Papermaking waste pulp grafted tartaric acid intercalated mg / al-ldhs adsorbent, preparation method therefor, and use thereof
By grafting the fiber composite with tartaric acid intercalated Mg/Al-LDHs, a grafted papermaking waste pulp adsorbent is formed, which solves the problems of low cellulose reactivity and easy agglomeration, significantly improves the adsorption capacity, and reduces wastewater The concentration of metal ions achieves efficient treatment and sustainable development of papermaking waste pulp.
Patent Information
- Application Number
- PCT/CN2023/109460
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-07-27
- Publication Date
- 2024-10-24
AI Technical Summary
When existing adsorbent materials are used to treat papermaking waste pulp, cellulose has low reactivity and is easy to agglomerate, resulting in insufficient ability to adsorb metal ions. Moreover, the cost is high and the adsorption capacity is limited. It is difficult to effectively reduce the concentration of metal ions in wastewater, affecting water quality and the environment. .
The fiber composite was prepared from papermaking waste pulp sediment, and grafted with tartaric acid intercalated Mg/Al-LDHs and the cross-linking agent N,N-methylenebisacrylamide to form papermaking waste pulp grafted tartaric acid intercalated Mg/ Al-LDHs adsorbent improves its hydrophilicity and dispersion, and enhances its adsorption capacity for metal ions.
It significantly improves the adsorption capacity of the adsorbent, reduces the concentration of heavy metal ions in wastewater, solves the problem of papermaking waste pulp pollution, reduces the cost of the adsorbent, and achieves sustainable development.
Smart Images

Figure CN2023109460_24102024_PF_FP_ABST
Abstract
Description
A papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent and its preparation method and application
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on April 17, 2023, with application number CN202310407417.9 and invention name “A papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent and its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The invention belongs to the technical field of adsorption materials, and particularly relates to a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs (magnesium-aluminum-based layered double hydroxide) adsorbent, and a preparation method and application thereof. Background Art
[0003] Water pollution in my country is mainly caused by serious pollution sources such as metal ions and organic matter. When these pollutants enter natural water bodies, the pollution caused exceeds the self-purification capacity of the water body, which will lead to physical, chemical and biological changes in the water body and cause water quality deterioration. These pollutants enter the human body through drinking water or the food chain, causing varying degrees of damage to human health. How to reduce the concentration of metal ions in wastewater, improve water quality, thereby improving water recycling efficiency and reducing pollution to environmental water bodies is one of the most important directions and purposes of adsorbent research for many researchers. Among the existing sewage treatment methods, adsorption is the most widely used method. For a long time, many scientific researchers at home and abroad have been committed to the research and development and application of adsorbents. However, defects such as high cost, limited adsorption capacity and difficulty in regeneration have limited the widespread use of existing adsorption materials and also promoted people's research on adsorption materials with high economic benefits and adsorption capacity.
[0004] Chinese patent CN103638905B discloses a method for adsorbing heavy metals using tartaric acid intercalated hydrotalcite, which comprises: (1) preparing a salt solution of magnesium nitrate, aluminum nitrate and a sodium hydroxide alkaline solution, and preparing carbonated hydrotalcite by coprecipitation; (2) preparing a tartaric acid solution; (3) placing carbonated hydrotalcite in the tartaric acid solution, performing ion exchange at 120°C for 12 hours, and then filtering, washing and drying to obtain tartaric acid intercalated hydrotalcite. The tartaric acid intercalated hydrotalcite prepared in this patent can quickly adsorb Cu in water. 2+ However, when tartaric acid ions are intercalated into the interlayers of layered double hydroxides (LDHs) as organic acid radicals, their hydrophilicity is lower than that of unintercalated LDHs, and this cannot effectively solve the problem of LDHs easily agglomerating in water, making it unfavorable for the adsorption of metal ions in wastewater.
[0005] On the other hand, the booming paper industry has led to serious pollution and damage to the environment and global ecosystems. Even with the most modern and efficient operating technologies, producing one ton of paper generates at least 50 cubic meters of waste pulp. If this waste pulp is directly discharged, it will inevitably cause significant pollution to our environment. To effectively address my country's serious pollution problems and achieve sustainable development of the paper industry and the country, recycling and reusing waste liquid and applying it to other areas is of great significance to the green economy.
[0006] In order to rationally utilize papermaking waste pulp, Chinese patent CN101396649A discloses a liquid pollutant adsorbent. The liquid pollutant adsorbent is prepared by modifying a fiber composite made from papermaking waste pulp precipitates using a penetrant. This fully utilizes the effective components of the papermaking waste pulp precipitates, opens up a new approach for the treatment of papermaking waste pulp precipitates, and reduces environmental pollution. Although cellulose contains a large number of hydroxyl groups, most of the hydroxyl groups are strongly hydrogen-bonded, forming a highly crystalline cellulose in a multi-layered coiled manner. Only some of the free hydroxyl groups can be used for the adsorption of metal ions. Therefore, cellulose's ability to adsorb metals is not strong. In addition, the cellulose content in waste paper pulp is not high, making the waste paper pulp's ability to adsorb metal ions even weaker.
[0007] Summary of the Invention
[0008] In view of the above shortcomings of the existing technology, the purpose of the present invention is to provide a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent and its preparation method and application. The preparation method provided by the present invention can simultaneously solve the problems of low cellulose reaction activity and easy agglomeration of organic intercalated LDHs in papermaking waste pulp, and prepare an adsorbent with excellent and efficient adsorption performance for heavy metal ions. At the same time, it rationally utilizes papermaking waste pulp and solves the pollution problem of papermaking waste pulp.
[0009] In order to achieve the above object, the present invention provides the following technical solutions:
[0010] The present invention provides a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent, which is prepared by the following method: first, Mg / Al-LDHs is intercalated with tartaric acid to obtain tartaric acid intercalated Mg / Al-LDHs; papermaking waste pulp precipitate is used as a raw material to prepare a granular fiber composite, and then the fiber composite and the tartaric acid intercalated Mg / Al-LDHs are grafted with a crosslinking agent to obtain the papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
[0011] Preferably, the cross-linking agent is N,N-methylenebisacrylamide.
[0012] Preferably, the mass ratio of the fiber composite to the tartaric acid intercalated Mg / Al-LDHs is 1:(0.3-3.5).
[0013] The present invention also provides a method for preparing the papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent described in the above scheme, comprising the following steps:
[0014] S1. Preparing a granular fiber composite using papermaking waste pulp sediment as raw material;
[0015] S2. Sodium tartrate was added to deionized water free of CO2 and stirred thoroughly to obtain a tartaric acid solution; the pretreated Mg / Al-LDHs were then added to the tartaric acid solution, the pH of the mixture was adjusted to 10-11, and then stirred and refluxed at 50-70°C for 24-36 hours, followed by filtration, washing, and drying to obtain tartaric acid-intercalated Mg / Al-LDHs;
[0016] S3. Lithium chloride was dissolved in N,N-dimethylacetamide and ultrasonically dispersed, and the fiber composite obtained in step S1 was added thereto. The mixture was then stirred at 90-110° C. for 2-3 hours under a protective gas atmosphere to obtain solution A. The tartaric acid-intercalated Mg / Al-LDHs obtained in step S2 was dissolved in an acetic acid solution and ultrasonically dispersed to obtain solution B.
[0017] S4. Stirring the solution A and solution B obtained in step S3, adding N,N-methylenebisacrylamide, stirring at 30-50°C for 1-2 hours, then adjusting the pH value of the solution to 9-10, and then stirring at 60-80°C for 1-2 hours, filtering, washing, drying and grinding in sequence to obtain a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
[0018] The present invention uses papermaking waste pulp sediment as raw material to prepare a fiber composite, and prepares tartaric acid intercalated Mg / Al-LDHs through an anion exchange method. Finally, the tartaric acid intercalated Mg / Al-LDHs is grafted onto the fiber composite through a cross-linking reaction to obtain a cellulose-grafted tartaric acid intercalated Mg / Al-LDHs adsorbent. On the one hand, the fiber composite contains a large number of hydroxyl groups, which can significantly improve the hydrophilicity of the adsorbent after grafting. On the other hand, after grafting, an adsorbent with a large rigid structure can be obtained. From the above two aspects, the dispersion and solubility of the adsorbent in wastewater are improved, and its contact with metal ions is increased, thereby improving the problem of tartaric acid intercalation causing the hydrophilicity of the adsorbent to decrease. At the same time, through grafting, more adsorption groups in the fiber composite and tartaric acid intercalated Mg / Al-LDHs can be exposed, increasing the possibility of contact with metal ions and thus enhancing its ability to adsorb metal ions. Under the synergistic effect of the fiber composite, tartaric acid intercalated Mg / Al-LDHs and N,N-methylenebisacrylamide, the dispersion ability of the adsorbent in water can be improved, and the ability of the adsorbent to adsorb metal ions can be improved. At the same time, the problems of low cellulose reaction activity in papermaking waste pulp and easy agglomeration of tartaric acid intercalated LDHs are solved, thereby significantly improving the adsorption capacity of the prepared cellulose grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
[0019] Preferably, the step S1 is: washing the papermaking waste pulp precipitate with deionized water and anhydrous ethanol repeatedly for 3 to 5 times, then drying it at 80 to 100° C., crushing it and passing it through a 200-mesh sieve to obtain a granular fiber composite.
[0020] Preferably, in step S2, the mass ratio of sodium tartrate to Mg / Al-LDHs is (8-10):25.
[0021] Preferably, in step S2, the pretreatment method of the Mg / Al-LDHs is: calcining the Mg / Al-LDHs at 450-550°C for 3-5 hours. The present invention removes CO3 between the LDHs layers through pretreatment. 2- .
[0022] Preferably, in step S3, the mass ratio of the fiber composite, lithium chloride, and N,N-dimethylacetamide is (4-6):(6-9):(85-90); and the mass ratio of the tartaric acid-intercalated Mg / Al-LDHs to the acetic acid solution is 1:(45-55). Hydrogen bonds within and between cellulose molecules induce the formation of crystalline regions, which hinder the contact between the solvent and the cellulose molecules. The main function of lithium chloride is to activate and pretreat the cellulose. After activation and pretreatment, some hydrogen bonds in the cellulose are broken, the molecular chains acquire a more relaxed configuration, and the tightly packed crystalline regions become more easily contacted with the solvent, thereby dissolving the cellulose more rapidly.
[0023] Preferably, in step S4, the mass ratio of solution A to solution B is 1:(1-7); the mass ratio of solution A to N,N-methylenebisacrylamide is 1:(0.2-2.2).
[0024] The present invention also provides the use of the papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent described in the above scheme or the papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent obtained by the preparation method described in the above scheme in wastewater treatment.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. By grafting the fiber composite onto tartaric acid-intercalated Mg / Al-LDHs, the present invention not only retains the ability of tartaric acid-intercalated Mg / Al-LDHs to adsorb copper ions, but also increases the hydroxyl groups in the fiber composite as binding sites for copper ions. Under the combined action of the two, the adsorbent's adsorption capacity for metal ions is significantly improved.
[0027] 2. After tartaric acid is intercalated into Mg / Al-LDHs, it cannot effectively inhibit the agglomeration of Mg / Al-LDHs. The present invention uses N,N-methylenebisacrylamide as a cross-linking agent to graft the fiber composite and tartaric acid intercalated Mg / Al-LDHs. As a dialdehyde linker, the polarized structure of the carbonyl group of N,N-methylenebisacrylamide makes it easy to undergo nucleophilic reaction with polar groups and bind tightly, so that the fiber composite grafted tartaric acid intercalated Mg / Al-LDHs adsorbent of the present invention has a large rigid structure, so it has better dispersibility in water than matrix LDHs. The present invention allows more adsorption groups in the fiber composite and tartaric acid intercalated Mg / Al-LDHs to be exposed through the grafting of N,N-methylenebisacrylamide, thereby increasing the possibility of contact with metal ions. In addition, N,N-methylenebisacrylamide has an amino group, which can further enhance the adsorption capacity of copper ions. Under the synergistic effect of fiber composite, tartaric acid intercalated Mg / Al-LDHs and N,N-methylenebisacrylamide, not only the dispersion ability of the adsorbent in wastewater can be improved, but also the metal ion adsorption capacity of the adsorbent can be enhanced, thereby obtaining an adsorbent with excellent adsorption capacity.
[0028] 3. The preparation method of the present invention can not only solve the problem of heavy metal ion adsorption in industrial wastewater, but also reduce the cost of wastewater adsorbents, while solving the pollution treatment problem of papermaking waste pulp, and ultimately achieve sustainable development.
[0029] 4. The papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent prepared by the present invention can achieve an equilibrium adsorption capacity of 60.5 mg / g for copper ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0031] FIG1 is an infrared spectrum of cellulose and papermaking waste pulp precipitates;
[0032] Figure 2 shows the XRD patterns of cellulose and papermaking waste pulp precipitates. DETAILED DESCRIPTION
[0033] To further illustrate the present invention, the applicant will now provide a detailed description of the present invention with reference to the accompanying drawings and specific embodiments, with the goal of enabling those skilled in the art to clearly understand the present invention. However, the following embodiments should not be construed as limiting the scope of protection of the present invention to any extent.
[0034] In the following examples and comparative examples, the papermaking waste pulp precipitate was sourced from Vinda Group;
[0035] Figure 1 is an infrared spectrum of cellulose and papermaking waste pulp sediment. As can be seen from Figure 1, the 1040, 1400, 1700, 2950, and 3400 cm-1 spectrum of cellulose -1 There are absorption peaks on the left and right, which are CO, CH, C=O, CH and OH groups. In the spectrum of papermaking waste pulp sediment, there are absorption peaks at 1040, 1400, 1700, 2950, 3400 cm -1 There are also absorption peaks on the left and right, corresponding to the cellulose spectrum, but the intensity of the peaks is slightly lower than that of cellulose. Based on this, it can be judged that the main material of the papermaking waste pulp precipitate is cellulose.
[0036] Figure 2 is the XRD spectrum of cellulose and papermaking waste pulp precipitate. As can be seen from Figure 2, cellulose has obvious characteristic peaks at 14, 16, 22 and 34°, and the peaks are sharp, indicating that cellulose has good crystallinity; the papermaking waste pulp precipitate has weaker peaks at 14, 16, 22 and 34°. On the one hand, based on the infrared spectrum, it is further explained that the main material of the papermaking waste pulp precipitate is cellulose. On the other hand, the papermaking waste pulp precipitate has weaker crystallinity than cellulose, so that more hydroxyl groups can be exposed. Compared with natural cellulose, the ability to adsorb metal ions in wastewater is enhanced.
[0037] Sodium tartrate, magnesium aluminum-based layered double hydroxide, dilute hydrochloric acid, anhydrous lithium chloride, N,N-dimethylacetamide, and N,N-methylenebisacrylamide were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. All raw materials are common raw materials on the market.
[0038] Example 1
[0039] This embodiment discloses a method for preparing a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent, comprising the following steps:
[0040] S1. The papermaking waste pulp precipitate was washed three times with distilled water and anhydrous ethanol, dried at 80°C to a moisture content of 10%, and then pulverized and passed through a 200-mesh sieve to obtain a fine granular fiber composite;
[0041] S2. Sodium tartrate was added to deionized water at 80°C (with a mass ratio of 1:90) and the mixture was stirred thoroughly to dissolve to obtain a tartaric acid solution. Mg / Al-LDHs was then placed in a muffle furnace, heated to 450°C, and calcined for 5 h to remove CO2 from the interlayer of the Mg / Al-LDHs. 2- Finally, after the muffle furnace temperature was lowered to 200°C, the Mg / Al-LDHs were quickly taken out and added to a three-necked flask placed in a water bath. The prepared tartaric acid solution was then added according to a mass ratio of sodium tartrate to Mg / Al-LDHs of 8:25. After stirring evenly, the pH value of the mixture was adjusted to 10 with dilute hydrochloric acid. The mixture was then stirred and refluxed at 50°C for 36 hours, cooled to room temperature, filtered, washed three times with deionized water, and dried at 90°C for 12 hours to obtain tartaric acid-intercalated Mg / Al-LDHs.
[0042] S3. Anhydrous lithium chloride and N,N-dimethylacetamide were added to a flask, and ultrasonic vibration was performed to dissolve the anhydrous lithium chloride in the N,N-dimethylacetamide. The fiber composite obtained in step S1 was then added, with the mass ratio of the fiber composite, anhydrous lithium chloride, and N,N-dimethylacetamide being 6:9:85. Then, under nitrogen protection, the mixture was uniformly stirred at 90°C for 3 hours and allowed to stand at room temperature to obtain solution A. The tartaric acid-intercalated Mg / Al-LDHs obtained in step S2 and acetic acid solution (2 wt%) were mixed in a mass ratio of 1:45 and dispersed and dissolved by ultrasonic vibration to obtain solution B.
[0043] S4. Under nitrogen protection, solution A and solution B were mixed in a mass ratio of 1:6.8, stirred at a constant speed at room temperature for 1 h, and then N,N-methylenebisacrylamide was added. The mass ratio of solution A to N,N-methylenebisacrylamide was 1:2.2. Stirring was continued at 30°C for 2 h. The pH value of the solution was adjusted to 9 with 1 mol / L NaOH, and then stirred at 80°C for 1 h. Finally, the solution was filtered, washed with anhydrous ethanol and deionized water three times respectively, dried at 90°C for 12 h, ground and passed through a 200-mesh sieve to obtain a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
[0044] Example 2
[0045] This embodiment discloses a method for preparing a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent, comprising the following steps:
[0046] S1. The papermaking waste pulp precipitate was washed three times with distilled water and anhydrous ethanol, dried at 100°C to a moisture content of 10%, and then pulverized and passed through a 200-mesh sieve to obtain a fine granular fiber composite;
[0047] S2. Sodium tartrate was added to deionized water at 80°C (with a mass ratio of 1:90) and the mixture was stirred thoroughly to dissolve to obtain a tartaric acid solution. Mg / Al-LDHs was then placed in a muffle furnace, heated to 500°C, and calcined for 4 h to remove CO2 from the interlayer of the Mg / Al-LDHs. 2- Finally, after the muffle furnace temperature was lowered to 200°C, the Mg / Al-LDHs were quickly taken out and added to a three-necked flask placed in a water bath. The prepared tartaric acid solution was then added according to a mass ratio of sodium tartrate to Mg / Al-LDHs of 9:25. After stirring evenly, the pH value of the mixture was adjusted to 10 with dilute hydrochloric acid. The mixture was then stirred and refluxed at 60°C for 24 hours, cooled to room temperature, filtered, washed three times with deionized water, and dried at 80°C for 12 hours to obtain tartaric acid-intercalated Mg / Al-LDHs.
[0048] S3. Anhydrous lithium chloride and N,N-dimethylacetamide were added to a flask, and anhydrous lithium chloride was dissolved in N,N-dimethylacetamide by ultrasonic oscillation. The fiber composite obtained in step S1 was then added, with the mass ratio of fiber composite, anhydrous lithium chloride, and N,N-dimethylacetamide being 5:7:88. The mixture was then stirred uniformly at 100°C for 2 h under nitrogen protection and allowed to stand at room temperature to obtain solution A. The tartaric acid-intercalated Mg / Al-LDHs obtained in step S2 and acetic acid solution (2 wt%) were mixed in a mass ratio of 1:50 and dispersed and dissolved by ultrasonic oscillation to obtain solution B.
[0049] S4. Under nitrogen protection, solution A and solution B were mixed in a mass ratio of 1:3.3, stirred at room temperature at a constant speed for 1 hour, and then N,N-methylenebisacrylamide was added. The mass ratio of solution A to N,N-methylenebisacrylamide was 1:1. Stirring was continued at 40°C for 1.5 hours, and the pH value of the solution was adjusted to 9 with 1 mol / L NaOH. Then, it was stirred at 70°C for 1 hour, and finally filtered. The solution was washed with anhydrous ethanol and deionized water three times respectively, dried at 80°C for 12 hours, ground and passed through a 200-mesh sieve to obtain a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
[0050] Example 3
[0051] This embodiment discloses a method for preparing a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent, comprising the following steps:
[0052] S1. The papermaking waste pulp precipitate was washed three times with distilled water and anhydrous ethanol, dried at 100°C to a moisture content of 10%, and then pulverized and passed through a 200-mesh sieve to obtain a fine granular fiber composite;
[0053] S2. Sodium tartrate was added to deionized water at 80°C (with a mass ratio of 1:90) and the mixture was stirred thoroughly to dissolve to obtain a tartaric acid solution. Mg / Al-LDHs was then placed in a muffle furnace, heated to 550°C, and calcined for 3 h to remove CO2 from the interlayer of the Mg / Al-LDHs. 2- Finally, after the muffle furnace temperature was lowered to 100°C, the Mg / Al-LDHs were quickly removed and added to a three-necked flask placed in a water bath. The prepared tartaric acid solution was then added according to a mass ratio of sodium tartrate to Mg / Al-LDHs of 10:25. After stirring evenly, the pH value of the mixture was adjusted to 10 with dilute hydrochloric acid. The mixture was then stirred and refluxed at 70°C for 24 hours, cooled to room temperature, filtered, washed three times with deionized water, and dried at 80°C for 12 hours to obtain tartaric acid-intercalated Mg / Al-LDHs.
[0054] S3. Anhydrous lithium chloride and N,N-dimethylacetamide were added to a flask, and ultrasonic vibration was performed to dissolve the anhydrous lithium chloride in the N,N-dimethylacetamide. The fiber composite obtained in step S1 was then added, with the mass ratio of the fiber composite, anhydrous lithium chloride, and N,N-dimethylacetamide being 4:6:90. The mixture was then stirred uniformly at 110°C for 2 hours under nitrogen protection and allowed to stand at room temperature to obtain solution A. The tartaric acid-intercalated Mg / Al-LDHs obtained in step S2 and acetic acid solution (2 wt%) were mixed in a mass ratio of 1:55 and dispersed and dissolved by ultrasonic vibration to obtain solution B.
[0055] S4. Under nitrogen protection, solution A and solution B were mixed in a mass ratio of 1:1.7, stirred at room temperature at a uniform speed for 2.5 h, and then N,N-methylenebisacrylamide was added. The mass ratio of solution A to N,N-methylenebisacrylamide was 1:0.4. Stirring was continued at 50°C for 1 h, and the pH value of the solution was adjusted to 9 with 1 mol / L NaOH. Then, it was stirred at 60°C for 2 h, and finally filtered. The mixture was washed with anhydrous ethanol and deionized water three times respectively, dried at 90°C for 12 h, ground and passed through a 200-mesh sieve to obtain a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
[0056] Example 4
[0057] This embodiment is substantially the same as embodiment 2, except that in step S4, the mass ratio of solution A to solution B is 1:1, and the mass ratio of solution A to N,N-methylenebisacrylamide is 1:0.3.
[0058] Comparative Example 1
[0059] This comparative example discloses a method for preparing a fiber composite adsorbent, comprising the following steps:
[0060] S1. The papermaking waste pulp precipitate was washed three times with distilled water and anhydrous ethanol, dried at 100°C to a moisture content of 10%, and then pulverized and passed through a 200-mesh sieve to obtain a fine granular fiber composite;
[0061] S2. Anhydrous lithium chloride and N,N-dimethylacetamide were added to a flask, and ultrasonic vibration was applied to dissolve the anhydrous lithium chloride in the N,N-dimethylacetamide. The fiber composite obtained in step S1 was then added, with the mass ratio of the fiber composite, anhydrous lithium chloride, and N,N-dimethylacetamide being 5:7:88. The mixture was then stirred uniformly at 100°C for 2 h under nitrogen protection and allowed to stand at room temperature to obtain Solution A.
[0062] S3. Under nitrogen protection, solution A obtained in step S2 was stirred at a constant speed at room temperature for 2.5 h, and then the pH value of the solution was adjusted to 9 with 1 mol / L NaOH, and then stirred at 70°C for 1 h. Finally, it was filtered, washed with anhydrous ethanol and deionized water three times respectively, dried at 80°C for 12 h, ground and passed through a 200-mesh sieve to obtain a fiber composite adsorbent.
[0063] Comparative Example 2
[0064] This comparative example discloses a method for preparing a tartaric acid intercalated Mg / Al-LDHs adsorbent, comprising the following steps:
[0065] S1. Sodium tartrate was added to deionized water at 80°C (mass ratio of sodium tartrate to deionized water was 1:90), and the mixture was stirred thoroughly to dissolve to obtain a tartaric acid solution. Mg / Al-LDHs was then placed in a muffle furnace, heated to 500°C, and calcined for 4 h to remove CO3 from the interlayer of Mg / Al-LDHs. 2- Finally, after the muffle furnace temperature was lowered to 200°C, the Mg / Al-LDHs were quickly taken out and added to a three-necked flask placed in a water bath. The prepared tartaric acid solution was then added according to a mass ratio of sodium tartrate to Mg / Al-LDHs of 9:25. After stirring evenly, the pH value of the mixture was adjusted to 10 with dilute hydrochloric acid. The mixture was then stirred and refluxed at 60°C for 24 hours, cooled to room temperature, filtered, washed three times with deionized water, and dried at 80°C for 12 hours to obtain tartaric acid-intercalated Mg / Al-LDHs.
[0066] S2. The tartaric acid-intercalated Mg / Al-LDHs obtained in step S1 and acetic acid solution (2 wt %) were mixed in a mass ratio of 1:50 and dispersed and dissolved by ultrasonic oscillation to obtain solution B;
[0067] S3. Under nitrogen protection, solution B obtained in step S2 was stirred at a constant speed at room temperature for 2.5 h, and then the pH value of the solution was adjusted to 9 with 1 mol / L NaOH, and then stirred at 70°C for 1 h. Finally, it was filtered, washed with anhydrous ethanol and deionized water three times, respectively, dried at 80°C for 12 h, ground and passed through a 200 mesh sieve to obtain a tartaric acid intercalated Mg / Al-LDHs adsorbent.
[0068] Comparative Example 3
[0069] This comparative example is basically the same as Example 2, except that: in step S4, the cross-linking agent N,N-methylenebisacrylamide is not added, and a blend of the fiber composite and the tartaric acid-intercalated Mg / Al-LDHs is obtained.
[0070] Comparative Example 4
[0071] This comparative example discloses a method for preparing a papermaking waste pulp grafted Mg / Al-LDHs adsorbent, comprising the following steps:
[0072] S1. The papermaking waste pulp precipitate was washed three times with distilled water and anhydrous ethanol, dried at 100°C to a moisture content of 10%, and then pulverized and passed through a 200-mesh sieve to obtain a fine granular fiber composite;
[0073] S2. Anhydrous lithium chloride and N,N-dimethylacetamide were added to a flask, and ultrasonic vibration was used to dissolve the anhydrous lithium chloride in the N,N-dimethylacetamide. The fiber composite obtained in step S1 was then added, with the mass ratio of the fiber composite, anhydrous lithium chloride, and N,N-dimethylacetamide being 5:7:88. The mixture was then stirred uniformly at 100°C for 2 h under nitrogen protection and allowed to stand at room temperature to obtain solution A. Mg / Al-LDHs and acetic acid solution (2 wt %) were mixed in a mass ratio of 1:50 and dispersed and dissolved by ultrasonic vibration to obtain solution B.
[0074] S3. Under nitrogen protection, solution A and solution B were mixed in a mass ratio of 1:3.3, stirred at a constant speed at room temperature for 1 hour, and then N,N-methylenebisacrylamide was added. The mass ratio of solution A to N,N-methylenebisacrylamide was 1:1. Stirring was continued at 40°C for 1.5 hours. The pH value of the solution was adjusted to 9 with 1 mol / L NaOH, and then stirred at 70°C for 1 hour. Finally, it was filtered, washed with anhydrous ethanol and deionized water three times respectively, dried at 80°C for 12 hours, ground and sieved through a 200-mesh sieve to obtain a papermaking waste pulp grafted Mg / Al-LDHs adsorbent.
[0075] That is, compared with Example 2, this comparative example does not use tartaric acid to intercalate Mg / Al-LDHs.
[0076] Comparative Example 5
[0077] This comparative example is basically the same as Example 2, except that the mass ratio of solution A to solution B in step S4 is 1:0.02.
[0078] Application Examples
[0079] Analytical reagent grade Cu(NO3)·3H2O was added to deionized water to prepare 1L of Cu with an initial concentration of 200 mg / L. 2+ solution, and then weigh 1g of the adsorbent prepared in Examples 1 to 4 and Comparative Examples 1 to 5 and add Cu 2+ The solution was stirred at a constant speed for 3 h at 25 ° C, and the adsorbed Cu 2+ concentration.
[0080] The equilibrium adsorption capacity was calculated according to the following formula:
[0081] Where q e is the equilibrium adsorption capacity, the unit is mg / g; C o is the initial concentration of metal ions in the wastewater before adsorption, expressed in mg / L; C eis the equilibrium concentration of metal ions in the remaining waste liquid after adsorption, and the unit is mg / L; m is the mass of the adsorbent, and V is the volume of the metal waste liquid. The test results are shown in Table 1.
[0082] Table 1 Adsorption of Cu by adsorbents prepared in Examples 1 to 4 of the present invention and Comparative Examples 1 to 5 2+ Performance test results
[0083] The data in Table 1 demonstrate that the papermaking waste pulp grafted tartaric acid-intercalated Mg / Al-LDHs adsorbent prepared by the present invention exhibits excellent copper ion adsorption performance. Comparing Example 2 with Comparative Examples 1-3, it can be seen that the equilibrium adsorption capacity is significantly reduced in both Comparative Example 1, which directly uses the fiber composite as the adsorbent, and Comparative Example 2, which directly uses tartaric acid-intercalated Mg / Al-LDHs as the adsorbent.
[0084] In Comparative Example 3, no cross-linking agent was added, and no grafting reaction occurred between the fiber composite and the tartaric acid intercalated Mg / Al-LDHs. It was just a simple composite, and the dispersibility of the adsorbent deteriorated, and the equilibrium adsorption capacity was also significantly reduced. This shows that compared with using the fiber composite, tartaric acid intercalated Mg / Al-LDHs alone, or simply composite the two, grafting the fiber composite and tartaric acid intercalated Mg / Al-LDHs can improve the adsorption capacity of the adsorbent for copper ions. This may be because by grafting the fiber composite onto the tartaric acid intercalated Mg / Al-LDHs, under the interaction between the fiber composite and the tartaric acid intercalated Mg / Al-LDHs, while improving the adsorption capacity of the adsorbent, it can also improve the dispersion ability of the adsorbent in wastewater. On the one hand, it can solve the problem of hydroxyl blocking and low reaction activity in the fiber composite, and on the other hand, it can solve the problem of easy agglomeration of tartaric acid intercalated Mg / Al-LDHs, thereby significantly improving the adsorption capacity of the prepared adsorbent for copper ions.
[0085] Compared with Example 2, Comparative Example 4 did not use tartaric acid to intercalate Mg / Al-LDHs, and the proportion of tartaric acid intercalated Mg / Al-LDHs in Comparative Example 5 was extremely small. The adsorption capacity of the adsorbents prepared in Comparative Examples 4 and 5 was significantly reduced.
[0086] Although the embodiments of the present invention have been shown and described and the present invention has been described in detail, they are only some of the embodiments of the present invention, rather than all of the embodiments. For those skilled in the art, it can be understood that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and other embodiments can be obtained without creativity. These embodiments all fall within the scope of protection of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent, characterized in that: The invention is prepared by the following method: firstly, tartaric acid is used to intercalate Mg / Al-LDHs to obtain tartaric acid intercalated Mg / Al-LDHs; a granular fiber composite is prepared by using papermaking waste pulp precipitate as a raw material, and then the fiber composite is grafted with tartaric acid intercalated Mg / Al-LDHs by a crosslinking agent to obtain a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
2. The papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent according to claim 1, characterized in that: The cross-linking agent is N,N-methylenebisacrylamide.
3. The papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent according to claim 1, characterized in that: The mass ratio of the fiber composite to the tartaric acid intercalated Mg / Al-LDHs is 1:(0.3-3.5).
4. The method for preparing the papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Using papermaking waste slurry precipitate as raw material to prepare a granular fiber composite; S2. Sodium tartrate is added to deionized water without CO2 and stirred to obtain a tartaric acid solution; then the pretreated Mg / Al-LDHs is added to the tartaric acid solution, the pH value of the mixture is adjusted to 10-11, and then stirred and refluxed at 50-70°C for 24-36h, filtered, washed and dried in sequence to obtain tartaric acid intercalated Mg / Al-LDHs; S3. dissolving lithium chloride in N,N-dimethylacetamide and ultrasonically dispersing the mixture, adding the fiber composite obtained in step S1, and stirring at 90-110° C. for 2-3 hours under a protective gas atmosphere to obtain solution A; dissolving the tartaric acid intercalated Mg / Al-LDHs obtained in step S2 in an acetic acid solution and ultrasonically dispersing the mixture to obtain solution B; S4. The solution A and solution B obtained in step S3 are mixed and stirred, and then N,N-methylenebisacrylamide is added, and stirred at 30-50° C. for 1-2 hours, and then the pH value of the obtained mixed solution is adjusted to 9-10, and stirred at 60-80° C. for 1-2 hours, and filtered, washed, dried and ground in sequence to obtain a papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent.
5. The preparation method according to claim 4, characterized in that: The step S1 is: washing the papermaking waste pulp precipitate with deionized water and anhydrous ethanol repeatedly for 3 to 5 times, then drying it at 80 to 100° C., crushing it and passing it through a 200-mesh sieve to obtain the granular fiber composite.
6. The preparation method according to claim 4, characterized in that: In the step S2, the mass ratio of sodium tartrate to Mg / Al-LDHs is (8-10):
25.
7. The preparation method according to claim 4, characterized in that: In the step S2, the method for pretreating the Mg / Al-LDHs is: calcining the Mg / Al-LDHs at 450-550° C. for 3-5 hours.
8. The preparation method according to claim 4, characterized in that: In step S3, the mass ratio of the fiber composite, lithium chloride and N,N-dimethylacetamide is (4-6):(6-9):(85-90); the mass ratio of the tartaric acid intercalated Mg / Al-LDHs to the acetic acid solution is 1:(45-55).
9. The preparation method according to claim 4, characterized in that: In the step S4, the mass ratio of the solution A to the solution B is 1:(1-7); the mass ratio of the solution A to N,N-methylenebisacrylamide is 1:(0.2-2.2).
10. Use of the papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent according to any one of claims 1 to 3 or the papermaking waste pulp grafted tartaric acid intercalated Mg / Al-LDHs adsorbent obtained by the preparation method according to any one of claims 4 to 8 in wastewater treatment.
Citation Information
Patent Citations
Liquid pollutant adsorbent and preparation method thereof
CN101396649A
Method for adsorbing heavy metals with tartaric acid intercalated hydrotalcite
CN103638905A
Carboxymethyl cellulose ion intercalated hydrotalcite-like composite material, and preparation method and application thereof
CN104874365A
Layered dual metal hydroxides / cellulose porous composite material and preparation method thereof
CN108690223A
Cellulose / magnesium-aluminum layered bimetallic oxide aerogel as well as preparation method and application thereof
CN113617302A
Cited By
Gasoline engine particle trap with low expansion coefficient and preparation method thereof