Neural electrode, neural device and methods of fabrication thereof

The rGO-based neural electrode with a nano-textured morphology addresses the limitations of existing electrodes by providing low impedance and high charge injection capacity, enabling stable and high-density neuronal recording over months without tissue damage or modification issues.

WO2024215255A1PCT designated stage expired Publication Date: 2024-10-17NATIONAL UNIVERSITY OF SINGAPORE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/SG2024/050237
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2024-04-08
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Current neural electrodes face challenges in achieving low impedance, high charge injection capacity, and long-term stability due to high interface impedance between neurons and metal, leading to poor electrochemical performance and tissue reactions.

Method used

A neural electrode with a reduced graphene oxide (rGO) fiber core and a sheath, featuring a nano-textured morphology to increase surface area, is developed, which eliminates the need for additional surface modifications and maintains low impedance and high charge injection capacity over time.

Benefits of technology

The rGO-based neural electrode achieves ultralow impedance and ultrahigh-density neuronal recording with high signal-to-noise ratio, enabling chronic and stable neural interface for extended periods without tissue damage or modification layer delamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SG2024050237_17102024_PF_FP_ABST
    Figure SG2024050237_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to a neural electrode comprising at least one probe, the probe having a reduced graphene oxide (rGO) fiber core and a sheath encapsulating the rGO fiber core; wherein the rGO fiber core is characterised by a cross sectional diameter of about 5 µm to about 100 µm; wherein an end of the rGO fiber core is substantially exposed from the sheath and is characterised by a cross sectional diameter of about 5 µm to about 100 µm; and wherein the end of the rGO fiber core comprises a nano- textured morphology in order to increase its surface area thereof. The present disclosure also relate to a neural device, methods of manufacture and use of the neural device thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Neural Electrode, Neural Device and Methods of Fabrication Thereof

[0002] Technical Field

[0003] The present invention relates, in general terms, to a neural electrode, a neural device and their methods of fabrication thereof.

[0004] Background

[0005] Neural electrodes provide an interface for the effective information transmission between the nervous system and external devices, which not only can be used in fundamental neuroscience research, such as exploring the mechanisms of cognitive processes and the neural basis of sensory information processing, but also help find cures for many neurological diseases. For example, recording brain activity by neural electrodes may identify the neural firing patterns related to epileptic activity, which can be used to locate epileptic lesions. In terms of neuromodulation, cochlear implants help deaf patients restore their hearing. Deep brain stimulations are used to relieve Parkinson's symptoms, and spinal cord stimulators help relieve neuropathic pain.

[0006] A functional microelectrode is required to communicate with an individual neuron to record bio-signals, while delivering sufficient amount of electrical charge to depolarize the neural tissue and initiate a response. Despite many significant breakthrough discoveries and technological innovations in this field, the existing microelectrode technologies have met significant challenges and limitations.

[0007] The ideal neural electrodes should have good biocompatibility, low impedance, and high charge injection capacity for the high-quality, low-damage, and long-term stable neural recording and regulation. Traditional neural electrodes fabricated from hard materials, such as metals and semiconductors, causing inflammation and glial hyperplasia in the tissues around the electrodes.

[0008] Electrode impedance is strongly correlated with the effective surface area of the electrode. Increasing its value can reduce the impedance and lower the thermal noise amplitude. A small metal electrode may have a large electrochemical impedance. resulting in a low signal-to-noise ratio.

[0009] Therefore, ideally the electrophysiological recording should identify the densely-packed nearby neurons over chronic timescales with minimum invasion. It requires invasive probe to directly interface with individual neuron near 1 :1 size ratio in each channel and assemble all the channels at neuronal density. However, broad adoption of such ideal design in neural electrophysiological recording probe is limited by the poor electrochemical performance of current metallic electrodes. This is due to the high interface impedance between neurons and metal induced low coupling efficiency causing low signal-to-noise ratio of recording signals.

[0010] Current advances in penetrating neural probes have been achieving some but not all the stringent requirements. The silicon probe, microelectrode array and Utah array, have leveraged complementary fabrication technology and materials engineering to expand the number and density of metallic recording sites. Increasing metallic site to 10 times larger than neuron may lower down impedance and subsequently reduce the noise level of recording signal, but it is not suitable for high-fidelity recording due to the low yield of single-unit sorting and large volume trauma induced significant gliosis and related deleterious tissue reaction. Surface modification of recording site is a well-known alternative for almost all the existing neural interfaces to permit the development of small and high-density probes. It either imports additional active layer or physically etch the smooth metal surface to nanoporous structure to increase the effective electrochemical surface area achieving low-impedance ionic-electronic transduction. For instance, metal wire tetrode of 17 urn 90%platinum / 10% iridium wires, a gold standard of the smallest unit of triangulation analysis of single-unit sorting, requires electroplating of platinum nanoparticles or PEDOT:PSS to decrease the impedance. It is challenging to perform stable chronic recording from such probes for months with minimum immunohistochemical response as it has high chance of modification layer delamination due to the weak interfacial adhesion and low environmental stability of coating layer or metal nanoparticle dissolution due to high relative surface area exposed. However, with surface modification, the latest silicon depth probe has achieved dense coverage along a plane perpendicular to the brain surface. While other geometries including Utah array and microelectrode array have been targeting to sample across a plane parallel to the brain surface, which offer important advantages in precise electrophysiology towards cellular medicine and brain functional organization. The areal spacing of recording sites has been narrowed down to 100 μm in large array. An alternative to commonly used metallic electrode is the graphene-based fiber probes, which has been validated for in vivo electrophysiology, and particularly attractive because of electrochemical inertness and competence, biocompatibility, as well as versatile fabrication and integration to flexible electronics or biomarker sensors. Hybrid of graphene fiber and platinum coating, graphene and polymer composite, and 70 μm thick graphene fiber were demonstrated for acute or chronic in vivo recording. With significant advances, the graphene-based probes can help address current challenges in compact neural probe design achieving high-density and high-yield single-unit recording and modulation, but have not yet been demonstrated to meet the potentially promising performance.

[0011] It would be desirable to overcome or ameliorate at least one of the above-described problems.

[0012] Summary

[0013] The present disclosure relates to a neural electrode comprising at least one probe, the probe having a reduced graphene oxide (rGO) fiber core and a sheath encapsulating the rGO fiber core; wherein the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; wherein an end of the rGO fiber core is substantially exposed from the sheath and is characterised by a cross sectional diameter of about 5 μm to about 100 μm; and wherein the end of the rGO fiber core comprises a nano-textured morphology in order to increase its surface area thereof.

[0014] In some embodiments, the rGO fiber core comprises intercalated and / or stacked rGO sheets, wherein the rGO sheets are aligned parallel to a longitudinal axis of the rGO fiber and wherein the rGO sheets are folded onto each other in a perpendicular direction relative to the longitudinal axis of the rGO fiber.

[0015] In some embodiments, the rGO fiber core is characterised by a cross sectional diameter of about 10 μm to about 20 μm. In some embodiments, the cross sectional diameter of the rGO fiber core is characterised by a relative standard deviation of less than 0.15.

[0016] In some embodiments, the rGO fiber core comprises nanotunnels between the rGO sheets, wherein the nanotunnels are characterised by a width of about 0.5 nm to about 500 nm.

[0017] In some embodiments, the end of the rGO fiber core has a cross sectional diameter which is substantially similar to the core of the rGO fiber.

[0018] In some embodiments, the end of the rGO fiber core comprises rGO sheets folded onto each other in a perpendicular direction relative to the longitudinal axis of the rGO fiber.

[0019] In some embodiments, the end of the rGO fiber core is characterised by an exposed cross sectional area of about 50 μm2to about 1000 μm2.

[0020] In some embodiments, the nano-textured morphology comprises a tip, wherein the tip is characterised by a morphology selected from a cone, or a pyramid.

[0021] In some embodiments, the rGO fiber core is characterised by a Young's modulus of about 10 GPa to about 50 GPa.

[0022] In some embodiments, the rGO fiber core is characterised by a cross sectional area of about 50 μm2to about 3500 μm2.

[0023] In some embodiments, the sheath comprises an insulator.

[0024] In some embodiments, the insulator is selected from parylene C, SU-8, polyimide, polyurethane, or a combination thereof.

[0025] In some embodiments, the sheath is characterised by a thickness of about 0.5 μm to about 10 μm.

[0026] In some embodiments, the probe is electrically connected to a wire or metal trace. In some embodiments, when the neural electrode comprises an array of probes, the probes spaced apart from each other and are adhered together by a hard polymer or a soft polymer.

[0027] In some embodiments, the neural electrode comprises at least 4 probes.

[0028] In some embodiments, the neural electrode is characterised by a cross sectional diameter is about 80 μm to about 100 μm.

[0029] In some embodiments, the neural electrode is characterised by an areal density of about 500 electrodes / mm2to about 4000 electrodes / mm2.

[0030] In some embodiments, the neural electrode is characterised by an impedance of about 0.0005 MΩ to about 1 MΩ.

[0031] In some embodiments, the neural electrode is characterised by a charge injection capacity of about 1.5 mC / cm2to about 10 mC / cm2.

[0032] In some embodiments, the neural electrode comprises an array of probes, wherein the array of probes is characterised by a probe density of about 500 probe / mm2to about 4000 probe / mm2.

[0033] The present disclosure also relates to a neural device, comprising : a) a neural electrode as disclosed herein; and b) a microdrive electrically connected to the neural electrode.

[0034] In some embodiments, the neural device further comprises computing means having a data processing algorithm.

[0035] The present disclosure also relates to a method of fabricating a neural electrode, the neural electrode comprising at least one probe, the probe having a reduced graphene oxide (rGO) fiber core and a sheath encapsulating the rGO fiber core, the method comprising : a) loading a solution of graphene oxide (GO) sheets and a reducing agent into a tubing in order to form a rGO gel; b) evaporating the rGO gel in order to form a rGO fiber; c) coating the rGO fiber with an insulator in order to form a rGO fiber core encapsulated with a sheath; and d) breaking the rGO fiber core and sheath in order to substantially expose an end of the rGO fiber core from the sheath; wherein the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; wherein an end of the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; and wherein the end of the rGO fiber core comprises a nano-textured morphology in order to increase its surface area thereof.

[0036] In some embodiments, the reducing agent is ascorbic acid.

[0037] In some embodiments, method further comprises a step after step a) of washing the rGO gel.

[0038] In some embodiments, the method further comprises a step after step c) of elastocapillary assembling at least one probe in order to form the neural electrode.

[0039] In some embodiments, the breaking step comprises: a) partially embedding the rGO fiber core and sheath in a polymer; b) cryo-freezing the partially embedded rGO fiber core and sheath; c) breaking the partially embedded rGO fiber core and sheath at an interface of the embedment; and d) dissolving the polymer of step a) in a solvent.

[0040] In some embodiments, the polymer is selected from OCT™, polyvinyl alcohol, and / or polyethylene glycol.

[0041] In some embodiments, when the neural electrode comprises an array of probes, the method further comprises a step of adhering the probes together with a hard polymer or a soft polymer.

[0042] The present disclosure also provides a method of isolating a neuron using the neural device as disclosed herein.

[0043] Brief description of the drawings

[0044] Embodiments of the present invention will now be described, by way of non-limiting example, with reference to the drawings in which:

[0045] Figure 1 shows stress-concentrated breaking-down technique to expose the electrode tip. a, Schematics of stress-concentrated breaking-down method (Natural cut (Ncut)). It involves partially coating the frozen optimal cutting temperature (OCT) compound on probe, increasing the diameter at one end, and hence causing significant bending stiffness difference between coating and uncoating part. It leads to naturally breakdown of the probe from the coating-uncoating point upon applying force, leaving a sharp exposure of graphene edge with well-preserved nanotexture and nanotunnels, b-c, SEM images of cross-section of the bare microfiber (b) and microfiber with parylene C (c) exposed by Ncut. d, Enlarged SEM images in c by viewing from top and tilted angle. It shows wavy nanotunnels and nanoedges, e, Schematics of scissors cutting in air (Acut) directly. It causes the deformation of the microfiber due to shear force from the scissors cutting, f-g, SEM images of cross-section of bare microfiber (f) and microfiber with parylene C (g) that were exposed by Acut. It shows deformed microfiber and the parylene C which reduced the exposed electrode area resulting in impedance spiking. Scale bar is 5 μm in b, c, f and g, 500 nm on the top and 250 nm at bottom in d.

[0046] Figure 2 is an overview of the monolithic high-density NeuroEdge, a, The schematic of NeuroEdge array interface with individual neurons at near 1:1 number ratio within an overall cross-section dimension of less than 100 μm. b, Scanning electron microscope (SEM) image of cross-section of a 20-channel NeuroEdge array. The NeuroEdge is coated with 2-μm parylene C for insulation and the NeuroEdge array is bundled via elastocapillary force-induced self-assembly from photoresist SU-8 bath followed by UV curing, c, Confocal image of neuron in the cortical area of a mouse brain labelled with neuronal nuclei (NeuN). The NeuroEdge and neurons show a similar density, d, Schematic of NeuroEdge tip. It featurs nanotexture, nanoedges and nanotunnels at the tip allowing for large relative electrochemical surface area and ion / electron coupling along nanotunnels, e, SEM images of the cross-section of NeuroEdge. The tip of NeuroEdge is sharply exposed using stress-concentrated breaking technique Where the I, II, III mark the nanotexture, nanotunnel and nanoedge, respectively, f, Comparison of the probe density of NeuroEdge, multielectrode array (MEA), and silicon probe regarding in the lateral direction within 100 μm x 100 μm region, g, Comparison of impedance (Z) of NeuroEdge, metal with a coating (ME-coat) and bare metal (ME-bare) with electrode dimensions comparable to the neuron cell body (~10 μm). The ideal impedance for electrophysiological recording is below 106 Ω. The NeuroEdge is within the ideal working range. The ME-coat initially falls in the working range, but moves out of the range over time due to the delamination and degradation of the modification layer. The ME-bare is far from the ideal working range. Scale bar is 25 μm in b and c, and 0.5 μm in e.

[0047] Figure 3 shows the fabrication process of NeuroEdge. Fabrication includes four key steps, incorporating solution-processable self-assemblies and stress-concentrated break-down. Specifically, in step I, to maximize the in vivo biocompatibility and realize the small form factor while streamline fabrication, solution-processable graphene oxide (GO) sheets were employed to form reduced graphene oxide (rGO) gel fiber through in situ 3D self-assembly and reduction with only water and vitamin C, a natural antioxidant that is widely employed as a food additive and can compete with the highly toxic hydrazine in terms of its reducing capability. Step II involves restricted self-alignment, driven by water evaporation induced self-assembly, to form a straight microelectrode fiber (II) from the gel fiber. The photograph reveals the prepared microfiber is significantly slimmer than the hair and fingerprint. In step III, to maximize array density, elastocapillary self-assembly was employed, merging the parylene C insulated microfibers into a bundle during the withdrawal from a bath of diluted SU-8 solution. The small form factor of microfiber enabled the elastocapillary self-assembly by providing a balanced adhesion energy arising from van der Waals force and probe stiffness. Such assembly cannot be extended to metal wires in similar neuronal size or larger metal probes as their stiffness will exceed the capillary adhesion force, preventing the formation of bundles. The grand challenge of this high-density configuration is to maintain a low impedance while reduce the recording site to neuronal size. Therefore, in step IV we developed a stress-concentrated break down method to expose the bundle tip end. The rGO sheet stack are well exposed preserving the nanoedge, nanotexture and nanotunnels, which accounts for the low impedance. During the whole process, the absence of toxic or organic solvent aligned with small size of probe, prioritizes the biocompatibility essentials for implantable probes. The solution processable technology allows for precise tuning of the probe to any desirable size. The stitched rGO sheets via van der Waals force enable highly flexibility and robustness of the NeuroEdge. Figure 4 shows step II of fabrication process of NeuroEdge. We examined three approaches for creating rGO microfiber from gel fiber with the goal of minimizing axial footprint size and fluctuation in diameter, a, Schematic of free-standing approach and the SEM images of the prepared microfiber. The gel fiber was exposed to air and underwent natural evaporation of water within the gel fiber. The evaporation process allows the rGO sheets to contact each other and shrink. However, the uneven evaporation rate, influenced by distinct radii of curvature at different locations along the gel fiber, led to uneven movement of rGO sheets, resulting in varying diameters at different locations. The SEM shows deep folding or crumpling of rGO sheets, b, Schematic of wet-mounting approach and the SEM images of the prepared fiber. The gel fiber was placed on a glass substrate. As water evaporated, the high surface tension of water caused the gel fiber to wet the hydrophilic glass, expanding its axial footprint. The bottom layer of rGO sheets were adhered to the glass due to interface tension between water and glass, minimizing crumpling and allowing for the stacking of rGO sheets layer-by-layer. The SEM images show the outer rGO sheets appear much flatter compared to those in a. with a footprint of 70 μm. c, Schematic of restricted solvent evaporation induced self-assembly (SEIA) and the SEM images of the resulting fiber. The gel fiber was anchored at both ends on a plastic substrate, and underwent solvent evaporation induced self-assembly of the rGO sheets along the anchoring direction. The absence of interface tension allowed the rGO sheets to freely assembly while being confined to the mounting direction, resulting in a small diameter and a straight longitudinal alignment. The SEM images showed the diameter is only 12 μm which is 5- fold smaller compared to b. d-e, Schematics of viewing direction and the SEM images from cross-section for fiber that was prepared by methods in b (d) and c (e). The folding of rGO sheets in e from restricted SEIA method resulted in a wavy pattern, while flattened rGO sheets from the wet-mounting method showed a layered pattern. It highlights the advantage of the method in c for reducing the diameter. Scale bar is 100, 10 and 0.5 μm for SEM images from top to bottom in a, b and c, and 0.5 μm in d and e.

[0048] Figure 5 shows a-b, Raman characterization (a) and X-ray photoelectron spectroscopy (XPS) (b) for NeuroEdge. The inset in a is the Raman scan of the exposed tip end of NeuroEdge. The D / G ratio is predominantly around 1.3. The XPS result showed a significantly increased ratio of carbon-to-oxygen compared to graphene oxide (GO). It indicates that the GO has been successfully converted to reduced graphene oxide (rGO). Figure 6 shows electrochemical characterization of NeuroEdge, a, Impedance at 1 kHz of NeuroEdge compared with reported metal electrodes (Metal), surface modified metal electrodes (Modified), and carbon-based electrodes (Carbon), b Impedance of NeuroEdge compared with that of conventional metal wires Pt / Ir (iridium 10%) in different diameters, c, Specific impedance at 1 kHz of NeuroEdge compared with Pt / Ir and PEDOT:PSS modified Pt / Ir. Values are mean ± s.d. d, Specific impedance at 1 kHz of NeuroEdge as a function of charging time compared with PEDOT:PSS modified Pt / Ir under a biphasic pulse. Charge density, 1 mC cm-2; pulse width, 1 ms; interphase delay, 50 ps; pulse frequency, 25 Hz. e, Specific impedance at 1 kHz of NeuroEdge as a function of soaking time in PBS compared with PEDOT:PSS modified Pt / Ir. f, Cyclic voltammetry (CV) of PEDOTiPSS modified Pt / Ir at different soaking period scanning at a 100 mV S-l sweep rate in the voltage range of -0.6 to 0.9 V versus Ag |AgCI. The minimum current kept dropping down by 24 times at 6-week marked in dashed circle, g. CV of NeuroEdge in the voltage range of -1.6 to 1.3 V versus Ag |AgCI. The minimum current was relatively stable with a change of < 10% at 6-month. h, Impedance of NeuroEdge over 6-month soaking in phosphate buffered saline (PBS, 0.01 M), indicating a relatively stable electrochemical performance. The scale bar is 1 μm in d and e.

[0049] Figure 7 shows in vivo high-density and high-quality recording and spike-sorting with NeuroEdge, a, Schematics of a mouse brain with implantation showing the location of 16-channel NeuroEdge, ground screw (GND), and supporting screw, as well as a 16- channel NeuroEdge neural interface (right side), b, Representative 10-min neural recording from channel 1 (Chi) in the cortex shows both local field potential (LFP) (0.1- 9000 Hz) and spontaneous spiking signal (300-9000 Hz), c, A typical waveform before and after high-pass (HP) filtering at 300 Hz in b marked by a red line, displaying clear depolarization, repolarization and relative refractory periods. The waveforms before and after filtering are almost identical in shape with a high amplitude of 600 μV. d, e. Power spectrum density (PSD) (d), and spectrogram (e) of the recorded signal (0.1-9000 Hz). The smooth average value of PSD shown in dark line in d and continuous horizontal PSD at different frequency demonstrate no significant external environment noise in the recording, f, g, Amplitude (f) and SNR (g) in maximum and average of the recorded signal after 300-9000 Hz band-pass filtering, h-j. Triangulation spike sorting using Offline Sorter. It mainly includes three steps. First, filter the raw data with a second order Butterworth HP filtering (h). Second, detect the waveform cross the positive-going threshold and extract the waveform in a 1.13-ms time window with a pre-threshold period of 0.26 ms and dead time of 1.03 ms. (i). Spikes are stored for all 4 channels whenever any 1 of the 4 crosses the threshold. The waveforms crossing the threshold and their intervals exceeding the dead time will be detected. Only positive-peaked APs are extracted because they are encountered most frequently. All the detected spikes are shown in the raster plot. Third, spike clustering based on principle components analysis (PCA) (j). It groups spikes with similar feature vectors that represent the activity of a single neuron. Each point on the plot represents a spike exceeding the defined threshold. Seven clusters are projected onto the first two principal components and marked as N1 to N7. k. Average spike waveforms on 4 channels for each putative neuron. I, Representative dense neural recording from 16-channel in cortex revealed clear and strong LFP and spiking signal (0.1-9000 Hz, left) and filtered spontaneous spiking signal (300-9000 Hz, right), m, n, Raster plot (m) and average waveforms (n) of the sorted units from the recording in I.

[0050] Figure 8 shows implantation of NeuroEdge, a. Schematics of fabrication and implantation of the NeuroEdge drive into mouse brain, b, Photograph of one representative probe, c, Photograph of the implantation of the probe into brain. NeuroEdge was attached onto a movable drive. With a clockwise turn of the screw on drive, the electrode was loaded down around 180 μm.

[0051] Figure 9 shows NeuroEdge resolves heterogeneity in the acoustic frequency response of neighboring neurons in mice auditory cortex, a, Schematic set-up for the auditory stimuli and recordings. The sound card supplies two channels. One is the click channel to align the timeline of the electrophysiological recording and the stimuli, and another is the tone channel to deliver auditory stimuli. There are 78 frequencies spanning 0.5- 42 kHz in1 / 2 octave with a duration of 100 ms and interstimulus interval of 1.3 s. b, Representative recording and its spectrogram during the stimulus duration in a marked by red background, c, Representative electrophysiological recording from NeuroEdge during pre-stimulation and stimulation spanning 0.5-42 kHz. d. Time-domain spike density (SD) colormaps and average spike density curves of representative putative neurons in a time window crossing the stimuli duration, e, Frequency-domain stimuli response of the same representative neurons in d. The red lines are the fitted curves, f, Average SD ratio for each putative neuron responding to full frequency from 0.5 to 42 kHz (All), lower frequency marked in f1 and higher frequency marked in f2 in d. The center frequency of f1 and f2 is 2.6 kHz and 9.5 kHz, respectively. The black solid line represents the SD ratio from the whole channel including all the neurons, g, Representative cross-correlograms of neurons under no stimulation and stimulation with full frequency of 0.5-42 kHz, f1and f2 h, Cross-correlation matrices of pairwise neurons under no stimulation and stimulation with full frequency of 0.5-42 kHz, f1 and f2.

[0052] Figure 10 shows auditory stimulation setup and data processing, a, Schematics of the auditory stimulation setup. It contains two channels, with the trigger channel marking the timestamp of the stimulation tone aligned with the recorded signal. Each frequency is stimulated for 100 ms, and interstimulus interval is 1.3 s to leave enough rest time for the neuron to recover from the last stimulus, b. Schematics of data processing. The filter signal was realigned by interval of 1.3 s, and each corresponds to a sound frequency, c. Peristimulus raster plot.

[0053] Figure 11 shows chronic assessment of recording stability, functionality and biocompatibility of NeuroEdge, a, A photograph of a mouse implanted with NeuroEdge and a schematic of the chronic recording timeline, b, Representative electrophysiological recording from NeuroEdge at Ml, M3 and M6. BP filtering of 300-9000 Hz was applied, c-d, Performance of the electrophysiological recording stability. The average values of SNR and noise level (c), NeuroEdge impedance and spike amplitude (d) all remained stable for 6 months, e-f, Peristimulus spike raster plot (e) and spike density (f) in response to 78 frequencies spanning 0.5-42 kHz at month 1, 3 and 6. It shows a similar spike density increase in the stimulus window responding to the acoustic stimuli at the same probe implantation location L1 at Ml and 3, and remained functional after moving down the probe by ~150 μm to L2 at M6. g, Frequency response distribution of representative near-by single units in mice at M6. h, Chronic-biocompatibility of pristine NeuroEdge and PEDOT: PSS / Au coated NeuroEdge after 3-month implantation. Neurons, microglia and astrocytes are immunohistochemically stained with NeuN (red), Ibal(red) and GFAP (green), respectively, i, Analysis of the neuron cells (NeuN), activated microglia (Ibal) and astrocyte cells (GFAP) around insertion position across the entire immunohistochemical images. Values are shown mean ± s.d. using one-way t-test (*P<0.05, **P<0.01).

[0054] Detailed description

[0055] The present disclosure is predicated on the understanding that compared to the modification of traditional electrode materials, the development of graphene-based neural electrodes is a relatively simple and cost-effective method. Owing to its excellent bio and neuroelectronic properties, graphene is an ideal material for future neural probes. Graphene is a two-dimensional nanomaterial with a single atomic layer composed of sp2-hybridized carbon atoms. As an active material for neural electrodes, graphene has many advantages over other materials that include: (1) high mechanical flexibility that allows close contacts with soft brain tissues and formation of a stable electrode-neuron interface; (2) good electrical conductivity and excellent carrier mobility (up to 100,000 cm2.V-1'S-1), which promote the highly sensitive detection of neuroelectric signals by a graphene field-effect transistor; (3) a single atomic layer thickness and ultra-high specific surface area combined with unique electrical properties, which ensure low electrochemical impedance and high charge injection capabilities of graphene neural electrodes that lay the foundation for the effective electrical stimulation of neural tissues; and (4) high transparency and transmittance of a single-layer graphene (up to 97.3%).

[0056] A porous electrode materials may be used to obtain a neural electrode with a larger effective surface area but smaller geometric size. However, traditional porous electrode materials has bad mechanical property, which is not easy to handle or insert into tissue. In contrast, graphene sheets may be obtained by exfoliation, and graphene fiber electrodes with highly active graphene edge and large relative surface area are produced after tip exposure. Therefore, graphene electrodes can record electrophysiological signals while observing changes in cells and blood vessels under the electrodes with electrophysiological activity. Owing to their high transparency, graphene neural electrodes can also be combined with other technologies (such as optogenetics) for the optical regulation of neuroelectric activities.

[0057] The present disclosure concerns a graphene fiber based pristine neural electrode and neural probe array, which may enable ultralow-impedance and ultrahigh-density neuronal recording and modulation achieving a neuron-to-neuron functionality discrimination and accurate electronic medicine therapy for months. It may be used for chronically stable neural interface for lots of promising application that could alter our living status. For instance, the brain-machine interface, neuronal modulation for deepbrain disease, prosthesis helping disables. The probe array may record the signal from nervous system with high signal-to-noise ratio and long-term stability. The individual probe can be down to single neuronal size, and more than 15 vertical aligned probes can be bonded together in the horizontal direction at an area of cross-section of individual human hair, which enables the probe density close to the neuron density in the cortex area of brain. The unique texture structure on the exposed cross-section end has high electrochemical activity and large surface area, resulting in an ultra-low impedance, which is even better than modified probe with metal nanoparticles or conducting polymer. Such high electrochemical activity at extremely low exposed area allows for high-quality recording and modulation at high-density, which turns out a high- quality spike-sorting to identify single-units at higher yield and higher density. It helps further allocate the functionality of brain at higher resolution to individual near-by neurons.

[0058] Accordingly, the present disclosure relates to a neural electrode comprising at least one probe, the probe having a reduced graphene oxide (rGO) fiber core and a sheath encapsulating the rGO fiber core; wherein the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; wherein an end of the rGO fiber core is substantially exposed from the sheath and is characterised by a cross sectional diameter of about 5 μm to about 100 μm; and wherein the end of the rGO fiber core comprises a nano-textured morphology in order to increase its surface area thereof.

[0059] It was found that by stress concentrating an end of the rGO fiber and sheath and subsequently breaking it, the cross sectional diameter (and hence cross sectional area) of the end of the rGO fiber core is maintained relative to the body of the rGO fiber core. In this regard, the end of the rGO fiber core is not deformed. Further, nano-textured morphology may be created at the end of the rGO fiber core which may increase its surface area, higher electrochemical activity and thus low impedance is enabled for large array or individual fiber. In contrast, a normal cut (using scissors) will cause the tib end to collapse and the sheath on the surface of fiber to deform and cover the end of the rGO fiber, causing large impedance. By stress concentrating the end of the rGO fiber, ultralow-impedance recording and ultrahigh charge injection capacity may be obtained. As the rGO fiber has a diameter of less than 100 μm, or preferably less than 20 μm, which is similar to neuronal size, this further adds to the improved quality for recording and modulation. In contrast, pure metal probe cannot achieve neuronal size while meeting the impedance requirement, and modified probe can reach this size but with extra risk of modification layer detach causing worse long-term stability.

[0060] It was found that the electrode (and probe) as disclosed herein does not need an additional modification layer to lower down impedance or improve charge injection capacity. The modified layer has a high chance to delaminate or fatigue with time. This will cause failure in recording, and at the same time damage the tissue to induce immune response. Accordingly, in some embodiments, the probe is pristine. This means that the probe is not further functionalised or modified. In some embodiments, the probe is void of surface modifications.

[0061] In some embodiments, the rGO fiber core comprises intercalated and / or stacked rGO sheets. The sheets are physically connected together but leave nanovoids between the rGO sheets. In some embodiments, the rGO sheets are characterised by an intersheet distance of about 0.5 nm to about 500 nm. In some embodiments, the rGO sheets are axially aligned. The alignment may be along a longitudinal direction of the rGO fiber core. In some embodiments, the probe comprises nanotunnels between the rGO. The nanotunnels may be formed due of the spacing between the intercalated and / or stacked rGO sheets. The nanotunnels may be about 0.5 nm to about 500 nm in width. In other embodiments, the intersheet distance and / or nanotunnels is about 0.5 nm to about 450 nm, about 0.5 nm to about 400 nm, about 0.5 nm to about 350 nm, about 0.5 nm to about 300 nm, about 0.5 nm to about 250 nm, about 0.5 nm to about 200 nm, about 0.5 nm to about 150 nm, about 0.5 nm to about 100 nm, or about 0.5 nm to about 50 nm.

[0062] In some embodiments, rGO fiber core comprises a single linear rGO fiber. The rGO fiber core may be formed as a straight fiber. In some embodiments, the rGO fiber core is characterised by a uniform and straight morphology. This is due to the restricted selfassembly of rGO sheets, and optionally the restricted drying of the rGO gel in order to form the rGO fiber. As shown in Figure 9, in the restricted self-assembly of rGO sheets, the rGO sheets in the rGO gel are induced to self-assemble along an anchoring direction. The resulting rGO fiber has a small diameter (at least 5 times smaller than a fiber formed from a wet mounting approach) as a result of the rGO sheets stacking more closely to each other. The rGO sheets are also aligned within the rGO fiber in a straight longitudinal alignment relative to the rGO fiber. A cross sectional view of the rGO fiber shows that the rGO sheets are folded on each other resulting in a wavy pattern as observed under SEM, which indicates that the rGO sheets curled onto each other.

[0063] In some embodiments, rGO fiber comprises rGO sheets, wherein the rGO sheets are aligned parallel to a longitudinal axis of the rGO fiber. In some embodiments, the rGO sheets are folded onto each other in a perpendicular direction relative to the longitudinal axis of the rGO fiber. In some embodiments, a cross section of the rGO fiber comprises folded rGO sheets.

[0064] In some embodiments, the rGO fiber core is characterised by a Young's modulus of about 10 GPa to about 50 GPa. In some embodiments, the Young's modulus is about 10 GPa to about 45 GPa, about 10 GPa to about 40 GPa, about 10 GPa to about 35 GPa, about 10 GPa to about 30 GPa, about 10 GPa to about 25 GPa, about 10 GPa to about 20 GPa, or about 10 GPa to about 15 GPa.

[0065] In some embodiments, the rGO fiber core is characterised by a bending stiffness of about 2 x 10-2nN m2to about 8 x I0-2nN m2. In some embodiments, the rGO fiber core is characterised by a bending stiffness of about 2 x 10'2nN m2to about 7.5 x 10"2nN m2, about 2 x 10'2nN m2to about 7 x 10'2nN m2, about 2 x 10'2nN m2to about 6.5 x 10'2nN m2, about 2 x 10'2nN m2to about 6 x 10'2nN m2, about 2 x 10'2nN m2to about 5.5 x 102nN m2, about 2 x 102nN m2to about 5 x 102nN m2, about 2 x I0-2nN m2to about 4.5 x I0-2nN m2, or about 2 x 10'2nN m2to about 4 x 10'2nN m2. In some embodiments, the rGO fiber core is characterised by a bending stiffness of 4 x 10-2nN m2.

[0066] In some embodiments, the rGO fiber core is characterised by a cross sectional area of about 50 μm2to about 3500 μm2. In other embodiments, the cross sectional area is about 100 μm2to about 3500 μm2, about 200 μm2to about 3500 μm2, about 300 μm2to about 3500 μm2, about 400 μm2to about 3500 μm2, about 500 μm2to about 3500 μm2, about 600 μm2to about 3500 μm2, about 700 μm2to about 3500 μm2, about 800 μm2to about 3500 μm2, about 900 μm2to about 3500 μm2, about 1000 μm2to about 3500 μm2, about 1500 μm2to about 3500 μm2, about 2000 μm2to about 3500 μm2, about 2500 μm2to about 3500 μm2, or about 3000 μm2to about 3500 μm2.

[0067] In some embodiments, the cross sectional diameter of the rGO fiber core is about 10 μm to about 100 μm, about 10 μm to about 90 μm, about 10 μm to about 80 μm, about 10 μm to about 70 μm, about 10 μm to about 60 μm, about 10 μm to about 50 μm, about 10 μm to about 40 μm, about 10 μm to about 30 μm, or about 10 μm to about 20 μm. In some embodiments, the cross sectional diameter of the rGO fiber core is about 12 μm to about 15 μm. In some embodiments, the cross sectional diameter of the rGO fiber core is characterised by a relative standard deviation of less than 0.15. A consistent diameter was found to be advantageous for the low impedance.

[0068] In some embodiments, the end of the rGO fiber core is undeformed. This is shown in Figure 6. In this regard, the end of the rGO fiber retains a cross sectional diameter similar to the core of the rGO fiber. In some embodiments, the end of the rGO fiber has a cross sectional diameter which is substantially the same as the core of the rGO fiber. As disclosed herein, the present method of forming the probe does not deform the sheath nor the rGO fiber core.

[0069] The end of the rGO fiber is undeformed in that the intersheet spacing of rGO sheets and / or nanotunnels is substantially similar to that in the rGO fiber core. In a cross sectional view, the rGO sheets also maintain its folded configuration onto each other. The edge or end is also not covered by the sheath if present. As this edge is maintained similar to the core of the fiber, electrical signals from a brain may be transferred at low impedance.

[0070] In some embodiments, the end of the rGO fiber core is characterised by a surface unevenness of about 5 nm to about 900 nm. In other embodiments, the end of the rGO fiber core comprises a tip. The tip may protrude from the sheath, or may be levelled with an interface of the sheath.

[0071] In some embodiments, the tip is characterised by a morphology selected from a cone, or a pyramid. Other shapes may also be possible. It was found that a protrusion is sufficient to provide a low impedance, as it improves contact with the neural tissue.

[0072] In some embodiments, the end of the rGO fiber core is characterised by an exposed cross sectional area of about 50 μm2to about 3500 μm2. In other embodiments, the exposed cross sectional area is about 100 μm2to about 3500 μm2, about 200 μm2to about 3500 μm2, about 300 μm2to about 3500 μm2, about 400 μm2to about 3500 μm2, about 500 μm2to about 3500 μm2, about 600 μm2to about 3500 μm2, about 700 μm2to about 3500 μm2, about 800 μm2to about 3500 μm2, about 900 μm2to about 3500 μm2, about 1000 μm2to about 3500 μm2, about 1500 μm2to about 3500 μm2, about 2000 μm2to about 3500 μm2, about 2500 μm2to about 3500 μm2, about 3000 μm2to about 3500 μm2, about 50 μm2to about 3000 μm2, about 50 μm2to about 2500 μm2, about 50 μm2to about 2000 μm2, about 50 μm2to about 1500 μm2, or about 50 μm2to about 1000 μm2.

[0073] In some embodiments, the end of the rGO fiber core is characterised by a cross sectional diameter of about 10 μm to about 100 μm, about 10 μm to about 90 μm, about 10 μm to about 80 μm, about 10 μm to about 70 μm, about 10 μm to about 60 μm, about 10 μm to about 50 μm, about 10 μm to about 40 μm, about 10 μm to about 30 μm, or about 10 μm to about 20 μm. In some embodiments, the end of the rGO fiber core is characterised by a cross sectional diameter of about 12 μm to about 15 μm.

[0074] In some embodiments, the sheath comprises an insulator. An electrical insulator is a material in which electric current does not flow freely. The atoms of the insulator have tightly bound electrons which cannot readily move. The property that distinguishes an insulator is its resistivity; insulators have higher resistivity than semiconductors or conductors.

[0075] In some embodiments, the insulator is selected from parylene C, SU-8, polyimide, polyurethane, or a combination thereof. In some embodiments, the insulator is parylene C.

[0076] In some embodiments, the sheath is characterised by a thickness of about 0.5 μm to about 10 μm. In other embodiments, the thickness is about 0.5 μm to about 9 μm, about 0.5 μm to about 8 μm, about 0.5 μm to about 7 μm, about 0.5 μm to about 6 μm, about 0.5 μm to about 5 μm, about 0.5 μm to about 4 μm, about 0.5 μm to about 3 μm, about 0.5 μm to about 2 μm, or about 0.5 μm to about 1 μm.

[0077] In some embodiments, the probe comprises nanotunnels between the rGO, wherein the nanotunnels are filled with an electrolyte. The electrolyte may be a salt solution. The electrolyte may be phosphate buffered saline or body fluid. The nanotunnels may be filled with an electrolyte when used, or the probe may be dry without electrolyte inside nanotunnels if not in use. In some embodiments, the probe is electrically connected to a wire or metal trace. For example, a stainless steel wire may be used. The probe may be connected to the wire via the other end of the rGO fiber.

[0078] In some embodiments, when the neural electrode comprises an array of probes. The probes may be adhered together by a hard polymer or a soft polymer. In this regard, a single sheath may be used to encapsulate the probes while still maintaining electrical separation relative to each other. For example, epoxy, polyimide, polyurethane, PEG, PVA and / or PDMS may be used. The epoxy may be SU-8.

[0079] In some embodiments, the neural electrode comprises at least 4 probes. In some embodiments, the neural electrode comprises at least 16 probes. The neural electrode may comprise an array of probes. The array may be a square array or a circular array. The probe may be arrayed such that they are spaced apart from each other.

[0080] Due to the small size of the probes, ultrahigh density array may be achieved. This improves the recording or modulation resolution to be individual neuron cell.

[0081] In some embodiments, the neural electrode is characterised by a cross sectional diameter of about 10 μm to about 100 μm, about 20 μm to about 100 μm, about 30 μm to about 100 μm, about 40 μm to about 100 μm, about 50 μm to about 100 μm, about 60 μm to about 100 μm, about 70 μm to about 100 μm, or about 80 μm to about 100 μm. In some embodiments, the cross sectional diameter is about 100 μm.

[0082] In some embodiments, the neural electrode is characterised by an areal density of about 500 electrodes / mm2to about 4000 electrodes / mm2. In some embodiments, the areal density is about 800 electrodes / mm2to about 4000 electrodes / mm2, about 1000 electrodes / mm2to about 4000 electrodes / mm2, about 1500 electrodes / mm2to about 4000 electrodes / mm2, about 2000 electrodes / mm2to about 4000 electrodes / mm2, about 2500 electrodes / mm2to about 4000 electrodes / mm2, about 3000 electrodes / mm2to about 4000 electrodes / mm2, or about 1000 electrodes / mm2to about 3500 electrodes / mm2.

[0083] In some embodiments, the neural electrode is characterised by an impedance of about 0.0005 MΩ to about 1 MΩ. In some embodiments, the impedance is about 0.0005 MΩ to about 0.9 MΩ, about 0.0005 MΩ to about 0.8 MΩ, about 0.0005 MΩ to about 0.7 MQ, about 0.0005 MΩ to about 0.6 MΩ, about 0.0005 MQ to about 0.5 MQ, about 0.0005 MQ to about 0.4 MQ, about 0.0005 MQ to about 0.3 MQ, about 0.0005 MQ to about 0.2 MQ, about 0.0005 MQ to about 0.1 MQ, about 0.0005 MQ to about 0.09 MQ, about 0.0005 MQ to about 0.08 MQ, about 0.0005 MQ to about 0.07 MQ, about 0.0005 MQ to about 0.06 MQ, or about 0.0005 MQ to about 0.05 MQ. Preferably, the impedance is about 0.04 MQ.

[0084] In some embodiments, the impedance is substantially the same over a period of at least 50 days.

[0085] In some embodiments, when the neural electrode has an electrode size of about 100 μm2, the impedance is less than about 0.5 MQ.

[0086] In some embodiments, the neural electrode is characterised by a charge injection capacity of about 1.5 mC / cm2to about 10 mC / cm2. In other embodiments, the charge injection capacity is about 2 mC / cm2to about 10 mC / cm2, about 3 mC / cm2to about 10 mC / cm2, about 4 mC / cm2to about 10 mC / cm2, about 5 mC / cm2to about 10 mC / cm2, or about 6 mC / cm2to about 10 mC / cm2.

[0087] In some embodiments, the neural electrode is characterised by a specific impedance around 20 MQ μm2over 3000 min.

[0088] In some embodiments, the neural electrode is characterised by a phase angle at 1 kHz of about -20°.

[0089] In some embodiments, the neural electrode is characterised by a depolarization, repolarization and / or refractory period with amplitude of about 100 μV to about 800 μV. In other embodiments, the depolarization, repolarization and / or refractory amplitude is about 100 μV to about 750 μV, about 100 μV to about 700 μV, about 100 μV to about 650 μV, about 100 μV to about 600 μV, about 100 μV to about 550 μV, about 100 μV to about 500 μV, about 100 μV to about 450 μV, about 100 μV to about 400 μV, about 100 μV to about 350 μV, or about 100 μV to about 200 μV. In some embodiments, the neural electrode is characterised by a signal to noise ratio (SNR) of about 20 dB to about 40 dB. In other embodiments, the signal to noise ratio (SNR) is about 20 dB to about 38 dB, about 20 dB to about 36 dB, about 20 dB to about 34 dB, about 20 dB to about 32 dB, about 20 dB to about 30 dB, about 20 dB to about 28 dB, or about 20 dB to about 26 dB.

[0090] In some embodiments, the neural electrode comprises an array of probes, wherein the array of probes is characterised by a probe density of about 500 probe / mm2to about 4000 probe / mm2.

[0091] The present disclosure also relates to a neural device, comprising : a) a neural electrode as disclosed herein; and b) a microdrive electrically connected to the neural electrode.

[0092] In some embodiments, the neural device further comprises a control system. The control system may be a computer implemented system. This may involve a computer programme which regulates the generation of electric signals to the neuron, and / or receive a feedback signal from the neuron.

[0093] The control system may be configured with data processing means, such as data processing algorithm. The data processing algorithm may involve clustering a signal obtained from the neural electrode into at least 3 clusters, at least 4 clusters, or at least 7 clusters. Principle component analysis may be used.

[0094] With improved neuron identification resolution, brain region in the single-cell level among closely-packed neurons may be targeted. As such, the electrode and / or device may be used as a tool or therapy media to explore the function of our brain or do precision medicine. This may unlock more secrets of our brain and improve the quality of electronic medicine. Further the lowest impedance achieved enable the high SNR recording at the neuronal size without any additional modification. To improve the neuron identification resolution, the recording site should be small enough to be close to the neuron size, but the impedance of probe will be inversely spiked, which will fail the recording as there is big noise caused by the large impedance. Traditional metal wire all need to be surface-modified (PEDOT or metal nanoparticle) before using as singunit recording probe. But it has trade-off for the modification because the weak interface adhesion between the original probe and the modification layer will cause the detachment and the modification layer itself is not stable in the in vivo environment. Additionally, the raw material may be obtained cheaply, is biocompatible and is environmental friendly to fabricate while maintain high performance. In contrast, current commercial probes cost thousands of dollars.

[0095] The present disclosure also relates to a method of fabricating a neural electrode, the neural electrode comprising at least one probe, the probe having a reduced graphene oxide (rGO) fiber core and a sheath encapsulating the rGO fiber core, the method comprising : a) loading a solution of graphene oxide (GO) sheets and a reducing agent into a tubing in order to form a rGO gel; b) evaporating the rGO gel in order to form a rGO fiber; c) coating the rGO fiber with an insulator in order to form a rGO fiber core encapsulated with a sheath; and d) breaking the rGO fiber core and sheath in order to substantially exposed an end of the rGO fiber core from the sheath; wherein the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; wherein an end of the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; and wherein the end of the rGO fiber core comprises a nano-textured morphology in order to increase its surface area thereof.

[0096] The rGO gel is formed in the tubing. After the rGO gel is formed, it is removed from the tubing and the aqueous medium evaporated in order to allow for restricted selfassembly of the rGO sheets to form a straight thin rGO fiber. In this regard, the rGO gel may be tethered or fixed to a substrate at only its ends thereof with its body remain unsupported. This removes external forces which may influence the self-assembly of the rGO sheets.

[0097] In some embodiments, the reducing agent is a non-toxic reducing agent. In some embodiments, the reducing agent is ascorbic acid. In some embodiments, the graphene oxide is reacted with the reducing agent at about 95 °C for at least 1 h.

[0098] In some embodiments, the rGO gel is cylindrical.

[0099] In some embodiments, the tubing is a glass capillary tubing with an inner diameter of about 200 μm. This will provide a rGO fiber with a core of about 10-15 μm in diameter.

[0100] In some embodiments, the rGO gel is washed in a water bath. The rGO gel may be washed through a repeat exchange of an aqueous medium. The rGO gel may be washed for at least 2 to 3 times.

[0101] In some embodiments, the method further comprises a step after step c) of elastocapillary assembling the at least one probe in order to form the neural electrode. In elastocapillary assembly, the fibers are immersed in an adhesive solution (SU-8 solution) and upon withdrawing the fibers from the adhesive solution, the fibers are bonded together as a bundle due to the elastocapillary force. The small form factor of microfiber enabled the elastocapillary self-assembly by providing a balanced adhesion energy arising from van der Waals force and probe stiffness. Such assembly cannot be extended to larger metal probes as their stiffness will exceed the capillary adhesion force, preventing the formation of bundles.

[0102] In some embodiments, the method further comprises a step after step b) of electrically connecting the rGO fiber to a wire or metal trace.

[0103] In some embodiments, the breaking step comprises: a) at least partially embedding the rGO fiber core and sheath in a polymer; b) cryo-freezing the at least partially embedded rGO fiber core and sheath; c) breaking the partially embedded rGO fiber core and sheath at an interface of the embedment; and d) dissolving the polymer of step a) in a solvent.

[0104] In some embodiments, the polymer is a water soluble polymer. In some embodiments, the polymer is OCT™. OCT may be dissolved in an aqueous medium or an organic solvent. In some embodiments, the polymer is polyvinyl alcohol and / or polyethylene glycol.

[0105] In some embodiments, step c) comprises fracturing the rGO fiber core to form an end. A rapid force may be applied. Due to the bending stiffness mismatch at the coating boundary, stress is created which results in a natural fracture. This exposes the graphene edge nanotexture with well-preserved nanoedge-nanotunnel architecture.

[0106] In some embodiments, when the neural electrode comprises an array of probes, the method further comprises a step of adhering the probes together with a hard polymer or soft polymer. The hard polymer may be epoxy.

[0107] In some embodiments, the plurality of probes is bonded using SU-8.

[0108] The present disclosure also concerns a method of fabricating a neural device, comprising electrically connecting a neural electrode as disclosed herein to a microdrive.

[0109] In some embodiments, the method further comprises electrically connecting the neural device to a control system. The control system may be configured with data processing means, such as data processing algorithm. The data processing algorithm may involve clustering a signal obtained from the neural electrode into at least 3 clusters, at least 4 clusters, or at least 7 clusters. Principle component analysis may be used.

[0110] The neural electrode and device may be used to track neuron activity chronically with almost maximum SNR for spontaneous electrophysiological signal, and high resolution to record and identify the evoked signal, as month long stable recording with high quality may be obtained.

[0111] The present disclosure also provides a method of isolating a neuron using the neural device as disclosed herein. The method may be an in vivo method, or an in vitro method.

[0112] Accordingly, the method of isolating a neuron may be in a subject in need thereof. The neuron may be located in the auditory cortex. In particular, the neuron may be located at cortical laminae in the auditory cortex. In some embodiments, the method further isolates neighbouring neurons.

[0113] The present disclosure also provides a method of diagnosing a neural condition or disease in a subject in need thereof using the neural device as disclosed herein.

[0114] The method may comprise a step of connecting the neural device to a brain of the subject. The neural device may be connected to the brain of the subject via an end of the probe, which has the rGO fiber exposed. The probe may be implanted into the cortex, hippocampus, and / or thalamus. The cortex may be an auditory and / or visual cortex. The neural device may be connected to a cortical laminae in the auditory cortex. The method may comprise a step of collecting neural signals obtained from the subject. For example, the neural signals may be obtained by stimulating the subject visually or by sound. The signals may then be analysed using principal component analysis. In this regard, the signals may be categorised into single unit events based on the unequal response to different stimuli.

[0115] In some embodiments, the neural device is connected to the subject for about 5 days to about 6 months. In other embodiments, the duration is for at least 1 month.

[0116] Example

[0117] High-density single-unit recording among closely-spaced neurons over long durations is crucial for understanding the cellular-level functional architecture of the brain. Existing brain probes, however, laterally sample neurons in the same cortical layer far more sparsely than neuronal density, preventing precise interrogation of neuron-to-neuron functional connectivity, and suffer from long-term instability due to electrode surface modification. Here we report a monolithic graphene-edge probe that achieves monthlong single-unit recording at 2000 electrodes / mm2, approaching cortical neuronal density. The probe directly interfaces with neurons through exposed nanoedges and electrolyte-filling nanotunnels constructed by self-aligned reduced graphene oxide nanoflakes. The monolithic electrode structure ensures a low specific impedance of 20 MΩ μm2without any surface modification. The improved density and impedance enable stable electrophysiological recording with high signal-to-noise ratio (> 20 dB) as well as discrimination of individual neuron spikes over 6 months. We demonstrate the capability of the probe to interrogate a single auditory cortical layer at neuronal density, revealing previously unobserved heterogeneities in the acoustic frequency response and dynamic connectivity among individual neighboring neurons. The probe provides a tool for the precise interrogation of local microcircuitry at the neural density of the brain.

[0118] Recording extracellular action potentials at high spatiotemporal resolution is crucial for understanding brain functions and investigating the pathophysiology of neurological diseases, as well as advancing precision brain-computer interfaces. In particular, most neuronal interactions and computations occur within spatially localized regions containing closely spaced neuron populations. Owing to the variable function, morphology, and plasticity of individual neurons, electrophysiological activity within even submillimeter-scale brain regions can be cooperative yet highly heterogeneous. Thus, precise interrogation of complex local micro-circuits among such tightly packed neurons requires methods to chronically record neural activity at the spatial resolution matching neuronal density, and temporal resolution matching the submillisecond dynamics of action potential. However, this remains a substantial challenge with existing neural recording technologies. Optical readout techniques such as calcium imaging are limited by poor temporal resolution or low signal-to-noise ratio (SNR). Recent advances in silicon probe and flexible electronics technology, such as the Neuropixels probe, have enabled millisecond-resolution recording of large neuron populations, but the spatial resolutions in the lateral direction remain low (<2 electrodes per 100 μm). This limitation arises from the inherent 2D planar nature of semiconductor manufacturing techniques, which restrict their ability to accurately identify single unit within cortical layer and interrogate the intralaminar connectivity of brain circuits. To date, the highest lateral density with high channel count is achieved by microelectrode arrays, such as the Utah array, possessing an 100 μm interelectrode spacing, which is still much larger than the average neuron-to-neuron distance (<25 μm).

[0119] A key challenge in increasing recording density is the attenuated signal-to-noise ratio (SNR) caused by the increased electrochemical impedance of electrodes as they approach cellular-scale dimensions. Surface modification techniques are currently the only approach to address this issue and have been employed to decrease electrode impedance in both rigid silicon and flexible probes. However, surface modification methods inherently limit long-term recording due to material instability in physiological conditions. For example, conductive polymers coatings, such as poly(3,4- ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS) based modification, while reduce electrode impedance, are prone to delamination and degradation, and therefore remain concerns for chronic implantation. Additionally, nanoparticle-coated platinum / iridium-based tetrodes, which are widely used for neural recording and triangulation of spike sorting, have limited effective lifetimes because of corrosion of the nanoparticle-based modification layer and associated cytotoxicity to surrounding tissue. These factors limit the long-term use of microelectronic probes in brain-machine interfaces and neuroscience studies, where high-quality and precise chronic interrogation of electrophysiological activities is essential.

[0120] Here, we report a monolithic graphene nanoedge probe (NeuroEdge) that achieves a channel density of >2000 electrodes / mm2at <25 μm interelectrode spacing, approaching cortical neuronal density, and long-term recording stability in the brain. The probe integrates more than 16 channels within a diameter of 100 μm, comparable to human hair, using a self-assembly fabrication strategy. We achieved an ultralow impedance even at neuronal dimensions (20 MΩ μm2) without the need for any surface modification by exposing highly electrochemically-active, nanotextured graphene edges and nanoporous tunnels at the probe tip. We demonstrate neural recording with SNR exceeding 20 dB, and discrimination of high-density single units within a cortical layer via multiple-channel based spike-sorting over 6 months of recording. We further use the probe in auditory experiments to resolve heterogeneities in the acoustic frequency response of neighboring neurons and reveal frequency-dependent changes in functional connectivity within a single auditory cortical layer in mice.

[0121] Design, fabrication and characterization of NeuroEdge

[0122] The probe array was designed to be neuronal size in each channel with equivalent circular diameter of 12-15 μm and inter-channel spacing below cortical neuron-to- neuron distance (Fig. 2a-c, Fig. 3). This configuration allows each channel to access an overlapping volume of neurons, enabling the triangulation sorting of single neuron across multiple channels, which allows a high-quality single-unit discriminability compared to single-channel based spike-sorting. Besides, the array was designed to be less than 100 μm in cross-section for each bundle to minimize tissue displacement and implant-induced inflammatory response. Specifically, NeuroEdge array has a high density of more than 2000 electrodes / mm2in the intralaminar cortical plane, which is 4-fold denser than the tetrodes, 8 times higher than Neuropixels and 16 times higher than the Utah arrays across the lateral region of 100 μm x 100 μm (Fig. 2b and f).

[0123] To meet the configuration design requirements, we developed a solution-processible self-assembly approach and a stress-concentrated breaking technique to fabricate NeuroEdge. Specifically, in-situ 3D self-assembly of reduced graphene oxide with nontoxic reductant, vitamin C, to produce a single microelectrode gel, which then underwent restricted shrinking driven by water-evaporation to form a straight thin microelectrode fiber. Subsequently, parylene C coated microelectrode fibers were integrated into a bundle via facile elastocapillary self-assembly (Fig. 3, 4, 5). These self-assembly processes allow for high precision, versatility and biocompatibility by excluding numerous techniques and toxic chemical or any organic solvent. To expose the graphene nanoedge in the cross-section of the fiber, with the aim of reducing electrochemical impedance, a stress-concentrated breaking technique was developed. We constructed the stress-concentrated point by coating a water-soluble polymer, polyvinyl alcohol, on part of the rGO bundle followed by solidification in liquid nitrogen. When a rapid force is applied on the uncoated part, the bending stiffness mismatch at the coating boundary leads to a natural fracture that expose the graphene edge nanotexture with well- preserved nanoedge-nanotunnel architecture (Fig. 1, 2d-e). In contrast, conventional exposing methods, such as scissors cutting, freezing-assisted cracking, and high-energy cutting (laser or burning) cause deformation or damage of rGO nanosheets resulting in a substantially reduced electrochemical performance or inaccurately expanded geometric size. The self-assemblies and stress-concentrated breaking technique provided a facile and effective approach for fabrication of ultrahigh density neural probes with arbitrary and large channel count.

[0124] The NeuroEdge has a significantly lower electrochemical impedance compared with bare metallic electrodes and modified electrodes (Fig. 2g). The well-organized unique nanoedge-nanotunnel architecture shown in SEM images (Fig. 2e) led to active and large relative electrochemical surface area. The electrolyte-filled nanotunnel serves as an additional ionic conduction pathway in parallel with the electronic conduction pathway formed via stitched graphene nanoflakes. The ionic and electronic interactions between these two pathways are likely to further reduce the impedance of the monolithic electrode, which can be interpreted with a modified transmission line model. As a result, the NeuroEdge electrode, despite having a small size comparable to an individual neuron, can achieve a low impedance of < 0.2 MΩ at 1 kHz, which is 20-fold lower than platinum / iridium (Pt / Ir) electrodes, 5 times lower than PEDOT:PSS modified electrodes and beyond other modified electrodes with CNT, porous TiN and IrO? etc. (Fig. 2g, 6a-c). Thus, NeuroEdge has 4.5-fold lower thermal noise compared with the Pt / Ir electrode and 2.5-fold lower compared with the Pt / Ir / PEDOT:PSS electrode.

[0125] NeuroEdge offers high electrochemical stability by eliminating surface modifications such as PEDOT:PSS coating, porous TiN deposition or platinum nanoparticle plating, which are prone to delamination or degradation under chronic electrochemical and physiological stress. As shown in Fig. 6d, NeuroEdge maintains a specific impedance around 20 MΩ μm2over 3000 min of current pulses at a charge density of 1 mC cm2, which is among the typical activation thresholds for cortical microstimulation. In contrast, PEDOT:PSS coated Pt / Ir electrode exhibits a transient increase of 2.3 times in impedance within 5 min under the same current pulsing condition. This is due to the delamination of the PEDOT:PSS layer shown in the inset SEM images, where no PEDOT:PSS was left after the delivery of electrical pulses. To further assess the stability for chronic implantation purpose, we soaked the electrodes in phosphate-buffered saline (PBS) and compared the electrochemical performance over a 2-month period. Fig. 6e shows that the PEDOT:PSS coated Pt / Ir electrode exhibited over 50% impedance change and partial delamination, whereas NeuroEdge showed a consistent impedance over 50 days of soaking without obvious change.

[0126] Cyclic voltammetry measurement results further confirm that the NeuroEdge has higher electrochemical stability compared to existing microelectrodes. As seen in Fig. 6f and g, NeuroEdge has a wider water electrolysis window versus Ag |AgCI (-1.6 to 1.3 V) compared to that of Pt / Ir (-0.6 to 0.8 V). the Pt / It / PEDOT:PSS modified electrode exhibited a sharp 24-fold decrease of minimum current at the left end of the CV curve at 6-week soaking (Fig. 6f), while NeuroEdge only changed by 10% over 6 months (Fig. 6g). This is attributed to the PEDOT:PSS delamination and Pt / Ir corrosion. In comparison, NeuroEdge shows stable CV and EIS curves over 6 months (Fig. 6g and h). The capacitive behaviour of NeuroEdge, evidenced by the lack of redox peak in the CV curve, ensures minimal toxic side product from redox reaction at the electrode interface in a physiological environment. It is in agreement with reported results that carbon usually has much greater resistance to electrochemical corrosion than metals used in neural probes.

[0127] On top of the superior electrochemical performance, the unique nanostructure of NeuroEdge also leads to a high mechanical robustness for practical handling and surgical usage. A single bare NeuroEdge fiber, which is only 1.5% of human hair in axial area, can mechanically support a load 1000 times its own weight. The tensile measurement shows a modulus of 19.5 ± 3.4 GPa, and a bending stiffness of (4.0 ± 0.4) x 10'2nN m2for NeuroEdge, which is 10-fold softer than the metallic electrode while still providing adequate mechanical strength for surgical procedures.

[0128] High-density and high-fidelity recording in vivo with NeuroEdge

[0129] We assessed the high-density and high-fidelity recording capability of NeuroEdge by implanting a 4-channel and a 16-channel (< 100 μm in axial diameter) bundle into a mouse cortex, respectively (Fig. 7a, 8). The recordings were acquired at 4-day postimplantation. Each channel of NeuroEdge was registered with strong electrophysiological signals. Fig. 7b shows a typical 10-min raw electrophysiological data from a 4-channel NeuroEdge, including both high-fidelity local field potential (LFP) and action potential (AP). The spiking signal after band-pass filtering at 300-9000 Hz is consistently stable (Fig. 7b). The average AP amplitude is 150 μV. We observed as high as 600 μV AP with a sharp depolarization, repolarization and relative refractory period (Fig. 7c). The power spectrum density of the recording data was found to be smooth as a function of frequency (Fig. 7d) and the spectrogram displayed continuous horizontal strips for various frequency bands (Fig. 7e), providing an indication of stable recording without discernible noise. Over the entire recording period, SNR maintained stable with an average value around 20 dB and maximum value of 30 dB (Fig. 7f and g). Together, the above analyses suggested that the NeuroEdge is capable of recording high-quality spontaneous action potential.

[0130] The combination of superior electrode density and high SNR enable NeuroEdge to simultaneously oversamples the same neurons with higher fidelity, particularly lower- amplitude distant neurons, and more channels compared with existing neural probe, such as tetrode and Neuropixel. As a result, NeuroEdge has higher discriminability of neighbouring neuron population for investigating microcircuit functional organization. The independently extracted individual spikes from each channel are shown in Fig. 7h and i, which are represented in raster plots. It shows simultaneous recording of individual neurons on all four channels, evidenced by similar cross-channel firing patterns, laying the foundation for highly accurate triangulation. The spike clustering projections based on the 4-channel recording are illustrated in Fig. 7j, showing 2.25 ± 0.75 single units per channel on average. Principal components analysis (PCA) reveals 7 clearly separated clusters in three projections after removing sparsely firing units, multi-units, and noise units. The clusters that overlap in the PC1 / PC2 projection become completely distinguishable when observed in eitherthe PC1 / PC3 or PC2 / PC3 projections. The average waveforms of each unit on all four channels exhibit similar spike shapes yet varying amplitudes, suggesting that the spikes were from the same neuron type but at different distances from each channel (Fig. 7k). The interspike intervals (ISI) histogram of all 7 units feature a refractory period of more than 2 ms that render them consistent with single-unit activities.

[0131] To interrogate a larger intralaminar neuronal population, a 16-channel NeuroEdge was used for hours-long electrophysiological recording. Representative LFP (Fig. 71) shows similar wave patterns across all channels and the AP exhibits close spike timing, indicating localized high-density electrophysiological recording. As a result, the <100- μm array identified more than 40 well-isolated single units across multiple channels. Each unit has no overlap in spike timings (Fig. 7m) and shows distinct average waveforms (Fig. 7n), suggesting an absence of duplicated units. The 16-channel NeuroEdge allows for a laminar recording at density of more than 4000 units per electrode mm2, approaching the neuronal density.

[0132] Investigating heterogeneity of frequency preference among neighboring neurons in auditory cortex

[0133] Frequency is the main acoustic parameter that is thought to be topographically mapped in most auditory cortex. Studies identified fine-scale frequency architectonic inhomogeneity across cortical laminae in the auditory cortex. However, the existence of local heterogeneity in frequency preference across neighboring neurons within a cortical layer remains inconclusive or incomplete. This is largely because there is a lack of tools or methods that combine both high temporal resolution and high lateral spatial resolution (matching cellular density). To address this challenge, we implanted NeuroEdge (with sub-25 μm spatial resolution) into mouse auditory cortex to record closely spaced neurons in response to tone frequencies spanning 0.5-42 kHz in Vi octaves (Fig. 9a and 10). The recorded local field potential (LFP) shows an increased negative deflection near tone onset, which is sustained for the entire 100-ms stimulus window (Fig. 9b). The filtered spiking signal reveals that the neurons have unequal responsivity to different sound frequencies, with distinct variation in firing rate from the highest of 16 Hz to almost zero (Fig. 9c).

[0134] Fig. 9d illustrates the characteristic frequency response in peristimulus raster plot from 12 representative sorted single units. It shows an average 2.7-fold increase in spike density, computed as the ratio of peak over baseline, during the stimulus window. However, all units exhibit different spike density increases ranging from 1 to 5 (Fig. 9d- f). For instance, unit 7 (N7) shows a 4.4-fold spike density increase, while unit 1 (Nl) exhibits almost no change. The diversity in spike density changes of near-by neurons within the stimulus window indicates that the near-by neurons are not equally activated by the external acoustic stimulus.

[0135] By observing neural responses to acoustic stimuli at varying frequencies, we found that all the units share common best frequency peaks around 2.6 kHz and 9.5 kHz, indicating they are from a vicinity region (Fig. 9e). However, each unit has its own frequency preference. For instance, units 7 and 12 (N7, N12) show strong response to low frequencies (<4 kHz), while units 6, 10 and 11 (N6, N10, Nil) show elevated response to higher frequencies (>4 kHz), and unit 9 (N9) presents response both below and above 4 kHz (Fig. 9g). Such frequency preference suggests heterogeneous responsivity among near-by neurons, agreeing with previously reported results using optical methods. We quantify the responsivity difference under different frequency range by calculating the SD ratio of neurons under acoustic stimuli at lower frequency fl centering 2.6 kHz and higher frequency f2 centering 9.5 kHz (Fig. 9f). We found distinct preference of the units to fl and f2. Particularly, N7 showed preference to fl (lower frequency) with an SD ratio of 13.2 at fl, that is three times that at f2 of 4.2. In contrast, N10 showed opposite preference at f2 (higher frequency) with an SD ratio of 8.7 compared to 3.2 at fl.

[0136] We further investigate whether and how functional connectivity of near-by neurons in single cortical layer is modulated by varying acoustic frequencies. From the examination of cross-correlograms between N6 and N9 (Fig. 9g), a discernible peak at -3 ms under full frequency (0.5-42 kHz) stimuli, suggests increased excitatory functional connectivity due to the acoustic stimulation. This augmented excitatory connectivity persists at both fl and f2 frequency bands. However, N1 and N5 pairwise reveal frequency-specific connectivity, specifically an excitatory functional connection at fl frequency band and an absent connection at f2 frequency band. Examining the interaction strength (coefficient ratio) reveals an increase in both the number and strength of functional connections with acoustic stimulation (Fig. 9h). Notably, substantial variability in connectivity responses is observed in relation to lower and higher frequencies (Fig. 9h).

[0137] These results demonstrate the capability of NeuroEdge probes to discriminate substantial heterogeneity of neuronal tuning at cellular level within a localized cortical region which has been previously understudied, and reveal the dynamic functional connectivity with frequency specificity among neighboring neurons within a functional microcircuit in the auditory cortex. NeuroEdge provides a versatile tool for investigating the neural basis of behavior, extending beyond organization across the depth of the cortex to within the intralaminar cortical layer.

[0138] Chronic in vivo biocompatibility and functionality assessment

[0139] We investigated the chronic functionality of NeuroEdge by evaluating the stability of recorded electrophysiological signals, the acoustic frequency response of single units, and the biocompatibility of the implanted probe in the mouse brain (Fig. 11a). Representative electrophysiological recordings at month 1 (Ml), month 3 (M3), and month 6 (M6) all exhibit prominent and high-amplitude action potential. (Fig. 11b). The SNR was consistently above 20 dB with a noise level below 7 μV across the entire experimental duration of 6 months (Fig. 11c). The average spike amplitude remained stable. NeuroEdge with size comparable to neuron also maintained a low impedance in vivo of around 0.5 MΩ over 6 months (Fig. lid). The sustained high SNR and low impedance of NeuroEdge enable neural activities monitoring with high-fidelity over an extended period without deterioration in yield and quality.

[0140] We further investigated the chronic functionality of NeuroEdge in respond to acoustic frequency. The frequency preference of neurons has negligible change over 3 months, and the spike density increase remains unchanged (~ 2.6-fold increase in both Ml and M3) (Fig. lie and f). In addition, after 6-month post-implantation, NeuroEdge retains its full ability to resolve responding frequency heterogeneities in the auditory cortex (Fig. 11g). Altogether, the results demonstrated the stable functionality of NeuroEdge for recording neural activity and successfully discriminating diverse response differences to auditory stimuli over 6 months.

[0141] To access long-term biocompatibility, we compared the neuroinflammatory responses to pristine and modified neural interfaces in mouse cortex, specifically using bare NeuroEdge and PEDOT: PSS / Au-modified probe of similar size. Immunohistochemical studies were performed on horizontal brain slices near the implantation sites to assess the presence of neuronal nuclei, microglia cells and astrocyte cells via immunostaining with neuronal nuclei (NeuN), ionized calcium-binding adaptor molecule 1 (Ibal, positive marker for microglia cell) and glial fibrillary acidic protein (GFAP, positive marker for astrocyte cell) (Fig. llh). We observed no significant morphology change of NeuN and Ibal stained cells in the area surrounding implanted NeuroEdge sites at 3-month postimplantation, and the intensity values are in the same range as the non-implanted contralateral cortex section (Fig. Hi). The good biocompatibility of NeuroEdge can be ascribe to the chemical inertness and small tissue lateral displacement (<100 μm). However, we observed a 20 % increase in Ibal intensity and 40% in GFAP intensity in the area surrounding the PEDOT:PSS / Au coated probe compared to the pristine NeuroEdge, suggesting glial scar encapsulation of microglia cells and astrocyte cells that were triggered by the implant. We further found a significant increase by near the implantation site of PEDOT:PSS / Au modified probe, indicating serious activation of. This could be due to PEDOT:PSS degradation / disintegration in physiological solution and poor interface adhesion between metal and PEDOT:PSS, leading to delamination or diffusion of disintegrated dopants and unreacted monomers. Overall, the chronic immunostaining study indicates that the NeuroEdge is suitable for long-term implantation without substantial neuroinflammatory response.

[0142] Conclusion

[0143] We have demonstrated high resolution and highly stable brain probes, NeuroEdge, that can measure the longitudinal neuronal activity of closely spaced neurons. NeuroEdge can overcome two key limitations of state-of-the-art silicon probes such as NeuroPixels. First, unlike existing proves that rely on planar processing steps and have limited spatial resolution due to their large lateral spacing between the electrodes, NeuroEdge can directly interface with neurons through exposed nanoedges and electrolyte-filling nanotunnels constructed by self-aligned reduced graphene oxide nanoflakes, enabling a channel density of >2000 electrodes / mm2that approaches cortical neuronal density. Second, unlike existing probes that have limited stability - NeuroEdges exploits graphene edges to achieve a low specific impedance of 20 MΩ μm2without relying on unstable surface modification, thereby achieving long-term stability over six months. With the increased resolution and stability, NeuroEdge enables electrophysiological recording with a high signal-to-noise ratio (>20 dB), with the ability to distinguish individual neuron spikes over six months. In addition, NeuroEdge resolves heterogeneities in the acoustic frequency response and reveals functional connectivity among neighboring neurons in the mouse auditory cortex, providing a fundamentally new brain probe that can precisely interrogate local microcircuitry at the neural density of the brain.

[0144] Beyond the auditory cortex, we envision that NeuroEdge, which has the capability of millisecond temporal resolution, cellular-scale spatial resolution, and monolithic-design- enabled chronic stability, will significantly contribute to the study of neural microcircuits and their functional architecture in many brain regions, especially those with dense neuron nuclei or fine-grained functional division, such as the hippocampus, visual cortex and thalamus. It can be broadly applied to investigate functional connectivity and plasticity in microcircuits and how they are affected by neurological disorders. The capabilities of NeuroEdge also position it as a highly promising solution for clinical bioelectronics applications. Particularly, it could facilitate the develoμment of braincomputer interfaces, where precise control of closely spaced neurons is required for the restoration of fine motor and sensory functions. Further improvements will be dedicated to exploring new configurations with more channels to cover larger brain areas. Additionally, we envision that the NeuroEdge can be used for detection of both action potentials and neurochemical concentrations by leveraging the inherently exceptional electrochemical activity of graphene edges.

[0145] Methods

[0146] Fabrication of graphene edge probes (NeuroEdge)

[0147] Aqueous dispersion of graphene oxide (GO) (Suzhou Tanfeng Graphene Technology CO., LTD, 10 mg ml1) was diluted to 6 mg mF1with water. Then, 85 mg of ascorbic acid (Sigma-Aldrich) was added to 1 ml of the GO dispersion and ultrasonicated for 5 min. The resulting GO / ascorbic acid mixture dispersion was loaded into glass capillary tubing, sealed with Teflon tape, and reacted at 95 °C for 1 h, resulting in a reduced graphene oxide (rGO) gel fiber in the capillary tubing. The gel fiber was extracted, and soaked in a water bath for 10 min, followed by changing the water and repeating for another 10 min. The gel fiber was then placed on a flat plastic polystyrene substrate to constrict the self-assembly alignment of rGO fiber during water-evaporation driven drying. The diameter of the rGO fiber was determined by the inner diameter of the glass capillary tubing, with a diameter of 10-15 μm synthesized from 200 μm of capillary tubing. To facilitate the drive assembly, a 50 μm stainless steel wire (793400, A-M system) was connected to the fiber using silver nanowire ink. The bare rGO fiber was coated with a 1-2 μm thick of parylene C to insulate the side wall of the fiber. The tip of the fiber was exposed via a strain-concentrated breaking. First, optimal cutting temperature (OCT, PVA solution) compound was coated on the surface of parylene C-coated rGO fiber, and frozen in liquid nitrogen. The OCT liquid solidified at the low temperature, encapsulating the entire rGO fiber, leaving a short fiber exposed at the tip end. Second, using spring scissors to press down on the free tip end, the fiber was broken down from the point right alongside the OCT embedding part. The fiber was taken out from liquid nitrogen and the melted liquid OCT was then washed away with water. After exposing the tip end of the rGO fiber, the sample was referred to as a graphene edge probe (NeuroEdge).

[0148] Fabrication of NeuroEdge array

[0149] The rGO fibers coated with parylene C were bundled with elastoca pi llary self-assembly by withdrawing the free-moving end of the fibers from the bath of diluted SU-8 solution (SU-8 2002, Kayaku Advanced Materials, Inc.). The assembly was baked in oven at 100 oC for 10 min to evaporate the solvent in SU-8 and then exposed to 365 nm UV lamp for 5 min to bond the rGO fibers permanently to a thin array. The tip end of the array was exposed using strain-concentrated breaking method as described in the previous section.

[0150] Assembly of implantation micro-drives

[0151] The stainless steel wire that is connected to NeuroEdge was tightened inside receptacle (ED85100-ND, Digi-key) by putting back the original pin. Two holes in receptacle were left to connect with the reference and ground wires for in vivo electrophysiological recording. The moving stage inside trimmer potentiometer was exposed to place the PI tubing part of the NeuroEdge array which was secured with adhesive (Loctite 404, Ted Pella). To create a strong bond of NeuroEdge on the moving stage, the adhesive was left overnight to allow full curing. The NeuroEdge tip end was adjusted to pass the bottom of the potentiometer by 1-2 mm to facilitate implantation into the brain. The receptacle was secured on the top of the trimmer potentiometer. Moreover, the stainless steel wires were left bend to facilitate the moving down of the NeuroEdge.

[0152] Characterize the exposed tip area of NeuroEdge

[0153] The size and morphology of the NeuroEdge tip end were analyzed with a Field-emission Scanning Electron Microscopy (FESEM) (FEI Verios460). The NeuroEdge array was attached to a 70° SEM stub with its tip slightly higher than the top side and grounded using silver ink on the bottom end of NeuroEdge to ensure electrical connection to double-sided carbon conductive tape adhered on the stub. The sample was not coated with additional Pt or Au to allow detection of the nanoscale graphene edges, the nanotextures and the nanotunnels. The sample holder stage was tilted to allow for the tip end to be viewed vertically or at a 45-degree angle relative to the FESEM detector.

[0154] Mechanical characterization

[0155] Tensile testing experiments were performed using an Instron instrument (Instron model 68SC-1). Stress-strain curves were obtained under ambient conditions with 10-mm- long samples at a constant strain rate of lmm / min. Values of Young's modulus were determined based on data from at least five samples. Bending stiffness (D) of the probe is defined as

[0156] D = El where E and I represent the elastic modulus and moment of inertia, respectively.

[0157] For a cross-sectional area A, the moment of inertia is calculated as

[0158] Characterization of NeuroEdge in PBS solution

[0159] The electrochemical performance of NeuroEdge was characterized in a phosphate buffer solution (PBS, 150 mM) using an Ag / AgCI electrode as a reference and a platinum mesh as a counter. Electrochemical impedance spectroscopy (EIS) was conducted over a frequency range of 100 to 100k Hz with a perturbation of 10 mV RMS sinusoidal excitation voltage (Biologic SP200). Cyclic voltammetry (CV) curves were acquired at a sweep rate of 100 mV / s between negative and positive potential limits of -1.6 and 1.3 V versus Ag / AgCI. The current pulse was delivered by applying a rectangular charge- balanced biphasic current pulse with the cathodic phase applied first which is a common practice for in vivo stimulation(Gamry reference 600+). The interpulse delay between cathodal and anodal phase was set to 50 us to visualize the interpulse potential. The pulse width was 1 ms, and the charge density was controlled to be 1 mC cm-2. The long-term stability study of NeuroEdge was performed by soaking it in 150 mM PBS for half a year.

[0160] PEDOT:PSS modified metal electrodes as control group

[0161] A metal electrode was electroplated with poly(3,4-ethylenedioxythiophene): poly(styrene sulfonate) (PEDOT:PSS) from a 0.1 M PSSNa (Sigma-Aldrich) aqueous solution with 0.01 M EDOT (Sigma-Aldrich) under galvanostatic conditions using an Ag / AgCI electrode as a reference and a platinum wire as a counter. The current density was controlled to be around 0.4 mA / cm2 to allow slow electrodeposition for enhanced adhesion and total electrodeposition charge density was around 600 mC / cm2 to minimize the risk of PEDOT:PSS layer cracking. After electrodeposition, the electrode was immersed in DI water for 15 min to wash away any weakly attached PEDOT:PSS on the surface. The electrochemical performance was characterized using EIS, CV and CIC measurements, with potential limits of -0.6 to 0.8 V versus Ag |AgCI, following the same process as the NeuroEdge characterization.

[0162] Ethical approval and animal handling

[0163] All animal procedures are approved by the Institutional Animal Care and Use Committee (IACUC) at National University of Singapore and were conducted in accordance with NACLAR guidelines. Male C57BL / 6 wild-type mice aged 8-12 weeks were purchased from Jackson Laboratory, and housed in a room maintained for a 12-hour light / dark cycle with ad libitum access to food and water. Before surgery, the mice were group- housed with 4 mice per cage while after surgery, the mice were individually housed with toys and brown paper provided in their cages. The mice were allowed to acclimate for at least 3 days before being used in the experiments.

[0164] Chronic implantation of NeuroEdge array to parietal lobe cortex

[0165] Mice were anesthetized via intraperitoneal injection of ketamine / xylazine mixture in saline (100 and 10 mg per kg mouse, respectively), and subcutaneous injection of analgesic buprenorphine (0.1 mg per kg mouse). The depth of anesthesia was monitored with the toe pinch reflex. The top of the head of the mice were shaved, and then placed in a stereotaxic frame (David Kopf Instruments), with ear bars securing the head and gel applied on the eyes to keep them moist. The exposed skin on the top of the head was cleaned with alcohol and iodine, and cut along the midline to expose the skull. After cleaning the skull with saline, two small holes were drilled, one on the right forehead and one on left part of back head for metal supporting screws (3SSCS94F008,1 / 4-28, Fastenere) using 0.9 mm diameter burr (19007-09, Fine Science Tools) with microdrill (78001, World Precision Instruments), respectively. Before mounting the forehead screw, a stainless-steel wire was soldered to the screw head for grounding and reference that would be connected to the electrode drive later. A craniotomy was performed on the right skull for electrode implantation using 1.8 mm diameter trephine (18004-18, Fine Science Tools). The prepared drive with NeuroEdge was secured on an insertion tool that was mounted on the stereotaxic frame holder. The drive was then lowered down to the brain with the NeuroEdge tip facing towards the coordinates relative to bregma of -1.9 mm AP, 1.4 mm ML, 0.5-1.0 mm DV. The dura was partially removed surrounding the NeuroEdge penetration point, and sterile saline was applied to keep the craniotomy moist. The drive was fixed onto the skull using cement (C&.B Metabond, Parkell Inc.) with Kwik-Sil (Word Precision Instruments Inc.) applied to the craniotomy area. After the cement and Kwik-Sil had complete cured, the insertion tool was removed, and a plastic tubing was placed outside the drive to protect it. The drive and plastic tubing were then secured together on the skull with dental cement (Rapid repair Meliodent), and the gap between them on the top was sealed as well to keep the craniotomy isolated from the ambient environment. The mice with implantation were returned to their cage after waking up from anesthesia. The mice were closely monitored for 3 days after surgery, and the NeuroEdge was moved down around 100 μm on the third day.

[0166] In vivo electrophysiological recording

[0167] An Intan recording system, which includes an RHD USB interface board and RHD headstage with an RHD2132 chip (Intan Technologies), was connected to the receptacle connector of the drive using an in-house adaptor. The mice were maintained at an anaesthetized state using 1-2 % isoflurane (Baxter Healthcare Corporation). This helped to minimize the trial-to-trial variation arising from the effects of attention, arousal, and body movements to facilitate the performance investigation of electrode itself. To minimize the noise from the environment, the mice were placed inside a Faraday cage, and the cage was grounded via the ground connector in the USB interface board. The RHX Data Acquisition Software was used to record the local field potential (LFP) and action potential (AP). The data acquisition was performed in the frequency width of 0.1- 9000 Hz with a sampling rate of 30 kHz, and the in vivo impedance was measured at 1 kHz before recording.

[0168] Auditory stimulation and recording

[0169] For auditory stimulation recording, the NeuroEdge was implanted into the left-side auditory cortex (AC) at coordinates relative to bregma of -2.2 mm AP, -4.0 mm ML, 0.6 mm DV, using the same recording and implantation setup as previously described. Pure tones were generated with a sound card (Sound Blaster Audigy Rx) and Matlab software, and amplified via an audio amplifier (Samson Servo 120a) before being presented to the mice's ear via loudspeaker (XT25TG30-04, Peerless by Tymphany) at a distance of 15 cm. The output of the speaker was measured with a free-field microphone (4939-A- 011, Briiel & Kjaer) placed at the same location as the mouse's head facing the speaker. The output was read in dB sound pressure level (SPL). The pure tones were arranged from 0.5 to 42 kHz in 1 / 12 octave steps. The duration was 100 ms including 6 ms cosine2 onset / offset ramp and inter-tone interval of 1300 ms. To align the acoustic stimuli timeline with the recording channels, the click channel from the same connection ports on the sound card with the same onset and offset timeline settings as the tone channel was directly connected to an analog-to-digital converter (ADC) port in the Intan USB interface board and the voltage of the acoustic click channel was recorded. Recording sessions lasted up to 2 h. To allow investigation of electrode performance only, the mice were kept under shallow anesthesia, responding with a light withdrawal reflex to tail or toe pinch but remaining quiet and motionless without indication of pain or distress. Deep anesthesia was maintained with a higher concentration of isoflurane, and the mice showed no response to tail or toe pinch.

[0170] Data analysis

[0171] All electrophysiological data were analyzed using Matlab (Mathworks) and sorted with Offline Sorter (OFS, Plexon) using the principal components of the waveforms. A 10-20 min dataset with continuous recording was used for analysis unless otherwise stated. In brief, the raw recording data was filtered using Butterworth bandpass filters (filtfilt function in Matlab) at 0.1-300 Hz for the local field potential (LFP) and 300-9000 Hz for action potential (AP) extraction. A custom Matlab script was used to create the power density spectrum in the frequency domain and the spectrogram in time domain based on the raw data to check the recording quality and noise. The amplitude of action potential was calculated using peak to peak detection. The signal-to-noise ratio (SNR) was expressed in decibels from 20 x In (RMS(S) / RMS(N)), where S is the waveform peak and N is the noise of the recording after removing the detected spikes. The SNR was evaluated based on the average spike amplitude over a 10-min recording. For sorting and clustering into OFS, the raw recording data was converted to a binary data format and imported to OFS. The data was then filtered with 2-pole Butterworth high- pass filter at a cutoff frequency of 500 Hz. Spikes at different channels were detected and extracted in a 1.13 ms time window with a prethreshold period of 0.26 ms and dead time of 1.03 ms. All the spike sorting results were triangulated on 4 neighboring channels. The 16-channel NeuroEdge was grouped in a 4x4 array, and timestamp comparison was applied to the original sorted single units to remove duplicated ones. Interspike intervals (ISI), auto-correlograms and cross-correlograms were exported from OFS and plotted using custom Matlab scripts. The recording data under acoustic stimuli was analyzed using custom Matlab scripts with the Gaussian spike density (SD) algorithm based on the average neural response in the form of the peristimulus time histogram (PSTH). The response strength to different auditory frequency was evaluated via the SD peak around stimulation window compared with the SD during rest time. Allocation of the spikes to the corresponding frequency of the acoustic stimulation was done by comparing the timestamp of spikes in each putative single neuron with the timeline of the trigger channel.

[0172] Immunohistochemistry

[0173] To minimize the impact of probe size on immunohistochemistry (IHC) results, mice were implanted with NeuroEdge and NeuroEdge with thin coating of 100 nm Au / 1-2 μm PEDOT:PSS for fair comparison. After 3 months of implantation, the mice were perfused with saline and 4% paraformaldehyde (PFA) (Sigma-Aldrich) in 0.1 M PB. The fixed brain was extracted and post-fixed in 4% PFA overnight at 4 oC, then immersed in 30% sucrose in 0.1 M PB until the brain sunk to the bottom. The brain was frozen with OCT and sectioned to 45 μm lateral slices at -20 oC using a Cryostat (Leica CM3050s). The individual serial sections were collected into 96-well plates filled with cryoprotection solution and stored at -20 oC until use. The slices were washed with tris-buffered saline (TBS) twice and incubated in blocking solution containing 0.2% Triton X-100 (Sigma- Aldrich) and 3% donkey serum (GeneTex GTX73205) in TBS for 1 h at room temperature. The slices were then incubated with primary antibodies, including mouse anti-NeuN (MAB377, 1 :100, Sigma), chicken anti-GFAP (ab4674, 1 : 1000, Abeam) and rabbit anti-Ibal (019-19471, 1: 1000, Wako) in blocking solution for 1 day at 4 oC. The slices were washed with TBS twice for 10 min each, and incubated with secondary antibodies at room temperature for 4 h, including donkey anti-mouse Alexa Fluro 647 (715-605-151, 1:250, Jackson ImmunoResearch), donkey anti-chicken Alexa Fluro 488 (703-545-155, 1 :250, Jackson ImmunoResearch) and donkey anti-goat cy3 (705-165- 147, 1 :250, Jackson ImmunoResearch). After washing with TBS twice, the slices were mounted on polylysine coated glass slide (Epredia Polysine) with Antifade Mounting Medium (Vector Laboratories, H-1200-10) and coverslips. Images were acquired using a confocal laser scanning microscope with a 20x air objective lens (Olympus FV3000). Quantification of expressed area was analyzed with ImageJ.

[0174] It will be appreciated that many further modifications and permutations of various aspects of the described embodiments are possible. Accordingly, the described aspects are intended to embrace all such alterations, modifications, and variations that fall within the spirit and scope of the appended claims.

[0175] Throughout this specification and the claims which follow, unless the context requires otherwise, the word "comprise", and variations such as "comprises" and "comprising", will be understood to imply the inclusion of a stated integer or step or group of integers or steps but not the exclusion of any other integer or step or group of integers or steps.

[0176] Throughout this specification and the claims which follow, unless the context requires otherwise, the phrase "consisting essentially of", and variations such as "consists essentially of" will be understood to indicate that the recited element(s) is / are essential i.e. necessary elements of the invention. The phrase allows for the presence of other non-recited elements which do not materially affect the characteristics of the invention but excludes additional unspecified elements which would affect the basic and novel characteristics of the method defined.

[0177] The reference in this specification to any prior publication (or information derived from it), or to any matter which is known, is not, and should not be taken as an acknowledgment or admission or any form of suggestion that that prior publication (or information derived from it) or known matter forms part of the common general knowledge in the field of endeavour to which this specification relates.

Claims

Claims1. A neural electrode comprising at least one probe, the probe having a reduced graphene oxide (rGO) fiber core and a sheath encapsulating the rGO fiber core; wherein the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; and wherein an end of the rGO fiber core is substantially exposed from the sheath and is characterised by a cross sectional diameter of about 5 μm to about 100 μm; and wherein the end of the rGO fiber core comprises a nano-textured morphology in order to increase its surface area thereof.

2. The neural electrode according to claim 1, wherein the rGO fiber core comprises intercalated and / or stacked rGO sheets, wherein the rGO sheets are aligned parallel to a longitudinal axis of the rGO fiber and wherein the rGO sheets are folded onto each other in a perpendicular direction relative to the longitudinal axis of the rGO fiber.

3. The neural electrode according to claim 1 or 2, wherein the rGO fiber core is characterised by a cross sectional diameter of about 10 μm to about 20 μm.

4. The neural electrode according to any one of claims 1 to 3, wherein the cross sectional diameter of the rGO fiber core is characterised by a relative standard deviation of less than 0.15.

5. The neural electrode according to any one of claims 2 to 4, wherein the probe comprises nanotunnels between the rGO sheets, wherein the nanotunnels are characterised by a width of about 0.5 nm to about 500 nm.

6. The neural electrode according to any one of claims 1 to 5, wherein the end of the rGO fiber core has a cross sectional diameter which is substantially similar to the core of the rGO fiber.

7. The neural electrode according to any one of claims 1 to 6, wherein the end of the rGO fiber core comprises rGO sheets folded onto each other in a perpendicular direction relative to the longitudinal axis of the rGO fiber.

8. The neural electrode according to any one of claims 1 to 7, wherein the end of the rGO fiber core is characterised by an exposed cross sectional area of about 50 μm2to about 1000 μm2.

9. The neural electrode according to any one of claims 1 to 8, wherein the nano- textured morphology comprises a tip, wherein the tip is characterised by a morphology selected from a cone, or a pyramid.

10. The neural electrode according to any one of claims 1 to 9, wherein the rGO fiber core is characterised by a Young's modulus of about 10 GPa to about 50 GPa.

11. The neural electrode according to any one of claims 1 to 10, wherein the rGO fiber core is characterised by a cross sectional area of about 50 μm2to about 3500 μm2.

12. The neural electrode according to any one of claims 1 to 11, wherein the sheath comprises an insulator.

13. The neural electrode according to claim 12, wherein the insulator is selected from parylene C, SU-8, polyimide, polyurethane, or a combination thereof.

14. The neural electrode according to any one of claims 1 to 13, wherein the sheath is characterised by a thickness of about 0.5 μm to about 10 μm.

15. The neural electrode according to any one of claims 1 to 14, wherein the probe is electrically connected to a wire or metal trace.

16. The neural electrode according to any one of claims 1 to 15, wherein when the neural electrode comprises an array of probes spaced apart from each other, wherein the probes are adhered together by a hard polymer or a soft polymer.

17. The neural electrode according to any one of claims 1 to 16, wherein the neural electrode comprises at least 4 probes.

18. The neural electrode according to any one of claims 1 to 17, wherein the neural electrode is characterised by a cross sectional diameter is about 80 μm to about 100 μm.

19. The neural electrode according to any one of claims 1 to 18, wherein the neural electrode is characterised by an areal density of about 500 electrodes / mm2to about 4000 electrodes / mm2.

20. The neural electrode according to any one of claims 1 to 19, wherein the neural electrode is characterised by an impedance of about 0.0005 MΩ to about 1 MΩ.

21. The neural electrode according to any one of claims 1 to 20, wherein the neural electrode is characterised by a charge injection capacity of about 1.5 mC / cm2to about 10 mC / cm2.

22. The neural electrode according to any one of claims 1 to 21, wherein when the neural electrode comprises an array of probes, wherein the array of probes is characterised by a probe density of about 500 probe / mm2to about 4000 probe / mm2.

23. A neural device, comprising : a) a neural electrode according to any one of claims 1 to 22; and b) a microdrive electrically connected to the neural electrode.

24. The neural device according to claim 23, wherein the neural device further comprises computing means having a data processing algorithm.

25. A method of fabricating a neural electrode, the neural electrode comprising at least one probe, the probe having a reduced graphene oxide (rGO) fiber core and a sheath encapsulating the rGO fiber core, the method comprising: a) loading a solution of graphene oxide (GO) sheets and a reducing agent into a tubing in order to form a rGO gel; b) evaporating the rGO gel in order to form a rGO fiber; c) coating the rGO fiber with an insulator in order to form a rGO fiber core encapsulated with a sheath; andd) breaking the rGO fiber core and sheath in order to substantially exposed an end of the rGO fiber core from the sheath; wherein the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; wherein an end of the rGO fiber core is characterised by a cross sectional diameter of about 5 μm to about 100 μm; and wherein the end of the rGO fiber core comprises a nano-textured morphology in order to increase its surface area thereof.

26. The method according to claim 25, wherein the reducing agent is ascorbic acid.

27. The method according to claim 25 or 26, wherein method further comprises a step after step a) of washing the rGO gel.

28. The method according to any one of claims 25 to 27, wherein method further comprises a step after step c) of elastocapillary assembling the at least one probe in order to form the neural electrode.

29. The method according to any one of claims 25 to 28, wherein the breaking step comprises: a) partially embedding the rGO fiber core and sheath in a polymer; b) cryo-freezing the partially embedded rGO fiber core and sheath; c) breaking the partially embedded rGO fiber core and sheath at an interface of the embedment; and d) dissolving the polymer of step a) in a solvent.

30. The method according to claim 29, wherein the polymer is selected from OCT™, polyvinyl alcohol, and / or polyethylene glycol.

31. A method of diagnosing a neuron using the neural device according to claim 23

Citation Information

Patent Citations

  • Methods of making and bioelectronic applications of metalized graphene fibers

    US20220305253A1