High-brightness high-luminous-efficiency complex-phase fluorescent ceramic for laser illumination and preparation method therefor

By introducing SrAl2O4 into Ce:LuAG ceramics, a complex-phase fluorescent ceramic with high brightness and high luminous efficiency is prepared, which solves the problems of poor thermal stability and low light conversion efficiency of Ce:LuAG ceramics and is suitable for high-power LEDs/LDs devices. The sintering temperature and preparation cost are reduced.

WO2024216829A1PCT designated stage expired Publication Date: 2024-10-24XUZHOU NORMAL UNIVERSITY +3
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/117952
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-09-11
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Due to its cubic crystal structure, Ce:LuAG transparent ceramic phosphor has problems of poor thermal stability and low light conversion efficiency, and its high sintering temperature limits its large-scale application.

Method used

The second phase SrAl2O4 is introduced into the ceramic matrix, and Ce:YAG composite phase fluorescent ceramics are prepared through discharge plasma sintering, which improves the uniformity of emitted light and light extraction efficiency and reduces the sintering temperature.

Benefits of technology

The thermal stability and light conversion efficiency of ceramics are significantly improved, and complex-phase fluorescent ceramics with high brightness and high luminous efficiency are realized, which are suitable for high-power LEDs/LDs devices and reduce preparation costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023117952_24102024_PF_FP_ABST
    Figure CN2023117952_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A high-brightness high-luminous-efficiency complex-phase fluorescent ceramic for laser illumination and a preparation method therefor. The complex-phase fluorescent ceramic is prepared from Ce:LuAG powder and SrAl2O4 power as ceramic raw material powder by using a spark plasma sintering method, wherein Ce:LuAG serves as a ceramic body, and SrAl2O4 is introduced as a second phase. The introduction of the second phase, i.e., SrAl2O4 remarkably inhibits grain growth of LuAG, and makes the particle distribution of a Ce:LuAG ceramic small and uniform, and the prepared complex-phase fluorescent ceramic has high brightness and high luminous efficiency. The fluorescent ceramic has better luminescence characteristics, and solves the problems in the prior art of poor thermal stability, low light conversion efficiency and the like, and the preparation method for the complex-phase ceramic is simple, involves a short process and a low sintering temperature, can be applied to high-power LEDs / LDs devices, and greatly improves the application value of the devices.
Need to check novelty before this filing date? Find Prior Art

Description

A high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting and its preparation method Technical Field

[0001] The present invention belongs to the technical field of fluorescent ceramics, and in particular relates to a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting and a preparation method thereof. Background Art

[0002] LuAG is the abbreviation of lutetium aluminum garnet, and its chemical formula is Lu3Al5O 12 It is a solid solution formed by Lu2O3 and Al2O3, belongs to the cubic crystal system, has a garnet structure, does not have a birefringence effect, and can be made into transparent ceramics with excellent optical properties. At the same time, due to its high density (6.73g / cm 3 , equivalent to 94% of the density of BGO), high melting point (2010°C), high effective atomic number (Z eff =60), good mechanical properties, and can maintain stable optical and physical and chemical properties under long-term radiation conditions.

[0003] Ce:LuAG transparent ceramic phosphor has been widely studied as a promising candidate material for color converters for white light-emitting diode (LED) lighting due to its excellent thermal and chemical stability. The Shanghai Institute of Ceramics used a solid-phase reaction method to prepare transparent LuAG:Ce ceramics under vacuum sintering conditions at 1760°C for 10 hours. Its transmittance is low, at 56% in the visible light range. In addition, the high sintering temperature of 1760°C also limits its large-scale application. Patent CN 110550945 B discloses a method for preparing LuAG:Ce transparent ceramics and LuAG:Ce transparent ceramics, which can solve the problems of the low transmittance of LuAG:Ce ceramics in the visible light range in the prior art and the large-scale application limited by the high sintering temperature during preparation.

[0004] However, Ce:LuAG transparent ceramic phosphor has a cubic crystal structure, and although it has a high transmittance, it also causes the blue light emitted by the InGaN chip to be reflected by the Ce:LuAG phosphor. 3+ The absorption of yellow light is less, the yellow light conversion efficiency is low, and there are problems such as poor thermal stability and low light conversion efficiency. Summary of the Invention

[0005] In response to the above-mentioned technical deficiencies, the purpose of the present invention is to provide a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting and a preparation method thereof. The fluorescent ceramic has better luminous properties and solves the problems of poor thermal stability and low light conversion efficiency in the prior art. The preparation method of the composite ceramic is simple, time-saving, and has a low sintering temperature. It can be applied to high-power LEDs / LDs devices, greatly enhancing the application value of the device.

[0006] To address these issues, a second phase is introduced into the ceramic matrix to control its transmittance and enhance the optical path. SrAl2O4 is selected as the second phase in the preparation of Ce:YAG composite fluorescent ceramics. The introduction of SrAl2O4 significantly improves the uniformity of the emitted light from the composite fluorescent ceramic, making it more suitable for white-light laser diode illumination.

[0007] SrAl2O4, a widely used traditional ceramic, has attracted widespread attention due to its unique properties. Compared to Al2O3, SrAl2O4 is a hexagonal system with a lower refractive index, which helps reduce total internal reflection losses and improve light extraction efficiency. Furthermore, the vacuum sintering temperature of SrAl2O4 is the same as that of Ce:LuAG, facilitating the one-step vacuum sintering process for the preparation of SrAl2O4-Ce:LuAG.

[0008] The specific technical solutions adopted in the present invention are as follows:

[0009] The first object of the present invention is to provide a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting. The composite fluorescent ceramic is prepared by spark plasma sintering using Ce:LuAG powder and SrAl2O4 powder as ceramic raw material powders, wherein Ce:LuAG is used as the ceramic main body and SrAl2O4 is introduced as the second phase. The prepared composite fluorescent ceramic has high brightness and high luminous efficiency.

[0010] A second object of the present invention is to provide a method for preparing a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting, comprising the following steps:

[0011] S1: Weigh Ce:LuAG powder and SrAl2O4 powder according to the mass ratio respectively as ceramic raw material powders, wherein SrAl2O4 powder accounts for 5% to 25% of the total mass of the ceramic raw material powders;

[0012] S2: Ce:LuAG powder and SrAl2O4 powder were blended, anhydrous ethanol was added, and the mixture was thoroughly mixed by ball milling;

[0013] S3: The slurry obtained after ball milling is taken out and dried to obtain a dry powder;

[0014] S4: The dried powder is subjected to spark plasma sintering in a vacuum state and cooled to room temperature to obtain a composite fluorescent ceramic.

[0015] Furthermore, in step S1, the particle size of the Ce:LuAG powder is 1 μm to 1.3 μm, the particle size of the SrAl2O4 powder is 1.5 μm to 2 μm, and the purity of both is above 99.99%.

[0016] Furthermore, in step S2, the ball milling speed is 180-250 rpm, and the ball milling time is 15-30 h.

[0017] Furthermore, in step S3, the drying temperature is 70-90° C., and the drying time is 8-12 hours.

[0018] Furthermore, in step S4, the spark plasma sintering has a sintering pressure of 50-100 MPa, a pulse current of 200-400 A, a heat preservation sintering time of 20-50 min, and a sintering temperature of 1650° C.-1800° C.

[0019] The beneficial effects of the present invention are:

[0020] 1. The vacuum sintering temperature of SrAl2O4 used in the present invention is the same as that of Ce:LuAG, which facilitates one-step vacuum sintering, is lower in cost and more environmentally friendly;

[0021] 2. The present invention adopts SrAl2O4-Ce:LuAG composite phase. By introducing the SrAl2O4 second phase, the grain growth of LuAG is significantly inhibited, making the Ce:LuAG particle distribution small and uniform, and effectively improving the light extraction rate;

[0022] 3. The SrAl2O4-Ce:LuAG composite prepared by the present invention has high thermal stability and low thermal quenching rate (92% @ 150°C). Compared with pure Ce:LuAG fluorescent ceramics, it has better luminescence properties. Under the excitation of a 20W blue light LD chip, there is no luminescence saturation. Especially when the input power is 4-5W, the maximum luminous flux of 20 wt% SrAl2O4-Ce:LuAG can reach 800-1000 lm, greatly enhancing the application value of the device.

[0023] 4. The present invention prepares SrAl2O4-Ce:LuAG composite ceramics with high brightness and high luminous efficiency through SPS sintering. The preparation method is simple, takes a short time, and has a low sintering temperature. It can be applied to high-power LEDs / LDs devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0025] 1 is a comparison diagram of XRD of samples SrAl2O4-Ce:LuAG, LuAG and SrAl2O4 prepared in Example 2 of the present invention;

[0026] 2 is an EL spectrum of the sample SrAl2O4-Ce:LuAG prepared in Example 2 of the present invention under 450nm LD chip excitation;

[0027] 3 is a comparison chart of the relationship between the luminous flux and the LD chip input power of the sample prepared in Example 1 of the present invention in which SrAl2O4 accounts for 25% of the total mass of the ceramic raw materials, the 20% sample prepared in Example 2, and the pure Ce:LuAG sample. Implementation Method

[0028] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0029] The Ce:LuAG powder and SrAl2O4 powder used in the following examples are both commercially available products. Example

[0030] According to the chemical formula SrAl2O4-Ce:LuAG, SrAl2O4 accounts for 25% of the total mass of the ceramic raw materials. According to the stoichiometric ratio of the corresponding raw materials, 60g of Ce:LuAG powder with a purity of 99.99% and a particle size of 1.2 μm and 15g of SrAl2O4 powder with a purity of 99.99% and a particle size of 1.7 μm were weighed. The Ce:LuAG powder and SrAl2O4 powder were blended, anhydrous ethanol was added, and the mixture was thoroughly mixed by ball milling. The resulting powder was dried in a 90°C oven for 12 hours to obtain a dry powder. The dried powder was wrapped with graphite paper and subjected to spark plasma sintering in a vacuum state. The sintering pressure was 80MPa, the pulse current was 300A, the sintering time was 40min, and the sintering temperature was 1700°C. The composite ceramic was obtained by cooling to room temperature.

[0031] When excited by a blue light LD chip with a wavelength of around 450nm, it emits high-brightness broadband yellow light around 540nm. Compared with pure Ce:LuAG, it exhibits excellent luminescence performance under the excitation of blue light LD. When the input power is 4.5W, 25 wt% SrAl2O4-Ce:LuAG reaches a maximum luminous flux of 800 lm. Example

[0032] According to the chemical formula SrAl2O4-Ce:LuAG, SrAl2O4 accounts for 20% of the total mass of the ceramic raw materials. According to the stoichiometric ratio of the corresponding raw materials, 60g of Ce:LuAG powder with a purity of 99.99% and a particle size of 1.2 μm and 12g of SrAl2O4 powder with a purity of 99.99% and a particle size of 1.7 μm were weighed. The Ce:LuAG powder and SrAl2O4 powder were blended, anhydrous ethanol was added, and the mixture was thoroughly mixed by ball milling. The resulting powder was dried in a 90°C oven for 12 hours to obtain a dry powder. The dried powder was wrapped with graphite paper and subjected to spark plasma sintering in a vacuum state. The sintering pressure was 80MPa, the pulse current was 300A, the sintering time was 40min, and the sintering temperature was 1700°C. The composite ceramic was obtained by cooling to room temperature.

[0033] When excited by a blue light LD chip with a wavelength of around 450nm, it emits high-brightness broadband yellow light around 540nm. When the input power is 5W, 20wt% SrAl2O4-Ce:LuAG does not show luminescence saturation, and the luminous flux can reach 1000 lm. Example

[0034] According to the chemical formula SrAl2O4-Ce:LuAG, SrAl2O4 accounts for 10% of the total mass of the ceramic raw materials. According to the stoichiometric ratio of the corresponding raw materials, 60g of Ce:LuAG with a purity of 99.99% and a particle size of 1.2 μm, 60g of SrAl2O4 with a purity of 99.99% and a particle size of 1.7 μm were weighed respectively. 4 6g of powder. Ce:LuAG powder and SrAl2O4 powder were blended, anhydrous ethanol was added, and the mixture was thoroughly mixed by ball milling. The resulting powder was dried in an oven at 90°C for 12 hours to obtain a dry powder. The dried powder was wrapped with graphite paper and then subjected to spark plasma sintering in a vacuum state at a sintering pressure of 80 MPa, a pulse current of 300 A, a sintering time of 40 minutes, and a sintering temperature of 1700°C. The mixture was cooled to room temperature to obtain a composite ceramic.

[0035] When excited by a blue light LD chip with a wavelength of around 450nm, it emits high-brightness broadband yellow light around 540nm. When the input power is 3.3W, the 10wt% SrAl2O4-Ce:LuAG reaches a maximum luminous flux of 600lm. Example

[0036] According to the chemical formula SrAl2O4-Ce:LuAG, SrAl2O4 accounts for 5% of the total mass of the ceramic raw materials. According to the stoichiometric ratio of the corresponding raw materials, 60g of Ce:LuAG with a purity of 99.99% and a particle size of 1.2 μm, 60g of SrAl2O4 with a purity of 99.99% and a particle size of 1.7 μm were weighed respectively.4 3g of powder. Ce:LuAG powder and SrAl2O4 powder were blended, anhydrous ethanol was added, and the mixture was thoroughly mixed by ball milling. The resulting powder was dried in an oven at 90°C for 12 hours to obtain a dry powder. The dried powder was wrapped with graphite paper and subjected to spark plasma sintering in a vacuum state at a sintering pressure of 80 MPa, a pulse current of 300 A, a sintering time of 40 minutes, and a sintering temperature of 1700°C. The composite ceramic was obtained by cooling to room temperature.

[0037] When excited by a blue light LD chip with a wavelength of around 450nm, it emits high-brightness broadband yellow light around 540nm. When the input power is 2.4W, the 5 wt% SrAl2O4-Ce:LuAG reaches a maximum luminous flux of 400lm.

[0038] Figure 1 is an XRD comparison chart of the sample SrAl2O4-Ce:LuAG prepared in Example 2 of the present invention, LuAG, and SrAl2O4; as shown in Figure 1, the diffraction peaks of the 20 wt% SrAl2O4-Ce:LuAG sample correspond well to the standard PDF cards of SrAl2O4 and LuAG, and no other impurities are produced, indicating that the sample has good crystallization performance.

[0039] FIG2 is an EL spectrum of the sample SrAl2O4-Ce:LuAG prepared in Example 2 of the present invention under excitation of a 450nm LD chip; when the input power is 5 W, the luminous flux reaches 1000 lm.

[0040] Figure 3 shows the relationship between the luminous flux and the input power of the LD chip for samples prepared in Examples 1 and 2 of the present invention, with SrAl2O4 accounting for 25% and 20% of the total ceramic raw material mass, as well as pure Ce:LuAG. As shown in Figure 3, compared to pure Ce:LuAG, the 20 wt% SrAl2O4-Ce:LuAG exhibits superior luminescence performance under blue LD excitation. At an input power of 5 W, the 20 wt% SrAl2O4-Ce:LuAG does not reach luminescence saturation, and its maximum luminous flux reaches 1000 lm.

[0041] Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if such changes and modifications fall within the scope of the claims and their equivalents, the present invention is intended to include such changes and modifications.

Claims

1. A high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting, characterized in that: The composite fluorescent ceramic is prepared by a spark plasma sintering method using Ce:LuAG powder and SrAl2O4 powder as ceramic raw material powders, wherein Ce:LuAG is used as the ceramic main body and SrAl2O4 is introduced as the second phase. The prepared composite fluorescent ceramic has high brightness and high luminous efficiency.

2. A method for preparing the high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: The following steps are involved: S1: Weigh Ce:LuAG powder and SrAl2O4 powder according to the mass ratio as ceramic raw material powders, wherein SrAl2O4 powder accounts for 5% to 25% of the total mass of the ceramic raw material powders; S2: Ce: LuAG powder and SrAl2O4 powder are blended and then anhydrous ethanol is added, and the mixture is fully mixed by ball milling; S3: taking out the slurry obtained after ball milling and drying it to obtain dry powder; S4: The dried powder is subjected to spark plasma sintering in a vacuum state, and then cooled to room temperature to obtain a composite fluorescent ceramic.

3. The method for preparing a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 2, characterized in that: In step S1, the particle size of the Ce:LuAG powder is 1 μm to 1.3 μm, the particle size of the SrAl2O4 powder is 1.5 μm to 2 μm, and the purity of both is above 99.99%.

4. The method for preparing a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 2, characterized in that: In step S2, the ball milling speed is 180-250 rpm, and the ball milling time is 15-30 h.

5. The method for preparing a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 2, characterized in that: In step S3, the drying temperature is 70-90° C. and the drying time is 8-12 hours.

6. The method for preparing a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 2, characterized in that: In step S4, the sintering pressure of the spark plasma sintering is 50-100 MPa, the pulse current is 200-400 A, the heat preservation sintering time is 20-50 min, and the sintering temperature is 1650° C.-1800° C.

Citation Information

Patent Citations

  • Ce:YAG based transparent ceramic being used for fluorescence conversion of white LED and containing Sr and preparation method thereof

    CN104177079A

  • Method for preparing multiphase translucent fluorescent ceramic and LED module

    CN107540368A

  • Fluorescent ceramic as well as preparation method and application thereof

    CN111995397A

  • Three-phase fluorescent ceramic with high thermal conductivity and high thermal stability for laser illumination and preparation method of three-phase fluorescent ceramic

    CN115215646A

  • High-brightness high-luminous-efficiency complex-phase fluorescent ceramic for laser illumination and preparation method of high-brightness high-luminous-efficiency complex-phase fluorescent ceramic

    CN116425544A