Polyester resin and preparation method therefor
By controlling the content ratios of germanium, zinc, and phosphorus in the polymerization process of polyester resin with specific diol and dicarboxylic acid components, the issues of heat resistance, chemical resistance, and appearance are addressed, resulting in a high-performance resin with enhanced mechanical and color properties.
Patent Information
- Application Number
- PCT/KR2024/003454
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-03-20
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional polyester resins produced with terephthalic acid and ethylene glycol lack sufficient heat resistance, chemical resistance, and exhibit poor appearance characteristics such as high yellowness and haze, limiting their productivity and transparency in molded products.
A polyester resin is developed with specific content ratios of germanium (Ge), zinc (Zn), and phosphorus (P) within the ranges 1≤Ge/Zn≤30 and 1≤(Ge+Zn)/P≤15, using these elements as catalysts and stabilizers in the polymerization process, along with various diol and dicarboxylic acid components, to enhance mechanical strength, heat resistance, chemical resistance, and color characteristics.
The solution results in polyester resin with improved heat resistance, chemical resistance, impact resistance, and excellent color characteristics, maximizing productivity and intrinsic viscosity, while maintaining high efficiency in the polymerization process.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Polyester resin and its manufacturing method
[0001] The present invention relates to a polyester resin having excellent color characteristics while exhibiting properties such as high heat resistance, chemical resistance, and impact resistance, and a method for producing the polyester resin.
[0002] Among polymers, polyester resins are widely used in various fields due to their high mechanical strength, heat resistance, chemical resistance, and impact resistance. In particular, films and plates manufactured using polyester resins exhibit excellent transparency and mechanical strength, leading to their widespread application in cases, boxes, partitions, shelves, panels, packaging, building materials, and interior and exterior finishes.
[0003] These polyester resins can be manufactured through a process of directly esterifying and / or transesterifying an acid component and a diol component in the presence of a polymerization catalyst, followed by condensation polymerization. Terephthalic acid (TPA) has been typically used as the acid component, and ethylene glycol (EG) has been typically used as the diol component. However, polyester resins manufactured using these components do not have sufficient heat resistance, chemical resistance, etc., so recently, various aliphatic or aromatic cyclic diol components (e.g., isosorbide (ISB), cyclohexanedimethanol (CHDM), etc.) are being introduced into the manufacture of polyester resins.
[0004] However, the polyester resin manufactured by introducing the above cyclic diol component has high yellowness index (YI), haze, etc., and when using it to manufacture a molded product, there is a problem that the appearance characteristics (e.g., transparency) of the molded product are poor. In addition, the polymerization reaction efficiency between the raw material components for manufacturing the polyester resin is not at a satisfactory level, so there is a limit to increasing the productivity of the polyester resin.
[0005] Therefore, it is necessary to develop a technology that can provide molded products with excellent appearance properties while increasing the productivity of polyester resin.
[0006] In order to solve the above-described conventional problems, the inventors of the present invention have conducted various studies, and as a result, they have confirmed that a polyester resin with excellent color characteristics can be manufactured with high efficiency (increased productivity) by controlling the content ratio between specific elements included in the polyester resin within a specific range.
[0007] Accordingly, the object of the present invention is to provide a polyester resin having excellent color characteristics along with basic physical properties and high productivity, and a method for producing the same.
[0008] To solve the above problem, the present invention provides a polyester resin comprising a diol repeating unit derived from a diol component and a dicarboxylic acid repeating unit derived from a dicarboxylic acid component, and in which the content ratios of germanium (Ge), zinc (Zn), and phosphorus (P) satisfy the following equations 1 and 2:
[0009] [Formula 1]
[0010] 1≤Ge / Zn≤30
[0011] [Formula 2]
[0012] 1≤(Ge+Zn) / P≤15
[0013] In addition, the present invention provides a method for producing a polyester resin, comprising the steps of: introducing a diol component and a dicarboxylic acid component into a reactor; introducing at least one of a germanium (Ge)-containing catalyst and a zinc (Zn)-containing catalyst and a phosphorus (P)-containing stabilizer into the reactor; producing an oligomer by esterifying the diol component and the dicarboxylic acid component in the presence of the catalyst and the stabilizer; and subjecting the oligomer to a condensation polymerization reaction, wherein the content ratios of germanium (Ge), zinc (Zn), and phosphorus (P) satisfy the above formulae 1 and 2.
[0014] The present invention provides a polyester resin having high mechanical strength, heat resistance, chemical resistance, impact resistance, and excellent color characteristics (e.g., transparency) by introducing a catalyst and stabilizer of a specific component (e.g., a germanium (Ge)-containing catalyst, a zinc (Zn)-containing catalyst, a phosphorus (P)-containing stabilizer) into a reaction process of a polyester resin, and controlling the content ratio between specific elements included in the polyester resin.
[0015] In addition, the present invention can provide a polyester resin having a desired intrinsic viscosity (IV) while maximizing the productivity of the polyester resin by manufacturing the polyester resin so that the content ratio between specific elements included in the polyester resin is controlled.
[0016] Hereinafter, the present invention will be described in detail. Herein, the present invention is not limited to the contents described below, and may be modified in various forms as long as the gist of the invention is not changed.
[0017] The word "comprising" or "including" in this specification is intended to specify particular features, regions, steps, processes, elements and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements and / or components, unless specifically stated to the contrary.
[0018] All numbers and expressions indicating the amounts of components, reaction conditions, etc. described in this specification can be understood to be modified by the term “about” in all cases unless otherwise specified.
[0019]
[0020] polyester resin
[0021] The polyester resin according to the present invention comprises a diol repeating unit derived from a diol component; a dicarboxylic acid repeating unit derived from a dicarboxylic acid component; and at least one element selected from the group consisting of germanium (Ge), zinc (Zn), and phosphorus (P), which will be specifically described as follows.
[0022] The diol repeating unit included in the polyester resin according to the present invention is derived from the diol component. The above diol component is not particularly limited, but specifically, ethylene glycol, cyclohexanedimethanol, isosorbide, diethylene glycol, neopentyl glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, 4-(hydroxymethyl)cyclohexylmethyl It may include at least one selected from the group consisting of 4-(hydroxymethyl)cyclohexanecarboxylate (CHDM derivative), 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol (CHDM derivative), bis-2-hydroxyethyl terephthalate, and recycled bis-2-hydroxyethyl terephthalate.
[0023] For example, the diol component may include a first diol component comprising ethylene glycol, and a second diol component (comonomer component) comprising at least one (specifically, at least two, at least three, or at least four) selected from the group consisting of cyclohexanedimethanol, isosorbide, diethylene glycol, bis-2-hydroxyethyl terephthalate, recycled bis-2-hydroxyethyl terephthalate, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol.
[0024] Here, the second diol component may include two or more or three or more selected from the group consisting of cyclohexanedimethanol, isosorbide, diethylene glycol, bis-2-hydroxyethyl terephthalate, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, and recycled bis-2-hydroxyethyl terephthalate.
[0025] When the diol component includes the first diol component and the second diol component, the diol repeating unit may include a first diol repeating unit (structural unit) derived from the first diol component and a second diol repeating unit (structural unit) derived from the second diol component. The content of the first diol repeating unit (content of the first diol repeating unit included in the polyester resin) is not particularly limited, but may be 5 to 95 mol%, 10 to 90 mol%, 10 to 85 mol%, 15 to 85 mol%, or 20 to 70 mol% based on the total mole number of the diol repeating unit. In addition, the content of the second diol repeating unit (the content of the second diol repeating unit included in the polyester resin) is not particularly limited, but may be 5 to 95 mol%, 10 to 90 mol%, 10 to 85 mol%, 15 to 85 mol%, or 20 to 70 mol% based on the total mole number of the diol repeating unit. When the content of the first diol repeating unit and the content of the second diol repeating unit are each within the above range, a polyester resin having excellent heat resistance, chemical resistance, color characteristics, and productivity can be provided.
[0026] In addition, when the second diol component includes at least one comonomer selected from the group consisting of cyclohexanedimethanol, isosorbide, diethylene glycol, bis-2-hydroxyethyl terephthalate, recycled bis-2-hydroxyethyl terephthalate, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, the diol repeating unit may include a repeating unit (structural unit) derived from the comonomer. For example, the content of the repeating unit derived from cyclohexanedimethanol (the content of the repeating unit derived from cyclohexanedimethanol included in the polyester resin) is not particularly limited, but may be 1 to 10 mol%, 2 to 9 mol%, 3 to 8 mol%, or 3 to 7 mol% based on the total mole number of the diol repeating unit. The content of the repeating unit derived from isosorbide (the content of the repeating unit derived from isosorbide included in the polyester resin) is not particularly limited, but may be 1 to 70 mol%, 2 to 65 mol%, 3 to 60 mol%, or 4 to 60 mol% based on the total mole number of the diol repeating unit. The content of the repeating unit derived from the above diethylene glycol (the content of the repeating unit derived from the diethylene glycol included in the polyester resin) is not particularly limited, but may be 1 to 10 mol%, 1 to 9 mol%, 1 to 8 mol%, or 1 to 7 mol% based on the total mole number of the diol repeating unit. The content of the repeating unit derived from the above recycled bis-2-hydroxyethyl terephthalate (the content of the repeating unit derived from the recycled bis-2-hydroxyethyl terephthalate included in the polyester resin) is not particularly limited, but may be 1 to 100 mol%, 2 to 100 mol%, 3 to 100 mol%, 4 to 100 mol%, 4 to 95 mol%, or 4 to 90 mol% based on the total mole number of the diol repeating unit.
[0027] The dicarboxylic acid repeating unit included in the polyester resin according to the present invention may be derived from the dicarboxylic acid component. The above dicarboxylic acid component is not particularly limited, but may specifically include at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, diphenyl dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, dimethyl 1,4-cyclohexane dicarboxylate, dimethyl 1,3-cyclohexane dicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, and azelaic acid.
[0028] For example, the dicarboxylic acid component may include at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl phthalate, and dimethyl isophthalate, and preferably, may include isophthalic acid, terephthalic acid, or a combination thereof.
[0029] When the dicarboxylic acid component includes the isophthalic acid and / or the terephthalic acid, the dicarboxylic acid repeating unit may include an isophthalic acid repeating unit (structural unit) derived from the isophthalic acid, a terephthalic acid repeating unit (structural unit) derived from the terephthalic acid, or a combination thereof. The content of the isophthalic acid repeating unit (content of the isophthalic acid repeating unit included in the polyester resin) is not particularly limited, but may be 1 to 10 mol%, 2 to 10 mol%, 3 to 10 mol%, or 4 to 10 mol% based on the total mole number of the dicarboxylic acid repeating unit. In addition, the content of the terephthalic acid repeating unit (the content of the terephthalic acid repeating unit included in the polyester resin) is not particularly limited, but may be 1 to 100 mol%, 2 to 100 mol%, 3 to 100 mol%, 4 to 100 mol%, 90 to 96 mol%, 90 to 97 mol%, 90 to 98 mol%, or 90 to 99 mol% based on the total mole number of the dicarboxylic acid repeating unit. When the content of the isophthalic acid repeating unit and the content of the terephthalic acid repeating unit are each within the above range, a polyester resin having excellent heat resistance, chemical resistance, impact resistance, and productivity can be provided.
[0030] The elements included in the polyester resin according to the present invention may include at least one selected from the group consisting of germanium (Ge), zinc (Zn), and phosphorus (P). In this case, the elements germanium (Ge), zinc (Zn), and phosphorus (P) may satisfy the content ratio (weight ratio) according to the following equations 1 and 2.
[0031] [Formula 1]
[0032] 1≤Ge / Zn≤30
[0033] [Formula 2]
[0034] 1≤(Ge+Zn) / P≤15
[0035] Specifically, when the polyester resin includes the germanium (Ge) and the zinc (Zn), the Ge / Zn ratio, which is the content ratio between them, may be 1 to 30. More specifically, the Ge / Zn ratio may be 1.1 to 29, 1.2 to 29, 1.3 to 28, 1.4 to 28, 1.5 to 27, 1.6 to 27, 1.8 to 26, 2 to 24, 2.5 to 22, 3 to 20, 5 to 19, 8 to 17, or 9 to 16. When the Ge / Zn ratio is within the above range, a polyester resin having remarkably excellent color characteristics and a desired intrinsic viscosity (IV) can be provided.
[0036] Meanwhile, when the polyester resin includes the germanium (Ge), the zinc (Zn), and the phosphorus (P), the content ratio therebetween, the (Ge+Zn) / P ratio, may be 1 to 15. Specifically, the (Ge+Zn) / P ratio may be 1.1 to 14.8, 1.2 to 14.6, 1.3 to 14.4, 1.4 to 14.2, 1.5 to 14, 1.6 to 13.8, 1.8 to 13.4, 2 to 13.2, 2.5 to 13, 3 to 12.5, 3.3 to 12, 3.5 to 11, 3.8 to 10, or 4 to 9.5. As the (Ge+Zn) / P ratio is within the above range, a polyester resin having excellent heat resistance, chemical resistance, and color characteristics can be provided with high efficiency. In particular, when the (Ge+Zn) / P ratio is within the above range, the productivity of the polyester resin can be maximized.
[0037] The germanium (Ge), an element included in the polyester resin according to the present invention, may be derived from a germanium (Ge)-containing catalyst. The germanium (Ge)-containing catalyst may not be particularly limited as long as it is commonly known. Specifically, the germanium (Ge)-containing catalyst may include at least one selected from the group consisting of a salt of a germanium (Ge)-containing aliphatic carboxylic acid, a salt of a germanium (Ge)-containing aromatic carboxylic acid, a salt of a germanium (Ge)-containing halogenated carboxylic acid, a salt of a germanium (Ge)-containing hydroxycarbonate, a salt of a germanium (Ge)-containing mineral, a germanium (Ge)-containing organosulfonate, a germanium (Ge)-containing organosulfate, a germanium (Ge)-containing alkoxide, a germanium (Ge)-containing acetylacetonate, a germanium (Ge)-containing oxide, a germanium (Ge)-containing metal, and a germanium (Ge)-containing hydroxide.
[0038] The salt of the aliphatic carboxylic acid containing germanium (Ge) is not particularly limited, but may specifically be a formate, acetate (e.g., germanium acetate), propionate, butyrate, oxalate, acrylate, or methacrylate containing germanium (Ge).
[0039] The salt of the aromatic carboxylic acid containing germanium (Ge) is not particularly limited, but may specifically be benzoate containing germanium (Ge).
[0040] The salt of the above-mentioned germanium (Ge)-containing halogenated carboxylic acid is not particularly limited, but may specifically be trichloroacetate or trifluoroacetate containing germanium (Ge).
[0041] The salt of the above germanium (Ge)-containing hydroxycarbonate is not particularly limited, but may specifically be lactate, citrate, or oxalate containing germanium (Ge).
[0042] The salt of the above germanium (Ge)-containing mineral is not particularly limited, but may specifically be a carbonate, sulfate, nitrate, phosphate, phosphonate, phosphinate, hydrogen sulfate, hydrogen carbonate, hydrogen phosphate, sulfite, thiosulfate, hydrochloride, hydrobromide, chloride (e.g., germanium tetrachloride), chlorate, bromide, or boromate containing germanium (Ge).
[0043] The above-mentioned germanium (Ge)-containing organosulfonate is not particularly limited, but may specifically be 1-propane-sulfonate, 1-pentane sulfonate, or naphthalenesulfonate containing germanium (Ge).
[0044] The above germanium (Ge)-containing organosulfate is not particularly limited, but may specifically be lauryl sulfate containing germanium (Ge).
[0045] The above germanium (Ge)-containing alkoxide is not particularly limited, but may specifically be methoxy, ethoxy, propoxy, iso-propoxy, or butoxy containing germanium (Ge).
[0046] The above germanium (Ge)-containing oxide is not particularly limited, but may specifically be germanium dioxide (GeO2), etc.
[0047] The content of germanium (Ge) derived from such a germanium (Ge)-containing catalyst is not particularly limited, but may be 10 to 500 ppm, 30 to 500 ppm, 40 to 490 ppm, 80 to 490 ppm, 105 to 480 ppm, 120 to 480 ppm, 130 to 470 ppm, 140 to 460 ppm, 150 to 450 ppm, 155 to 430 ppm, or 155 to 420 ppm based on the total weight of the polyester resin. As the content of germanium (Ge) is within the above range, the above formulas 1 and 2 are satisfied, and thus a polyester resin having excellent color characteristics can be manufactured with high efficiency.
[0048] The zinc (Zn), which is an element included in the polyester resin according to the present invention, may be derived from a zinc (Zn)-containing catalyst. The zinc (Zn)-containing catalyst may not be particularly limited as long as it is commonly known. Specifically, the zinc (Zn)-containing catalyst may include at least one selected from the group consisting of zinc acetate, zinc acetate dihydrate, zinc chloride, zinc sulfate, zinc sulfide, zinc carbonate, zinc citrate, and zinc gluconate.
[0049] The content of zinc (Zn) derived from such a zinc (Zn)-containing catalyst is not particularly limited, but may be 5 to 200 ppm, 6 to 200 ppm, 7 to 190 ppm, 8 to 190 ppm, 9 to 180 ppm, 9 to 170 ppm, 10 to 170 ppm, 10 to 160 ppm, 10 to 155 ppm, 11 to 150 ppm, or 16 to 150 ppm based on the total weight of the polyester resin. As the content of zinc (Zn) is within the above range, the above formulas 1 and 2 are satisfied, and thus a polyester resin having excellent color characteristics can be manufactured with high efficiency.
[0050] The phosphorus (P), which is an element included in the polyester resin according to the present invention, may be derived from a phosphorus (P)-containing stabilizer. The phosphorus (P)-containing stabilizer may not be particularly limited as long as it is commonly known. Specifically, the phosphorus (P)-containing stabilizer may include at least one selected from the group consisting of phosphoric acid, trimethyl phosphate, triethyl phosphate, triphenyl phosphate, and triethylphosphonoacetate.
[0051] The content of phosphorus (P) derived from such phosphorus (P)-containing stabilizer is not particularly limited, but may be 1 to 250 ppm, 1 to 245 ppm, 2 to 245 ppm, 2 to 240 ppm, 3 to 235 ppm, 3 to 230 ppm, 4 to 225 ppm, 4 to 220 ppm, 10 to 215 ppm, 20 to 210 ppm, or 25 to 205 ppm based on the total weight of the polyester resin. As the content of phosphorus (P) is within the above range, the above formulas 1 and 2 are satisfied, and thus a polyester resin having excellent color characteristics can be manufactured with high efficiency.
[0052] Meanwhile, the polyester resin according to the present invention may or may not further include elements derived from additives used in the production of the polyester resin (e.g., titanium (Ti), silicon (Si), antimony (Sb), tin (Sn), aluminum (Al), etc.), in addition to the germanium (Ge), zinc (Zn), and phosphorus (P).
[0053] In this way, the present invention can provide a polyester resin having excellent basic physical properties such as heat resistance, chemical resistance, and impact resistance while significantly improving color characteristics by including germanium (Ge), zinc (Zn), and phosphorus (P), which are specific elements among various elements included in the polyester resin, in the polyester resin so as to satisfy Equations 1 and 2. In addition, the present invention can provide a polyester resin having a desired intrinsic viscosity (IV) while maximizing the productivity of the polyester resin by manufacturing the polyester resin so that the germanium (Ge), zinc (Zn), and phosphorus (P) satisfy Equations 1 and 2.
[0054] Specifically, the polyester resin according to the present invention may exhibit a col-b value of -4 to +4 in a pellet state, thereby exhibiting excellent color characteristics (e.g., transparency). More specifically, the col-b value in the pellet state may be -4 to +3.5, -3.8 to +3, -3.6 to +2.6, -3.3 to +2, or -3 to +1.5. The col-b represents the 'complementary color of yellow to blue' among the color systems established by the International Standard Color Measurement Organization (CIE (Commission International d'Eclairage)), and can be measured using UltraScan PRO (manufactured by Hunterlab).
[0055] In addition, the polyester resin according to the present invention may have an intrinsic viscosity (IV) at 35°C of 0.6 to 1.3 dl / g, specifically 0.6 to 1.28 dl / g, 0.6 to 1.25 dl / g, 0.6 to 1.23 dl / g, 0.6 to 1.2 dl / g, or 0.6 to 1.15 dl / g. As the intrinsic viscosity is within the above range, the processability of the polyester resin can be secured.
[0056] The polyester resin according to the present invention may be a homopolymer or a copolymer. Specifically, the polyester resin may be selected from the group consisting of polyethylene terephthalate (PET), polyethylene terephthalate glycol (PETG), polyester sulfone (PES), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polybutylene adipate-co-terephthalate (PBAT), polypropylene adipate-co-terephthalate (PPAT), polycyclohexanedimethyl terephthalate (PCT), and thermoplastic polyester elastomer (TPEE).
[0057] The polyester resin according to the present invention may be in the form of chips, pellets, or powder.
[0058]
[0059] Method for manufacturing polyester resin
[0060] The present invention provides a method for producing the polyester resin described above. Specifically, the method for producing a polyester resin according to the present invention comprises the steps of: (S-1) introducing a diol component and a dicarboxylic acid component into a reactor; (S-2) introducing at least one of a germanium (Ge)-containing catalyst and a zinc (Zn)-containing catalyst and a phosphorus (P)-containing stabilizer into the reactor; (S-3) producing an oligomer by esterifying the diol component and the dicarboxylic acid component in the presence of the catalyst and the stabilizer; and (S-4) subjecting the oligomer to a condensation polymerization reaction, which will be described in detail as follows.
[0061]
[0062] Step (S-1): Input of raw ingredients
[0063] The above step (S-1) is a step of introducing a diol component and a dicarboxylic acid component into a reactor. Descriptions of each of the diol component and the dicarboxylic acid component are the same as those described above, and thus are omitted.
[0064] When the diol component and the dicarboxylic acid component are introduced into the reactor, the molar ratio between them (number of moles of diol component / number of moles of dicarboxylic acid) is not particularly limited, but considering the efficiency of the polymerization reaction and condensation polymerization reaction described below, it may be 1.1 to 2, 1.1 to 1.9, 1.1 to 1.8, or 1.1 to 1.7.
[0065] The above reactor may be a batch reactor or a continuous reactor.
[0066]
[0067] Step (S-2): Addition of catalyst and stabilizer
[0068] The above step (S-2) is a step of introducing at least one of a germanium (Ge)-containing catalyst and a zinc (Zn)-containing catalyst and a phosphorus (P)-containing stabilizer into the reactor. Descriptions of the germanium (Ge)-containing catalyst, the zinc (Zn)-containing catalyst, and the phosphorus (P)-containing stabilizer are the same as those described above, and therefore are omitted.
[0069] Meanwhile, the above reactor may further include the germanium (Ge)-containing catalyst and / or the zinc (Zn)-containing catalyst and the phosphorus (P)-containing stabilizer, as well as other additives including at least one selected from the group consisting of commonly known catalysts, coloring agents, crystallizers, antioxidants, and branching agents.
[0070] The catalyst may be a methylate of sodium or magnesium; an acetate, borate, fatty acid salt, or carbonate of Cd, Mn, Co, Ca, Ba, etc.; or an oxide or hydrate of Mg, Pb, Mn, Ti, Sb, Sn, Al, etc. For example, the catalyst may be tetraethyl titanate, acetyltripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, 2-ethylhexyl titanate, lactate titanate, octylene glycol titanate, triethanolamine titanate, acetylacetonate titanate, ethyl acetoacetic ester titanate, isostearyl titanate, titanium dioxide, or a combination thereof.
[0071] As the above coloring agent, organic compounds such as cobalt compounds, anthraquionone compounds, perinone compounds, azo compounds, and methine compounds (e.g., cobalt acetate, cobalt propionate, Clarient's Polysynthren Blue RLS toner, Clarient's Solvaperm Red BB toner) can be used.
[0072] As the above crystallizing agent, a crystal nucleating agent, an ultraviolet absorber, a polyolefin resin, a polyamide resin, etc. can be used.
[0073] As the above antioxidant, hindered phenol compounds, phosphite compounds, thioether compounds, etc. can be used.
[0074] As the above branching agent, trimellitic anhydride, trimellitic anhydride, trimellitic acid, etc. can be used.
[0075] This step (S-2) may be performed after the step (S-1) or simultaneously with the step (S-1). In addition, the germanium (Ge)-containing catalyst, the zinc (Zn)-containing catalyst, the phosphorus (P)-containing stabilizer, and the other additives may be added when performing the step (S-3) and / or step (S-4) described below.
[0076]
[0077] Step (S-3): Esterification reaction
[0078] The above step (S-3) is a step of producing an oligomer by esterifying the diol component and the dicarboxylic acid component in the presence of at least one of the germanium (Ge)-containing catalyst and the zinc (Zn)-containing catalyst and the phosphorus (P)-containing stabilizer.
[0079] The conditions under which the esterification reaction is performed may not be particularly limited. Specifically, the temperature at which the esterification reaction is performed may be 200 to 300°C, and more specifically, 220 to 300°C, 230 to 295°C, 240 to 290°C, 250 to 285°C, or 260 to 280°C. In addition, the pressure at which the esterification reaction is performed may be 0.1 to 5 kgf / ㎠, and specifically, 0.2 to 4.5 kgf / ㎠, 0.3 to 4 kgf / ㎠, 0.4 to 3.5 kgf / ㎠, or 0.5 to 3 kgf / ㎠. In addition, the time for which the esterification reaction is performed may be 2 to 10 hours, and specifically, 3 to 9 hours, 3.5 to 8.5 hours, 3.5 to 8 hours, or 4 to 7.5 hours. As the esterification reaction is performed under the above conditions, an oligomer having a desired molecular weight can be obtained in high yield while minimizing the production of side products.
[0080]
[0081] Step (S-4): Condensation polymerization reaction
[0082] The above step (S-4) is a step of subjecting the above oligomer to a condensation polymerization reaction.
[0083] The conditions under which the polycondensation reaction is performed may not be particularly limited. Specifically, the temperature at which the polycondensation reaction is performed may be 220 to 300°C, and more specifically, 230 to 300°C, 240 to 295°C, 250 to 290°C, or 260 to 285°C. In addition, the pressure at which the polycondensation reaction is performed may be a pressure (reduced pressure) lower than atmospheric pressure (e.g., 1 atm). In addition, the time for which the polycondensation reaction is performed may be 1 to 24 hours, and specifically, 1 to 20 hours, 2 to 15 hours, 3 to 10 hours, or 3.5 to 8 hours. When the polycondensation reaction is performed under the above conditions, a polyester resin (polymer) having the desired intrinsic viscosity and color characteristics can be efficiently produced while ensuring smooth discharge of by-products.
[0084]
[0085] The polyester resin of the present invention manufactured through the above steps (S-1) to (S-4) can have a content ratio of germanium (Ge), zinc (Zn), and phosphorus (P) satisfying the following equations 1 and 2. The explanation of the Ge / Zn ratio of the following equation 1 and the explanation of the (Ge+Zn) / P ratio of the following equation 2 are the same as those described above, and therefore are omitted.
[0086] [Formula 1]
[0087] 1≤Ge / Zn≤30
[0088] [Formula 2]
[0089] 1≤(Ge+Zn) / P≤15
[0090] The method for producing a polyester resin according to the present invention can provide a polyester resin having excellent color characteristics and high productivity by producing a polyester resin satisfying the above formulas 1 and 2.
[0091] Specifically, when manufacturing a polyester resin using the method for manufacturing a polyester resin according to the present invention, productivity is improved, and the manufacturing method has a process consumption rate (T) according to the following formula 3 c ) may be less than 65%. More specifically, the process consumption rate (T c ) may be 64% or less, 62% or less, 61% or less, 60% or less, 59% or less, 57% or less, 55% or less, 53% or less, 51% or less, 48% or less, or 45% or less (e.g., 5 to less than 65%, 10 to 63%, 15 to 60%, 20 to 58%, 25 to 53%, 30 to 50%, or 35 to 48%).
[0092] [Formula 3]
[0093] T c (%) = (T c2 / T c1 +T c2 ) × 100
[0094] In the above equation 3,
[0095] T c1 is the time consumed for the esterification reaction (time consumed in step (S-3)) during the manufacturing process of polyester resin,
[0096] T c2 is the time consumed for polycondensation reaction during the manufacturing process of polyester resin (time consumed in step (S-4)).
[0097] In addition, when manufacturing a polyester resin using the method for manufacturing a polyester resin according to the present invention, productivity is improved, and the manufacturing method can exhibit a productivity improvement index (PI) of 1 or more according to the following formula 4. Specifically, the productivity improvement (PI) may be 1.1 or more, 1.13 or more, 1.15 or more, 1.18 or more, 1.2 or more, 1.23 or more, 1.25 or more, 1.28 or more, 1.3 or more, 1.33 or more, 1.36 or more, 1.4 or more, 1.45 or more, 1.5 or more, 1.65 or more, 1.75 or more, 1.9 or more, or 2 or more (e.g., 1 to 2.5, 1.11 to 2.3, 1.15 to 2.1, 1.2 to 2, 1.25 to 1.95, or 1.35 to 1.93).
[0098] [Formula 4]
[0099] PI = IV × (T c1 +T c2 / T c2 )
[0100] In the above equation 4,
[0101] IV is the intrinsic viscosity of the polyester resin,
[0102] T c1 is the time consumed for esterification reaction during the manufacturing process of polyester resin,
[0103] T c2 is the time consumed in the polycondensation reaction during the manufacturing process of polyester resin.
[0104] Meanwhile, the steps (S-1) to (S-4) may be performed continuously, and by-products (e.g., side products, unreacted diol components, unreacted dicarboxylic acid components, etc.) generated in the steps (S-3) and / or (S-4) may undergo a process of recovery and purification. Thereafter, the purified product (e.g., ethylene glycol, etc.) obtained through the purification process may be reused as a reaction raw material.
[0105] The present invention is described in more detail through the following examples. However, the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention.
[0106]
[0107] [Example 1]
[0108] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 531.2 kg / hr), terephthalic acid (TPA, 1388.7 kg / hr), ethylene glycol (EG, 415.0 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 150.6 kg / hr), isosorbide (ISB, 61.1 kg / hr), and diethylene glycol (DEG, 22.2 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0109] Next, a Zn catalyst (Zinc acetate, 0.09 kg / hr), a Ge catalyst (GeO2, 1.3 kg / hr), a Ti catalyst (0.19 kg / hr), phosphoric acid (phosphoric acid, 0.021 kg / hr), a blue toner (0.008 kg / hr), and a red toner (0.002 kg / hr) were continuously fed into the continuous reactor.
[0110] Next, the temperature of the continuous reactor was gradually increased to 260°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 0.5 kgf / cm2 and a temperature of 260°C for 7 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0111] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 265°C while maintaining the pressure of the polycondensation reactor below atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.60 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 7 hours.
[0112] Next, the reactants discharged from the polycondensation reactor were introduced into a solid-state polymerization reactor, and the temperature of the solid-state polymerization reactor was gradually increased to 200°C under a nitrogen atmosphere, and then the solid-state polymerization reaction was performed at 200°C. When the solid-state intrinsic viscosity (IV) of the reactants in the solid-state polymerization reactor reached 1.3 dl / g, the reactants were discharged from the solid-state polymerization reactor to produce a pellet-type polyester resin (copolymer).
[0113]
[0114] [Example 2]
[0115] Terephthalic acid (TPA, 1578.9 kg / hr), ethylene glycol (EG, 357.7 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 547.8 kg / hr), isosorbide (ISB, 185.2 kg / hr), and diethylene glycol (DEG, 10.1 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0116] Next, a Zn catalyst (Zinc acetate, 0.06 kg / hr), a Ge catalyst (GeO2, 5.3 kg / hr), a Ti catalyst (0.19 kg / hr), phosphoric acid (phosphoric acid, 0.167 kg / hr), a blue toner (0.005 kg / hr), and a red toner (0.001 kg / hr) were continuously fed into the continuous reactor.
[0117] Next, the temperature of the continuous reactor was gradually increased to 255°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 2 kgf / cm2 and a temperature of 255°C for 5 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0118] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.7 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 7 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0119]
[0120] [Example 3]
[0121] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 112.0 kg / hr), terephthalic acid (TPA, 1390.9 kg / hr), ethylene glycol (EG, 47.4 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 889.1 kg / hr), isosorbide (ISB, 377.7 kg / hr), and diethylene glycol (DEG, 9.3 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0122] Next, a Zn catalyst (Zinc acetate, 0.88 kg / hr), a Ge catalyst (GeO2, 13.3 kg / hr), phosphoric acid (phosphoric acid, 0.938 kg / hr), blue toner (0.006 kg / hr), and red toner (0.002 kg / hr) were continuously fed into the continuous reactor.
[0123] Next, the temperature of the continuous reactor was gradually increased to 265°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 1 kgf / cm2 and a temperature of 265°C for 4 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0124] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 270°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.75 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 6 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0125]
[0126] [Example 4]
[0127] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 982.8 kg / hr), terephthalic acid (TPA, 481.7 kg / hr), isophthalic acid (IPA, 642.3 kg / hr), ethylene glycol (EG, 28.0 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 487.5 kg / hr), isosorbide (ISB, 188.3 kg / hr), and diethylene glycol (DEG, 20.5 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0128] Next, a Zn catalyst (Zinc acetate, 0.18 kg / hr), a Ge catalyst (GeO2, 9.3 kg / hr), a Ti catalyst (0.19 kg / hr), phosphoric acid (phosphoric acid, 1.042 kg / hr), and blue toner (0.01 kg / hr) were continuously fed into the continuous reactor.
[0129] Next, the temperature of the continuous reactor was gradually increased to 268°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 3 kgf / cm2 and a temperature of 268°C for 5 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0130] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 280°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.85 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 4 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0131]
[0132] [Example 5]
[0133] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 962.4 kg / hr), terephthalic acid (TPA, 943.4 kg / hr), ethylene glycol (EG, 13.7 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 818.4 kg / hr), isosorbide (ISB, 645.4 kg / hr), and diethylene glycol (DEG, 10.0 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0134] Next, a Zn catalyst (Zinc acetate, 0.06 kg / hr), a Ge catalyst (GeO2, 8.8 kg / hr), phosphoric acid (phosphoric acid, 0.313 kg / hr), blue toner (0.01 kg / hr), and red toner (0.004 kg / hr) were continuously fed into the continuous reactor.
[0135] Next, the temperature of the continuous reactor was gradually increased to 270°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 3 kgf / cm2 and a temperature of 270°C for 5 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0136] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 280°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.65 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 4 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0137]
[0138] [Example 6]
[0139] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 553.7 kg / hr), terephthalic acid (TPA, 1447.5 kg / hr), ethylene glycol (EG, 4.5 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 627.8 kg / hr), isosorbide (ISB, 1167.0 kg / hr), and diethylene glycol (DEG, 11.6 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0140] Next, a Zn catalyst (Zinc acetate, 0.58 kg / hr), a Ge catalyst (GeO2, 5.3 kg / hr), phosphoric acid (phosphoric acid, 0.146 kg / hr), blue toner (0.01 kg / hr), and red toner (0.004 kg / hr) were continuously fed into the continuous reactor.
[0141] Next, the temperature of the continuous reactor was gradually increased to 275°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 3 kgf / cm2 and a temperature of 275°C for 5 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0142] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 277°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.6 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 4 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0143]
[0144] [Comparative Example 1]
[0145] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 159.4 kg / hr), terephthalic acid (TPA, 937.4 kg / hr), ethylene glycol (EG, 451.3 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 90.4 kg / hr), and isosorbide (ISB, 36.6 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0146] Next, a Ge catalyst (GeO2, 0.8 kg / hr), a Ti catalyst (0.11 kg / hr), phosphoric acid (0.125 kg / hr), blue toner (0.003 kg / hr), and red toner (0.001 kg / hr) were continuously fed into the continuous reactor.
[0147] Next, the temperature of the continuous reactor was gradually increased to 255°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 2 kgf / cm2 and a temperature of 255°C for 6 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0148] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 265°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.7 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 11 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0149]
[0150] [Comparative Example 2]
[0151] Terephthalic acid (TPA, 878.5 kg / hr), ethylene glycol (EG, 146.6 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 533.4 kg / hr), isosorbide (ISB, 226.6 kg / hr), and diethylene glycol (DEG, 5.6 kg / hr) were continuously fed into a continuous reactor connected to a column and a condenser that could be cooled by water.
[0152] Next, a Zn catalyst (Zinc acetate, 0.11 kg / hr), a Ge catalyst (GeO2, 0.8 kg / hr), a blue toner (0.003 kg / hr), and a red toner (0.001 kg / hr) were continuously fed into the continuous reactor.
[0153] Next, the temperature of the continuous reactor was gradually increased to 265°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 1 kgf / cm2 and a temperature of 265°C for 5 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0154] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 275°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.75 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 5 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0155]
[0156] [Comparative Example 3]
[0157] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 577.4 kg / hr), terephthalic acid (TPA, 566.1 kg / hr), ethylene glycol (EG, 8.2 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 491.0 kg / hr), isosorbide (ISB, 387.2 kg / hr), and diethylene glycol (DEG, 6.0 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0158] Next, a Zn catalyst (Zinc acetate, 0.7 kg / hr), a Ge catalyst (GeO2, 1.6 kg / hr), phosphoric acid (phosphoric acid, 0.025 kg / hr), blue toner (0.004 kg / hr), and red toner (0.001 kg / hr) were continuously fed into the continuous reactor.
[0159] Next, the temperature of the continuous reactor was gradually increased to 275°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 1 kgf / cm2 and a temperature of 275°C for 5 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0160] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 280°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.5 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 10 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0161]
[0162] [Comparative Example 4]
[0163] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 144.4 kg / hr), terephthalic acid (TPA, 849.1 kg / hr), ethylene glycol (EG, 219.6 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 491.0 kg / hr), isosorbide (ISB, 387.2 kg / hr), and diethylene glycol (DEG, 6.0 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0164] Next, a Zn catalyst (Zinc acetate, 0.18 kg / hr), a Ge catalyst (GeO2, 1.6 kg / hr), phosphoric acid (phosphoric acid, 0.438 kg / hr), blue toner (0.006 kg / hr), and red toner (0.003 kg / hr) were continuously fed into the continuous reactor.
[0165] Next, the temperature of the continuous reactor was gradually increased to 275°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 1 kgf / cm2 and a temperature of 275°C for 4 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0166] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 280°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.5 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 12 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0167]
[0168] [Comparative Example 5]
[0169] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 166.1 kg / hr), terephthalic acid (TPA, 977.0 kg / hr), ethylene glycol (EG, 225.7 kg / hr), 1,4-cyclohexanedimethanol (CHDM, 376.7 kg / hr), isosorbide (ISB, 700.2 kg / hr), and diethylene glycol (DEG, 6.9 kg / hr) were continuously fed into a continuous reactor connected to a column and a water-cooled condenser.
[0170] Next, a Zn catalyst (Zinc acetate, 0.04 kg / hr), a Ge catalyst (GeO2, 6.4 kg / hr), phosphoric acid (phosphoric acid, 0.088 kg / hr), blue toner (0.006 kg / hr), and red toner (0.003 kg / hr) were continuously fed into the continuous reactor.
[0171] Next, the temperature of the continuous reactor was gradually increased to 275°C under a nitrogen atmosphere, and an esterification reaction (ES) was performed at a pressure of 1 kgf / cm2 and a temperature of 275°C for 5 hours to obtain an oligomer. At this time, the esterification reaction was performed while discharging by-products such as ethylene glycol and water to the outside of the continuous reactor.
[0172] Next, the oligomer was transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at a temperature of 280°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the melt intrinsic viscosity (IV) of the reactant in the polycondensation reactor reached 0.6 dl / g, the reactant was discharged from the polycondensation reactor. At this time, the polycondensation reaction took 8 hours. Thereafter, the discharged reactant was pelletized to produce a pellet-type polyester resin (copolymer).
[0173]
[0174] The conditions for the polyester resin manufacturing process of each of Examples 1 to 6 and Comparative Examples 1 to 5 are summarized in Table 1 below.
[0175]
[0176] Classification ES Reaction consumption time (h) PA Reaction consumption time (h) Melt intrinsic viscosity (IV, dl / g) Example 1770.6 Example 2570.7 Example 3460.75 Example 4540.85 Example 5540.65 Example 6540.6 Comparative Example 16110.7 Comparative Example 2550.75 Comparative Example 35100.5 Comparative Example 44120.5 Comparative Example 5580.6
[0177]
[0178] [Example 1]
[0179] The contents of germanium (Ge), zinc (Zn), and phosphorus (P) remaining in the pellet-type polyester resins manufactured in Examples 1 to 6 and Comparative Examples 1 to 5 were analyzed, and the content ratios therebetween were calculated and shown in Table 2 below. The analysis of germanium (Ge), zinc (Zn), and phosphorus (P) was performed using inductively coupled plasma atomic emission spectroscopy (ICP-AES).
[0180]
[0181] [Example 2]
[0182] The color of the pellet-type polyester resins manufactured in Examples 1 to 6 and Comparative Examples 1 to 5 was analyzed, and the results are shown in Table 2 below. The color analysis was performed by measuring the chromaticity and brightness of the pellet-type polyester resins using a Varian Cary 5 UV / Vis / NIR spectrophotometer equipped with a diffuse reflectance accessory. Next, transmission data was obtained with Illuminant D65 at an observer angle of 2°, and this was processed through a color analysis device in the Grams / 32 software to calculate the Hunter Lab value, thereby producing col-b.
[0183]
[0184] [Example 3]
[0185] Based on the consumption time of each reaction consumed in manufacturing pellet-type polyester resin in Examples 1 to 6 and Comparative Examples 1 to 5, the process consumption rate (T) according to the following Equation 3 c ) was produced, and the results are shown in Table 2 below.
[0186] [Formula 3]
[0187] T c (%) = (T c2 / T c1 +T c2 ) × 100
[0188] In the above equation 3,
[0189] T c1 is the time consumed in the esterification reaction (ES) during the manufacturing process of polyester resin,
[0190] T c2 is the time consumed in the polycondensation reaction (PA) during the manufacturing process of polyester resin.
[0191]
[0192] [Example 4]
[0193] Based on the intrinsic viscosity (IV) of the pellet-type polyester resins manufactured in Examples 1 to 6 and Comparative Examples 1 to 5 and the consumption time in each reaction, the productivity improvement (PI) according to Equation 4 below was calculated, and the results are shown in Table 2 below.
[0194] [Formula 4]
[0195] PI = IV × (T c1 +T c2 / T c2 )
[0196] In the above equation 4,
[0197] IV is the intrinsic viscosity of the polyester resin,
[0198] T c1 is the time consumed in the esterification reaction (ES) during the manufacturing process of polyester resin,
[0199] T c2 is the time consumed in the polycondensation reaction (PA) during the manufacturing process of polyester resin.
[0200]
[0201] Distinction Ge / Zn(Ge+Zn) / Pellet col-bT c(%)PI Example 12.713.8-3.550 %1.2 Example 2165.3-2.558 %1.2 Example 32.73.10.160 %1.25 Example 49.31.6-1.844 %1.91 Example 526.44.61.544 %1.46 Example 61.69.33.544 %1.35 Comparative Example 1Zn-free 10.565 %1.98 Comparative Example 21.3P-free 4.550 %1.5 Comparative Example 30.4357.567 %0.75 Comparative Example 41.60.9875 %0.67 Comparative Example 53211.88.562 %0.98
[0202] Referring to Table 2 above, it can be confirmed that the polyester resins of Examples 1 to 6, in which the Ge / Zn ratio and the (Ge+Zn) / P ratio fall within the scope of the present invention, have excellent color characteristics and high productivity.
[0203] Meanwhile, it can be confirmed that the polyester resin of Comparative Example 1, in which a zinc (Zn)-containing catalyst was not used, and the polyester resin of Comparative Example 2, in which a phosphorus (P)-containing stabilizer was not used, have poor color characteristics or productivity. In particular, it can be confirmed that Comparative Examples 3 to 5, in which the Ge / Zn ratio and the (Ge+Zn) / P ratio are outside the range of the present invention, have significantly poor color characteristics and very poor productivity.
Claims
1. A diol repeating unit derived from a diol component; and Contains a dicarboxylic acid repeating unit derived from a dicarboxylic acid component, A polyester resin having a content ratio of germanium (Ge), zinc (Zn) and phosphorus (P) satisfying the following equations 1 and 2: [Formula 1] 1≤Ge / Zn≤30 [Formula 2] 1≤(Ge+Zn) / P≤15 2. In paragraph 1, The above diol component is ethylene glycol, cyclohexanedimethanol, isosorbide, diethylene glycol, neopentyl glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, A polyester resin comprising at least one selected from the group consisting of 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, bis-2-hydroxyethyl terephthalate, and recycled bis-2-hydroxyethyl terephthalate.
3. In paragraph 1, The above Diol ingredient, a first diol component comprising ethylene glycol; and A polyester resin comprising a second diol component comprising at least one selected from the group consisting of cyclohexanedimethanol, isosorbide, diethylene glycol, bis-2-hydroxyethyl terephthalate, recycled bis-2-hydroxyethyl terephthalate, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol.
4. In paragraph 1, The above germanium (Ge) is derived from a germanium (Ge) containing catalyst, A polyester resin wherein the zinc (Zn) is derived from a zinc (Zn)-containing catalyst.
5. In paragraph 4, A polyester resin, wherein the germanium (Ge)-containing catalyst comprises at least one selected from the group consisting of a salt of a germanium (Ge)-containing aliphatic carboxylic acid, a salt of a germanium (Ge)-containing aromatic carboxylic acid, a salt of a germanium (Ge)-containing halogenated carboxylic acid, a salt of a germanium (Ge)-containing hydroxycarbonate, a salt of a germanium (Ge)-containing mineral, a germanium (Ge)-containing organosulfonate, a germanium (Ge)-containing organosulfate, a germanium (Ge)-containing alkoxide, a germanium (Ge)-containing acetylacetonate, a germanium (Ge)-containing oxide, a germanium (Ge)-containing metal, and a germanium (Ge)-containing hydroxide.
6. In paragraph 4, A polyester resin, wherein the zinc (Zn)-containing catalyst comprises at least one selected from the group consisting of zinc acetate, zinc acetate dihydrate, zinc chloride, zinc sulfate, zinc sulfide, zinc carbonate, zinc citrate, and zinc gluconate.
7. In paragraph 1, A polyester resin wherein the above phosphorus (P) is derived from a phosphorus (P)-containing stabilizer.
8. In paragraph 7, A polyester resin, wherein the phosphorus (P)-containing stabilizer comprises at least one selected from the group consisting of phosphoric acid, trimethyl phosphate, triethyl phosphate, triphenyl phosphate, and triethylphosphonoacetate.
9. In paragraph 1, A polyester resin, wherein the dicarboxylic acid component comprises at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, diphenyl dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, dimethyl 1,4-cyclohexane dicarboxylate, dimethyl 1,3-cyclohexane dicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, and azelaic acid.
10. In paragraph 1, A polyester resin having a col-b value of -4 to +4 in a pellet state.
11. Step of introducing a diol component and a dicarboxylic acid component into a reactor; A step of introducing at least one of a germanium (Ge)-containing catalyst and a zinc (Zn)-containing catalyst and a phosphorus (P)-containing stabilizer into the above reactor; A step of producing an oligomer by esterifying the diol component and the dicarboxylic acid component in the presence of the catalyst and the stabilizer; and Comprising a step of subjecting the above oligomer to a condensation polymerization reaction, A method for manufacturing a polyester resin in which the content ratios of germanium (Ge), zinc (Zn), and phosphorus (P) satisfy the following equations 1 and 2: [Formula 1] 1≤Ge / Zn≤30 [Formula 2] 1≤(Ge+Zn) / P≤15 12. In paragraph 11, A method for producing a polyester resin, wherein the above esterification reaction is performed at a temperature of 200 to 300°C.
13. In paragraph 11, A method for producing a polyester resin, wherein the above polycondensation reaction is performed at a temperature of 220 to 300°C for 1 to 24 hours.
14. In paragraph 11, Process consumption rate (T) according to the following equation 3 c ) is less than 65%, a method for manufacturing a polyester resin: [Formula 3] T c (%) = (T c2 / T c1 +T c2 ) × 100 In the above equation 3, T c1 is the time consumed for esterification reaction during the manufacturing process of polyester resin, T c2 is the time consumed in the polycondensation reaction during the manufacturing process of polyester resin.
15. In paragraph 11, A method for manufacturing a polyester resin having a productivity improvement index (PI) of 1 or more according to the following formula 4: [Formula 4] PI = IV × (T c1 +T c2 / T c2 ) In the above equation 4, IV is the intrinsic viscosity of the polyester resin, T c1 is the time consumed for esterification reaction during the manufacturing process of polyester resin, T c2 is the time consumed in the polycondensation reaction during the manufacturing process of polyester resin.
Citation Information
Patent Citations
Preparation method of polyester resin
KR1020130132138A
Novel polyester resin and method for preparation of the same
KR1020160053716A
Preparation method of polyester resin
KR1020160059287A
Isosorbide and neophentyl glycol copolymerized polyester resin and method of preparation thereof
KR1020160146080A
Polyester resin composition and process for manufacturing the same
WO2012007958A1