compound is preferably at least one selected from the group consisting of hydroxides, halides, sulfates, carbonates, and hydrogencarbonates of alkali metals or alkaline earth metals.

[0030] In a preferred embodiment, the catalyst compound is potassium hydroxide (KOH), sodium hydroxide (NaOH), calcium hydroxide (Ca(OH) 2 ), or a combination thereof. Particularly preferably, the catalyst compound is a combination of potassium hydroxide and calcium hydroxide, and the ratio of potassium hydroxide to calcium hydroxide is in the range of 1:1 to 2:1 by weight. By using such a mixture containing calcium hydroxide, the final SiO 2 This is preferable in that it can suppress distortion in the hardened body and provide a hardened body with higher strength. Here, a mixture of sodium hydroxide and calcium hydroxide can also be used instead of potassium hydroxide.

[0031] The amount of catalyst compound to be added is not particularly limited, but preferably, SiO 2 The amount of the catalyst compound is in the range of 0.01 to 50 parts by weight based on the raw material. The catalyst compound can be added in the form of a solution in which the catalyst compound is dissolved, and preferably, the solution contains 10 to 30% by weight of the catalyst compound.

[0032] SiO in step a) 2 The amount of the raw material present can be set as appropriate, but is preferably 1 to 50 parts by weight, more preferably 1 to 30 parts by weight, per 100 parts by weight of the alcohol compound.

[0033] In a preferred embodiment, the mixture obtained in step a) does not contain a starting aprotic organic solvent, such as acetals or ethers, such as dimethoxypropane.

[0034] The amount of alkali metal compound or alkaline earth metal compound added in step a) is preferably SiO 2 It is 1 to 20 parts by weight, more preferably 13 to 20 parts by weight, per 100 parts by weight of the raw material containing

[0035] <Step b)> Next, in step b) of the production method of the present invention, the mixture obtained in step a) is heat-treated at a relatively low temperature to promote the reaction toward the right side of the above reaction formula (1), thereby producing SiO 2 SiO in raw materials 2 A part or all of the tetraalkoxysilane component (Si(OR) 4 ) is converted into SiO. 2 At least a portion of the raw material is in a liquefied state or a gelled state (alkali silica gel).

[0036] The heat treatment in step b) is preferably carried out at a temperature in the range of 40 to 300°C, more preferably in the range of 90 to 200°C. The heating time can be appropriately set depending on the amount of reactants, etc., but is typically in the range of 1 hour to 10 days, preferably 5 to 8 days. The heat treatment is typically preferably carried out at a temperature of about 110°C for 7 days.

[0037] Step b) can be carried out under any pressure conditions, but is usually 0.1 MPa or more, preferably 0.5 MPa or more, more preferably 1.0 MPa or more, and usually 60 MPa or less, preferably 30 MPa or less, more preferably 20 MPa or less. Therefore, step b) can be carried out in a pressure-resistant and heat-resistant reactor such as an autoclave.

[0038] <Step c)> Step c) in the production method of the present invention is a step of pressing the partially liquefied treated product obtained in step b) under heated conditions (i.e., hot pressing). As a result, SiO 2 The components are regenerated and SiO 2 A hardened body in which the raw materials are directly bonded to each other is obtained, and SiO 2 This can increase the strength of the cured body. The hot press is preferably a physical press, i.e., it applies mechanical stress to compress the mixture. Therefore, the reactor may be provided with a means for pressing inside the reactor. For example, such a pressing means may be a metal plate with punch holes that can be driven vertically, which is placed inside the reactor and used to press the solid components in the mixture. In this case, the dimensions of the metal plate may be slightly smaller than the inner diameter of the reactor, allowing the liquid components in the mixture to escape upward through gaps with the reactor wall, thereby applying pressure only to the solid components.

[0039] The hot pressing in step c) is preferably carried out under high temperature and high pressure conditions. For example, the temperature can be in the range of 20 to 200°C, preferably 30 to 150°C, and the pressure can be in the range of 0.1 to 100 MPa, preferably 1.5 to 20 MPa.

[0040] The time for hot pressing can be appropriately set depending on the amount of reactants, etc., but is typically in the range of 10 seconds to 1 hour, preferably 1 to 30 minutes.

[0041] Preferably, at least a part of the treated product obtained in step c) is in a gelled state, and not completely in a state of SiO 2 It also includes components that have not hardened.

[0042] <Step d)> In the production method of the present invention, it is preferable to optionally carry out, as step d), a step of heating and calcining the treated product obtained in step c). By calcining at a high temperature, SiO 2 The hydrogen bonds on the surface of the inclusions can be converted into covalent bonds by a dehydration (condensation) reaction, and SiO 2 The strength of the inclusions can be increased.

[0043] The heating temperature in the calcination may be preferably in the range of 300 to 800° C., more preferably 500 to 800° C. The calcination time may be appropriately set depending on the amount of reactants, etc., but may typically be in the range of 1 to 24 hours, preferably 2 to 8 hours.

[0044] Furthermore, the dehydration reaction can be promoted more efficiently by carrying out the heating and baking under a reduced pressure environment. Here, "reduced pressure" includes a vacuum state.

[0045] In a preferred embodiment, the method may further include a step of drying the treated product obtained in step c) at 200° C. or less before the heating and calcining in step d).

[0046] Surprisingly, when a combination of sodium hydroxide and calcium hydroxide is used as the catalyst compound, SiO 2 having the desired properties can be obtained even if the heating and calcination in step d) is not performed for a short time or at all. 2 A hardened body was obtained.

[0047] 2. SiO obtained by the manufacturing method of the present invention 2 Physical properties of the cured product, i.e., SiO obtained by the manufacturing method of the present invention 2 The hardened product has excellent physical properties such as compressive strength and porosity, making it suitable as a concrete substitute.

[0048] More specifically, SiO obtained by the manufacturing method of the present invention 2 The cured product preferably has a compressive strength of 16 MPa or more, more preferably 20 MPa or more. 2 The hardened body has a compressive strength in the range of 16 to 50 MPa, more preferably in the range of 20 to 50 MPa.

[0049] The compressive strength of the cured product can be measured by a method known in the art. For example, 2After drying the cured product, the surface is cut using a low-speed cutter or the like, and a test is performed using a universal testing machine. The compressive strength fc (MPa) can be calculated by applying the load measured by the load cell to the following formula: where P is the maximum load (N) and d is the diameter (mm).

[0050] In particular, SiO obtained by the manufacturing method of the present invention 2 The hardened product maintains a relatively high compressive strength even after immersion in water, and is suitable for use in environments where water is present, which is a unique feature not found in conventional products. 2 The hardened body can maintain a compressive strength after immersion in water of preferably 50% or more, more preferably 70% or more, of that before immersion.

[0051] Thus, in another aspect, the present invention provides a method for producing a SiO 2 are bonded to each other by chemical bonds 2 A hardened body, the compressive strength of which after immersion in water is maintained at 50% or more of that before immersion. 2 The compressive strength of the hardened product after immersion in water is preferably 20 MPa or more, more preferably 25 MPa or more.

[0052] In addition, SiO obtained by the manufacturing method of the present invention 2 The cured body preferably has a porosity of 40% or less, more preferably 20% or less, and even more preferably 10% or less. 2 It has higher strength than the hardened body, and can be used as a concrete substitute to enhance its strength. When used in applications where high thermal insulation and sound insulation are required, SiO 2 It can also be made into a hardened product.

[0053] SiO 2 The porosity of the cured body corresponds to the "open porosity" defined in JIS R1634:1998. The porosity can be measured by a known method, for example, by the Archimedes method. 2The weight of the cured body containing the alcohol compound etc. was measured, and then the SiO 2 The contents are dried to an absolutely dry state, and the weight is measured. The porosity (%) can be calculated from the measured weight using the following formula.

[0054] Furthermore, as described above, the SiO obtained by the manufacturing method of the present invention 2 The cured product may be in a gel form in part, so in another aspect, the present invention provides a cured product comprising SiO 2 are bonded to each other by chemical bonds 2 A cured body component and a tetraalkoxysilane component (Si(OR) 4 ) and the gel composition.

[0055] The SiO of the present invention 2 The hardened product and compositions containing the same can be used for a variety of purposes, such as construction materials such as building materials and structural materials, raw materials for industrial products and crafts (e.g., containers, molds, tableware, decorative items, etc.), etc. In particular, when used as a construction material, it is useful as a concrete substitute material that can be produced without using cement.

[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0057] 1. SiO 2 Production of hardened body [Material] SiO 2 Commercially available silica sand (ST Craft) was used as the raw material. The chemical composition of the silica sand measured by fluorescent X-ray analysis was as shown in Table 1 below. Furthermore, according to the particle size distribution of the silica sand shown in Figure 1, 98.5% or more of the particles were less than 250 μm.

[0058] Silica sand was mixed with 0 to 40% by weight of KOH (weight % of KOH relative to the weight of silica sand), placed in a cylindrical container made of stainless steel foil, and stored in an autoclave. Ethanol (15 ml) of 0 to 99.5% by volume was added to the mixture. The autoclave was heated at 110°C for 7 days under saturated ethanol vapor pressure. The resulting mixed powder was hot-pressed at 105°C and 2.5 MPa for 1 minute, and then dried at 105°C for another 7 days. Finally, it was sintered at 500°C for 3 hours to obtain SiO 2 A cured product was obtained. An image of the obtained cured product is shown in Figure 2 (the raw material is on the left, and the cured product is on the right).

[0059] When the sample in the autoclave was observed before the hot pressing treatment, it was found to be in the form of a wet powder containing liquid, and no hardened body had been formed. This is because the desired SiO2 was not obtained by heat treatment at a relatively low temperature of about 110°C alone. 2 This indicates that no hardened product was obtained.

[0060] The obtained SiO 2 The compressive strength and porosity of the hardened specimens were measured. Compressive strength was measured using a universal testing machine (UH-1000kNC, Shimadzu Corporation) at a loading rate of 0.5 kN / min. Porosity was measured using 20 mm diameter × 30 mm diameter test specimens according to the Archimedes' principle in accordance with GB / T 8489-2006.

[0061] 1. Various conditions in the manufacturing process were changed and a comparative study was carried out.

[0062] 2-1. Examination of alcohol compound concentration SiO 2 The concentration of ethanol added to the raw material was varied in the range of 60 to 99.5% by volume (v / v%), and SiO 2 Cured bodies were prepared and their compressive strength and porosity were measured under the following reaction conditions: KOH content: 20 wt%, autoclave heating conditions: 110°C, 7 days, hot pressing conditions: 105°C, 2.5 MPa, 1 minute, drying time: 7 days, and firing conditions: 500°C, 3 hours.

[0063] The obtained SiO 2The compressive strength and porosity of the hardened body are shown in Figure 3. As a result, as the ethanol concentration increased, the compressive strength increased, reaching a maximum value of 38.55 MPa at an ethanol concentration of 90%. On the other hand, when the ethanol concentration was further increased to 99.5%, the compressive strength decreased to 7.88 MPa. This tendency is also due to the fact that when the ethanol concentration is too high, new SiO 2 This is thought to be because the formation of silica sand is prevented, while the ethanol concentration is too low, which reduces the solubility of silica sand in ethanol.

[0064] The porosity also decreased with increasing ethanol concentration, reaching a minimum value (17.93%) at an ethanol concentration of 90%. On the other hand, when the ethanol concentration was further increased to 99.5%, the porosity exceeded 30%. This is because the porosity decreased and SiO 2 It is believed that the higher compressive strength was achieved by the dense structure of the hardened body.

[0065] 2-2. Consideration of catalyst compound concentration Next, SiO 2 The concentration of KOH added to the raw material was changed in the range of 10 to 60 wt %, and SiO 2 Cured bodies were prepared and their compressive strength and porosity were measured. The reaction conditions were as follows: ethanol concentration: 90 v / v% (45 ml), autoclave heating conditions: 110°C, 7 days, hot pressing conditions: 105°C, 2.5 MPa, 1 minute, drying time: 7 days, firing conditions: 500°C, 3 hours. When no KOH was added, SiO 2 No hardened product was obtained.

[0066] The obtained SiO 2 The compressive strength and porosity of the hardened raw materials are shown in Figure 4. As a result, the maximum compressive strength (38.55 MPa) was obtained at a KOH concentration of 20% by weight. On the other hand, as the KOH concentration was increased further, the compressive strength gradually decreased. When these samples were analyzed using FT-IR analysis, it was found that the peaks resulting from the stretching of Si-O-Si bonds decreased with increasing KOH concentration. This is because when the KOH concentration exceeds a certain level, the SiO 2It is believed that the strength of the hardened body has decreased.

[0067] 2-3. Study of reaction time (heating time) Furthermore, the heating time (in the autoclave) after mixing the raw materials was changed in various ways, and the SiO 2 Cured bodies were prepared and their compressive strength and porosity were measured under the following reaction conditions: ethanol concentration: 90 v / v%, KOH content: 20 wt%, autoclave heating temperature: 110°C, hot pressing conditions: 105°C, 2.5 MPa, 1 minute, drying time: 7 days, and firing conditions: 500°C, 3 hours.

[0068] The obtained SiO 2 The compressive strength and porosity of the hardened raw material are shown in Figure 5. The compressive strength of the sample heated in an autoclave for one day was 2.82 MPa, but when heated for three days, it significantly increased to 20.43 MPa. Furthermore, when heated for six days, it increased to 38.31 MPa, and reached a maximum of 38.55 MPa after seven days. Conversely, the porosity of the compressive strength was at its lowest at 17.93% after seven days of heat treatment, and then tended to increase.

[0069] 2-4. Investigation of hot pressing and drying conditions The temperature and pressure in the hot pressing process and the subsequent drying process time were varied to obtain SiO 2 Cured bodies were prepared and their compressive strength and porosity were measured under the following reaction conditions: ethanol concentration: 90 v / v% (45 ml), KOH content: 20 wt%, autoclave conditions: 110°C, 6 days, hot press conditions: 20-105°C, 2.5-10 MPa, 1 minute, drying time: 1-7 days, and firing conditions: 500°C, 3 hours.

[0070] As a result, it was found that the compressive strength increased as the temperature and pressure in the autoclave heating conditions increased, as shown in Tables 2 to 4. Furthermore, the optimum drying time after heat treatment was 5 days.

[0071]

[0072] 2-5. Study of heating and firing conditions and strength changes after immersion in water The effects of the firing temperature and time after hot pressing on compressive strength and porosity were studied. In addition, the SiO 2 The change in compressive strength after immersing the hardened material in water for 24 hours was also examined. The reaction conditions were as follows: ethanol concentration: 90 v / v% (45 ml), KOH content: 20 wt%, autoclave conditions: 110°C, 6 days, hot press conditions: 105°C, 2.5 MPa, 1 minute, drying time: 3 days, and firing conditions: 500-800°C, 3-6 hours.

[0073] The results obtained are shown in Table 5 below.

[0074]

[0075] As a result, it was found that the compressive strength increased as the firing temperature increased and the firing time increased. In addition, when firing was performed at a temperature exceeding 700°C, the SiO 2 The hardened body maintained its compressive strength even after being immersed in water for 24 hours. In particular, when fired at 800°C for 3 hours, it retained 38.67 MPa even after being immersed in water, maintaining more than 80% of the compressive strength compared to before immersion.

[0076] 2-6. Examination of the type of catalyst compound SiO 2 Regarding the catalyst compound to be added to the raw materials, compounds other than KOH used in 1. were investigated. The reaction conditions were as follows: silica sand: 15 g, ethanol concentration: 90 v / v% (45 ml), catalyst compound content: 20 wt%, autoclave conditions: 110°C, 6 days, hot press conditions: 105°C, 2.5 MPa, 1 minute, drying time: 3 days, calcination conditions: 800°C, 3 hours.

[0077] First, as a catalyst compound, NaOH, Ca(OH) 2 A comparison of the results when 10% by weight of NaOH and KOH were used alone is shown in Table 6. As a result, it was found that the hardened body obtained when 10% by weight of NaOH was used had a higher compressive strength than when KOH was used.

[0078] A predetermined amount of Ca(OH)2 The results when the ratio was changed so that the total amount was 20 wt% are shown in Table 7. As a result, KOH:Ca(OH) 2 When the ratio was 4:2, the compressive strength of the hardened body was as high as 41.79 MPa.

[0079]

[0080] Next, a predetermined amount of Ca(OH) 2 and SiO using catalyst compounds whose ratios were changed so that the total amount was 10 wt %. 2 Surprisingly, NaOH and Ca(OH) 2 It was found that when the mixture of the above was used, a hardened body having high compressive strength could be obtained without any heating or sintering after hot pressing.

[0081] The compressive strength and porosity of the obtained hardened body are shown in Table 8. As a result, NaOH:Ca(OH) 2 When the ratio was 4:2, the compressive strength of the hardened body was as high as 49.71 MPa. In this case, the high compressive strength was maintained even after immersion in water.

Claims

1. SiO 2 A method for producing a cured body, comprising the steps of: a) forming a SiO 2 a) mixing a raw material containing the above-mentioned SiO with an alcohol compound and a catalyst compound, the catalyst compound being an alkali metal salt or an alkaline earth metal salt; b) heat-treating the mixture obtained in the above-mentioned step a); c) hot-pressing the treated product obtained in the above-mentioned step b); and d) optionally heating and calcining the treated product obtained in the above-mentioned step c), 2 The hardened body is SiO 2 SiO present on the surface of the raw material containing 2 The SiO 2 The manufacturing method of the present invention comprises the step of:

2. The method according to claim 1, wherein at least a portion of the treated product obtained in step c) is in a gelled state.

3. The method according to claim 1, wherein the hot pressing in step c) is carried out at a temperature in the range of 20 to 200° C. and a pressure in the range of 1 to 100 MPa.

4. The method according to claim 1, wherein the hot pressing time in step c) is from 10 seconds to 1 hour.

5. The method according to claim 1, wherein at least a portion of the treated product obtained in step b) is in a liquefied or gelled state.

6. The method according to claim 1, wherein the heating temperature in step b) is in the range of 90 to 200°C.

7. The method according to claim 1, wherein the heating time in step b) is from 1 hour to 10 days.

8. The method according to claim 1, further comprising a step of drying the treated product obtained in step c) at 200° C. or less before step d).

9. The method according to claim 1, wherein the heating and sintering in step d) is carried out at a temperature in the range of 300 to 800°C.

10. The method according to claim 1, wherein the heating and baking time in step d) is 1 to 24 hours.

11. The SiO 2 The method according to claim 1 , wherein the raw material containing the formula (I) comprises silica stone, silica sand, diatomaceous earth, quartz, or silica.

12. The SiO 2 2. The method of claim 1, wherein the feedstock containing is an inorganic material selected from sand, gravel, coal ash, biomass combustion ash, and combinations thereof.

13. The SiO 2 The raw material containing 10% by weight or more of SiO 2 The method of claim 1 , comprising:

14. The SiO 2 The method according to claim 1, wherein the raw material containing has a particle shape with a particle size in the range of 1 nm to 10 cm.

15. The method of claim 1, wherein the alcohol compound is ethanol.

16. The method according to claim 1, wherein the alcohol compound is a solution having an alcohol concentration of 50 to 95% by volume.

17. The method of claim 1, wherein the catalyst compound is at least one selected from the group consisting of hydroxides, halides, sulfates, carbonates, and hydrogen carbonates of alkali metals or alkaline earth metals.

18. The catalytic compound is potassium hydroxide (KOH), sodium hydroxide (NaOH), calcium hydroxide (Ca(OH) 2 ), or a combination thereof.

19. The process of claim 18, wherein the catalytic compound is a combination of potassium hydroxide and calcium hydroxide.

20. The method of claim 19, wherein the ratio of potassium hydroxide to calcium hydroxide is in the range of 1:1 to 2:1 by weight.

21. The method of claim 1, wherein the amount of catalyst compound added in the mixture is 10 to 60% by weight.

22. SiO 2 The inclusions are bonded together by chemical bonds to form SiO 2 A hardened body, the compressive strength of which after immersion in water is maintained at 50% or more of that before immersion. 2 Hardened body.

23. SiO according to claim 22, having a compressive strength of 20 MPa or more after immersion in water. 2 Hardened body.

24. SiO 2 The inclusions are bonded together by chemical bonds to form SiO 2 A cured body component and a tetraalkoxysilane component (Si(OR) 4 ). A gel composition comprising:

Citation Information

Patent Citations

  • Volcanic ejecta compound, method of producing the same, concrete composition, and cured product

    JP2019006610A

  • Manufacturing method of tetraalkoxysilane

    JP2019119736A

  • MANUFACTURING METHOD OF SiO2-CONTAINING HARDENED BODY

    JP2021127264A