Oriented polyester film and manufacturing method therefor
A stretched polyester film with controlled crystallinity, achieved through specific heat treatments, addresses the inefficiency in recycling processes by allowing simultaneous recycling with PET bottles, improving recycling efficiency by eliminating the need for film separation.
Patent Information
- Application Number
- PCT/KR2023/007889
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2023-06-08
- Publication Date
- 2024-10-17
AI Technical Summary
The recycling process for plastic containers like PET bottles is inefficient due to the need for pretreatment to separate polyester films, which have different crystallinity than the PET, preventing their simultaneous recycling.
A stretched polyester film with controlled crystallinity is developed by polymerizing a diol component and a dicarboxylic acid component, undergoing primary and secondary heat treatments to achieve a heat shrinkage rate of 40% or more at 80°C and specific melting temperatures, allowing it to be recycled without separation.
The film exhibits high crystallinity and heat shrinkability, enabling it to be recycled with PET bottles without pretreatment, thus enhancing recycling efficiency by eliminating the need for film separation.
Smart Images

Figure KR2023007889_17102024_PF_FP_ABST
Abstract
Description
Polyester stretch film and method for producing the same
[0001] The present invention relates to a polyester stretch film having heat shrinkability and controlled crystallinity, thereby increasing the efficiency of a recycling process, and a method for producing the polyester stretch film.
[0002] Among polymers, polyester resins are widely used in various fields due to their superior mechanical strength, heat resistance, transparency, and gas barrier properties. In particular, heat-shrinkable films manufactured using polyester resins exhibit high heat resistance and an appropriate heat shrinkage rate, making them suitable for packaging and / or labeling plastic containers such as PET bottles.
[0003] Meanwhile, while the use of plastic containers makes everyday life more convenient, their indiscriminate disposal and excessive use are causing serious environmental problems. Consequently, various measures are being developed to recycle used plastic containers.
[0004] The process of recycling the above waste plastic containers can be divided into a physical recycling process, such as washing and crushing, and a chemical recycling process, such as depolymerization. However, these recycling processes require preprocessing to separate the waste plastic by plastic type, which reduces the efficiency of the recycling process. For example, to recycle a PET bottle with a polyester film bonded as a label, the polyester film must be separated (removed) from the PET bottle. This is because the difference in crystallinity between the polyester resin contained in the polyester film and the PET contained in the PET bottle makes recycling impossible if the PET bottle is recycled while the polyester film is still bonded.
[0005] Therefore, in order to increase the efficiency of the recycling process, it is necessary to develop a technology that can omit the preprocessing work of separating (removing) polyester film from plastic containers such as PET bottles.
[0006] [Prior Art Literature]
[0007] [Patent Document]
[0008] (Patent Document 1) Republic of Korea Patent Publication No. 2009-0062882
[0009] In order to solve the above-mentioned conventional problems, the inventors of the present invention have conducted various studies, and as a result, they have confirmed that by controlling the crystallinity of a polyester stretch film manufactured using a polyester resin, a polyester stretch film can be obtained that can be recycled without separating (removing) it from a waste plastic container.
[0010] Accordingly, the object of the present invention is to provide a polyester stretch film with controlled crystallinity and a method for producing the same.
[0011] In order to solve the above problem, the present invention comprises a polyester resin in which a diol component and a dicarboxylic acid component are polymerized, and has a heat shrinkage rate in the main shrinkage direction of 40% or more at 80°C, and when analyzed by differential scanning calorimetry (DSC) after the first heat treatment and the second heat treatment, has a first melting temperature (T m1 ) and the second melting temperature (T m2 ) provides a polyester stretch film.
[0012] In addition, the present invention comprises a step of manufacturing a polyester resin by polymerizing a diol component and a dicarboxylic acid component; a step of manufacturing an elongated sheet from the polyester resin; and a step of heat-setting the elongated sheet, wherein the heat shrinkage in the main shrinkage direction at 80° C. is 40% or more, and after the first heat treatment and the second heat treatment, the first melting temperature (T) is 100° C. when analyzed by differential scanning calorimetry (DSC). m1 ) and the second melting temperature (Tm2 ) provides a method for manufacturing a polyester stretch film.
[0013] The polyester stretch film according to the present invention has two different melting temperatures (T) through heat treatment under specific conditions. m1 , T m2 ) can exhibit high crystallinity and excellent heat shrinkage.
[0014] Therefore, the polyester stretch film according to the present invention can be usefully used as a heat shrinkable film applied as a packaging and / or label for a plastic container (e.g., a PET bottle).
[0015] In addition, the polyester stretch film according to the present invention can have a crystallinity similar to that of a highly crystalline plastic container (e.g., a PET bottle) through heat treatment under specific conditions, so that recycling of the waste plastic container is possible without separating the polyester stretch film (e.g., the waste plastic container can be fed into the recycling process in a combined state with the polyester stretch film that has undergone the primary heat treatment and the secondary heat treatment). Accordingly, the present invention can increase the efficiency of the recycling process compared to the prior art.
[0016] Figure 1 is a graph showing the results of DSC analysis of a polyester stretch film according to Example 2 of the present invention.
[0017] Hereinafter, the present invention will be described in detail. Herein, the present invention is not limited to the contents described below, and may be modified in various forms as long as the gist of the invention is not changed.
[0018] The word "comprising" or "including" in this specification is intended to specify particular features, regions, steps, processes, elements and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements and / or components, unless specifically stated to the contrary.
[0019] In this specification, terms such as first, second, etc. are used to describe various components, and the components are not limited to these terms. These terms are used to distinguish one component from another.
[0020] All numbers and expressions indicating the amounts of components, reaction conditions, etc. described in this specification can be understood to be modified by the term “about” in all cases unless otherwise specified.
[0021]
[0022] Generally, the melting temperature (T) of polymer resins m ) is the crystallization temperature (T ), which is the temperature at which the crystalline portion of the polymer resin begins to melt. c ) is defined as the limit of the melting temperature (T m ) means that a large amount of heat (heat of fusion) is required to melt the crystalline portion of the polymer resin, which can be interpreted as the crystallinity of the polymer resin being maximized.
[0023] Based on these points, the polyester stretch film of the present invention, which includes a polyester resin, which is a polymer resin, can be obtained at a number of melting temperatures (T) through heat treatment under specific conditions. m ) can exhibit maximized crystallinity. That is, the polyester stretched film according to the present invention includes a polyester resin and has two different melting temperatures (T m1 , T m2 ) and exhibits high crystallinity, which is explained in detail as follows.
[0024]
[0025] Polyester stretch film
[0026] The polyester stretch film according to the present invention comprises a polyester resin in which a diol component and a dicarboxylic acid component are polymerized, and when analyzed by differential scanning calorimetry (DSC), the melting temperature (T m) did not show the first melting temperature (T ), but after the first and second heat treatments, when analyzed by differential scanning calorimetry (DSC), the first melting temperature (T ) m1 ) and the second melting temperature (T m2 ) is shown. Specifically, the polyester stretched film according to the present invention is a stretched film manufactured from a polyester resin, and by heat-treating at a first heat-treatment temperature and then heat-treating again at a second heat-treatment temperature, the crystallinity can be controlled to be high. For example, the polyester stretched film according to the present invention may be a polyester film manufactured by heat-treating a stretched film manufactured from a polyester resin at a first heat-treatment temperature and then heat-treating again at a second heat-treatment temperature.
[0027] The above first heat treatment temperature is not particularly limited, but may be 60 to 105°C, and specifically, 63 to 104°C, 66 to 103°C, 67 to 102°C, 68 to 100°C, 70 to 100°C, 70 to 98°C, 70 to 97°C, or 70 to 96°C.
[0028] In addition, the secondary heat treatment temperature is not particularly limited, but may be 140 to 220°C, and specifically, 141 to 219°C, 142 to 218°C, 143 to 217°C, 144 to 216°C, 145 to 215°C, 145 to 214°C, or 146 to 213°C.
[0029] As the first and second heat treatment temperatures are within the above ranges, the polyester stretched film according to the present invention can have high crystallinity at the required level and excellent heat shrinkage.
[0030] After the first and second heat treatments, the differential scanning calorimetry (DSC) used to analyze the polyester stretched film may be specifically modulated DSC (MDSC), and more specifically temperature-modulated DSC (TMDSC). When analyzing with the differential scanning calorimetry (DSC), a heating rate condition such as a heating rate of 10°C / min from room temperature (25°C±5°C) to 280°C may be applied.
[0031] According to the present invention, the first melting temperature (T) that appears during the first and second heat treatments m1 ) and the second melting temperature (T m2 ) are not particularly limited, but may be 150 to 230 ℃, respectively, and at this time, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) may be different from each other. Specifically, the first melting temperature (T m1 ) is the second melting temperature (T m2 ) may be lower.
[0032] That is, the first melting temperature (T m1 ) may be 150 to 230 ℃, specifically 152 to 225 ℃, 154 to 210 ℃, 156 to 205 ℃, 158 to 200 ℃, 160 to 198 ℃, 165 to 196 ℃, 170 to 195 ℃, 172 to 190 ℃, or 172 to 187 ℃. In addition, the second melting temperature (T m2 ) may be 150 to 230 ℃, specifically 155 to 230 ℃, 160 to 230 ℃, 165 to 230 ℃, 170 to 230 ℃, 175 to 229 ℃, 180 to 229 ℃, 185 to 228 ℃, 190 to 228 ℃, or 195 to 228 ℃. The first and second melting temperatures (Tm1 , T m2 ) As each range is within the above range, the polyester stretch film according to the present invention can have high crystallinity at the required level and excellent heat shrinkage, heat resistance and durability.
[0033] According to the present invention, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) may have a specific correlation.
[0034] Specifically, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) is the car (│T m1 - T m2 │) can represent a range of 10 to 60 ℃. More specifically, the difference (│T m1 - T m2 │) may be 10.5 to 58°C, 11 to 56°C, 11.5 to 54°C, 12 to 52°C, 12.5 to 50°C, 13 to 48°C, or 14 to 46°C.
[0035] Also, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) may exhibit a sum of fusion heats (fusion heats) of 3 J / g or more. Specifically, the first melting temperature (T m1 ) and the first heat of fusion (H1) and the second melting temperature (T m2 ) may be 3 J / g or more, 4 J / g or more, 5 J / g or more, 7 J / g or more, 9 J / g or more, 11 J / g or more, 13 J / g or more, 15 J / g or more, 17 J / g or more, 19 J / g or more, or 20 J / g or more. More specifically, the sum (H1+ H2) may be 3 to 25 J / g, 3.5 to 23 J / g, 4 to 21 J / g, 4.3 to 20 J / g, or 4.5 to 19.5 J / g.
[0036] Also, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) the ratio (H1 / H2) between the heat of fusion (heat of fusion) in each can be 0.1 to 10. Specifically, the second melting temperature (T m2 ) for the first melting temperature (T) for the second heat of fusion (H2) m1 ) may be 0.1 to 10, and more specifically, 0.2 to 9.5, 0.3 to 9, 0.4 to 8.5, 0.5 to 8, 0.6 to 7.9, 0.7 to 7.8, or 0.75 to 7.7.
[0037] The above first melting temperature (T m1 ) and the second melting temperature (T m2 ) is the correlation between the above difference (│T m1 - T m2 │), the polyester stretched film according to the present invention can have high crystallinity at the required level and excellent heat shrinkage, heat resistance and durability as the above sum (H1+H2) and the above ratio (H1 / H2) are each within the above range.
[0038] The polyester stretched film according to the present invention may have excellent heat shrinkage properties. Specifically, the polyester stretched film according to the present invention may have a heat shrinkage ratio in the main shrinkage direction of 40% or more at 80°C (e.g., when immersed in 80°C hot water for 10 seconds), and more specifically, may have a heat shrinkage ratio of 42% or more, 44% or more, 46% or more, 48% or more, 50% or more, 52% or more, 55% or more, or 60% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 80°C of the polyester stretched film may be 40 to 70%, 41 to 65%, 42 to 60%, 43 to 60%, 44 to 58%, or 45 to 56%.
[0039] In addition, the polyester stretched film according to the present invention may have a heat shrinkage ratio in the main shrinkage direction of 50% or more at 90°C (e.g., when immersed in 90°C hot water for 10 seconds), and specifically, 51% or more, 52% or more, 54% or more, 56% or more, 60% or more, 63% or more, 65% or more, or 70% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 90°C of the polyester stretched film may be 50 to 80%, 51 to 80%, 52 to 80%, 53 to 79%, 54 to 79%, or 55 to 78%.
[0040] The polyester stretched film according to the present invention may have a strain of 10% or less according to the following formula 1 when heated to 195°C after the first heat treatment and the second heat treatment. Specifically, the strain may be 0 to 10%, 0.01 to 9.5%, 0.01 to 9%, 0.03 to 8.8%, 0.03 to 8.5%, 0.05 to 8%, 0.05 to 7%, 0.08 to 5%, or 0.1 to 3%. As the strain is within the above range, the recyclability of the polyester stretched film may be excellent. Specifically, the temperature of 195°C is a temperature applied in a recycling process of waste plastic containers (e.g., PET bottles). Since the polyester stretched film according to the present invention has high crystallinity as it undergoes the first and second heat treatments, melting is minimized when heated to 195°C, so even if the recycling process is carried out while being combined with a waste plastic container, fusion with the waste plastic container does not occur, and thus recyclability can be excellent.
[0041] [Formula 1]
[0042] Strain (%) = (F m / F T )×100
[0043] In the above equation 1,
[0044] F m is the total number of melted polyester stretch film samples after heating to 195 ℃ (after first heat treatment and second heat treatment and heating to 195 ℃),
[0045] F T is the total number of polyester stretch film samples before heating to 195 ℃ (after the first and second heat treatments and before heating to 195 ℃),
[0046] The size of the above polyester stretch film sample is 1 cm in width and 1 cm in length.
[0047] The polyester stretched film according to the present invention has excellent heat shrinkability and high crystallinity, and thus can be usefully applied as a heat shrinkable film for packaging or labeling plastic containers (e.g., PET bottles). In particular, the polyester stretched film according to the present invention, by undergoing the first heat treatment and the second heat treatment processes, has a crystallinity similar to or equivalent to that of a plastic container (e.g., PET bottle) having high crystallinity (specifically, has a crystallinity similar to or equivalent to that of the polyethylene terephthalate (PET) component, which is a component of PET bottles), and thus, in the recycling process of used waste plastic containers, no fusion occurs with the plastic container, and thus the recycling process of waste plastic containers can be performed without going through a process of separating (removing) the polyester stretched film from the waste plastic container. Therefore, the present invention can increase the efficiency of the recycling process of waste plastic containers compared to the related art.
[0048] Meanwhile, the polyester resin included in the polyester stretch film according to the present invention may be a polyester resin in which a diol component and a dicarboxylic acid component are polymerized.
[0049] According to the present invention, the diol component may be a commonly known diol component. Specifically, the above diol component is bis-2-hydroxyethyl terephthalate, isosorbide, neopentyl glycol, ethylene glycol, cyclohexanedimethanol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl It may include at least one selected from the group consisting of 4-(hydroxymethyl)cyclohexanecarboxylate (CHDM derivative), 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol (CHDM derivative), recycled cyclohexanedimethanol, recycled ethylene glycol, recycled bis-2-hydroxyethyl terephthalate, and recycled diethylene glycol. Preferably, when considering the crystallinity, heat shrinkage, economic efficiency, etc. of the polyester stretched film, the diol component may include two or more (specifically, three or more, four or more, or five or more) selected from the group consisting of bis-2-hydroxyethyl terephthalate, isosorbide, ethylene glycol, cyclohexanedimethanol, neopentyl glycol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, and recycled bis-2-hydroxyethyl terephthalate.
[0050] For example, the diol component may include at least one (specifically, at least two, at least three, or at least four) selected from the group consisting of ethylene glycol and, as a comonomer, bis-2-hydroxyethyl terephthalate, isosorbide, cyclohexanedimethanol, neopentyl glycol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, and recycled bis-2-hydroxyethyl terephthalate.
[0051] When the diol component includes the ethylene glycol and the comonomer, the amounts of these components used are not particularly limited, but based on the total weight of the diol component, the amount of ethylene glycol used may be 10 to less than 100 wt%, 15 to 90 wt%, 20 to 85 wt%, 30 to 85 wt%, or 50 to 85 wt%, and the amount of the comonomer used may be more than 0 to 90 wt%, more than 0 to 85 wt%, 1 to 90 wt%, 1 to 50 wt%, 2 to 50 wt%, 10 to 85 wt%, 15 to 80 wt%, 15 to 70 wt%, or 15 to 50 wt%. In particular, when diethylene glycol is used as the comonomer, the amount of diethylene glycol used may be 0 to 50 wt%, 1 to 50 wt%, 2 to 50 wt%, 3 to 45 wt%, 4 to 40 wt%, or 5 to 35 wt%, based on the total weight of the diol component. Accordingly, the polyester resin according to the present invention may contain a structural unit derived from diethylene glycol in an amount of 0 to 50 wt%, 1 to 50 wt%, 2 to 50 wt%, 3 to 45 wt%, 4 to 40 wt%, or 5 to 35 wt%, based on the total weight of the polyester resin.
[0052] According to the present invention, the dicarboxylic acid component may be a commonly known dicarboxylic acid component. Specifically, the above dicarboxylic acid components are isophthalic acid, terephthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate (dimethyl terephthalate), phthalic anhydride, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, diphenyl dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, dimethyl 1,4-cyclohexane dicarboxylate, dimethyl 1,3-cyclohexane dicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, azelaic acid, recycled isophthalic acid, recycled terephthalic acid, recycled dimethyl isophthalate, and recycled dimethyl phthalate (recycled dimethyl It may include at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl phthalate, and dimethyl isophthalate. Preferably, considering the crystallinity and heat shrinkage properties of the polyester stretched film, the dicarboxylic acid component may include at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl phthalate, and dimethyl isophthalate.
[0053] Meanwhile, the recycled component (regenerated monomer) used as the above diol component and / or the above dicarboxylic acid component is not particularly limited, but may mean one obtained by subjecting a used waste polyester resin or waste polyester article to a commonly known recycling process (e.g., a depolymerization process).
[0054] According to the present invention, the polyester resin may have an intrinsic viscosity (IV) at 35°C of 0.5 to 1.2 dl / g, specifically 0.52 to 1.15 dl / g, 0.55 to 1.13 dl / g, 0.58 to 1.1 dl / g, 0.6 to 0.9 dl / g, 0.62 to 0.88 dl / g, 0.65 to 0.85 dl / g, 0.68 to 0.83 dl / g, or 0.7 to 0.8 dl / g. As the intrinsic viscosity is within the above range, the processability of the polyester resin can be secured.
[0055]
[0056] Method for manufacturing polyester stretch film
[0057] The present invention provides a method for manufacturing the above-described polyester stretched film. Specifically, the method for manufacturing the polyester stretched film according to the present invention comprises the steps of (S-1) polymerizing a diol component and a dicarboxylic acid component to manufacture a polyester resin; (S-2) manufacturing a stretched sheet from the polyester resin; and (S-3) heat-setting the stretched sheet, which will be described in detail as follows.
[0058]
[0059] Step (S-1): Polyester resin manufacturing
[0060] The above step (S-1) is a step for producing a polyester resin (copolymer) by polymerizing a diol component and a dicarboxylic acid component. Descriptions of each of the diol component and the dicarboxylic acid component for the polymerization are the same as those described above, and therefore are omitted.
[0061] The polymerization of the above diol component and the above dicarboxylic acid component can be carried out by a conventionally known method (e.g., liquid phase polymerization, solid phase polymerization, etc.), and a batch reactor or a continuous reactor can be used for the polymerization reaction. Specifically, the polymerization reaction can include an esterification reaction (esterification exchange reaction) in which the diol component and the dicarboxylic acid component are reacted to produce an oligomer, and a polycondensation reaction of the oligomer.
[0062] The temperature at which the esterification reaction takes place is not particularly limited, but considering the properties of the polyester resin and the polyester stretched film, it may be 230 to 270°C, 235 to 268°C, 240 to 265°C, or 240 to 260°C. In addition, the time at which the esterification reaction takes place is not particularly limited, but may be 1 to 24 hours, 2 to 22 hours, 3 to 20 hours, or 4 to 18 hours. In addition, the pressure at which the esterification reaction takes place is not particularly limited, but may be 0 to 5.0 kgf / cm. 2 , 0.1 to 4.5 kgf / cm 2 , 0.1 to 4.0 kgf / cm 2 , or 0.1 to 3.0 kgf / cm 2 It could be.
[0063] The temperature at which the polycondensation reaction takes place is not particularly limited, but considering the properties of the polyester resin and the polyester stretched film, it may be 245 to 290°C, 250 to 285°C, 255 to 280°C, or 255 to 270°C. In addition, the time at which the polycondensation reaction takes place is not particularly limited, but may be 1 to 24 hours, 2 to 24 hours, 5 to 22 hours, or 7 to 20 hours.
[0064] Meanwhile, an additive including at least one selected from the group consisting of a catalyst, a stabilizer, a coloring agent, a crystallizer, an antioxidant, and a branching agent may be added to the polymerization reaction.
[0065] The catalyst is not particularly limited, but specifically, methylates of sodium and magnesium; acetates, borates, fatty acid salts, or carbonates of Zn, Cd, Mn, Co, Ca, Ba, etc.; oxides or hydrates of Mg, Pb, Mn, Ti, Zn, Sb, Ge, etc. can be used. For example, the catalyst can be tetraethyl titanate, acetyltripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, triethanolamine titanate, acetylacetonate titanate, ethylacetoacetic ester titanate, isostearyl titanate, titanium dioxide, germanium dioxide, germanium tetrachloride, germanium ethyleneglycoxide, germanium acetate, or a combination thereof.
[0066] The above stabilizer is not particularly limited, but phosphorus compounds such as phosphoric acid, trimethyl phosphate, and triethyl phosphate can be used.
[0067] The above coloring agent is not particularly limited, but organic compounds such as cobalt compounds, anthraquionone compounds, perinone compounds, azo compounds, and methine compounds (e.g., cobalt acetate, cobalt propionate, Clarient's Polysynthren Blue RLS toner, Clarient's Solvaperm Red BB toner) can be used.
[0068] The above crystallizer is not particularly limited, but a crystal nucleating agent, an ultraviolet absorber, a polyolefin resin, a polyamide resin, etc. can be used.
[0069] The above antioxidant is not particularly limited, but hindered phenol compounds, phosphite compounds, thioether compounds, etc. can be used.
[0070] The above branching agent is not particularly limited, but trimellitic anhydride, trimellitic propane, trimellitic acid, etc. can be used.
[0071]
[0072] Step (S-2): Manufacturing of stretched sheets
[0073] The above step (S-2) is a step for manufacturing a stretched sheet from the polyester resin obtained in the above step (S-1). The manufacturing of the stretched sheet can be carried out by a conventionally known method, and specifically, the stretched sheet can be manufactured through a melting and casting process of the polyester resin, a uniaxial stretching process, a biaxial stretching process, etc.
[0074] The melting and casting process of the polyester resin may be performed through an extruder, and at this time, the melting temperature is not particularly limited, but may be 180 to 310°C, 200 to 310°C, 230 to 310°C, 240 to 300°C, or 250 to 290°C. By performing this process, an unstretched sheet may be obtained, and the obtained unstretched sheet may be passed to a stretching process. The unstretched sheet may be preheated to a predetermined temperature (e.g., 90 to 120°C) before undergoing the stretching process.
[0075] The above-described single-axis stretching process or two-axis stretching process may include a process of stretching the unstretched sheet obtained through the above-described melting and casting process in the machine direction (MD), the transverse direction (TD), or both directions. The stretching in the machine direction may be performed at a stretching ratio of 1 to 5 times, or 1.1 to 4.5 times, at a temperature of 55 to 180°C or 60 to 170°C. In addition, the stretching in the transverse direction may be performed at a stretching ratio of 1.5 to 6 times, or 2.5 to 5.5 times, at a temperature of 55 to 180°C or 60 to 170°C.
[0076]
[0077] Step (S-3): Open fixation
[0078] The above step (S-3) is a step of heat-setting the stretched sheet obtained in the above step (S-2). The temperature at which the stretched sheet is heat-set is not particularly limited, but may be similar to or higher than the stretching process temperature. Specifically, the heat-setting temperature may be 60 to 200°C, 65 to 190°C, 65 to 180°C, or 65 to 170°C. As the heat-setting temperature is within the above range, a polyester stretched film with increased crystallinity and mechanical strength can be manufactured.
[0079]
[0080] The polyester stretched film manufactured through this heat-setting process may have a heat shrinkage ratio in the main shrinkage direction of 40% or more at 80°C, and specifically, 42% or more, 44% or more, 46% or more, 48% or more, 50% or more, 52% or more, 55% or more, or 60% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 80°C may be 40 to 70%, 41 to 65%, 42 to 60%, 43 to 60%, 44 to 58%, or 45 to 56%.
[0081] In addition, the polyester stretched film manufactured through the above heat-setting process may have a heat shrinkage ratio in the main shrinkage direction of 50% or more at 90°C, and specifically, may be 51% or more, 52% or more, 54% or more, 56% or more, 60% or more, 63% or more, 65% or more, or 70% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 90°C may be 50 to 80%, 51 to 80%, 52 to 80%, 53 to 79%, 54 to 79%, or 55 to 78%.
[0082] The polyester stretch film of the present invention manufactured through the above steps has the first melting temperature (T) as described above when analyzed by the differential scanning calorimetry (DSC) after the first heat treatment and the second heat treatment. m1 ) and the second melting temperature (T m2 ) and can exhibit very high crystallinity and excellent heat shrinkage, heat resistance and durability.
[0083] The temperature of the first heat treatment is not particularly limited, but may be 60 to 105°C, and specifically, 63 to 104°C, 66 to 103°C, 67 to 102°C, 68 to 100°C, 70 to 100°C, 70 to 98°C, 70 to 97°C, or 70 to 96°C. For example, the first heat treatment may be performed by immersing the polyester stretched film obtained through the heat-setting process in the step (S-3) in hot water having the temperature range described above for 5 to 15 seconds. In addition, the first heat treatment may be performed by placing the polyester stretched film obtained through the heat-setting process into an oven having the temperature range described above and applying the temperature range to perform heat treatment for 5 to 15 seconds.
[0084] The secondary heat treatment temperature is not particularly limited, but may be 140 to 220°C, and specifically, 141 to 219°C, 142 to 218°C, 143 to 217°C, 144 to 216°C, 145 to 215°C, 145 to 214°C, or 146 to 213°C. For example, the secondary heat treatment may be performed by placing the primary heat-treated polyester stretched film into an oven and applying the temperature range described above to heat treat for 15 to 45 minutes.
[0085] The present invention is described in more detail through the following examples. However, the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention.
[0086]
[0087] [Example 1]
[0088] 1) Manufacturing of polyester resin (copolymer)
[0089] Into a 10 L reactor connected to a column and a water-cooled condenser, terephthalic acid (TPA, 7693.0 g), isosorbide (ISB, 96.7 g), ethylene glycol (EG, 2601.3 g), 1,4-cyclohexanedimethanol (CHDM, 1557.1 g), diethylene glycol (DEG, 1213.7 g), Ge catalyst (GeO2, 1.0 g), Ti catalyst (1.0 g), phosphoric acid (phosphoric acid, 1.5 g), blue toner (0.01 g), and red toner (0.005 g) were charged. Next, after raising the temperature of the reactor to 265 ℃, an esterification reaction (ES) was performed at 265 ℃ under a pressure of 2 kgf / ㎠ to obtain a transparent reactant.
[0090] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 270°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.77 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0091] 2) Manufacturing of polyester stretch sheet
[0092] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0093] 3) Open fixation
[0094] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0095] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 70°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 160°C for 30 minutes.
[0096]
[0097] [Example 2]
[0098] 1) Manufacturing of polyester resin (copolymer)
[0099] Into a 10 L reactor connected to a column and a water-cooled condenser, terephthalic acid (TPA, 7663.2 g), ethylene glycol (EG, 3345.5 g), 1,4-cyclohexanedimethanol (CHDM, 1255.7 g), neopentyl glycol (NPG, 106.7 g), diethylene glycol (DEG, 978.7 g), cyclohexanedimethanol derivative (CHDM derivative, 247.4 g), Ti catalyst (1.0 g), blue toner (0.01 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 255 ℃, and an esterification reaction (ES) was performed at 255 ℃ under a pressure of 1 kgf / ㎠ to obtain a transparent reactant.
[0100] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.65 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0101] 2) Manufacturing of polyester stretch sheet
[0102] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0103] 3) Open fixation
[0104] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0105] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 90°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 175°C for 30 minutes.
[0106]
[0107] [Example 3]
[0108] 1) Manufacturing of polyester resin (copolymer)
[0109] Into a 10 L reactor connected to a column and a water-cooled condenser, regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 1202.9 g), terephthalic acid (TPA, 7075.2 g), ethylene glycol (EG, 3488.9 g), 1,4-cyclohexanedimethanol (CHDM, 1363.9 g), diethylene glycol (DEG, 1063.0 g), Ti catalyst (1.0 g), blue toner (0.02 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 255 ℃, and an esterification reaction (ES) was performed at 255 ℃ under a pressure of 0.5 kgf / ㎠ to obtain a transparent reactant.
[0110] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.70 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0111] 2) Manufacturing of polyester stretch sheet
[0112] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0113] 3) Open fixation
[0114] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0115] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 95°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 155°C for 30 minutes.
[0116]
[0117] [Example 4]
[0118] 1) Manufacturing of polyester resin (copolymer)
[0119] Terephthalic acid (TPA, 7918.3 g), ethylene glycol (EG, 4080.5 g), 1,4-cyclohexanedimethanol (CHDM, 1068.5 g), diethylene glycol (DEG, 832.8 g), Ge catalyst (GeO2, 1.0 g), blue toner (0.05 g), and red toner (0.02 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 260 °C, and an esterification reaction (ES) was performed at 260 °C under a pressure of 1 kgf / cm2 to obtain a transparent reactant.
[0120] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 275°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.78 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0121] 2) Manufacturing of polyester stretch sheet
[0122] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0123] 3) Open fixation
[0124] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0125] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 95°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 165°C for 30 minutes.
[0126]
[0127] [Example 5]
[0128] 1) Manufacturing of polyester resin (copolymer)
[0129] Dimethyl phthalate (DMT, 7878.5 g), isosorbide (ISB, 494.9 g), ethylene glycol (EG, 4076.7 g), 1,4-cyclohexanedimethanol (CHDM, 1139.1 g), diethylene glycol (DEG, 887.8 g), Mn catalyst (Mn(II) acetate tetrahydrate, 1.5 g), Sb catalyst (Sb2O3, 1.8 g), and cobalt acetate (cobalt acetate, 0.8 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 240 ℃, and an esterification reaction (ES) was performed at 240 ℃ under a pressure of 0.1 kgf / ㎠ to obtain a transparent reactant.
[0130] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 255°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.85 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0131] 2) Manufacturing of polyester stretch sheet
[0132] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0133] 3) Open fixation
[0134] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0135] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 95°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 175°C for 30 minutes.
[0136]
[0137] [Example 6]
[0138] 1) Manufacturing of polyester resin (copolymer)
[0139] Terephthalic acid (TPA, 8279.3 g), ethylene glycol (EG, 4432.3 g), neopentyl glycol (NPG, 864.5 g), Ge catalyst (GeO2, 1.0 g), cobalt acetate (0.4 g), blue toner (0.03 g), and red toner (0.01 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 250°C, and an esterification reaction (ES) was performed at 250°C under a pressure of 1 kgf / cm2 to obtain a transparent reactant.
[0140] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.70 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0141] 2) Manufacturing of polyester stretch sheet
[0142] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0143] 3) Open fixation
[0144] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0145] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 95°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 160°C for 30 minutes.
[0146]
[0147] [Example 7]
[0148] 1) Manufacturing of polyester resin (copolymer)
[0149] In a 10 L reactor connected to a column and a water-cooled condenser, regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 2288.5 g), terephthalic acid (TPA, 5982.5 g), ethylene glycol (EG, 739.3 g), 1,4-cyclohexanedimethanol (CHDM, 1441.6 g), neopentyl glycol (NPG, 1301.4 g), diethylene glycol (DEG, 1123.6 g), Ge catalyst (GeO2, 1.0 g), blue toner (0.03 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 265 ℃, and an esterification reaction (ES) was performed at 265 ℃ under a pressure of 2 kgf / cm2 to obtain a transparent reactant.
[0150] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 270°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.78 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0151] 2) Manufacturing of polyester stretch sheet
[0152] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0153] 3) Open fixation
[0154] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0155] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 100°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 210°C for 30 minutes.
[0156]
[0157] [Comparative Example 1]
[0158] 1) Manufacturing of polyester resin (copolymer)
[0159] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 2256.8 g), terephthalic acid (TPA, 5899.6 g), ethylene glycol (EG, 824.5 g), 1,4-cyclohexanedimethanol (CHDM, 2487.8 g), diethylene glycol (DEG, 1939.0 g), Ge catalyst (GeO2, 1.0 g), blue toner (0.01 g), and red toner (0.01 g) were charged into a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 273 ℃, and an esterification reaction (ES) was performed at 273 ℃ under a pressure of 0.5 kgf / ㎠ to obtain a transparent reactant.
[0160] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.80 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0161] 2) Manufacturing of polyester stretch sheet
[0162] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0163] 3) Open fixation
[0164] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0165] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 110°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 225°C for 30 minutes.
[0166]
[0167] [Comparative Example 2]
[0168] 1) Manufacturing of polyester resin (copolymer)
[0169] In a 10 L reactor connected to a column and a water-cooled condenser, regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 2509.9 g), terephthalic acid (TPA, 6561.3 g), ethylene glycol (EG, 3281.5 g), 1,4-cyclohexanedimethanol (CHDM, 790.5 g), diethylene glycol (DEG, 616.1 g), Ti catalyst (1.0 g), blue toner (0.01 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 263 ℃, and an esterification reaction (ES) was performed at 263 ℃ under a pressure of 1 kgf / cm2 to obtain a transparent reactant.
[0170] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 275°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.70 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0171] 2) Manufacturing of polyester stretch sheet
[0172] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0173] 3) Open fixation
[0174] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0175] Thereafter, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 80°C for 10 seconds. Next, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 170°C for 30 minutes.
[0176]
[0177] [Comparative Example 3]
[0178] 1) Manufacturing of polyester resin (copolymer)
[0179] Terephthalic acid (TPA, 7918.3 g), ethylene glycol (EG, 4080.5 g), 1,4-cyclohexanedimethanol (CHDM, 1068.5 g), diethylene glycol (DEG, 832.8 g), Ge catalyst (GeO2, 1.0 g), blue toner (0.05 g), and red toner (0.02 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 260 °C, and an esterification reaction (ES) was performed at 260 °C under a pressure of 1 kgf / cm2 to obtain a transparent reactant.
[0180] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 275°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.78 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.
[0181] 2) Manufacturing of polyester stretch sheet
[0182] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.
[0183] 3) Open fixation
[0184] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 200°C.
[0185] Afterwards, in order to control the crystallinity of the polyester stretched film, the polyester stretched film was first heat-treated by immersing it in hot water at 65°C for 10 seconds.
[0186]
[0187] [Example 1]
[0188] Each of the heat-treated polyester stretched films in Examples 1 to 7 and Comparative Examples 1 to 3 was analyzed by differential scanning calorimetry (DSC) to determine the melting temperature (T m) was confirmed to appear, and the results are shown in Table 1 and Figure 1 below. The DSC analysis of the polyester stretched film was performed as follows.
[0189] DSC analysis device: Mettler Toledo's DSC 1 model was used.
[0190] Sample preparation: About 6 to 10 mg of the primary or primary and secondary heat-treated polyester stretch film was taken and filled into an aluminum pan.
[0191] Scan conditions: DSC curves were obtained by heating from room temperature to 280 ℃ at a rate of 10 ℃ and annealing at 280 ℃ for 3 minutes.
[0192] Melting temperature verification: The temperature at which an endothermic peak appears during the heating process in the obtained DSC curve was defined as the melting temperature. Based on the results obtained thereafter, the melting temperature (T m1 , T m2 ), │T m1 - T m2 │, H1+H2 and H1 / H2 were calculated. At this time, │T m1 - T m2 │Applies the value rounded to the second decimal place.
[0193]
[0194] [Example 2]
[0195] The heat shrinkage rate of each of the polyester stretched films (polyester stretched films before the first or first and second heat treatments) before heat treatment in Examples 1 to 7 and Comparative Examples 1 to 3 was evaluated as follows, and the results are shown in Table 1 below.
[0196] Sample preparation: Polyester stretch film was cut into 5 cm × 5 cm pieces and stored at room temperature (20°C).
[0197] Heat shrinkage at 80°C: After immersing a polyester stretched film sample in hot water at 80°C for 10 seconds, the change in length in the transverse direction (TD), which is the main shrinkage direction, was calculated by applying Equation 2 below.
[0198] Heat shrinkage at 90°C: After immersing a polyester stretched film sample in hot water at 90°C for 10 seconds, the change in length in the transverse direction (TD), which is the main shrinkage direction, was calculated by applying Equation 2 below.
[0199] [Formula 2]
[0200] Heat shrinkage (%) = {(F S1 -F S2 ) / F S1}×100
[0201] In the above equation 2,
[0202] F S1 is the transverse (TD) length of the polyester stretched film sample before hot water immersion,
[0203] F S2 is the transverse direction (TD) length of the polyester stretched film sample after immersion in hot water.
[0204]
[0205] [Example 3]
[0206] The recyclability of each of the heat-treated polyester stretch films in Examples 1 to 7 and Comparative Examples 1 to 3 was evaluated as follows, and the results are shown in Table 1 below.
[0207] Sample preparation: The first or first and second heat-treated polyester stretch film was cut into 1 cm × 1 cm pieces and stored at room temperature (20°C).
[0208] Test conditions: 100 polyester stretched film samples were placed on a Teflon-coated plate, heated in an oven at 195°C (PET recycling process temperature) for 30 minutes, and the strain of the polyester stretched film was calculated according to Equation 1 below. If the strain was less than 10%, the recyclability was evaluated as excellent, and in Equation 1 below, the case where the polyester stretched film sample melted was applied when the stretched film sample melted and stuck to the plate without falling off.
[0209] [Formula 1]
[0210] Strain (%) = (F m / F T )×100
[0211] In the above equation 1,
[0212] F m is the total number of polyester stretch film samples that melted after heating to 195 ℃,
[0213] F T is the total number of polyester stretch film samples before heating to 195 ℃.
[0214] ◎: Strain is 0 to 5%
[0215] ○: Strain exceeding 5% to 10%
[0216] ×: Strain exceeds 10%
[0217]
[0218] Classification T m1 (℃)T m2 (℃)│T m1 - T m2│(℃)H1+H2(J / g)H1 / H2Shrinkage(80℃, %)Shrinkage(90℃, %)RecyclabilityExample 1173.3196.923.67.533.355267◎Example 2172.52194.0821.616.611.914859◎Example 3181.5195.614.14.57.675568◎Example 4173.46199.3625.919.021.504557◎Example 5174.13227.7253.66.96.524455◎Example 6181.1208.1327.011.640.764655○Example 7181.49209.2127.78.111.174555○Comparative Example 1164.8--0.5-6570×Comparative Example 2188234.546.51.50.652535◎Comparative Example 3183.3--0.5-4557×
[0219] Referring to Table 1 above, two melting temperatures (T) as in the present invention m1 , T m2 ) (see Fig. 1) │T m1 - T m2 │, it can be confirmed that the polyester stretched films of Examples 1 to 7, in which H1+H2 and H1 / H2 are controlled within the scope of the present invention, have high heat shrinkage rates depending on temperature and ensure recyclability.
[0220] On the other hand, it can be confirmed that the polyester stretched film of Comparative Example 1 having a single melting temperature has significantly poor recyclability, and the polyester stretched film of Comparative Example 2 having a low usage amount of comonomer (e.g., diethylene glycol) has low heat shrinkage. In addition, it can be confirmed that the polyester stretched film of Comparative Example 3, which was heat treated only once, also has significantly poor recyclability.
Claims
1. Contains a polyester resin polymerized with a diol component and a dicarboxylic acid component, The thermal shrinkage rate in the main shrinkage direction at 80℃ is 40% or more, After the first and second heat treatments, the first melting temperature (T) was analyzed by differential scanning calorimetry (DSC). m1 ) and the second melting temperature (T m2 ), a polyester stretch film.
2. In paragraph 1, The above first melting temperature (T m1 ) is 150 to 230 ℃, and the second melting temperature (T m2 ) is 150 to 230 ℃, The above first melting temperature (T m1 ) and the second melting temperature (T m2 ) are different from each other, polyester stretch films.
3. In paragraph 1, The above first melting temperature (T m1 ) and the second melting temperature (T m2 ) of tea (│T m1 - T m2 │) A polyester stretch film having a temperature of 10 to 60°C.
4. In paragraph 1, The above first melting temperature (T m1 ) and the first heat of fusion (H1) and the second melting temperature (T m2 ) A polyester stretched film having a sum of the second heats of fusion (H2) (H1 + H2) of 3 J / g or more.
5. In paragraph 1, The second melting temperature (T m2 ) for the first melting temperature (T) for the second heat of fusion (H2) m1 ) has a ratio (H1 / H2) of the first heat of fusion (H1) of 0.1 to 10, a polyester stretched film.
6. In paragraph 1, A polyester stretched film having a primary heat treatment temperature of 60 to 105°C.
7. In paragraph 1, A polyester stretched film having a secondary heat treatment temperature of 140 to 220°C.
8. In paragraph 1, The above diol component is bis-2-hydroxyethyl terephthalate, isosorbide, neopentyl glycol, ethylene glycol, cyclohexanedimethanol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl A polyester stretched film comprising at least one selected from the group consisting of 4-(hydroxymethyl)cyclohexanecarboxylate, 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, recycled cyclohexanedimethanol, recycled ethylene glycol, recycled bis-2-hydroxyethyl terephthalate, and recycled diethylene glycol.
9. In paragraph 1, A polyester elongation, wherein the dicarboxylic acid component comprises at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, diphenyl dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, dimethyl 1,4-cyclohexane dicarboxylate, dimethyl 1,3-cyclohexane dicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, azelaic acid, recycled isophthalic acid, recycled terephthalic acid, recycled dimethyl isophthalate, and recycled dimethyl phthalate. Film.
10. In paragraph 1, A polyester stretched film having a heat shrinkage rate of 50% or more in the main shrinkage direction at 90°C.
11. In paragraph 1, A polyester stretch film, wherein the intrinsic viscosity (IV) of the polyester resin is 0.5 to 1.2 dl / g.
12. In paragraph 1, A polyester stretched film having a strain of 10% or less according to the following formula 1 when heated to 195°C after the first heat treatment and the second heat treatment: [Formula 1] Strain (%) = (F m / F T )×100 In the above equation 1, F m is the total number of polyester stretch film samples that melted after heating to 195 ℃, F T is the total number of polyester stretch film samples before heating to 195 ℃, The size of the above polyester stretch film sample is 1 cm in width and 1 cm in length.
13. A step of manufacturing a polyester resin by polymerizing a diol component and a dicarboxylic acid component; A step of manufacturing a stretched sheet from the above polyester resin; and Including a step of opening and fixing the above-mentioned extension sheet, The thermal shrinkage rate in the main shrinkage direction at 80℃ is 40% or more, After the first and second heat treatments, the first melting temperature (T) was analyzed by differential scanning calorimetry (DSC). m1 ) and the second melting temperature (T m2 ) and a method for manufacturing a polyester stretch film.
14. In paragraph 13, A method for manufacturing a polyester stretched film, wherein the first heat treatment temperature is 60 to 105°C.
15. In paragraph 13, A method for manufacturing a polyester stretched film, wherein the secondary heat treatment temperature is 140 to 220°C.
Citation Information
Patent Citations
A heat shrinkable stacked film and a heat shrinkable label using the same as substrate
KR1020090062882A
Fiber sheet
JP2008025047A
Method and apparatus for thermally processing crystalline thermoplastic resin film
KR100154331B1
Thermally shrinkable polyester-based film
KR1020010078083A
Blocking device of exposure of power cable disconnection portion
KR1020210043134A