Ink for a fuel cell electrode, process for the preparation of such an ink and an electrode, and fuel cell having such an electrode
The novel ink composition for fuel cell catalytic layers, using a specific mixture of water, alcohol, and polyalkylene glycol, addresses the challenge of forming thin, continuous, and crack-free catalytic layers on fuel cell membranes, ensuring excellent adhesion and electrochemical performance for industrial-scale production.
Patent Information
- Application Number
- PCT/EP2024/060447
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-24
AI Technical Summary
The challenge in fuel cell technology is to deposit a thin, homogeneous, and continuous catalytic layer on a proton exchange membrane or gas diffusion layer without cracking and damaging the membrane, while ensuring good adhesion and electrochemical performance, particularly during industrial processes like slot die deposition.
A novel ink composition is developed, comprising a dispersion of ionomer and supported catalyst in a mixture of water, alcohol with a single hydroxyl function, and polyalkylene glycol devoid of terminal OH functions, which stabilizes the ionomer network, provides adequate viscosity, and prevents rapid evaporation, ensuring a stable, crack-free, and adherent catalytic layer formation.
The ink achieves a homogeneous and crack-free catalytic layer with excellent adhesion and electrochemical performance, suitable for industrial-scale production, including roll-to-roll processes, without flammability risks during manufacturing and drying.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
[0001] DESCRIPTION
[0002] TITLE: Ink for fuel cell electrode, method for preparing such an ink and an electrode, and fuel cell incorporating such an electrode
[0003] The present invention relates to an ink for forming a catalytic layer or electrode of a fuel cell membrane electrode (CCM) or membrane electrode assembly (MEA). The invention also relates to a method for preparing this ink. It further relates to the manufacture of a membrane electrode and a membrane electrode assembly of a fuel cell. It also relates to such a membrane electrode, such a membrane electrode assembly, and a fuel cell comprising at least one such electrode, such a membrane electrode, or such a membrane electrode assembly.
[0004] In the field of fuel cells, it is known to insert a stack of electrochemical cells between two end plates, located on either side of this stack in a stacking direction, and possibly to arrange this stack in a housing. Electrochemical cells are formed by membrane-electrode assemblies and bipolar plates. A membrane-electrode assembly is sometimes called MEA, from the English "Membrane-Electrode Assembly", and generally comprises a base membrane (or proton exchange membrane), which can be coated on one or both sides with a catalytic layer comprising a catalyst, as well as a frame which supports this membrane.The frame may include openings which, in the stack, define fluid flow galleries within the stack of electrochemical cells for the distribution and recovery of these fluids in the corresponding fluid compartments of each cell. This frame is most often associated with at least one seal, sometimes called a "gasket", with which it also provides a sealing function to the flow of fluids within the stack.
[0005] The membrane, when coated with catalytic layers comprising a catalyst, is sometimes called CCM, from the English "Catalyst Coated Membrane" and in this case comprises three layers, namely, a membrane itself, a catalytic layer on the anode side and a catalytic layer on the cathode side. In some cases, the CCM comprises the membrane and a catalytic layer.
[0006] In the stack, a membrane-electrode assembly is interposed between two bipolar plates and thus delimits, between the bipolar plates, an anodic compartment on one side of the membrane-electrode assembly, in which the oxidation of dihydrogen occurs, and a cathodic compartment on the other side, in which the reduction of dioxygen occurs. On each side, the catalyst-coated membrane can be covered by a gas diffusion layer which is therefore received in the corresponding anodic or cathodic compartment and promotes contact between the chemical species present in the corresponding anodic or cathodic compartment and the membrane. Each gas diffusion layer also has an electron conduction role. These diffusion layers are sometimes called GDL, from the English "Gas Diffusion Layer".
[0007] It is known to manufacture a membrane-electrode assembly by attaching the catalyst-coated membrane to the frame, which in particular makes it possible to stiffen this membrane and facilitate its handling. This is done by tightly gluing the membrane to the frame. Once this operation has been carried out, it is known to immobilize the diffusion layer(s) on the pre-assembled membrane and frame, during an additional operation, for example by a hot pressing operation and / or by means of an adhesive.
[0008] The MEA membrane-electrode assembly therefore comprises a base membrane which is a proton exchange polymer membrane and which is coated, as previously mentioned, with a catalytic layer, generally on each of its two faces. This base membrane is often made of a polymer material which is an ionomer, generally a perfluorosulfonated acid ionomer or perfluorosulfonic acid (PFSA), preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether such as NAFION™, which has a very low thickness, generally less than 0.1 mm, while the catalytic layers are made from an ionomer and a supported catalyst, typically platinum supported by carbon and also of very low thickness, typically less than 0.05 mm. The deposition of these catalytic layers on the base membrane requires the use of water and volatile organic solvents, and their evaporation to leave a dry layer.
[0009] Given the extreme thinness of both the base membrane and the catalytic layers, it is understood that the difficulty is to achieve the deposition of a thin and perfectly homogeneous or continuous catalytic layer both after deposition and after drying, without the appearance in particular of imperfections such as cracks, and without the constituents of the catalytic layers, in particular water and solvents, damaging the base membrane itself at the time of application or drying. The invention therefore aims to design an ink making it possible to form one or more catalytic layers fulfilling these objectives. Furthermore, it would be interesting to be able to apply an ink by industrial processes, for example using slot die deposition, and even making it possible to produce MEAs using a roll-to-roll process.The ink must be suitable for this type of deposition in order to obtain the extremely thin, homogeneous and continuous layer mentioned in the previous paragraph, with good adhesion to the support and good electrochemical properties.
[0010] Ideally, this ink could also be deposited on the base membrane as well as on a gas diffusion layer (GDL).
[0011] It is to these technical problems that the invention intends to address more particularly by proposing a new ink composition, its preparation process, and its method of implementation, making it possible to produce a stable dried ink layer, adhering to the support, homogeneous and without cracks, on the surface of a membrane or a GDL without damaging them, and having good electrochemical performances. Other objectives of the invention will appear in the remainder of the description.
[0012] To this end, the invention relates to an ink advantageously capable of forming an electrode on a proton exchange membrane or on a gas diffusion layer (GDL), intended to form a fuel cell MEA. This ink comprises a dispersion of ionomer and supported catalyst in the form of particles, in a mixture of water, an alcohol comprising a single hydroxyl function, carried by a carbon chain, the latter comprising or not one or more aromatic cycles, and a polyalkylene glycol devoid of terminal OH functions.
[0013] According to one embodiment, the invention relates to an ink capable of forming an electrode on a base membrane or a gas diffusion layer of a fuel cell, comprising a dispersion of ionomer and catalyst supported in a mixture of water, an alcohol comprising a single hydroxyl function, carried by a carbon chain, the latter comprising or not one or more aromatic cycles, and a polyalkylene glycol devoid of terminal OH functions and having a number-average molecular mass Mn of between 200 and 1000, preferably between 200 and 500.
[0014] According to one embodiment, the invention relates to an ink comprising a dispersion of ionomer and supported catalyst in the form of particles, in a mixture of water, an alcohol comprising a single hydroxyl function, carried by a carbon chain, the latter comprising or not one or more aromatic cycles, and a polyalkylene glycol devoid of terminal OH functions. According to one embodiment, said ink is suitable for forming an electrode on a proton exchange membrane or on a gas diffusion layer (GDL), and may be intended to form a fuel cell MEA.
[0015] Preferably, this polyalkylene glycol has a number average molecular weight / W n between 200 and 1000, preferably between 200 and 500.
[0016] According to one embodiment, said polyalkylene glycol has terminal groups of the ether type -OAlk where Alk represents a linear or branched alkyl group comprising from 1 to 6 carbon atoms, in particular methyl.
[0017] In particular, said polyalkylene glycol has the repetition of 2 to 35 -(O-alkyl)- units, preferably -(O-ethyl)-, on average.
[0018] According to one embodiment, the alcohol is chosen from alcohols comprising a hydroxyl function carried by a linear or branched alkyl chain comprising from 1 to 12 carbon atoms, in particular from 2 to 6 carbon atoms.
[0019] In particular, the alcohol comprising a single hydroxyl function has a boiling point between 75 and 130°C, preferably between 75 and 100°C. It is preferably 1-propanol (propan-1-ol), 2-propanol (propan-2-ol), or a mixture of the two.
[0020] In particular, the polyalkylene glycol is a polyalkylene glycol dialkyl ether. It is preferably chosen from: polyethylene glycol dimethyl ether
[0021] (PEGDME), polyethylene glycol diethyl ether, polyethylene glycol dipropyl ether, polyethylene glycol dibutyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol dimethyl ether, polypropylene glycol diglycidyl ether, polypropylene glycol / polyethylene glycol copolymer with dibutyl ether termination, polyethylene glycol / polypropylene glycol / polyethylene glycol block copolymer with dibutyl ether termination. This is preferably PEGDME. Preferably, the polyalkylene glycol selected from this list has a number average molecular weight M n between 200 and 1000, preferably between 200 and 500.
[0022] This number-average molecular mass is defined as the average of the molar masses of the polyalkylene glycol macromolecules weighted by their mole fraction. It can be measured in particular by size exclusion chromatography, including via the ISO 16014-5:2019 standard.
[0023] The solvent part (water, alcohol, polyalkylene glycol dialkyl ether) of the ink composition has several functions. It combines water, the majority constituent, with a low-boiling alcohol and a high-boiling solvent capable of producing a binding effect. It allows the ionomer to be dispersed in colloidal form, while maintaining contact between chains to allow the formation of an ionomer network, it induces an interaction between the ionomer and the catalyst, it stabilizes the dispersion. It allows the appropriate viscosity to be conferred for the method of application of the ink on the base membrane or the GDL. It provides an evaporation rate that is not too rapid. It prevents internal swelling of the base membrane, which typically includes an ionomer.
[0024] The presence of polyalkylene glycol devoid of OH functions, such as PEGDME, plays a decisive role in achieving the objectives set by the invention, through the combination of at least two factors. The first factor is the polymer status. The second is a high boiling point reducing its volatility under operating conditions. This polymer can then play a role as a binder in the catalytic layer both in the applied ink and in the dried ink layer, and therefore makes it possible to improve the homogeneity of this layer. Advantageously, the polymer and the ionomer can contribute together to this role of binder. In addition and very advantageously, the fact of not having OH groups reduces the risk of flammability during the ink manufacturing process, during its application and during the drying step.This produces an ink layer that has a very good affinity for the base membrane or for the GDL, with a good level of adhesion, and which has good homogeneity, notably with the absence of cracks. Indeed, and in particular on this last point, it is necessary to avoid drying the ink layer too quickly: the polyalkylene glycol advantageously guarantees, thanks to its high boiling point, for example by being preferably higher than 250°C, that it does not evaporate during drying, and thus ensures the homogeneity of the dried ink layer. In addition, to guarantee the homogeneity of the ink layer, and in particular the absence of cracks, it is also important to ensure the correct viscosity of the ink when applying it to the substrate (i.e.) the proton exchange membrane or the gas diffusion layer (GDL). The viscosity of the ink depends in particular on the viscosity of each of its components, including polyalkylene glycol.It is known that, in general, the viscosity of a polymer is directly related to the number-average molecular mass. However, the inventors have found that a number-average molecular mass Mn of the polyalkylene glycol of between 200 and 1000 makes it possible, in a quite remarkable manner, to obtain an optimal viscosity for the invention. More precisely, a number-average molecular mass Mn of the polyalkylene glycol of between 200 and 500 makes it possible to further reduce the viscosity of the ink and therefore to further improve the homogeneity of the ink layer.
[0025] This precision of the number-average molecular mass advantageously makes it possible to restrict the average length of a polyalkylene glycol macromolecule, and therefore to guarantee the occurrence of the anti-cracking effect of the polyalkylene glycol without limiting the nature of all the repeating units and of the terminal groups.
[0026] Indeed, the length of each macromolecule is influenced by the length of all the repeating units, as well as the length of the terminal groups. However, the number-average molecular mass is a parameter dependent on the length of all the repeating units, for identical terminal groups. The ionomer is involved in electrochemical reactions, allowing the transport of protons and water. It also plays a role as a binder in the ink, giving the catalytic layer formed from it a certain mechanical resistance and adhesion properties to the base membrane or to the GDL, which combine advantageously with the properties provided by the polyalkylene glycol devoid of OH functions.
[0027] In particular, the ionomer comprises or consists of a perfluorosulfonic acid or perfluorosulfonic acid (PESA) ionomer. It is notably formed from a polytetrafluoroethylene backbone bearing side chains terminated by sulfonic acid groups. The ionomer used is preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether. Mention may be made of Nation® and Aquivion®. These copolymers are known to be characterized by so-called long side chains (LSC for "long side chain"), an example being Nation®, or by so-called short side chains (SSC for "short side chain"), an example being Aquivion®. These PFSA ionomers are also defined by their equivalent weight or "Equivalent Weight" in English (EW), representing the ratio of grams of polymer / moles of sulfonate ("grams polymer / mole sulfonate"). The Nation® has a high EW, between 1000 and 1100; the Aquivion® has a low EW, between 720 and 790.
[0028] The catalyst comprises or consists of a noble metal, several noble metals or an alloy of noble metals. This metal, these metals or this alloy of metals is combined with a carbon support to form the catalyst.
[0029] The noble metal is selected in particular from: platinum (Pt), palladium (Pd), ruthenium (Ru), iridium (Ir), gold (Au), osmium (Os), rhodium (Rh), osmium (Os), tungsten (W), lead (Pb), iron (Fe), chromium (Cr), cobalt (Co), nickel (Ni), manganese (Mn), vanadium (V), molybdenum (Mo), gallium (Ga), aluminum (Al) or any other metal having catalytic activity. Alloys of two or more of these metals include platinum (Pt)-palladium (Pd) alloys, platinum (Pt)-ruthenium (Ru) alloys, platinum (Pt)-iridium (Ir) alloys, platinum (Pt)-osmium alloys, platinum (Pt)-M alloys (M being Ti, V, Cr, Mo, W, Mn, Fe, Co, Rh, Ni, Cu, Ag, Au, Zn, Ga and / or Sn) or a combination thereof. The noble metal or noble metal alloy is combined with a carbon support to form what is called the supported catalyst.The carbon support may comprise or consist of: carbon black, activated carbon, carbon powder, acetylene black, ketjen black, carbon nanotubes, carbon nanofibers, carbon nanohorns, carbon beads, carbon nanowires, carbon nanohorns, carbon aerogels, carbon crerogels or carbon nanorings, or a mixture of two or more of these.
[0030] Advantageously, the catalyst comprises or consists of a platinum-based catalyst supported on a carbon support. The catalyst may also comprise or consist, for example, of a platinum and cobalt alloy supported on a carbon support (PtCo / C).
[0031] In one embodiment, the platinum or the platinum and cobalt alloy is supported on carbon nanoparticles. These may be carbon nanoparticles with a high specific surface area, and the metal or alloy is essentially located on the surface of the nanoparticles. They may also be porous carbon nanoparticles, and the metal or alloy is found in whole or in part in the pores of the nanostructure. The support nanoparticles, in particular made of carbon, have a nanometric size which may be between 10 and 100 nm.
[0032] Noble metals, such as platinum or platinum-cobalt alloys, can be in the form of nanoparticles. These nanoparticles have a nanometric size that can be between 1 and 10 nm.
[0033] The mass proportions of the various ingredients in the ink according to the invention may be, relative to the total mass of the ink resulting from this mixture: from 55 to 70% of water, from 2 to 15% of polyalkylene glycol devoid of OH functions, from 7 to 20% of alcohol comprising a single hydroxyl function, from 2 to 8% of ionomer, and from 5 to 7% of supported catalyst. According to a preferred method, in particular when PEGDME is used as polyalkylene glycol devoid of OH functions, the following mass proportions are retained, relative to the total mass of the ink resulting from this mixture: from 61 to 69% of water, from 2 or 4 to 14% of polyalkylene glycol, from 7, 10 or 15 to 20% of alcohol, from 3 to 6% of ionomer, and from 5 to 7% of supported catalyst. More preferably, it is a mixture: 62 to 66% water, 5 to 11% polyalkylene glycol, 17 to 19% alcohol, 3 to 4% ionomer, and 5.5 to 6.5% supported catalyst.A typical example for PEGDME is: about 63.1% water, about 9% PEGDME, about 18% alcohol, about 3.7% ionomer, and about 6.2% supported catalyst. The invention also relates to a method for preparing an ink capable of forming an electrode on a fuel cell membrane, in particular an ink as mentioned above, comprising: forming a dispersion by mixing i. an ionomer or electrolyte polymer, ii. water, iii. an alcohol comprising a single hydroxyl function, carried by a carbon chain, the latter comprising or not one or more aromatic rings, and iv. a polyalkylene glycol devoid of terminal OH functions and having a number-average molecular weight Mn of between 200 and 1000, preferably between 200 and 500, v. a supported catalyst in the form of particles.
[0034] Preferably, this method comprises the following steps: a. Forming a first dispersion A by mixing i., ii., iii., and iv., b. Forming a second dispersion B by mixing ii., iii., iv., and v., alcohol iii. and polyalkylene glycol iv. which may be the same or different in dispersions A and B, c. Mixing the two dispersions A and B, stirring, and obtaining the ink in the form of a dispersion of the ionomer i. and the supported catalyst v. in the mixture of water ii., alcohol iii. and polyalkylene glycol iv.
[0035] The compounds entering into the composition of the ink and implemented in this method under i., ii., iii., iv., and v. have been defined previously in the description of the inks according to the invention.
[0036] The method uses in particular, as alcohol iii.: 1-propanol, 2-propanol, or a mixture of both, and / or as polyalkylene glycol iv.: polyethylene glycol dimethyl ether (PEGDME), and / or as ionomer i. a perfluorosulfonated acid or perfluorosulfonic acid (PFSA) ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether, and / or, as supported catalyst, carbon particles supporting platinum and / or cobalt.
[0037] According to a preferred method, in step a., the following mass proportions are used, relative to the total mass of dispersion A: from 55 to 70% of water, from 2 to 15% of polyalkylene glycol iv., from 10 to 35% of alcohol iii., and from 8 to 20% of ionomer i. According to an even more preferred method, in particular when PEGDME is used as ingredient iv., in step a., the following mass proportions are used, relative to the total mass of dispersion A: from 58 to 69% of water, from 2 to 14% of polyalkylene glycol iv., from 12 to 20% of alcohol iii., and from 8 to 17% of ionomer i. A typical example for PEGDME is: about 63.1% water, about 9.1% PEGDME iv., about 18% alcohol iii., and about 9.8% ionomer i.
[0038] According to a preferred method, in step b., the following mass proportions are used, relative to the total mass of dispersion B: from 55 to 70% of water, from 1 to 15% of polyalkylene glycol iv., from 15 to 25% of alcohol iii., and from 6 to 13% of supported catalyst v. According to an even more preferred method, in particular when PEGDME is used as ingredient iv., in step b., the following mass proportions are used, relative to the total mass of dispersion B: from 62-70% of water, from 5 to 11% of polyalkylene glycol iv., from 17 to 20% of alcohol iii., and from 8 to 11% of supported catalyst v. A typical example for PEGDME is: about 63.1% water, about 9% PEGDME iv., about 18% alcohol iii., and about 9.9% supported catalyst v.
[0039] According to a preferred method, in step c., dispersions A and B are mixed so as to obtain the following mass proportions, relative to the total mass of the ink resulting from this mixture: from 55 to 70% of water, from 2 to 15% of polyalkylene glycol iv., from 7 to 20% of alcohol iii., 2 to 8% of ionomer i. and from 5 to 7% of supported catalyst v. According to an even more preferred method, in particular when PEGDME is used as ingredient iv., the dispersions A and B are mixed so as to obtain the following mass proportions, relative to the total mass of the ink resulting from this mixture: from 61 to 69% of water, from 2 or 4 to 14% of polyalkylene glycol iv., from 7, 10 or 15 to 20% of alcohol iii., from 3 to 6% of ionomer i. and from 5 to 7% of supported catalyst v. More preferably, it is a mixture: from 62 to 66% of water, from 5 to 11% of polyalkylene glycol, from 17 to 19% of alcohol, from 3 to 4% of ionomer, and from 5.5 to 6.5% of supported catalyst.A typical example for PEGDME is: about 63.1% water, about 9% PEGDME iv., about 18% alcohol iii., about 3.7% ionomer i. and about 6.2% supported catalyst v.
[0040] Each dispersion, and the mixing of dispersions A and B, can be carried out using a mechanical mixer, in particular a disperser, in particular an industrial disperser of the Ultra Turrax® type. The mixing can in particular be carried out at a temperature between 15 and 50°C.
[0041] The invention also relates to an ink obtained by implementing the preparation method described herein. This ink is capable of forming an electrode on a base membrane or a fuel cell GDL.
[0042] The invention also relates to a dried ink, capable in particular of constituting or constituting a catalytic layer or electrode on a base membrane or a GDL of a fuel cell, comprising an ionomer, a supported catalyst, and a polyalkylene glycol devoid of terminal OH functions. The latter has in particular a number-average molecular mass Mn of between 200 and 1000, preferably between 200 and 500.
[0043] This dried ink comprises in particular: a polyalkylene glycol dialkyl ether, preferably chosen from: polyethylene glycol dimethyl ether
[0044] (PEGDME), polyethylene glycol diethyl ether, polyethylene glycol dipropyl ether, polyethylene glycol dibutyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol dimethyl ether, polypropylene glycol diglycidyl ether, polypropylene glycol / polyethylene glycol copolymer with dibutyl ether termination, polyethylene glycol / polypropylene glycol / polyethylene glycol block copolymer with dibutyl ether termination, preferably PEGDME; and / or a perfluorosulfonic acid or perfluorosulfonic acid (PFSA) ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether; and / or a supported catalyst formed from carbon particles supporting platinum and / or cobalt.
[0045] The invention also relates to a membrane electrode which comprises a fuel cell base membrane. This membrane is a proton exchange polymer membrane, carrying on one or both of its faces a catalytic layer formed from an ink as described herein, dried, or a catalytic layer as obtained by implementing the method for forming such a layer as described herein. The base membrane comprises or is made of a polymer or ionomer material, in particular a perfluorosulfonated acid or perfluorosulfonic acid (PFSA) polymer or ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether such as NAFION® or Aquivion®.
[0046] More precisely, a first catalytic layer forms the cathode and a second catalytic layer forms the anode.
[0047] The catalytic layer(s) have a thickness of the order of 0.001 to 0.010 mm.
[0048] The catalytic layer(s) typically have a supported catalyst loading of about 0.1 to 0.5 mg / cm 2 .
[0049] The invention also relates to a membrane-electrode assembly which comprises a fuel cell base membrane, or proton exchange polymer membrane, carrying on one or both of its faces a catalytic layer formed from an ink as described here, dried, or a catalytic layer as obtained by implementing the method for forming such a layer as described here.
[0050] In particular, the base membrane comprises or is made of a polymeric material, in particular a perfluorosulfonic acid or perfluorosulfonic acid (PFSA) ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether such as NAFION®. The membrane thus coated can be held in a frame, thereby forming the membrane-electrode assembly.
[0051] More precisely, a first catalytic layer forms the cathode and a second catalytic layer forms the anode.
[0052] The catalytic layer(s) have a thickness of the order of 0.001 to 0.010 mm.
[0053] According to one feature, this base membrane comprises or is made of a polymeric material which is a perfluorosulfonic acid or perfluorosulfonic acid (PFSA) ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether such as NAFION™. It may in particular have a thickness of the order of 0.005 to 0.050 mm.
[0054] This base membrane may optionally be composed of several layers, one of which contains a perfluorosulfonic acid or perfluorosulfonic acid (PFSA) ionomer, alone or in association with one or more materials, of a polymeric nature or not.
[0055] A gas diffusion layer (GDL) is a porous, electrically conductive medium. It can be made of carbon fibers that are woven or knitted together, or are in the form of a nonwoven or matt textile. Depending on a characteristic, a GDL can be treated to give it an additional property, such as hydrophobicity, with a coating of a hydrophobic polymer (e.g., PTFE), loaded with carbon particles or fibers to maintain the electrically conductive character.
[0056] The invention then relates to a GDL carrying on one of its faces a catalytic layer formed from an ink as described here, dried, or a catalytic layer as obtained by implementing the method for forming such a layer as described here. The catalytic layer has a thickness of the order of 0.001 to 0.010 mm.
[0057] The invention therefore also relates to a membrane-electrode or a membrane-electrode assembly associating at least one base membrane carrying a catalytic layer according to the invention, and a GDL carrying a catalytic layer according to the invention. The base membrane carries a catalytic layer on a first face, the second face being devoid of it. The GDL carries a catalytic layer on a first face. It is via this face carrying the catalytic layer that the GDL is applied to the base membrane, on the second face of the latter, devoid of a catalytic layer.
[0058] The invention also relates to a fuel cell comprising several of these membrane-electrode or membrane-electrode assemblies. The invention also relates to a method for forming a catalytic layer on the surface of a base membrane or a GDL of a fuel cell, and, preferably, on a sheet from which base membranes or GDLs will then be cut to the required dimensions. It may be a large sheet usable in a roll-to-roll process, typically a sheet from a supply roll (or reel) passing through the coating station before being wound onto a receiving roll (or reel). It may also be a sheet of smaller dimensions, for a sheet-to-sheet process.
[0059] The catalytic layer is formed by coating, comprising the deposition of a layer of ink according to the invention, then drying it. The coating or deposition of the ink is preferably carried out by dispersion deposition techniques using application means allowing the deposition of the dispersion on the supports across the direction of advancement thereof. This can be carried out in particular using a slot die, a doctor blade or a bar coater. For double-sided coating, the sheet will be turned over to apply the ink in the same way to the opposite side. This will involve, for example, unwinding the sheet from the receiving roll, winding it onto another roll; then the sheet will be unwound again to apply the ink to the other side. The sheet coated with a catalytic layer on both sides will then be received on a receiving roll, before being cut to size.Traditionally, the sheet is covered with a backing film, particularly PET, which must therefore be removed before applying the ink.
[0060] The invention will be better understood and other advantages thereof will appear more clearly in light of the following description of embodiments of catalytic inks and their application to a base membrane for a fuel cell, given solely by way of example.
[0061] Example 1
[0062] Step 1. Dilution of the ionomer
[0063] 4.54 grams of ionomer (sold under the brand name Aquivion®) are introduced into a 50 milliliter bottle, along with 3.93 grams of deionized water, 2.10 grams of 1-propanol (Fisher, purity greater than 99%), and 1.05 grams of PEGDME (Sigma). This ionomer dilution is stirred by a magnetic stirrer for 1 hour.
[0064] Step 2. Dispersion of the catalyst
[0065] In a beaker, 2.47 grams of Pt / C catalyst (high surface area carbon) are mixed with 15.62 grams of deionized water and then mixed with a magnetic stirrer at room temperature. In a 150 milliliter beaker, 2.47 grams of Pt / C catalyst (high surface area carbon) are mixed with 15.62 grams of deionized water and then mixed with a magnetic stirrer at room temperature. With vigorous stirring, 4.44 grams of 1-propanol and 2.21 grams of PEGDME are added to the beaker. This dispersion containing the catalyst is stirred for 30 minutes at 1000 rpm by a dissolver.
[0066] Step 3. Preparing the ink
[0067] 11.05 grams of the ionomer dilution prepared in step 1 and 18.53 grams of the catalyst-containing dispersion prepared in step 2 are mixed in a 150 milliliter bottle for 30 minutes at 24,000 rpm by a rotor-stator mixer. The ink is then characterized by rheology to check if it is suitable for the deposition process. The rheological measurement consists of a viscosity measurement, at a shear rate between 0.01 and 1000 s -1 (per second) and at a temperature of 20°C. The ink has a shear-thinning behavior and has a viscosity of 1 pascal second for a shear rate of 1 s -1 (per second), measured at a temperature of 20°C.
[0068] Step 4. Depositing the ink
[0069] The ink is deposited onto a membrane (M775.15, Gore) using a bar coater. The desired amount of platinum is between 0.3 and 0.5 milligrams of platinum per square centimeter of membrane. To evaporate the solvent, the ink-coated membrane is heated to 40°C for several minutes.
[0070] Example 2
[0071] Step 1. Dilution of the ionomer
[0072] 30.3 grams of ionomer (sold under the brand name Aquivion®) are added to a 150 milliliter bottle, along with 26.4 grams of deionized water, 14.2 grams of 2-propanol (Fisher, purity greater than 99%), and 6.3 grams of PEGDME (Sigma). This ionomer dilution is stirred with a magnetic stirrer for 1 hour.
[0073] Step 2. Dispersion of the catalyst
[0074] In a 250 milliliter beaker, 12.7 grams of Pt / C (high surface area carbon) catalyst are mixed with 80.1 grams of deionized water and then mixed using a magnetic stirrer at room temperature. While stirring vigorously, 23.3 grams of 2-propanol and 10.3 grams of PEGDME are added to the beaker. This catalyst-containing dispersion is stirred for 15 minutes at 200 rpm using a propeller.
[0075] Step 3. Preparing the ink
[0076] 73.6 grams of the ionomer dilution prepared in step 1 and the entire catalyst-containing dispersion prepared in step 2 are mixed in a 250 milliliter bottle for 30 minutes at 15,000 rpm by a rotor-stator mixer. The ink is then characterized by rheology to check whether it is suitable for the deposition process. The rheological measurement consists of a viscosity measurement, at a shear rate between 0.01 and 1000 s-1 (per second) and at a temperature of 20°C. The ink has a shear-thinning behavior and has a viscosity of 1 pascal second for a shear rate of 1 s -1 (per second), measured at a temperature of 20°C.
[0077] Step 4. Depositing the ink
[0078] The ink is deposited onto a membrane (M775.15, Gore) using a bar coater. The desired amount of platinum is between 0.3 and 0.5 milligrams of platinum per square centimeter of membrane. To evaporate the solvent, the ink-coated membrane is heated to 40°C for several minutes.
[0079] Example 3
[0080] Step 1. Dilution of the ionomer
[0081] 30.4 grams of ionomer (sold under the brand name Aquivion®) are added to a 150 milliliter bottle, along with 27.9 grams of deionized water, 14.6 grams of 2-propanol (Fisher, purity greater than 99%), and 4.4 grams of PEGDME (Sigma). This ionomer dilution is stirred with a magnetic stirrer for 1 hour.
[0082] Step 2. Dispersion of the catalyst
[0083] In a 250 milliliter beaker, 12.7 grams of Pt / C (high surface area carbon) catalyst are mixed with 82.7 grams of deionized water and then mixed using a magnetic stirrer at room temperature. While stirring vigorously, 23.9 grams of 2-propanol and 7.2 grams of PEGDME are added to the beaker. This catalyst-containing dispersion is stirred for 15 minutes at 200 rpm using a propeller.
[0084] Step 3. Preparing the ink
[0085] 73.6 grams of the ionomer dilution prepared in step 1 and the entire catalyst-containing dispersion prepared in step 2 are mixed in a 250 milliliter bottle for 30 minutes at 15,000 rpm by a rotor-stator mixer. The ink is then characterized by rheology to check whether it is suitable for the deposition process. The rheological measurement consists of a viscosity measurement, at a shear rate between 0.01 and 1000 s -1 (per second) and at a temperature of 20°C. The ink has a shear-thinning behavior and has a viscosity of 1 pascal second for a shear rate of 1 s -1 (per second), measured at a temperature of 20°C.
[0086] Step 4. Ink Deposition The ink is deposited onto a membrane (M775.15, Gore) using a bar coater. The desired amount of platinum is between 0.3 and 0.5 milligrams of platinum per square centimeter of membrane. To evaporate the solvent, the ink-coated membrane is heated to 40°C for several minutes. Results:
[0087] In all 3 examples, the ink deposition was done on a membrane with a surface area of 36 cm 2 and drying did not raise any flammability issues. The appearance of the ink layers was observed with the naked eye; the surface appearance was homogeneous with little or no cracking. The electrochemical performance was satisfactory: > 0.65 V at 1 A / cm 2 .
Claims
CLAIMS 1. Ink capable of forming an electrode on a base membrane or a gas diffusion layer of a fuel cell, comprising a dispersion of ionomer and supported catalyst in the form of particles, in a mixture of water, an alcohol comprising a single hydroxyl function, carried by a carbon chain, the latter comprising or not one or more aromatic cycles, and a polyalkylene glycol devoid of terminal OH functions and having a number-average molecular mass Mn of between 200 and 1000, preferably between 200 and 500.
2. Ink according to claim 1, wherein: a. the alcohol has a boiling point of between 75 and 130°C, preferably between 75 and 100°C, and / or b. the polyalkylene glycol is a polyalkylene glycol dialkyl ether, preferably chosen from: polyethylene glycol dimethyl ether (PEGDME), polyethylene glycol diethyl ether, polyethylene glycol dipropyl ether, polyethylene glycol dibutyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol dimethyl ether, polypropylene glycol diglycidyl ether, polypropylene glycol / polyethylene glycol copolymer with dibutyl ether termination, polyethylene glycol / polypropylene glycol / polyethylene glycol block copolymer with dibutyl ether termination.
3. Ink according to claim 1 or 2, wherein: a. the alcohol iii. is 1-propanol, 2-propanol, or a mixture of the two, and / or b. the polyalkylene glycol iv. is polyethylene glycol dimethyl ether (PEGDME), and / or 4. An ink according to any one of claims 1 to 3, wherein: a. the ionomer i. comprises or consists of a perfluorosulfonated acid or perfluorosulfonic acid (PFSA) ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether, and / or b. the supported catalyst comprises carbon particles supporting platinum and / or cobalt.
5. Ink according to any one of claims 1 to 4, in which the mass proportions of the different ingredients are, relative to the total mass of the ink resulting from this mixture: from 55 to 70% water, from 2 to 15% polyalkylene glycol devoid of OH functions, from 7 to 20% alcohol comprising a single hydroxyl function, from 2 to 8% ionomer, and from 5 to 7% supported catalyst.
6. Method for preparing an ink capable of forming an electrode on a fuel cell membrane, comprising: forming a dispersion by mixing i. an ionomer, ii. water, iii. an alcohol comprising a single hydroxyl function, carried by a carbon chain, the latter comprising or not one or more aromatic cycles, and iv. a polyalkylene glycol devoid of terminal OH functions and having a number-average molecular mass Mn of between 200 and 1000, preferably between 200 and 500, v. a supported catalyst.
7. A method according to claim 6, comprising a. forming a first dispersion A by mixing i., ii., iii., and iv., b. forming a second dispersion B of ii., iii., iv., and v., alcohol iii. and polyalkylene glycol iv. which may be the same or different in dispersions A and B, c. mixing the two dispersions, stirring, and obtaining the ink in the form of a dispersion of the ionomer i. and the supported catalyst v. in the mixture of water ii., alcohol iii. and polyalkylene glycol iv.
8. Method according to claim 6 or 7, wherein: a. the alcohol iii. has a boiling point between 75 and 130 °C, preferably between 75 and 100 °C, and / or b. the polyalkylene glycol iv. is a polyalkylene glycol dialkyl ether, preferably chosen from: polyethylene glycol dimethyl ether (PEGDME), polyethylene glycol diethyl ether, polyethylene glycol dipropyl ether, polyethylene glycol dibutyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol dimethyl ether, polypropylene glycol dibutyl ether, polypropylene glycol / polyethylene glycol copolymer with dibutyl ether termination, polyethylene glycol / polypropylene glycol / polyethylene glycol block copolymer with dibutyl ether termination.
9. A method according to any one of claims 6 to 8, wherein: a. the alcohol iii. is 1-propanol, 2-propanol, or a mixture of both, and / or b. the polyalkylene glycol iv. is polyethylene glycol dimethyl ether (PEGDME).
10. A method according to any one of claims 6 to 9, wherein: a. the ionomer i. comprises or consists of a perfluorosulfonated acid or perfluorosulfonic acid (PESA) ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether, and / or b. the supported catalyst comprises carbon particles supporting platinum and / or cobalt.
11. Method according to any one of claims 6 to 10, in which, in step a., the following mass proportions are used, relative to the total mass of dispersion A: from 55 to 70% of water, from 2 to 15% of polyalkylene glycol iv., from 10 to 35% of alcohol iii., and from 8 to 20% of ionomer i.
12. Method according to any one of claims 6 to 11, in which, in step b., the following mass proportions are used, relative to the total mass of dispersion B: from 55 to 70% of water, from 1 to 15% of polyalkylene glycol iv., from 15 to 25% of alcohol iii., and from 6 to 13% of supported catalyst v.
13. Method according to any one of claims 6 to 12, in which, in step c., the dispersions A and B are mixed so as to obtain the following mass proportions, relative to the total mass of the ink resulting from this mixture: from 55 to 70% of water, from 2 to 15% of polyalkylene glycol iv., from 7 to 20% of alcohol iii., and from 2 to 8% of ionomer i. and from 5 to 7% of supported catalyst v.
14. Ink capable of forming an electrode on a base membrane or a fuel cell gas diffusion layer, obtained by implementing the method according to any one of claims 6 to 13.
15. Dried ink capable of constituting or constituting a catalytic layer or electrode on a fuel cell membrane, comprising a ionomer, a supported catalyst, and a polyalkylene glycol devoid of terminal OH functions and having a number-average molecular weight Mn of between 200 and 1000, preferably between 200 and 500.
16. Dried ink according to claim 15, wherein: a. the polyalkylene glycol is a polyalkylene glycol dialkyl ether, preferably selected from: polyethylene glycol dimethyl ether (PEGDME), polyethylene glycol diethyl ether, polyethylene glycol dipropyl ether, polyethylene glycol dibutyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol dimethyl ether, polypropylene glycol diglycidyl ether, polypropylene glycol / polyethylene glycol copolymer with dibutyl ether termination, polyethylene glycol / polypropylene glycol / polyethylene glycol block copolymer with dibutyl ether termination, preferably it is PEGDME, and / or b. the ionomer i. comprises or consists of a perfluorosulfonated acid or perfluorosulfonic acid (PFSA) ionomer, preferably a copolymer of tetrafluoroethylene and sulfonyl fluoride vinyl ether, and / or c. the supported catalyst comprises carbon particles supporting platinum and / or cobalt.
17. A method of forming a catalytic layer on the surface of a base membrane or a fuel cell gas diffusion layer, comprising depositing an ink layer according to any one of claims 1 to 5, on this surface using a slot die, a doctor blade or a bar coating machine, preferably in a roll-to-roll process.
18. Fuel cell membrane electrode or membrane electrode assembly, which comprises a fuel cell membrane carrying on one or both of its faces a catalytic layer formed from a dried ink according to claim 15 or 16, or a catalytic layer as obtained by applying and drying an ink according to any one of claims 1 to 5 and 14.
19. Fuel cell membrane electrode or membrane electrode assembly, further comprising a gas diffusion layer carrying on one side a catalytic layer formed from a dried ink according to claim 15 or 16, or a catalytic layer as obtained by application and drying of an ink according to any one of claims 1 to 5 and 14.
20. Fuel cell comprising a membrane electrode or a membrane electrode assembly according to claim 18 or 19.
Citation Information
Patent Citations
Inkjet ink for forming catalyst layer for fuel cell, catalyst layer for fuel cell and its manufacturing method, and catalyst layer-electrolyte film laminate
JP2010086674A
Electrode catalyst dispersion and ink composition
US20110262828A1
Catalyst ink for forming electrode catalyst layer and method of producing membrane electrode assembly
US20220302465A1