Wound cell and battery

By arranging active coatings with different diffusion coefficients on the negative electrode and positive electrode sheets of the wound battery core, the problems of lithium deposition and cycle capacity attenuation in the battery core are solved, and the service life of the battery is extended.

WO2024217210A1PCT designated stage expired Publication Date: 2024-10-24ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
PCT/CN2024/082418
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-03-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Due to the different circumferences of each turn of the wound battery core, the negative active material is unbalanced, resulting in lithium precipitation in the battery core and long-term cycle capacity attenuation, affecting the battery life.

Method used

A first active coating and a second active coating are respectively provided on both sides of the current collector of the negative electrode sheet and the positive electrode sheet. The first active coating is provided on the side of the current collector close to the curl center, and the second active coating is disposed on the side away from the curl center. On one side, the diffusion coefficient of the first active coating is smaller than that of the second active coating, which is controlled by adjusting parameters such as surface density, D50, aspect ratio, compacted density, and conductive agent content.

Benefits of technology

Effectively maintain long-term cycle battery capacity, improve lithium precipitation problems, and extend battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082418_24102024_PF_FP_ABST
    Figure CN2024082418_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A wound battery cell and a battery, relating to the technical field of batteries. A first active coating and a second active coating are respectively arranged on both sides of a current collector of a negative electrode sheet and / or a positive electrode sheet, the first active coating is arranged on the surface of the current collector close to one side of a rolling center, the second active coating is arranged on the surface of the side of the current collector away from the rolling center, and when the diffusion coefficient of the first active coating is smaller than that of the second active coating, the battery capacity during long-term cycle can be effectively kept, so that the problem of the second active coating being prone to lithium precipitation can be effectively solved, and the service life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Wound cells and batteries

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 17, 2023, with application number 202310407156.0 and application name “Wound Battery Cell and Battery”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of battery technology, and in particular to wound cells and batteries. Background Art

[0003] In recent years, with the continuous emergence of consumer electronic products such as smartphones, tablets, and electronic bracelets, and the rapid growth of the electric vehicle product market, lithium-ion batteries as the power source of these products have also received increasing attention. Among them, the service life of lithium-ion batteries is crucial.

[0004] For wound-structured battery cells, since the circumference of each circle of the wound battery cell is different, the negative electrode active materials corresponding to both sides of the surface arc near the center of the curl of the same folded negative electrode sheet are unbalanced, resulting in problems such as lithium plating in the battery cell and long-term cycle battery capacity attenuation, which seriously affects the battery life.

[0005] Therefore, it is necessary to provide a technical solution to the problems of lithium deposition and long-term cycle capacity attenuation in wound batteries.

[0006] Summary of the Invention

[0007] In view of this, the present invention provides a wound cell and a battery. The wound cell can effectively maintain the battery capacity over a long period of cycling, thereby improving the problem of lithium plating and extending the battery life.

[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0009] The present invention provides a wound battery cell, which includes a negative electrode sheet and / or a positive electrode sheet;

[0010] The negative electrode sheet includes a first negative electrode active coating, a current collector, and a second negative electrode active coating arranged in sequence; the first negative electrode active coating is arranged on a surface of the current collector close to the curling center; the second negative electrode active coating is arranged on a surface of the current collector away from the curling center; the diffusion coefficient of the first negative electrode active coating is smaller than the diffusion coefficient of the second negative electrode active coating;

[0011] The positive electrode sheet includes a first positive electrode active coating, a current collector, and a second positive electrode active coating arranged in sequence; the first positive electrode active coating is arranged on the surface of the current collector close to the curling center; the second positive electrode active coating is arranged on the surface of the current collector away from the curling center; the diffusion coefficient of the first positive electrode active coating is smaller than the diffusion coefficient of the second positive electrode active coating.

[0012] Preferably, the diffusion coefficient of the first negative electrode active coating is 1×10 -9 ~3×10 -8 cm 2 / s;

[0013] As a preference, the diffusion coefficient of the second negative electrode active coating is 1×10 -8 ~1×10 -7 cm 2 / s;

[0014] Preferably, the diffusion coefficient of the first positive electrode active coating is 1×10 -9 ~2×10 -8 cm 2 / s;

[0015] As a preference, the diffusion coefficient of the second positive electrode active coating is 5×10 -8 ~1×10 -7 cm 2 / s.

[0016] In the embodiments provided by the present invention, the diffusion coefficient of the first negative electrode active coating layer is smaller than the diffusion coefficient of the second negative electrode active coating layer, which can be controlled by at least one of the following methods:

[0017] (1) The surface density of the first negative electrode active coating layer is greater than the surface density of the second negative electrode active coating layer;

[0018] (2) D of the active material in the first negative electrode active coating 50 Greater than the D of the active material in the second negative electrode active coating 50 ;

[0019] (3) the aspect ratio of the active material in the first negative electrode active coating is smaller than the aspect ratio of the active material in the second negative electrode active coating;

[0020] (4) The compaction density of the first negative electrode active coating is greater than the compaction density of the second negative electrode active coating;

[0021] (5) The conductive agent content of the first negative electrode active coating layer is less than the conductive agent content of the second negative electrode active coating layer;

[0022] (6) The thickness of the first negative electrode active coating layer is less than the thickness of the second negative electrode active coating layer;

[0023] (7) The conductive agents of the first negative electrode active coating and the second negative electrode active coating are both tubular conductive agents, and the length of the conductive agent tube wall of the first negative electrode active coating is shorter than the length of the conductive agent tube wall of the second negative electrode active coating;

[0024] The diffusion coefficient of the first positive electrode active coating layer is smaller than the diffusion coefficient of the second positive electrode active coating layer, which can be controlled by at least one of the following methods:

[0025] (1) The surface density of the first positive electrode active coating layer is greater than the surface density of the second positive electrode active coating layer;

[0026] (2) D of the active material in the first positive electrode active coating 50 Greater than the D of the active material in the second positive electrode active coating 50 ;

[0027] (3) the aspect ratio of the active material in the first positive electrode active coating layer is smaller than the aspect ratio of the active material in the second positive electrode active coating layer;

[0028] (4) The compaction density of the first positive electrode active coating layer is greater than the compaction density of the second positive electrode active coating layer;

[0029] (5) The conductive agent content of the first positive electrode active coating layer is less than the conductive agent content of the second positive electrode active coating layer;

[0030] (6) The thickness of the first positive electrode active coating layer is less than the thickness of the second positive electrode active coating layer;

[0031] (7) The conductive agents of the first positive electrode active coating layer and the second positive electrode active coating layer are both tubular conductive agents, and the length of the tube wall of the conductive agent of the first positive electrode active coating layer is shorter than the length of the tube wall of the conductive agent of the second positive electrode active coating layer.

[0032] Preferably, the components of the first negative electrode active coating or the second negative electrode active coating include, in parts by weight:

[0033] Negative electrode active material 75-99.8wt%;

[0034] Conductive agent 0.5-15wt%;

[0035] Binder 0.5~15wt%.

[0036] Preferably, in the first negative electrode active coating or the second negative electrode active coating,

[0037] The negative electrode active material is independently selected from one or more of carbon-based graphite materials, other carbon-based materials or silicon-carbon materials, and lithium titanate; the carbon-based graphite material is selected from at least one of natural graphite, artificial graphite, and mesophase carbon spheres; the other carbon-based materials are selected from at least one of hard carbon, soft carbon, and graphene;

[0038] The conductive agent is independently selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube, and graphene; the carbon black is selected from at least one of SP, Ketjen black, and acetylene black;

[0039] The binder is independently selected from one or more of polyvinylidene fluoride, polymethyl methacrylate, polyvinyl alcohol, polytetrafluoroethylene, styrene-butadiene latex compounds, polyacrylate compounds, polyacrylonitrile, polytetrafluoroethylene, and polyethylene oxide.

[0040] Preferably, the components of the first positive electrode active coating or the second positive electrode active coating include, in parts by weight:

[0041] Positive electrode active material 75-99.8wt%;

[0042] Conductive agent 0.5-15wt%;

[0043] Binder 0.5~15wt%.

[0044] Preferably, in the first positive electrode active coating or the second positive electrode active coating,

[0045] The positive electrode active material is independently selected from one or more of lithium cobaltate, lithium iron phosphate, lithium manganese iron phosphate, sodium iron phosphate, lithium vanadium phosphate, sodium vanadium phosphate, lithium vanadium oxyphosphate, sodium vanadium oxyphosphate, lithium vanadate, lithium manganate, lithium nickelate, lithium nickel cobalt manganate, lithium-rich manganese-based materials or lithium nickel cobalt aluminum oxide;

[0046] The conductive agent is independently selected from one or more of conductive carbon black, Ketjen black, conductive fiber, conductive polymer, acetylene black, carbon nanotubes, graphene, flake graphite, conductive oxide, and metal particles;

[0047] The binder is independently selected from one or more of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, and styrene-butadiene rubber.

[0048] The types of the negative electrode active material, positive electrode active material, conductive agent, and binder are not limited thereto, and all types recognized by those skilled in the art are within the scope of protection of the present invention.

[0049] In the present invention, the first negative electrode active coating, the second negative electrode active coating, the first positive electrode active coating or the second positive electrode active coating may include, in addition to the above components, other functional components recognized in the art.

[0050] Preferably, the thickness of the first negative electrode active coating layer is 20 to 75 μm.

[0051] Preferably, the thickness of the second negative electrode active coating layer is 20 to 75 μm.

[0052] Preferably, the thickness of the first positive electrode active coating layer is 20 to 75 μm.

[0053] Preferably, the thickness of the second positive electrode active coating layer is 20 to 75 μm.

[0054] In the embodiment provided by the present invention, the current collector used for the negative electrode is selected from one or more of copper foil, carbon-coated copper foil, and perforated copper foil.

[0055] In the embodiment provided by the present invention, the current collector used for the positive electrode is selected from one or more of aluminum foil, carbon-coated aluminum foil, and perforated aluminum foil.

[0056] In the embodiment provided by the present invention, the wound battery cell may further include one or more of a positive electrode tab, a negative electrode tab, and a separator.

[0057] In some embodiments, the separator is selected from one or both of polyethylene and polypropylene.

[0058] In the embodiments provided by the present invention, the wound battery cell may be a conventional core structure, a tab-centered core structure, a tab-free core structure, a three-tab core structure, a multi-tab core structure, and the like.

[0059] The present invention also provides a battery, which includes the above-mentioned wound battery core.

[0060] According to an embodiment of the present invention, the battery further includes an electrolyte and / or a casing.

[0061] In some embodiments, the electrolyte is a non-aqueous electrolyte comprising a non-aqueous organic solvent and a lithium salt.

[0062] In some embodiments, the non-aqueous organic solvent is selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethylene carbonate, γ-butyrolactone, methylpropyl carbonate, and ethyl propionate.

[0063] In some embodiments, the lithium salt is selected from one or more of LiPF6, LiBF4, LiSbF6, LiClO4, LiCF3SO3, LiAlO4, LiAlCl4, Li(CF3SO2)2N, LiBOB and LiDFOB.

[0064] Compared with the prior art, the present invention has the following beneficial effects:

[0065] The present invention arranges a first active coating and a second active coating on both sides of the current collector of the negative electrode sheet and / or the positive electrode sheet, respectively. The first active coating is arranged on the surface of the current collector close to the curling center; the second active coating is arranged on the surface of the current collector away from the curling center. When the diffusion coefficient of the first active coating is smaller than the diffusion coefficient of the second active coating, the battery capacity of long-term cycle can be effectively maintained, the problem of easy lithium deposition of the second active coating can be effectively improved, and the service life of the battery can be extended. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] FIG1 is a schematic structural diagram of a negative electrode sheet provided in Examples 1-9 of the present invention;

[0067] FIG2 is a schematic structural diagram of a positive electrode sheet provided in Examples 1-9 of the present invention;

[0068] Figure 3 is a schematic diagram of a conventional winding core structure;

[0069] FIG4 is a schematic diagram of the structure of the winding core with the tab in the middle provided by Examples 1-9 of the present invention.

[0070] Description of reference numerals:

[0071] 1: negative electrode sheet; 1-1: negative electrode current collector; 1-2: first negative electrode active coating; 1-3: second negative electrode active coating;

[0072] 2: positive electrode sheet; 2-1: positive electrode current collector; 2-2: first positive electrode active coating; 2-3: second positive electrode active coating;

[0073] 3: positive electrode ear;

[0074] 4: negative electrode ear;

[0075] 5: Diaphragm. DETAILED DESCRIPTION

[0076] The present invention discloses wound cells and batteries. Those skilled in the art can refer to the contents herein and appropriately modify the process parameters to achieve the desired results. It is particularly important to note that all similar substitutions and modifications obvious to those skilled in the art are considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments. It is obvious that those skilled in the art can modify or appropriately alter and combine the methods and applications described herein to implement and apply the technology of the present invention without departing from the content, spirit, and scope of the present invention.

[0077] Explanation of terms:

[0078] The ion diffusion rate refers to the degree to which lithium ions diffuse within a particular material. It can be measured using a galvanostatic intermittent titration technique (GITT) under charge / discharge conditions. For example, the GITT can be used to measure the lithium ion diffusion rate at a 50% state of charge (SOC).

[0079] Areal density: In engineering materials, it is the mass per unit area of ​​a substance of a specified thickness.

[0080] Aspect ratio: refers to the ratio of the longest diameter passing through the interior of the particle to the longest diameter perpendicular to it; in this application, the aspect ratio is the ratio of the longest axis length inside the active material particle to the length of the diameter perpendicular to it.

[0081] Compacted density: During the manufacturing process of lithium-ion power batteries, compacted density has a significant impact on battery performance. The calculation method is: compacted density = surface density / material thickness.

[0082] The chemical components and materials used in the present invention can be obtained through commercial channels.

[0083] The present invention will be further described below in conjunction with the embodiments:

[0084] Examples 1 to 9

[0085] 1. Structure and composition

[0086] The wound battery cell of this embodiment includes a wound negative electrode sheet 1 , a wound positive electrode sheet 2 , a positive electrode tab 3 , a negative electrode tab 4 , and a separator 5 .

[0087] (1) Negative electrode

[0088] As shown in Figure 1, the negative electrode sheet 1 includes a negative electrode current collector 1-1, a first negative electrode active coating 1-2 and a second negative electrode active coating 1-3; the first negative electrode active coating is arranged on the surface of the negative electrode current collector close to the curling center; the second negative electrode active coating is arranged on the surface of the negative electrode current collector away from the curling center.

[0089] The diffusion coefficient of the first negative electrode active coating is smaller than that of the second negative electrode active coating. The diffusion coefficient of the first negative electrode active coating is 1×10 -9 ~3×10 -8 cm 2 / s, and the diffusion coefficient of the second negative electrode active coating is 1×10 -8 ~1×10 -7 cm 2 s.

[0090] The first negative electrode active coating comprises: 96.5 wt% active material (artificial graphite), 1.5 wt% conductive agent (conductive carbon black), and 2 wt% binder (sodium carboxymethyl cellulose). 50 13~16μm, surface density 0.008~0.016g / cm 2 , compacted density 1.3~2.2g / cm 3 The aspect ratio is 0.6 to 1.5. The coating thickness is 50 to 60 μm, and the tube wall length is 14 to 16 nm.

[0091] The second negative electrode active coating comprises: 96.5 wt% active material (artificial graphite), 2.3 wt% conductive agent (conductive carbon black), and 1.2 wt% binder (sodium carboxymethyl cellulose). 50 10~13μm, surface density 0.004~0.007g / cm 2 , compacted density 0.5~1.0g / cm 3 , the aspect ratio is 4 to 5. The coating thickness is 70 to 75 μm, and the tube wall length is 22 to 23 nm.

[0092] (2) Positive electrode

[0093] As shown in Figure 2, the positive electrode sheet 2 includes a positive electrode collector 2-1, a first positive electrode active coating 2-2 and a second positive electrode active coating 2-3; the first positive electrode active coating is arranged on the surface of the positive electrode collector close to the curling center; the second positive electrode active coating is arranged on the surface of the positive electrode collector away from the curling center.

[0094] The diffusion coefficient of the first positive electrode active coating is smaller than that of the second positive electrode active coating. The diffusion coefficient of the first positive electrode active coating is 1×10 -9 ~2×10 -8 cm 2 / s; the diffusion coefficient of the second positive electrode active coating is 5×10 -9 ~1×10 -7 cm 2 / s.

[0095] The first positive electrode active coating comprises: 97 wt% of active material (lithium cobalt oxide material), 1 wt% of conductive agent (acetylene black), and 2 wt% of binder (polyvinylidene fluoride). 50 15-17 μm, surface density 0.016-0.02 g / cm 2 , compacted density 3.2~4.0g / cm 3 , aspect ratio is 1 to 1.5. The coating thickness is 50 μm, and the tube wall length is 14 to 16 nm.

[0096] The second positive electrode active coating comprises: 97 wt% of active material (lithium cobalt oxide material), 1.8 wt% of conductive agent (acetylene black), and 1.2 wt% of binder (polyvinylidene fluoride). 50 14-16 μm, surface density 0.012-0.016 g / cm 2 , compacted density 1.8~2.5g / cm 3 , the aspect ratio is 3.5 to 5. The coating thickness is 65 μm, and the tube wall length is 22 to 23 nm.

[0097] 2. Preparation process

[0098] (1) 1 wt% acetylene black and 2 wt% polyvinylidene fluoride were added to 97 wt% lithium cobalt oxide, and then adjusted with N-methylpyrrolidone to form positive electrode slurry A. Acetylene black and polyvinylidene fluoride were added to lithium cobalt oxide, and then adjusted with N-methylpyrrolidone to form positive electrode slurry B. Positive electrode slurries A and B were applied to the surface of the current collector using a coating device, followed by drying, roller pressing, slitting, and sheeting to obtain positive electrode sheets.

[0099] (2) The negative electrode active material artificial graphite, the conductive agent conductive carbon black, and the binder sodium carboxymethyl cellulose were mixed in a ratio of (96.5wt%, 1.5wt%, 2wt%), and then deionized water was added to disperse the mixture to prepare a negative electrode slurry A with an appropriate solid content. The negative electrode active material artificial graphite, the conductive agent conductive carbon black, and the binder sodium carboxymethyl cellulose were mixed in a ratio of (96.5wt%, 2.3wt%, 1.2wt%), and then deionized water was added to disperse the mixture to prepare a negative electrode slurry B with an appropriate solid content. The negative electrode slurries A and B were then simultaneously coated on the negative electrode current collector using a coating device, and then dried, roller-pressed, slit, and sheeted to obtain a negative electrode sheet.

[0100] As shown in FIG3 , the wound battery cell of this embodiment has a conventional wound core structure.

[0101] This technical solution is also applicable to the tab-centered winding core structure (as shown in FIG4 ) and other winding core structures (such as tab-free winding core structure, three-tab winding core structure, multi-tab winding core structure, etc.).

[0102] Comparative Example 1

[0103] Similar to Example 1, except that: diffusion coefficient, D 50 , aspect ratio, cathode sheet formula and other parameters are different. Specific differences are shown in Table 1-1 and Table 1-2.

[0104] Comparative Example 2

[0105] Similar to Example 1, except that: diffusion coefficient, D 50 , aspect ratio, cathode sheet formula and other parameters are different. Specific differences are shown in Table 1-1 and Table 1-2.

[0106] Table 1-1

[0107] Table 1-2

[0108] Test Example 1 Cycle Life Test

[0109] The positive and negative electrodes of the battery cells of Examples 1-9 and Comparative Examples 1-2 were stacked together with a separator and wound into a core, which was then encapsulated with an aluminum-plastic film to form a battery cell. The cells were then subjected to processes such as liquid injection, aging, formation, and secondary packaging. Finally, the electrochemical properties of the lithium-ion batteries were tested.

[0110] The preparation method of the electrolyte includes: mixing propylene carbonate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a weight ratio of 1:1:0.5:1, and then adding LiPF6 to obtain the electrolyte, wherein the concentration of LiPF6 is 1 mol / L.

[0111] The cycle life and lithium deposition of the lithium-ion batteries prepared above were compared using the following test methods:

[0112] ① Cycle life: Charge at 3C rate to 4.4V, discharge at 1C rate for 500 cycles.

[0113] ② Lithium deposition test: fully charge at 5C, discharge at 0.5C, and dissect the battery cell after 20 charge and discharge cycles to check for lithium deposition.

[0114] The results are shown in Table 2.

[0115] Table 2

[0116] The results show that the capacity retention rates of Examples 1-9 after 500 cycles ranged from 91.25% to 92.60%, with no lithium deposition. The capacity retention rates of Comparative Examples 1-2 after 500 cycles were 85.1% and 82.7%, respectively, but lithium deposition did occur. It can be seen that the capacity retention rates of Examples 1-9 after 500 cycles were significantly improved, and no lithium deposition occurred.

[0117] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A wound battery cell, characterized in that: The wound battery cell includes a negative electrode sheet and / or a positive electrode sheet; The negative electrode sheet comprises a first negative electrode active coating, a current collector and a second negative electrode active coating arranged in sequence; the first negative electrode active coating is arranged on a surface of the current collector close to a curling center; the second negative electrode active coating is arranged on a surface of the current collector away from a curling center; the diffusion coefficient of the first negative electrode active coating is smaller than the diffusion coefficient of the second negative electrode active coating; The positive electrode sheet includes a first positive electrode active coating, a current collector and a second positive electrode active coating arranged in sequence; the first positive electrode active coating is arranged on the surface of the current collector close to the curling center; the second positive electrode active coating is arranged on the surface of the current collector away from the curling center; the diffusion coefficient of the first positive electrode active coating is not higher than the diffusion coefficient of the second positive electrode active coating.

2. The wound battery cell according to claim 1, characterized in that: The diffusion coefficient of the first positive electrode active coating layer is smaller than the diffusion coefficient of the second positive electrode active coating layer.

3. The wound battery cell according to claim 1 or 2, characterized in that: The diffusion coefficient of the first negative electrode active coating is 1×10 -9 ~3×10 -8 cm 2 / s; The diffusion coefficient of the second negative electrode active coating is 1×10 -8 ~1×10 -7 cm 2 / s; The diffusion coefficient of the first positive electrode active coating is 1×10 -9 ~2×10 -8 cm 2 / s; The diffusion coefficient of the second positive electrode active coating is 5×10 -8 ~1×10 -7 cm 2 / s.

4. The wound battery cell according to any one of claims 1 to 3, characterized in that: The diffusion coefficient of the first negative electrode active coating is smaller than the diffusion coefficient of the second negative electrode active coating, which is regulated by at least one of the following methods: (1) The surface density of the first negative electrode active coating is greater than the surface density of the second negative electrode active coating; (2) D of the active material in the first negative electrode active coating 50 Greater than the D of the active material in the second negative electrode active coating 50 ; (3) the aspect ratio of the active material in the first negative electrode active coating is smaller than the aspect ratio of the active material in the second negative electrode active coating; (4) The compaction density of the first negative electrode active coating is greater than the compaction density of the second negative electrode active coating; (5) The conductive agent content of the first negative electrode active coating is less than the conductive agent content of the second negative electrode active coating; (6) The thickness of the first negative electrode active coating is less than the thickness of the second negative electrode active coating; (7) The conductive agents of the first negative electrode active coating and the second negative electrode active coating are both tubular conductive agents, and the length of the tube wall of the conductive agent of the first negative electrode active coating is shorter than the length of the tube wall of the conductive agent of the second negative electrode active coating; The diffusion coefficient of the first positive electrode active coating is smaller than the diffusion coefficient of the second positive electrode active coating, which is regulated by at least one of the following methods: (1) The surface density of the first positive electrode active coating is greater than the surface density of the second positive electrode active coating; (2) D of the active material in the first positive electrode active coating 50 Greater than the D of the active material in the second positive electrode active coating 50 ; (3) the aspect ratio of the active material in the first positive electrode active coating is smaller than the aspect ratio of the active material in the second positive electrode active coating; (4) The compaction density of the first positive electrode active coating is greater than the compaction density of the second positive electrode active coating; (5) The conductive agent content of the first positive electrode active coating is less than the conductive agent content of the second positive electrode active coating; (6) The thickness of the first positive electrode active coating is less than the thickness of the second positive electrode active coating; (7) The conductive agents of the first positive electrode active coating and the second positive electrode active coating are both tubular conductive agents, and the length of the tube wall of the conductive agent of the first positive electrode active coating is shorter than the length of the tube wall of the conductive agent of the second positive electrode active coating.

5. The wound battery cell according to any one of claims 1 to 4, characterized in that: In parts by weight, the components of the first negative electrode active coating or the second negative electrode active coating include: Negative electrode active material 75-99.8wt%; Conductive agent 0.5-15wt%; Binder 0.5~15wt%.

6. The wound battery cell according to claim 5, characterized in that: In the first negative electrode active coating or the second negative electrode active coating, The negative electrode active material is independently selected from one or more of carbon-based graphite materials, other carbon-based materials or silicon-carbon materials, and lithium titanate; the carbon-based graphite material is selected from at least one of natural graphite, artificial graphite, and mesophase carbon spheres; the other carbon-based materials are selected from at least one of hard carbon, soft carbon, and graphene; The conductive agent is independently selected from carbon black, conductive graphite, carbon fiber, carbon nanotube, graphene One or more of; the carbon black is selected from at least one of SP, Ketjen black, and acetylene black; The binder is independently selected from one or more of polyvinylidene fluoride, polymethyl methacrylate, polyvinyl alcohol, polytetrafluoroethylene, styrene-butadiene latex compounds, polyacrylate compounds, polyacrylonitrile, polytetrafluoroethylene, and polyethylene oxide.

7. The wound battery cell according to any one of claims 1 to 6, characterized in that: In parts by weight, the components of the first positive electrode active coating or the second positive electrode active coating include: Positive electrode active material 75-99.8wt%; Conductive agent 0.5-15wt%; Binder 0.5~15wt%.

8. The wound battery cell according to claim 7, characterized in that: In the first positive electrode active coating or the second positive electrode active coating, The positive electrode active material is independently selected from one or more of lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate, sodium iron phosphate, lithium vanadium phosphate, sodium vanadium phosphate, lithium vanadium oxyphosphate, sodium vanadium oxyphosphate, lithium vanadate, lithium manganate, lithium nickel oxide, lithium nickel cobalt manganate, lithium-rich manganese-based materials or lithium nickel cobalt aluminum oxide; The conductive agent is independently selected from one or more of conductive carbon black, Ketjen black, conductive fiber, conductive polymer, acetylene black, carbon nanotubes, graphene, flake graphite, conductive oxide, and metal particles; The binder is independently selected from one or more of polyvinylidene fluoride, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, and styrene-butadiene rubber.

9. The wound battery cell according to any one of claims 1 to 8, characterized in that: The thickness of the first negative electrode active coating, the second negative electrode active coating, the first positive electrode active coating or the second positive electrode active coating is 20 to 75 μm.

10. A battery, characterized in that: The battery comprises the wound battery cell according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Lithium ion battery cathode and preparation method and application thereof and lithium ion battery

    CN111785923A

  • Negative plate and preparation method and application thereof

    CN112086620A

  • Lithium battery negative plate, wound battery cell and lithium ion battery

    CN112736217A

  • Negative plate and application thereof

    CN114242941A

  • Positive plate, preparation method thereof and battery comprising positive plate

    CN115588730A

Cited By

  • Negative pole piece, winding battery cell and lithium ion battery

    CN119361599A

  • Negative plate and battery

    CN119764325A

  • Negative electrode sheet, cylindrical battery, battery pack and electric tool

    WO2026103105A1