Gallium arsenide single crystal substrate and method for producing same

The novel cleaning method for gallium arsenide single crystal substrates, involving alkaline and acid treatments, effectively addresses the issue of incomplete oxide film removal, resulting in substrates with high specularity and reduced haze values, thereby improving epitaxial film quality.

WO2024218823A1PCT designated stage expired Publication Date: 2024-10-24SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/015310
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current methods for producing gallium arsenide single crystal substrates fail to achieve high specularity surfaces, leading to increased haze values in epitaxial films due to incomplete removal of oxide films, which affects device characteristics.

Method used

A novel cleaning method involving alkaline and acid treatments, followed by a second alkaline cleaning and heat treatment, is employed to create a gallium-rich oxide film with improved wettability, allowing for effective wet etching and reduced haze values in epitaxial films.

Benefits of technology

The method results in gallium arsenide single crystal substrates with high specularity surfaces and reduced haze values in epitaxial films, enhancing device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023015310_24102024_PF_FP_ABST
    Figure JP2023015310_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This gallium arsenide single crystal substrate has a main surface having a circular shape, and has a first integrated intensity ratio, a second integrated intensity ratio, a third integrated intensity ratio, a fourth integrated intensity ratio, and a fifth integrated intensity ratio. The second integrated intensity ratio is 0.9-1.05, the third integrated intensity ratio and the fourth integrated intensity ratio are not greater than 1.0, the fifth integrated intensity ratio is not greater than 0.8, and the ratio of the first integrated intensity ratio to the second integrated intensity ratio is 0.5-1.
Need to check novelty before this filing date? Find Prior Art

Description

Gallium arsenide single crystal substrate and method for manufacturing same

[0001] The present disclosure relates to gallium arsenide single crystal substrates and methods for manufacturing the same.

[0002] Japanese Patent Laid-Open Publication No. 06-045318 (Patent Document 1) proposes a gallium arsenide single crystal substrate (hereinafter also referred to as "GaAs single crystal substrate") that enables thermal cleaning, an operation for removing oxide films, to be performed at low temperatures and in a short time. It is said that this can be achieved by artificially forming an As-rich interfacial transition layer with a thickness of 3 Å or less on the surface of the GaAs single crystal substrate. Japanese Patent Laid-Open Publication No. 2008-300747 (Patent Document 2) proposes providing a GaAs wafer that is clean enough to remove impurities and oxides on the surface by at least thermally cleaning the surface of the GaAs single crystal substrate.

[0003] Japanese Patent Laid-Open No. 06-045318 Japanese Patent Laid-Open No. 2008-300747

[0004] A gallium arsenide single crystal substrate according to the present disclosure is a gallium arsenide single crystal substrate having a circular main surface. The gallium arsenide single crystal substrate has first, second, third, fourth, and fifth integrated intensity ratios. The first and third integrated intensity ratios are obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate, based on X-ray photoelectron spectroscopy, in which X-rays are irradiated onto the center of the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 30°. The second and fifth integrated intensity ratios are obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted to the outside of the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°. The fourth integrated intensity ratio is obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted to the outside of the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 45°. The first integrated intensity ratio and the second integrated intensity ratio are ratios of the sum of the integrated intensities of elemental arsenic present as diarsenic pentoxide, diarsenic trioxide, gallium arsenide, and metallic arsenic to the sum of the integrated intensities of elemental gallium present as digallium monoxide, digallium trioxide, and gallium arsenide. The third integrated intensity ratio, the fourth integrated intensity ratio, and the fifth integrated intensity ratio are ratios of the sum of the integrated intensities of elemental arsenic present as diarsenic pentoxide and diarsenic trioxide to the sum of the integrated intensities of elemental gallium present as digallium monoxide and gallium trioxide.The second integrated intensity ratio is 0.9 or more and 1.05 or less. The third integrated intensity ratio and the fourth integrated intensity ratio are 1.0 or less. The fifth integrated intensity ratio is 0.8 or less. A ratio of the first integrated intensity ratio to the second integrated intensity ratio is 0.5 or more and 1 or less.

[0005] A method for producing a gallium arsenide single crystal substrate according to the present disclosure is a method for producing a gallium arsenide single crystal substrate having a circular major surface, the method comprising the steps of: preparing a gallium arsenide single crystal substrate precursor having a circular surface; and cleaning the gallium arsenide single crystal substrate precursor to obtain the gallium arsenide single crystal substrate. The cleaning step includes the steps of: polishing the surface of the gallium arsenide single crystal substrate precursor to form the polished surface; cleaning the polished surface with a first alkaline cleaning solution to form the polished surface as an alkali-cleaned surface; cleaning the alkali-cleaned surface with an acid cleaning solution containing 0.3 mass ppm to 0.5 mass % acid to form the alkali-cleaned surface as an acid-cleaned surface; rotating the acid-cleaned surface in a circumferential direction at a rotation speed of 1000 rpm or more, while supplying a second alkaline cleaning solution to the acid-cleaned surface at a flow rate of 0.1 L / min to 5 L / min for 30 seconds to 5 minutes to clean the acid-cleaned surface and form the acid-cleaned surface into a second alkaline-cleaned surface; and heat-treating the second alkaline-cleaned surface in an inert gas atmosphere under conditions of 1.1 atmospheres to 3 atmospheres and 150°C to 300°C to form the second alkaline-cleaned surface into the main surface. The first alkaline cleaning solution contains 0.1 mass % to 10 mass % of a first base. The first base contains at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide. The second alkaline cleaning solution contains 0.3 mass ppm to 0.5 mass % of a second base. The second base contains at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide.

[0006] FIG. 1 is an example of a graph showing the relationship between the measurement depth from the main surface of a GaAs single crystal substrate according to this embodiment (horizontal axis), the ratio of the integrated intensity of all arsenic elements to the integrated intensity of all gallium elements (vertical axis), and the ratio of the integrated intensity of arsenic elements present as arsenic oxides to the integrated intensity of gallium elements present as gallium oxides (vertical axis). FIG. 2 is an explanatory diagram schematically illustrating the configuration of an analysis system using X-ray photoelectron spectroscopy (XPS). FIG. 3A is a graph showing an example of a background-corrected Ga 3d spectrum obtained based on XPS in which X-rays are irradiated onto the center of the main surface of a GaAs single crystal substrate according to this embodiment. FIG. 3B is a graph showing an example of a background-corrected As 3d spectrum obtained based on XPS in which X-rays are irradiated onto the center of the main surface of a GaAs single crystal substrate according to this embodiment. Fig. 4 is an explanatory diagram illustrating five measurement points set on a GaAs single crystal substrate having a diameter of 75 mm or more and less than 150 mm in this embodiment. Fig. 5 is an explanatory diagram illustrating nine measurement points set on a GaAs single crystal substrate having a diameter of 150 mm or more and 205 mm or less in this embodiment. Fig. 6 is a flow chart showing a method for manufacturing a GaAs single crystal substrate according to this embodiment.

[0007] [Problem to be Solved by the Present Disclosure] Haze is one method for evaluating the specularity (i.e., the presence or absence of steps) of the surface of an epitaxial film, and it is known that an increase in this value correlates with a decrease in device characteristics. Haze refers to the amount of scattered light caused by surface irregularities and minute defects and foreign particles present on the surface when a laser beam is irradiated onto the surface of an epitaxial film. Haze is expressed as the ratio of the amount of scattered light to the amount of laser light incident on the surface. Haze is expressed in parts per million (ppm). The smaller the haze value, the more specular the surface is and the fewer steps there are. These steps are derived from stacking faults that occur, for example, when an epitaxial film is grown on a GaAs single crystal substrate. Because these stacking faults depend on the specularity of the main surface of the GaAs single crystal substrate, there is a demand for reducing the haze value by realizing GaAs single crystal substrates with highly specular main surfaces.

[0008] In addition to the thermal cleaning described above, wet etching is known as a method for removing oxide films from the main surfaces to obtain GaAs single crystal substrates with highly specular main surfaces. Wet etching involves removing oxide films from the main surfaces using a sulfuric acid-based aqueous solution containing sulfuric acid and hydrogen peroxide, or an NH4OH-based aqueous solution containing ammonium hydroxide and hydrogen peroxide. However, due to poor wettability, the oxide films are sometimes not sufficiently removed by wet etching. In such cases, GaAs single crystal substrates with sufficiently specular main surfaces cannot be obtained, and the haze value of epitaxial films grown on the main surfaces is also difficult to sufficiently reduce.

[0009] In view of the above, an object of the present disclosure is to provide a gallium arsenide single crystal substrate and a method for manufacturing the same that enable the formation of an epitaxial film with a reduced haze value, thereby improving device characteristics.

[0010] [Effects of the Present Disclosure] According to the present disclosure, it is possible to provide a gallium arsenide single crystal substrate and a method for manufacturing the same that can improve device characteristics by enabling the formation of an epitaxial film with a reduced haze value.

[0011] [Summary of the Embodiments] First, an overview of the embodiments of the present disclosure will be described. The present inventors have conducted extensive research to solve the above-mentioned problems and have completed the present disclosure. That is, the present inventors have focused on obtaining a highly specular main surface of a gallium arsenide single crystal substrate by performing a novel cleaning method on a gallium arsenide single crystal substrate precursor having a circular surface cut from a gallium arsenide single crystal. Specifically, in addition to performing both conventionally known liquid-phase treatments, namely, alkaline cleaning with an alkaline solution and acid cleaning with an acidic solution, a second alkaline cleaning and a heat treatment were newly performed. As a result, it was discovered that the wettability of the oxide film of a GaAs single crystal substrate obtained by the above-mentioned novel cleaning method is improved when the oxide film has a composition that is richer in gallium than arsenic overall and this tendency is maintained up to the interface between the oxide film and the GaAs single crystal constituting the gallium arsenide single crystal substrate. This allows a GaAs single crystal substrate having a highly specular main surface to be obtained by wet etching, thereby achieving a GaAs single crystal substrate on which an epitaxial film with a reduced haze value can be formed, thereby completing the present disclosure.

[0012] Next, embodiments of the present disclosure will be described. [1] A gallium arsenide single crystal substrate according to one aspect of the present disclosure is a gallium arsenide single crystal substrate having a circular main surface. The gallium arsenide single crystal substrate has a first integrated intensity ratio, a second integrated intensity ratio, a third integrated intensity ratio, a fourth integrated intensity ratio, and a fifth integrated intensity ratio. The first integrated intensity ratio and the third integrated intensity ratio are obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy, in which X-rays are irradiated onto the center of the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 30°. The second and fifth integrated intensity ratios are obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted to the outside of the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°. The fourth integrated intensity ratio is obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted to the outside of the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 45°. The first integrated intensity ratio and the second integrated intensity ratio are ratios of the sum of the integrated intensity of elemental arsenic present as diarsenic pentoxide, the integrated intensity of elemental arsenic present as diarsenic trioxide, the integrated intensity of elemental arsenic present as gallium arsenide, and the integrated intensity of elemental arsenic present as metallic arsenic to the sum of the integrated intensity of elemental gallium present as digallium monoxide, the integrated intensity of elemental gallium present as digallium trioxide, and the integrated intensity of elemental gallium present as gallium arsenide.The third integrated intensity ratio, the fourth integrated intensity ratio, and the fifth integrated intensity ratio are ratios of the sum of the integrated intensity of the arsenic element present as diarsenic pentoxide and the integrated intensity of the arsenic element present as diarsenic trioxide to the sum of the integrated intensity of the gallium element present as digallium monoxide and the integrated intensity of the gallium element present as digallium trioxide. The second integrated intensity ratio is 0.9 or more and 1.05 or less. The third integrated intensity ratio and the fourth integrated intensity ratio are 1.0 or less. The fifth integrated intensity ratio is 0.8 or less. The ratio of the first integrated intensity ratio to the second integrated intensity ratio is 0.5 or more and 1 or less.

[0013] A gallium arsenide single crystal substrate having such characteristics can have the oxide film effectively removed by wet etching and has a main surface with high specularity, making it possible to form an epitaxial film with a reduced haze value.

[0014] [2] The second integrated intensity ratio is preferably equal to or greater than 0.9 and less than 1.04, which allows the oxide film to be removed more effectively by wet etching.

[0015] [3] The gallium arsenide single crystal substrate preferably has an oxide film on the main surface thereof having a thickness of 2 nm or less, which allows the oxide film to be more effectively removed by wet etching.

[0016] [4] The contact angle of the oxide film is preferably 20 degrees or less, so that the oxide film with good wettability can be more effectively removed by wet etching.

[0017] [5] The gallium arsenide single crystal substrate preferably has a diameter of 75 mm or more and 205 mm or less. This allows the gallium arsenide single crystal substrate having a diameter of 75 mm or more and 205 mm or less to have a main surface with high specularity, thereby enabling the formation of an epitaxial film with a reduced haze value.

[0018] [6] The gallium arsenide single crystal substrate preferably has the following characteristics. The gallium arsenide single crystal substrate has a diameter of 75 mm or more and less than 150 mm. The gallium arsenide single crystal substrate has a sixth integrated intensity ratio and a seventh integrated intensity ratio. The sixth integrated intensity ratio and the seventh integrated intensity ratio are obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which X-rays are irradiated onto five measurement points on the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°. The sixth integrated intensity ratio is the ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentoxide, the integrated intensity of the arsenic element present as diarsenic trioxide, the integrated intensity of the arsenic element present as gallium arsenide, and the integrated intensity of the arsenic element present as metallic arsenic to the sum of the integrated intensity of the gallium element present as digallium monoxide, the integrated intensity of the gallium element present as digallium trioxide, and the integrated intensity of the gallium element present as gallium arsenide. The seventh integrated intensity ratio is the ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentoxide and the integrated intensity of the arsenic element present as diarsenic trioxide to the sum of the integrated intensity of the gallium element present as digallium monoxide and the integrated intensity of the gallium element present as digallium trioxide. The standard deviation and average value of the ratio of the seventh integrated intensity ratio to the sixth integrated intensity ratio satisfy the relationship of standard deviation / average value ≦ 0.039. When the diameter is represented by D and two mutually orthogonal axes on the main surface that pass through the center of the main surface are represented by the X and Y axes, the X- and Y-axis coordinates (X, Y) of the five measurement points are (0, 0), (D / 4, 0), (0, D / 4), (-D / 4, 0), and (0, -D / 4). The units of D and X and Y in the coordinates (X, Y) are mm. As a result, in a gallium arsenide single crystal substrate having a diameter of 75 mm or more and less than 150 mm, by effectively removing the oxide film using wet etching, a main surface with high specularity and no in-plane variation can be obtained, thereby enabling the formation of an epitaxial film with a reduced haze value.

[0019] [7] The gallium arsenide single crystal substrate preferably has the following characteristics. The gallium arsenide single crystal substrate has a diameter of 150 mm or more and 205 mm or less. The gallium arsenide single crystal substrate has an eighth integrated intensity ratio and a ninth integrated intensity ratio. The eighth integrated intensity ratio and the ninth integrated intensity ratio are obtained by determining a spectrum of the detected intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which X-rays are irradiated onto nine measurement points on the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°. The eighth integrated intensity ratio is the ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentoxide, the integrated intensity of the arsenic element present as diarsenic trioxide, the integrated intensity of the arsenic element present as gallium arsenide, and the integrated intensity of the arsenic element present as metallic arsenic to the sum of the integrated intensity of the gallium element present as digallium monoxide, the integrated intensity of the gallium element present as digallium trioxide, and the integrated intensity of the gallium element present as gallium arsenide. The ninth integrated intensity ratio is the ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentoxide and the integrated intensity of the arsenic element present as diarsenic trioxide to the sum of the integrated intensity of the gallium element present as digallium monoxide and the integrated intensity of the gallium element present as digallium trioxide. The standard deviation and mean value of the ratio of the ninth integrated intensity ratio to the eighth integrated intensity ratio satisfy the relationship: standard deviation / mean value≦0.022. When the diameter is represented by D and two axes passing through the center of the main surface and perpendicular to each other on the main surface are represented by the X and Y axes, the X- and Y-axis coordinates (X, Y) of the nine measurement points are (0, 0), (D / 4, 0), (0, D / 4), (-D / 4, 0), (0, -D / 4), (D / 2-10, 0), (0, D / 2-10), (-(D / 2-10), 0), and (0, -(D / 2-10)). The units of D and X and Y in the coordinates (X, Y) are mm.As a result, in a gallium arsenide single crystal substrate having a diameter of 150 mm or more and 205 mm or less, by effectively removing the oxide film using wet etching, it is possible to obtain a main surface with high specularity without in-plane variation, and thereby form an epitaxial film with a reduced haze value.

[0020] [8] The gallium arsenide single crystal substrate preferably has an epitaxial film on the main surface, the maximum haze of the surface of the epitaxial film being 100 ppm or less, and the average haze of the surface of the epitaxial film being 2.5 ppm or less. This makes it possible to provide a gallium arsenide single crystal substrate having an epitaxial film with a reduced haze value formed on the main surface.

[0021] [9] A method for producing a gallium arsenide single crystal substrate according to one aspect of the present disclosure is a method for producing a gallium arsenide single crystal substrate having a circular major surface, the method including the steps of: preparing a gallium arsenide single crystal substrate precursor having a circular surface; and cleaning the gallium arsenide single crystal substrate precursor to obtain the gallium arsenide single crystal substrate. The cleaning step includes the steps of: polishing the surface of the gallium arsenide single crystal substrate precursor to form the polished surface; cleaning the polished surface with a first alkaline cleaning solution to form the polished surface as an alkali-cleaned surface; cleaning the alkali-cleaned surface with an acid cleaning solution containing 0.3 mass ppm to 0.5 mass % acid to form the alkali-cleaned surface as an acid-cleaned surface; rotating the acid-cleaned surface in a circumferential direction at a rotation speed of 1000 rpm or more, while supplying a second alkaline cleaning solution to the acid-cleaned surface at a flow rate of 0.1 L / min to 5 L / min for 30 seconds to 5 minutes to clean the acid-cleaned surface and form the acid-cleaned surface into a second alkaline-cleaned surface; and heat-treating the second alkaline-cleaned surface in an inert gas atmosphere under conditions of 1.1 atmospheres to 3 atmospheres and 150°C to 300°C to form the second alkaline-cleaned surface into the main surface. The first alkaline cleaning solution contains 0.1 mass % to 10 mass % of a first base. The first base contains at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide. The second alkaline cleaning solution contains 0.3 mass ppm to 0.5 mass % of a second base. The second base contains at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide. By using a method for producing a gallium arsenide single crystal substrate having such characteristics, a gallium arsenide single crystal substrate having a main surface with high specularity can be obtained.

[0022]

[10] The method preferably includes the step of forming an epitaxial film on the main surface, whereby an epitaxial film with a reduced haze value can be formed on the main surface.

[0023] [Details of the embodiment] One embodiment according to the present disclosure (hereinafter also referred to as "the present embodiment") will be described in further detail below, but the present disclosure is not limited thereto. The following description may be made with reference to the drawings, and the same or corresponding elements in this specification and the drawings will be denoted by the same reference numerals, and the same description will not be repeated. Furthermore, the scale of the drawings has been adjusted appropriately to facilitate understanding of each component, and the scale of each component shown in the drawings does not necessarily coincide with the scale of the actual component.

[0024] In this specification, the expression "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is specified for A and only a unit is specified for B, the units of A and B are the same. Furthermore, when a compound or the like is expressed in this specification by a chemical formula, unless the atomic ratio is particularly limited, it is understood to include any conventionally known atomic ratio, and should not necessarily be limited to only those within a stoichiometric range.

[0025] As used herein, the "main surface" of a gallium arsenide single crystal substrate refers to both of the two circular faces of the substrate. A gallium arsenide single crystal substrate falls within the scope of the present invention if at least one of the two faces satisfies the scope of the claims of the present disclosure. An epitaxial film may be disposed on the "main surface" of the gallium arsenide single crystal substrate. Furthermore, the term "plane" used in the term "in-plane" herein refers to the "main surface." Furthermore, when the diameter of a gallium arsenide single crystal substrate is described as "75 mm," this means that the diameter is approximately 75 mm (approximately 75 to 76.5 mm) or 3 inches. When the diameter is described as "100 mm," this means that the diameter is approximately 100 mm (approximately 95 to 105 mm) or 4 inches. When the diameter is described as "150 mm," this means that the diameter is approximately 150 mm (approximately 145 to 155 mm) or 6 inches. When the diameter is described as "200 mm," this means that the diameter is approximately 200 mm (approximately 195 to 205 mm), or 8 inches. The diameter can be measured using a conventionally known outer diameter measuring device such as a vernier caliper.

[0026] In the crystallographic descriptions in this specification, individual orientations are represented by [ ], collective orientations by < >, individual planes by ( ), and collective planes by {}. A negative index in crystallographic terms is usually represented by placing a "- (bar)" before the number, but when this is expressed in this specification, a negative sign is placed before the number.

[0027] [Gallium Arsenide Single Crystal Substrate] The gallium arsenide single crystal substrate (GaAs single crystal substrate) according to this embodiment is a GaAs single crystal substrate having a circular main surface. The GaAs single crystal substrate has a first integrated intensity ratio, a second integrated intensity ratio, a third integrated intensity ratio, a fourth integrated intensity ratio, and a fifth integrated intensity ratio. The first integrated intensity ratio and the third integrated intensity ratio are obtained by determining a spectrum of the detected intensity of gallium (Ga) and arsenic (As) 3d electrons versus the binding energy of photoelectrons emitted outside the GaAs single crystal substrate, based on X-ray photoelectron spectroscopy, in which X-rays are irradiated onto the center of the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 30°. The second and fifth integrated intensity ratios are obtained by determining a spectrum of detected intensities of Ga and As 3d electrons versus binding energy of photoelectrons emitted to the outside of the GaAs single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°. The fourth integrated intensity ratio is obtained by determining a spectrum of detected intensities of Ga and As 3d electrons versus binding energy of photoelectrons emitted to the outside of the GaAs single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 45°.

[0028] The first integrated intensity ratio and the second integrated intensity ratio are determined based on the Ga element present as digallium monoxide (GaO) (hereinafter, referred to as "Ga + ") and the Ga element present as digallium trioxide (Ga2O3) (hereinafter referred to as "Ga 3+ ") and the sum of the integrated intensity of Ga element present as gallium arsenide (GaAs) (hereinafter, this may be referred to as "Ga-As" for convenience) with respect to the integrated intensity of As element present as diarsenic pentoxide (As2O5) (hereinafter, this may be referred to as "As 5+ ") and the As element present as diarsenic trioxide (As2O3) (hereinafter referred to as "As3+ The third integrated intensity ratio, the fourth integrated intensity ratio, and the fifth integrated intensity ratio are the ratios of the sum of the integrated intensity of the Ga element (GaO) (hereinafter, for convenience, this may be referred to as "As-Ga") present as gallium arsenide (GaAs), the integrated intensity of the As element (hereinafter, for convenience, this may be referred to as "As-Ga") present as metallic arsenic (metallic As), and the integrated intensity of the As element (hereinafter, for convenience, this may be referred to as "metallic As"). + ) and the Ga element (Ga 3+ ) and the sum of the integrated intensity of the As element (As 5+ ) and the As element (As 3+ ) is a ratio of the sum of the integrated intensities of the first and second integrated intensity ratios. In the GaAs single crystal substrate, the second integrated intensity ratio is 0.9 or more and 1.05 or less. The third integrated intensity ratio and the fourth integrated intensity ratio are 1.0 or less. The fifth integrated intensity ratio is 0.8 or less. Furthermore, the ratio of the first integrated intensity ratio to the second integrated intensity ratio is 0.5 or more and 1 or less.

[0029] A GaAs single crystal substrate with these characteristics can have a main surface with high specularity by effectively removing the oxide film using wet etching, which allows the formation of an epitaxial film with a reduced haze value.

[0030] <Major Surface> The GaAs single crystal substrate has a circular major surface as described above. In this specification, the term "circular shape" used to describe the shape of the major surface includes not only a geometric circular shape but also a shape in which the major surface does not form a geometric circular shape due to the formation of at least one of a notch, an orientation flat (hereinafter also referred to as "OF"), and an index flat (hereinafter also referred to as "IF"). In other words, the term "a shape in which the major surface does not form a geometric circular shape" refers to a shape in which, among line segments extending from any point on the periphery of the major surface to the center of the main surface, the length of a line segment extending from any point on the notch, OF, or IF to the center of the main surface is shorter. In other words, in this specification, the shape of the main surface is considered to be "circular" based on the shape before the notch, OF, and IF are formed. Therefore, the position and size (length) of the center of the main surface and the diameter of the substrate are determined based on the circular shape before the notch, OF, IF, etc. are formed. It should be noted that the "shape in which the main surface does not form a geometrically circular shape" also includes a shape in which the lengths of all line segments extending from any point on the periphery of the main surface to the center of the main surface are not necessarily the same due to the shape of the GaAs single crystal before it is cut out as a GaAs single crystal substrate. In this case, the center of the main surface refers to the position of the center of gravity, and the diameter of the substrate refers to the length of the longest line segment extending from one point on the periphery of the substrate, through the center of the main surface, to another point on the periphery of the substrate.

[0031] <X-ray Photoelectron Spectroscopy (XPS) Using Synchrotron Radiation> In the course of developing GaAs single crystal substrates capable of forming epitaxial films with reduced haze values, the inventors focused on X-ray photoelectron spectroscopy (XPS) using synchrotron radiation, which can accurately analyze the state of the main surface of a GaAs single crystal substrate. Specifically, by performing XPS using synchrotron radiation, they attempted to identify the cause of the deterioration of the specularity of the main surface of the GaAs single crystal substrate and resolve the cause, thereby achieving a GaAs single crystal substrate capable of forming an epitaxial film with reduced haze values. Here, XPS refers to an analytical technique in which a sample is irradiated with X-rays and the kinetic energy distribution of photoelectrons emitted from the sample is measured to obtain information about the types, abundances, and chemical bonding states of elements present on the surface of the sample.

[0032] Typically, XPS analysis of the main surface of a GaAs single crystal substrate is often performed using X-rays with an energy fixed around 1.487 keV. However, when X-rays with an incident energy fixed around 1.487 keV are used and the photoelectron take-off angle is set to 30°, knowledge of the state of the main surface of the GaAs single crystal substrate is obtained by averaging the state over a region from the main surface to a depth of approximately 5 nm. This region corresponds to approximately 20 atomic layers in atomic terms. For this reason, it has been difficult to accurately analyze the state of the main surface of a GaAs single crystal substrate using X-rays with an incident energy fixed around 1.487 keV and changing the photoelectron take-off angle to obtain knowledge of the state of the main surface of a GaAs single crystal substrate. Furthermore, when XPS is used to obtain knowledge of the state of the main surface of a GaAs single crystal substrate by changing the photoelectron take-off angle, the measurement error with respect to the angle becomes too large, and the measurement error also increases due to the low ionization efficiency of the photoelectron intensity, making it difficult to perform accurate analysis.

[0033] In contrast, in the present disclosure, as described above, X-rays with an X-ray incident energy of 600 eV are used, and XPS is performed under conditions where the photoelectron take-off angle is set to 30°, 45°, or 85°, thereby making it possible to analyze the state of the main surface of a GaAs single crystal substrate.

[0034] When the XPS is performed under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 30°, the state of the main surface of the GaAs single crystal substrate is obtained by averaging the state over a region from the main surface to a depth of about 2.25 nm. When the XPS is performed under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 45°, the state of the main surface of the GaAs single crystal substrate is obtained by averaging the state over a region from the main surface to a depth of about 3.18 nm. When the XPS is performed under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°, the state of the main surface of the GaAs single crystal substrate is obtained by averaging the state over a region from the main surface to a depth of about 4.48 nm. In other words, it is now possible to analyze in detail the region from the main surface of the GaAs single crystal substrate to a depth of approximately 5 nm (corresponding to approximately 20 atomic layers) at intervals of approximately 1 to 3 atomic layers, thereby enabling the state of the main surface to be analyzed with even greater accuracy than before.

[0035] It is known that an oxide film of approximately 1 to 2 nm thick is formed on the main surface of a GaAs single crystal substrate after cleaning in a cleaning process. For this reason, attempts have been made to reduce the haze value of the surface of the epitaxial film by removing the oxide film by wet etching and then forming an epitaxial film on the main surface. However, the haze value of the surface of the epitaxial film remains relatively high even after the wet etching due to factors such as a portion of the oxide film remaining on the main surface. In response to this, the present inventors focused on a detailed analysis of the interface between the oxide film occupying the very surface of the main surface of the GaAs single crystal substrate and a layer consisting of gallium (Ga) and arsenic (As) immediately below the oxide film (hereinafter also referred to as the "main layer" of the GaAs single crystal substrate) (i.e., a region approximately 2 to 5 nm deep from the main surface of the GaAs single crystal substrate) using XPS with synchrotron radiation as described above. As a result, it was discovered that when the oxide film of the GaAs single crystal substrate is rich in gallium relative to arsenic as a whole and this tendency is maintained up to the interface between the oxide film and the GaAs single crystal, the wettability of the surface of the oxide film is improved, and therefore the oxide film can be effectively removed by the wet etching. In other words, it was discovered that by appropriately controlling the gallium composition of the oxide film, a main surface with high specularity can be obtained. Note that in this specification, the "surface" of the oxide film refers to the surface of the oxide film opposite to the GaAs single crystal substrate side.

[0036] <First Integrated Intensity Ratio, Second Integrated Intensity Ratio, Third Integrated Intensity Ratio, Fourth Integrated Intensity Ratio, and Fifth Integrated Intensity Ratio> The GaAs single crystal substrate according to this embodiment has a first integrated intensity ratio, a second integrated intensity ratio, a third integrated intensity ratio, a fourth integrated intensity ratio, and a fifth integrated intensity ratio. The first integrated intensity ratio and the third integrated intensity ratio are obtained by determining a spectrum of the detected intensity of Ga and As 3d electrons versus the binding energy of photoelectrons emitted outside the GaAs single crystal substrate, based on X-ray photoelectron spectroscopy in which X-rays are irradiated onto the center of the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 30°. The second and fifth integrated intensity ratios are obtained by determining a spectrum of detected intensities of Ga and As 3d electrons versus binding energy of photoelectrons emitted to the outside of the GaAs single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°. The fourth integrated intensity ratio is obtained by determining a spectrum of detected intensities of Ga and As 3d electrons versus binding energy of photoelectrons emitted to the outside of the GaAs single crystal substrate based on X-ray photoelectron spectroscopy in which the center of the main surface is irradiated with X-rays under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 45°.

[0037] The first integrated intensity ratio and the second integrated intensity ratio are determined based on the Ga element present as GaO (Ga + ) and the Ga element present as Ga2O3 (Ga 3+ ) and the integral intensity of Ga element present as GaAs (Ga-As) relative to the integral intensity of As element present as AsO (As 5+ ) and the integral intensity of the As element (As 3+ The third integrated intensity ratio, the fourth integrated intensity ratio, and the fifth integrated intensity ratio are the ratio of the sum of the integrated intensity of the Ga element (GaO) present as GaO (Ga +) and the Ga element present as Ga2O3 (Ga 3+ ) and the sum of the integrated intensities of the As element (As 5+ ) and the integral intensity of the As element (As 3+ ) and the sum of the integrated intensities.

[0038] If the first integrated intensity ratio, the second integrated intensity ratio, the third integrated intensity ratio, the fourth integrated intensity ratio, and the fifth integrated intensity ratio are represented by In1, In2, In3, In4, and In5, respectively, In1, In2, In3, In4, and In5 can be expressed by the following mathematical formulas.

[0039]

[0040] In the GaAs single crystal substrate, the second integrated intensity ratio is 0.9 or more and 1.05 or less. The third integrated intensity ratio and the fourth integrated intensity ratio are 1.0 or less. The fifth integrated intensity ratio is 0.8 or less. Furthermore, the ratio of the first integrated intensity ratio to the second integrated intensity ratio is 0.5 or more and 1 or less. It is preferable that the second integrated intensity ratio is 0.9 or more and less than 1.04.

[0041] 1 is an example of a graph showing the relationship between the measurement depth (horizontal axis) from the main surface of a GaAs single crystal substrate according to this embodiment, the ratio of the integrated intensity of the total arsenic element to the integrated intensity of the total gallium element (vertical axis), and the ratio of the integrated intensity of the arsenic element present as arsenic oxide to the integrated intensity of the gallium element present as gallium oxide (vertical axis). In FIG. 1 , the circular point near a measurement depth (horizontal axis) of about 2.25 nm corresponds to the first integrated intensity ratio, the circular point near a measurement depth (horizontal axis) of about 4.48 nm corresponds to the second integrated intensity ratio, the rectangular point near a measurement depth (horizontal axis) of about 2.25 nm corresponds to the third integrated intensity ratio, the rectangular point near a measurement depth (horizontal axis) of about 3.18 nm corresponds to the fourth integrated intensity ratio, and the rectangular point near a measurement depth (horizontal axis) of about 4.48 nm corresponds to the fifth integrated intensity ratio.

[0042] 1, the first integrated intensity ratio, the second integrated intensity ratio, the third integrated intensity ratio, the fourth integrated intensity ratio, and the fifth integrated intensity ratio are 0.99, 1.01, 0.9, 0.83, and 0.76, respectively, and the ratio of the first integrated intensity ratio to the second integrated intensity ratio is 0.98 (=0.99 / 1.01).

[0043] This relationship means that the oxide film occupying a depth of about 1 to 2 nm from the main surface has a composition that is richer in gallium than arsenic as a whole, and that this tendency is maintained up to the interface between the main layer and the oxide film (a depth of about 2 to 5 nm from the main surface). Specifically, the second integrated intensity ratio being 0.9 or more and 1.05 or less means that the oxide film has an intended thickness and is not thicker than intended. The third integrated intensity ratio and the fourth integrated intensity ratio being 1.0 or less means that the oxide film as a whole is richer in gallium than arsenic. The fifth integrated intensity ratio being 0.8 or less and the ratio of the first integrated intensity ratio to the second integrated intensity ratio being 0.5 or more and 1 or less means that the composition changes sharply at the interface between the main layer and the oxide film, and that the oxide film is maintained as a composition that is richer in gallium than arsenic up to the vicinity of the interface. In this case, it is presumed that the oxide film has good surface wettability and can be effectively removed by wet etching. As a result, when an epitaxial film is grown on the main surface of the GaAs single crystal substrate according to this embodiment after wet etching, both the maximum and average haze values ​​of the surface of the epitaxial film can be reduced compared to conventional methods (for example, the maximum haze value of the surface of the epitaxial film can be reduced to 100 ppm or less, and the average haze value can be reduced to 2.5 ppm or less). In this specification, the "surface" of the epitaxial film refers to the surface of the epitaxial film opposite to the GaAs single crystal substrate side.

[0044] On the other hand, when the first, second, third, fourth, and fifth integrated intensity ratios are obtained by performing the XPS on a conventional GaAs single crystal substrate, any of the following relationships is not satisfied: the second integrated intensity ratio does not satisfy the relationship of 0.9 to 1.05, the third integrated intensity ratio and the fourth integrated intensity ratio do not satisfy the relationship of 1.0 or less, the fifth integrated intensity ratio does not satisfy the relationship of 0.8 or less, or the ratio of the first integrated intensity ratio to the second integrated intensity ratio does not satisfy the relationship of 0.5 to 1. In such a GaAs single crystal substrate, there is a risk that a portion of the oxide film may remain on the main surface even after wet etching. Therefore, when an epitaxial film is formed on the main surface of the GaAs single crystal substrate after wet etching, steps may occur on the surface, resulting in large maximum and average haze values.

[0045] As described above, the present inventors have found for the first time that the haze on the surface of an epitaxial film formed on the main surface of a GaAs single crystal substrate depends on the amount of gallium relative to arsenic, and the amount of gallium oxide relative to arsenic oxide, in the oxide film (a region occupying a depth of approximately 1 to 2 nm from the main surface) and in the vicinity of the interface between the oxide film and the main layer (a region 2 to 5 nm deep from the main surface).

[0046] <Oxide Film> The GaAs single crystal substrate preferably has an oxide film on the main surface having a thickness of 2 nm or less. This allows the oxide film to be more effectively removed by wet etching. The thickness of the oxide film is more preferably 1.5 nm or less. The lower limit of the thickness of the oxide film is not particularly limited, but is, for example, 0.5 nm.

[0047] The thickness of the oxide film can be determined by analyzing the main surface of the GaAs single crystal substrate using a scanning transmission electron microscope (STEM) equipped with an energy dispersive X-ray spectroscopy (EDX), for example, a JEM-ARM300F2 (product name (product number) manufactured by JEOL Ltd.). Specifically, an electron beam is irradiated onto the center of the main surface of the GaAs single crystal substrate at an acceleration voltage of 200 kV, and the element-specific characteristic X-rays generated at the center of the main surface are spectroscopically detected and analyzed using the EDX, thereby performing a composition analysis. This is then subjected to a line analysis along the depth direction of the main surface, thereby determining the composition corresponding to each analysis depth from the surface of the main surface.

[0048] Furthermore, the thickness of the oxide film can be determined from the above composition analysis as follows. Specifically, the difference between the As and Ga contents along the analysis depth from the surface of the main surface is first determined, and a spectrum is plotted on a graph with the analysis depth on the horizontal axis and the difference on the vertical axis. Next, since the spectrum exhibits a shape with a peak similar to a Gaussian distribution, the half-width of this shape is determined, and this half-width can be used as the thickness of the oxide film. As described above, the GaAs single crystal substrate according to this embodiment has a composition rich in gallium (particularly gallium oxide) in the oxide film and near the interface between the oxide film and the main layer (a region 1 to 5 nm deep from the main surface). Therefore, based on the difference in the As and Ga contents along the analysis depth from the surface of the main surface, the thickness of the oxide film can be determined from the spectrum representing this difference.

[0049] <Wettability (Contact Angle)> The contact angle of the oxide film is preferably 20 degrees or less. This improves the wettability of the oxide film, allowing it to be more effectively removed by wet etching. The contact angle of the oxide film is more preferably 10 degrees or less. The lower limit of the contact angle of the oxide film is not particularly limited, but is, for example, 1 degree.

[0050] The contact angle of the oxide film can be determined by measuring the contact angle of a droplet of 2 μL of distilled water formed at the center of the main surface (the surface of the oxide film) at room temperature (20 to 25° C.) and a relative humidity of 40 to 60% using the θ / 2 method. A contact angle meter (for example, product name (product number) “Drop Master 500” manufactured by Kyowa Interface Science Co., Ltd.) can be used to observe the droplet.

[0051] <Diameter> The GaAs single crystal substrate preferably has a diameter of 75 mm or more and 205 mm or less. In other words, the diameter of the GaAs single crystal substrate is preferably 3 to 8 inches. This allows for the effective removal of oxide films by wet etching on GaAs single crystal substrates having a diameter of 75 mm or more and 205 mm or less, thereby obtaining a main surface with high specularity. Here, with regard to the diameter, even if the substrate does not have a geometrically circular shape due to the influence of OF, IF, etc., the substrate is considered to have a circular shape before the OF, IF, etc. are formed, and its size (diameter) is determined. The GaAs single crystal substrate preferably has a diameter of 100 mm or more and 205 mm or less, and also preferably has a diameter of 150 mm or more and 205 mm or less.

[0052] <Method for Analyzing GaAs Single Crystal Substrates by X-ray Photoelectron Spectroscopy (XPS) Using Synchrotron Radiation> Hereinafter, the method for analyzing GaAs single crystal substrates by XPS using synchrotron radiation will be described in further detail.

[0053] (Analysis System) Fig. 2 is an explanatory diagram that schematically illustrates the configuration of an analysis system that uses X-ray photoelectron spectroscopy. As shown in Fig. 2, the analysis system 100 includes an X-ray generation facility 10, a vacuum vessel 20, and an electron spectrometer 30. The X-ray generation facility 10, the vacuum vessel 20, and the electron spectrometer 30 are connected in this order. The internal spaces of the X-ray generation facility 10, the vacuum vessel 20, and the electron spectrometer 30 are maintained at an ultra-high vacuum. The pressure in the internal spaces of the X-ray generation facility 10, the vacuum vessel 20, and the electron spectrometer 30 is, for example, 4 x 10 -7 It is Pa.

[0054] The X-ray generating facility 10 generates X-rays called synchrotron radiation. As the X-ray generating facility 10, for example, the beamline "BL17" in the Saga Prefectural Kyushu Synchrotron Light Research Center can be used.

[0055] The X-ray generating equipment 10 generates X-rays of any energy within the energy range of 50 to 2000 eV at the above-mentioned "BL17" and can irradiate the GaAs single crystal substrate 1 placed in the vacuum chamber 20 with the X-rays. The X-ray generating equipment 10 illustrated in FIG. 2 has an X-ray source 11, slits 12 and 14, and a grating 13. The slits 12 and 14 are arranged on the upstream and downstream sides of the grating (spectroscope) 13, respectively. The slits 12 and 14 are, for example, four-quadrant slits.

[0056] The X-ray source 11 outputs synchrotron radiation (X-rays) radiated in a direction tangent to the direction of travel by bending the traveling direction of high-energy electrons in a circular accelerator using a magnetic field generated by a bending electromagnet.

[0057] The X-rays emitted from the X-ray source 11 have high brightness. Specifically, the number of X-ray photons emitted from the X-ray source 11 per second is 10 9 The X-ray intensity is 1 / 3 of the X-ray intensity emitted immediately after activation.

[0058] X-rays emitted from an X-ray source 11 are collimated by a collimating mirror or the like (not shown). A slit 12 allows a portion of the collimated X-rays to pass through. The X-rays that have passed through the slit 12 are monochromatized by a grating 13. A slit 14 limits the spread of the monochromatized X-rays.

[0059] The energy of the X-rays emitted from the X-ray generating facility 10 is determined by the slit width of the slits 12 and 14 and the ruling density of the grating 13. For example, by setting the slit width of the slits 12 and 14 to 30 μm and using a grating 13 with a ruling density of 400 l / mm at the center, and adjusting the exit angle of the grating, X-rays of 600 eV are emitted from the X-ray generating facility 10.

[0060] When X-rays from the X-ray generating equipment 10 are irradiated onto the GaAs single crystal substrate 1 placed in the vacuum chamber 20, photoelectrons are emitted from the GaAs single crystal substrate 1.

[0061] The electron spectrometer 30 measures the kinetic energy distribution of the photoelectrons emitted from the GaAs single crystal substrate 1. The electron spectrometer 30 has a hemispherical analyzer and a detector. The hemispherical analyzer separates the photoelectrons into different wavelengths. The detector counts the number of photoelectrons of each energy.

[0062] The angle θ1 between the traveling direction of X-rays incident on the GaAs single crystal substrate 1 from the X-ray generating equipment 10 and the main surface 1m of the GaAs single crystal substrate 1 is variable. The angle (hereinafter referred to as the "take-off angle θ2") between the traveling direction of photoelectrons captured by the electron spectrometer 30, among the photoelectrons emitted from the GaAs single crystal substrate 1, and the main surface 1m of the GaAs single crystal substrate 1 is also variable. In this embodiment, the take-off angle θ2 is set to 30°, 45°, or 85°. The angle θ1 is not particularly limited, but is set to, for example, 85°.

[0063] As the electron spectrometer 30, for example, a high-resolution XPS analyzer "R3000" manufactured by Scienta Omicron can be used.

[0064] (Depth from the Main Surface to be Analyzed) Some of the photoelectrons emitted to the outside of the GaAs single crystal substrate 1 by irradiation with X-rays lose energy due to inelastic scattering. Therefore, only a portion of the photoelectrons generated in the GaAs single crystal substrate 1 escape into vacuum while retaining the energy at the time of generation and reach the electron spectrometer 30. Photoelectrons escaping from the surface are generated at a depth equivalent to approximately three times the inelastic mean free path (IMFP) of the photoelectrons. Therefore, the depth d (nm) from the main surface of the GaAs single crystal substrate to be analyzed is expressed by the following formula: In the following formula, λ (nm) is the IMFP value, and θ is the take-off angle.

[0065]

[0066] Furthermore, as shown in "Method for Estimating the Inelastic Mean Free Path of Electrons Using the Tpp-2M Formula," Journal of Surface Analysis, Vol. 1, No. 2, 1995, λ (Å) is expressed by the following formulas:

[0067]

[0068] In each of the above formulas, A W is the atomic weight or molecular weight, N v is the number of valence electrons per atom or molecule, E p is the plasmon energy of free electrons (eV), ρ is the density (g / cm 3 ), E g indicates the band gap energy (eV). E indicates the kinetic energy (eV) of the photoelectron, which is calculated from the energy (eV) of the irradiated X-ray and the binding energy (eV) between the electron and the atomic nucleus.

[0069] By using the above formulas, the depth d (nm) from the main surface of the GaAs single crystal substrate to be analyzed can be determined. That is, the depth d (nm) from the main surface of the GaAs single crystal substrate is calculated using the above formulas, various parameter values ​​related to the 3d electrons of Ga and As elements, and the X-ray energy (600 eV). The depth d (nm) is as follows:

[0070] When the X-ray incident energy is 600 eV and the photoelectron take-off angle is 30°, the depth d is approximately 2.25 nm. When the X-ray incident energy is 600 eV and the photoelectron take-off angle is 45°, the depth d is approximately 3.18 nm. When the X-ray incident energy is 600 eV and the photoelectron take-off angle is 85°, the depth d is approximately 4.48 nm.

[0071] (Method of Calculating the First, Second, Third, Fourth, and Fifth Integrated Intensity Ratios) Hereinafter, a method of calculating the first, second, third, fourth, and fifth integrated intensity ratios at the main surface based on the above-described XPS will be described, first illustrating a method of calculating the first and third integrated intensity ratios. In this case, the XPS is performed using X-rays with an energy of 600 eV relative to the center of the main surface of the GaAs single crystal substrate. The take-off angle of the photoelectrons is set to 30°. This allows the kinetic energy distribution of the photoelectrons emitted from the GaAs single crystal substrate to be obtained.

[0072] The kinetic energy E of photoelectrons emitted from the GaAs single crystal substrate is the sum of the energy hν (eV) of the irradiated X-rays and the binding energy E of the electrons in the GaAs single crystal substrate. B (eV) and the work function φ (eV), it is expressed by the following formula: E=hν−E B -φ.

[0073] Using the above formula, a spectrum showing the binding energy distribution of photoelectrons is generated from the kinetic energy distribution of photoelectrons emitted from the GaAs single crystal substrate. In this embodiment, a Ga 3d spectrum and an As 3d spectrum showing the binding energy distribution of photoelectrons are generated based on the kinetic energy distribution of photoelectrons emitted from a position at a depth d (nm) from the main surface of the GaAs single crystal substrate. Here, in this specification, the term "Ga 3d spectrum" refers to a spectrum showing the detected intensity of photoelectrons emitted from the 3d orbital of Ga elements (GaO, GaO, and Ga contained in GaAs). The term "As 3d spectrum" refers to a spectrum showing the detected intensity of photoelectrons emitted from the 3d orbital of As elements (AsO, AsO, metallic As, and As contained in GaAs).

[0074] In particular, in the analysis using XPS, from the viewpoint of accurate measurement, Ga3d spectra and As3d spectra are obtained by narrow scanning a predetermined binding energy range. Specifically, by narrow scanning a binding energy range of 16 to 26 eV, the Ga3d spectrum can be plotted on a graph with the above range on the horizontal axis and the detection intensity on the vertical axis. By narrow scanning a binding energy range of 39 to 49 eV, the As3d spectrum can be plotted on a graph with the above range on the horizontal axis and the detection intensity on the vertical axis.

[0075] The narrow scan is performed under the conditions that the energy interval is 0.05 eV, the integration time at each energy value is 100 ms, and the number of integrations is 1 or more. The energy resolution E / ΔE is 3480.

[0076] As a result of the above, a Ga 3d spectrum LG as shown in FIG. 3A and an As 3d spectrum LA as shown in FIG. 3B can be obtained. FIG. 3A is a graph showing an example of a background-corrected Ga 3d spectrum obtained based on XPS in which X-rays are irradiated onto the center of the main surface of a GaAs single crystal substrate according to this embodiment. FIG. 3B is a graph showing an example of a background-corrected As 3d spectrum obtained based on XPS in which X-rays are irradiated onto the center of the main surface of a GaAs single crystal substrate according to this embodiment. As mentioned above, FIGS. 3A and 3B show examples of a Ga 3d spectrum and an As 3d spectrum, respectively, after background correction. That is, when obtaining the Ga 3d spectrum LG and the As 3d spectrum LA, background correction is performed using the Shirley method (reference: Kazuhiro Yoshihara, Journal of the Vacuum Society of Japan, 2013, Vol. 56, No. 6, pp. 243-247). This allows the determination of a background-corrected Ga spectrum L G based on the difference between the Ga spectrum obtained based on actual measurement and the background, and also allows the determination of a background-corrected As spectrum L A based on the difference between the As spectrum obtained based on actual measurement and the background.

[0077] When obtaining the Ga 3d spectrum LG, the Ga element (Ga + The peak of the detected intensity of Ga (Ga) is fixed at the position where the binding energy is 19.9 eV. 3+The peak position of the detected intensity of Ga-As is fixed at a position where the binding energy is 20.7 eV. Furthermore, the peak of the detected intensity of Ga element (Ga-As) present as GaAs is given a width at a position where the binding energy is approximately 19.2 to 19.7 eV. This is because when the above-mentioned X-ray photoelectron spectroscopy is performed on a GaAs single crystal, a charging shift may occur, and the Ga3d spectrum may shift by up to approximately 1 eV toward the higher energy side. Furthermore, since the peak of the detected intensity of Ga-As is affected by the main layer made of GaAs, it is difficult to fix it to a single value. Therefore, the peak position is given a width of 0.5 eV as described above.

[0078] When obtaining the As3d spectrum LA, the As element (As 5+ The peak of the detected intensity of As (As) is fixed at the position where the binding energy is 45.57 eV. 3+ The peak position of the detection intensity of As (As-Ga) is fixed to a position where the binding energy is 44.07 eV. Furthermore, the peak of the detection intensity of As element (metallic As) present as metallic As is given a width at a position where the binding energy is approximately 41.62 to 42.12 eV, and the peak of the detection intensity of As element (As-Ga) present as GaAs is given a width at a position where the binding energy is approximately 40.77 to 41.27 eV. This is because when the above-mentioned X-ray photoelectron spectroscopy is performed on a GaAs single crystal, a charging shift may occur, which may cause the As3d spectrum to shift by up to approximately 1 eV toward the higher energy side. Furthermore, since each peak of metallic As and As-Ga is affected by the main layer made of GaAs, it is difficult to fix it to a single value. Therefore, as described above, the peak position is given a width of 0.5 eV.

[0079] Next, the Ga3d spectrum LG after background correction obtained as described above is separated into the following three Gaussian functions Y1, Y2, and Y3 (hereinafter, this operation is also referred to as "peak separation"). As a result, the Ga element (Ga+ ), Ga element present as Ga2O3 (Ga 3+ ), and Ga element present as GaAs (Ga-As). Y1 = a1 * exp {(-(X - b1) 2 ) / c1 2} Y2=a2*exp{(-(X-b2) 2 ) / c2 2} Y3=a3*exp{(-(X-b3) 2 ) / c3 2} The Gaussian functions Y1, Y2, and Y3 are dimensionless, and in the Gaussian functions Y1, Y2, and Y3, X, b1, b2, b3, c1, c2, and c3 are eV, and a1, a2, and a3 are dimensionless.

[0080] The Gaussian functions Y1 to Y3 are such that the i-th component of Ga3d is the Gaussian function Gi=Ai*exp{(-(E-E1) 2 ) / Wi 2}, and the square of the difference with the actual measurement ([actual measurement - ΣGi] 2 ) is obtained by optimizing each variable (a1, a2, a3, b1, b2, b3, c1, c2, c3) so that the above-mentioned Ga + , Ga 3+ , and the value of the binding energy at the peak of the detected intensity of Ga—As are substituted.

[0081] That is, the variables (a1, a2, a3, b1, b2, b3, c1, c2, c3) are as follows: a1, a2, a3 are real numbers equal to or greater than 0. b1 = 19.9 eV b2 = 20.7 eV 19.2 eV ≦ b3 ≦ 19.7 eV 0.2 eV ≦ c1 ≦ 0.95 eV 0.2 eV ≦ c2 ≦ 0.95 eV 0.2 eV ≦ c3 ≦ 0.95 eV.

[0082] As a result, the Gaussian functions Y1, Y2, and Y3 are, for example, Ga peaks separated from the Ga spectrum LG of FIG. + Spectrum L2, Ga 3+ The Ga—As spectrum can be expressed as spectrum L1 and Ga—As spectrum L3, respectively.

[0083] Furthermore, the As3d spectrum LA after background correction obtained as described above can be expressed by peak separation into the following four Gaussian functions Y4, Y5, Y6, and Y7. This allows the As element (As 5+ ), As element present as As2O3 (As 3+ Four spectra can be obtained: Y4 = a4 * exp {(-(X - b4)}}, ... 2 ) / c4 2} Y5=a5*exp{(-(X-b5) 2 ) / c5 2} Y6=a6*exp{(-(X-b6) 2 ) / c6 2} Y7=a7*exp{(-(X-b7) 2 ) / c7 2} The units of the Gaussian functions Y4, Y5, Y6, and Y7 are dimensionless, and in the Gaussian functions Y4, Y5, Y6, and Y7, the units of X, b4, b5, b6, b7, c4, c5, c6, and c7 are eV, and the units of a4, a5, a6, and a7 are dimensionless.

[0084] The Gaussian functions Y4 to Y7 are such that the i-th component of As3d is a Gaussian function Gi = Ai * exp {(-(E-E1) 2 ) / Wi 2}, and the square of the difference with the actual measurement ([actual measurement - ΣGi] 2 ) is obtained by optimizing each variable (a4, a5, a6, a7, b4, b5, b6, b7, c4, c5, c6, c7) so that the above-mentioned As 5+ , As 3+ , metallic As, and As—Ga are substituted for the binding energy values ​​at the peaks of signal intensity.

[0085] That is, the variables (a4, a5, a6, a7, b4, b5, b6, b7, c4, c5, c6, c7) are as follows: a4, a5, a6, a7 are real numbers greater than or equal to 0. b4 = 45.57 eV b5 = 44.07 eV 41.62 eV ≦ b6 ≦ 42.12 eV 40.77 eV ≦ b7 ≦ 41.27 eV 0.2 eV ≦ c4 ≦ 0.95 eV 0.2 eV ≦ c5 ≦ 0.95 eV 0.2 eV ≦ c6 ≦ 0.95 eV 0.2 eV ≦ c7 ≦ 1.2 eV.

[0086] As a result, the Gaussian functions Y4, Y5, Y6, and Y7 are, for example, peak-separated As spectrums from the As spectrum LA in FIG. 3B. 5+ Spectrum L4, As 3+ These can be represented as spectrum L5, metallic As spectrum L6, and As-Ga spectrum L7, respectively. Metallic As is generated from the oxide film and the main layer by the reaction 2GaAs + As2O3 → Ga2O3 + 4As, and is therefore detected as an intensity by the XPS.

[0087] Note that the following correction can be made to determine the peak positions of each Gaussian function Y1 to Y7. First, the probability that photoelectrons are generated by X-rays, known as the photoionization efficiency (η), is considered to vary depending on the element, X-ray energy, etc., so the data posted on the following website is used as the value of η. Specifically, the photoionization efficiency (η) of X-rays with an incident energy of 600 eV is set to 0.28 for Ga3d and 0.42 for As3d.

[0088] https: / / vuo.elettra.eu / services / elements / WebElements.html (The data is based on JJ Yeh, Atomic Calculation of Photoionization Cross-Sections and Asymmetry Parameters, Gordon and Breach Science Publishers, Langhorne, PE(USA), 1993 and JJ Yeh and I. Lindau, Atomic Data and Nuclear Data Tables, 32, 1-155(1985)).

[0089] Furthermore, since the irradiation intensity of the X-rays used at the synchrotron radiation facility decays over time, a gold (Au) standard sample is measured at regular intervals to determine the decay ratio of the Au4f photoelectron intensity, and the X-ray irradiation dose is corrected based on this ratio.

[0090] In FIG. 3A, Ga 3+ The area between the spectrum L1 and the horizontal axis (X axis) is Ga 3+ corresponds to the number of photoelectrons emitted from the 3d orbital of Ga 3+ means the integrated intensity of Ga + The area between the spectrum L2 and the horizontal axis (X axis) is Ga + corresponds to the number of photoelectrons emitted from the 3d orbital of Ga + The area between the Ga—As spectrum L3 and the horizontal axis (X axis) corresponds to the number of photoelectrons emitted from the 3d orbitals of Ga—As, and therefore represents the integrated intensity of Ga—As.

[0091] In FIG. 3B, As 5+ The area between spectrum L4 and the horizontal axis (X axis) is As 5+ corresponds to the number of photoelectrons emitted from the 3d orbital of As 5+ As means the integrated intensity of 3+ The area between spectrum L5 and the horizontal axis (X axis) is As 3+ corresponds to the number of photoelectrons emitted from the 3d orbital of As 3+The area between the metal As spectrum L6 and the horizontal axis (X-axis) corresponds to the number of photoelectrons emitted from the 3d orbital of metal As, and thus represents the integrated intensity of metal As. The area between the As—Ga spectrum L7 and the horizontal axis (X-axis) corresponds to the number of photoelectrons emitted from the 3d orbital of As—Ga, and therefore represents the integrated intensity of As—Ga.

[0092] Therefore, based on the above-mentioned spectra and the areas obtained from the horizontal axis, Ga + and the integrated intensity of Ga 3+ The sum of the integrated intensity of Ga—As and the integrated intensity of Ga—As is 5+ and the integral intensity of As 3+ The ratio of the sum of the integrated intensity of As—Ga, the integrated intensity of As, and the integrated intensity of metal As can be calculated as the first integrated intensity ratio. + and the integrated intensity of Ga 3+ As for the sum of the integrated intensity of 5+ and the integral intensity of As 3+ The ratio of the sum of the integrated intensities of the first and second integrated intensities to the integrated intensities of the second and third integrated intensities can be calculated as a third integrated intensity ratio.

[0093] According to this embodiment, the second integrated intensity ratio and the fifth integrated intensity ratio can be calculated by the same method as that for calculating the first integrated intensity ratio and the third integrated intensity ratio described above, except that the XPS is performed under conditions of an incident energy of 600 eV and a photoelectron take-off angle of 85° with respect to the center of the main surface of the GaAs single crystal substrate. The fourth integrated intensity ratio can also be calculated by the same method as that for calculating the first integrated intensity ratio and the third integrated intensity ratio described above, except that the XPS is performed under conditions of an incident energy of 600 eV and a photoelectron take-off angle of 45° with respect to the center of the main surface of the GaAs single crystal substrate.

[0094] <Uniformity of the Main Surface of the GaAs Single Crystal Substrate> The characteristics of the GaAs single crystal substrate according to this embodiment are preferably uniform across the main surface. In other words, the GaAs single crystal substrate according to this embodiment is preferably capable of forming an epitaxial film with a reduced haze value, regardless of the position across the main surface. Specific examples of such a preferred GaAs single crystal substrate include the following aspects (first and second aspects).

[0095] (First Aspect) A GaAs single crystal substrate according to the first aspect has a diameter of 75 mm or more and less than 150 mm. The GaAs single crystal substrate preferably has a diameter of 75 mm or more and 105 mm or less. The GaAs single crystal substrate has a sixth integrated intensity ratio and a seventh integrated intensity ratio. The sixth integrated intensity ratio and the seventh integrated intensity ratio are obtained by determining a spectrum of the detected intensity of Ga and As 3d electrons versus the binding energy of photoelectrons emitted outside the GaAs single crystal substrate based on X-ray photoelectron spectroscopy, in which X-rays are irradiated onto five measurement points on the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°.

[0096] The sixth integrated intensity ratio is the Ga element present as GaO (Ga + ) and the Ga element present as Ga2O3 (Ga 3+ ) and the integral intensity of Ga element present as GaAs (Ga-As) relative to the integral intensity of As element present as AsO (As 5+ ) and the integral intensity of the As element (As 3+ The seventh integrated intensity ratio is the ratio of the sum of the integrated intensity of the Ga element (Ga-Ga) present as GaAs to the integrated intensity of the As element (metallic As) present as metallic As. + ) and the Ga element present as Ga2O3 (Ga 3+ ) and the sum of the integrated intensities of the As element (As 5+ ) and the integral intensity of the As element (As 3+) is the ratio of the sum of the integrated intensities of the seventh integrated intensity ratio to the sixth integrated intensity ratio. The standard deviation and average value of the ratio of the seventh integrated intensity ratio to the sixth integrated intensity ratio satisfy the relationship of standard deviation / average value≦0.039. The standard deviation and average value of the ratio of the seventh integrated intensity ratio to the sixth integrated intensity ratio satisfying the relationship of standard deviation / average value≦0.039 means that the oxide film has a gallium-rich composition without variation within the surface, and therefore the oxide film on the main surface can be removed by wet etching without variation within the surface. The lower limits of the standard deviation and average value of the ratio of the seventh integrated intensity ratio to the sixth integrated intensity ratio are 0, which is an ideal value. For example, the standard deviation and average value of the ratio of the seventh integrated intensity ratio to the sixth integrated intensity ratio may satisfy the relationship of standard deviation / average value≧0.026.

[0097] When the diameter is represented by D and two mutually orthogonal axes on the main surface that pass through the center of the main surface are represented by the X and Y axes, the X- and Y-axis coordinates (X, Y) of the five measurement points are (0, 0), (D / 4, 0), (0, D / 4), (-D / 4, 0), and (0, -D / 4). The units of D and X and Y in the coordinates (X, Y) are mm. As a result, in a GaAs single crystal substrate having a diameter of 75 mm or more and less than 150 mm, it is possible to effectively remove an oxide film by wet etching, obtain a main surface with high specularity without in-plane variation, and thereby form an epitaxial film with a reduced haze value.

[0098] (Second Aspect) A GaAs single crystal substrate according to the second aspect has a diameter of 150 mm or more and 205 mm or less. The GaAs single crystal substrate has an eighth integrated intensity ratio and a ninth integrated intensity ratio. The eighth integrated intensity ratio and the ninth integrated intensity ratio are obtained by determining a spectrum of the detected intensity of Ga and As 3d electrons versus the binding energy of photoelectrons emitted outside the GaAs single crystal substrate based on X-ray photoelectron spectroscopy, in which X-rays are irradiated onto five measurement points on the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°.

[0099] The eighth integrated intensity ratio is the Ga element present as GaO (Ga + ) and the Ga element present as Ga2O3 (Ga 3+ ) and the integral intensity of Ga element present as GaAs (Ga-As) relative to the integral intensity of As element present as AsO (As 5+ ) and the integral intensity of the As element (As 3+ The ninth integrated intensity ratio is the ratio of the sum of the integrated intensity of the Ga element (GaO) present as GaO (Ga-Ga) to the integrated intensity of the As element (As-Ga) present as metal As. + ) and the Ga element present as Ga2O3 (Ga 3+ ) and the sum of the integrated intensities of the As element (As 5+ ) and the integral intensity of the As element (As 3+ ) and the integrated intensity of the ninth integrated intensity ratio. The standard deviation and average value of the ratio of the ninth integrated intensity ratio to the eighth integrated intensity ratio satisfy the relationship of standard deviation / average value≦0.022. The standard deviation and average value of the ratio of the ninth integrated intensity ratio to the eighth integrated intensity ratio satisfying the relationship of standard deviation / average value≦0.022 means that the oxide film has a gallium-rich composition without variation within the surface, and therefore the oxide film on the main surface can be removed by wet etching without variation within the surface. The lower limits of the standard deviation and average value of the ratio of the ninth integrated intensity ratio to the eighth integrated intensity ratio are 0, which is an ideal value. For example, the standard deviation and average value of the ratio of the ninth integrated intensity ratio to the eighth integrated intensity ratio may satisfy the relationship of standard deviation / average value≧0.009.

[0100] When the diameter is represented by D and two mutually orthogonal axes on the main surface that pass through the center of the main surface are represented by the X and Y axes, the X- and Y-axis coordinates (X, Y) of the nine measurement points are (0, 0), (D / 4, 0), (0, D / 4), (-D / 4, 0), (0, -D / 4), (D / 2-10, 0), (0, D / 2-10), (-(D / 2-10), 0), and (0, -(D / 2-10)). The units of D and X and Y in the coordinates (X, Y) are mm. As a result, in a GaAs single crystal substrate having a diameter of 150 mm or more and 205 mm or less, it is possible to effectively remove an oxide film by wet etching, obtain a main surface with high specularity without in-plane variation, and thereby form an epitaxial film with a reduced haze value.

[0101] In the first and second aspects, the specific analytical methods for determining the sixth, seventh, eighth, and ninth integrated intensity ratios are the same as those described above in the section <Method for analyzing GaAs single crystal substrates by X-ray photoelectron spectroscopy (XPS) using synchrotron radiation>, and therefore, redundant description will not be repeated.

[0102] (Five Measurement Points and Nine Measurement Points) The GaAs single crystal substrate according to the first embodiment has a diameter of 75 mm or more and less than 150 mm. In this case, five measurement points are set on the main surface of the GaAs single crystal substrate according to the first embodiment, as follows: That is, to evaluate the effect of reducing the haze value of the epitaxial film due to a uniform in-plane distribution of the ratio of the seventh integrated intensity ratio to the sixth integrated intensity ratio, it is preferable to set five measurement points so that the distance between them is as large as possible, and measure the haze value generated in the epitaxial film grown in the vicinity of each of the five measurement points. In this case, it is preferable to measure the haze value in an area with a diameter of 20 mm or more. Therefore, five circular measurement targets with a diameter of 20 mm are set on the main surface of the GaAs single crystal substrate so that the distance between them is as large as possible. The center of each measurement target is set as a measurement point.

[0103] First, when two axes passing through the center of the main surface and perpendicular to each other on the main surface are defined as the X-axis and the Y-axis, the X-axis and Y-axis coordinates (X, Y) of the first of the five measurement points are set to (0, 0). The X-axis and Y-axis are set so that the notch formed in the GaAs single crystal substrate is located in the third quadrant of the XY coordinate plane, and the general angle of the half line passing through the notch with respect to the half line extending from the origin in the positive direction of the X-axis is 225°.

[0104] Furthermore, of the five measurement points, the second, third, fourth, and fifth measurement points are arranged at equal intervals on a circle consisting of a set of points spaced D / 4 from the center of the GaAs single crystal substrate. Specifically, the coordinates (X, Y) of the second measurement point are set to (D / 4, 0). The coordinates (X, Y) of the third measurement point are set to (0, D / 4). The coordinates (X, Y) of the fourth measurement point are set to (-D / 4, 0). The coordinates (X, Y) of the fifth measurement point are set to (0, -D / 4). D represents the diameter of the GaAs single crystal substrate, and the units of X and Y in D and the coordinates (X, Y) are mm.

[0105] The GaAs single crystal substrate according to the second embodiment has a diameter of 150 mm or more and 205 mm or less. In this case, four additional measurement points are set on the main surface of the GaAs single crystal substrate according to the second embodiment, in addition to the five measurement points set on the GaAs single crystal substrate according to the first embodiment, for a total of nine measurement points, as follows: That is, on the main surface of the GaAs single crystal substrate according to the second embodiment, in addition to the second, third, fourth, and fifth measurement points described above, four measurement targets each having a diameter of 20 mm are set on the outer periphery of these measurement points and so as not to overlap with the measurement targets including the second, third, fourth, and fifth measurement points. The center of each measurement target is set as a measurement point, and X-rays are irradiated toward the measurement points. Specifically, the coordinates (X, Y) of the sixth measurement point of the four additional measurement points are set to (0, D / 2-10). The coordinates (X, Y) of the seventh measurement point are set to (D / 2-10, 0). The coordinates (X, Y) of the eighth measurement point are set to (-(D / 2-10), 0). The coordinates (X, Y) of the ninth measurement point are set to (0, -(D / 2-10)). D represents the diameter of the GaAs single crystal substrate, and the units of D and X and Y in the coordinates (X, Y) are mm.

[0106] It is known that in the main surface of a large-diameter substrate having a diameter of 150 mm or more and 205 mm or less, such as the GaAs single crystal substrate according to the second aspect, characteristics tend to vary in the more outer peripheral region. Therefore, in order to evaluate the effect of reducing the haze value of an epitaxial film due to a uniform in-plane distribution of the ratio of the ninth integrated intensity ratio to the eighth integrated intensity ratio, it is desirable to measure the haze value of an epitaxial film grown in a more outer peripheral region in addition to the five measurement points described above. To address this, in addition to the five measurement points described above, four measurement targets with a diameter of 20 mm and their central measurement points are set in the more outer peripheral region, with the distance between them as large as possible.

[0107] Fig. 4 is an explanatory diagram illustrating five measurement points set on a GaAs single crystal substrate with a diameter of 75 mm or more and less than 150 mm in this embodiment. Fig. 5 is an explanatory diagram illustrating nine measurement points set on a GaAs single crystal substrate with a diameter of 150 mm or more and 205 mm or less in this embodiment.

[0108] 4, in the GaAs single crystal substrate according to the first embodiment, the X-axis and Y-axis are set so that the general angle of a half line passing through the notch 50 with respect to a half line extending from the origin in the positive direction of the X-axis is 225°. Next, a first measurement point P1 is set at the origin (0,0), which is the center of the GaAs single crystal substrate, and a measurement object A1 is set as a circular region with a diameter of 20 mm centered at the first measurement point P1.

[0109] Next, a second measurement point P2, a third measurement point P3, a fourth measurement point P4, and a fifth measurement point P5 are set on a circumference consisting of a set of points spaced a distance D / 4 from the center of the GaAs single crystal substrate. Furthermore, measurement targets A2, A3, A4, and A5 are set as circular regions with a diameter of 20 mm, each centered on the second measurement point P2, the third measurement point P3, the fourth measurement point P4, and the fifth measurement point P5, respectively.

[0110] For example, if the example shown in FIG. 4 is a GaAs single crystal substrate with a diameter of 75 mm, the coordinates (X, Y) (X and Y are both in mm; the same applies below) of the second measurement point P2, the third measurement point P3, the fourth measurement point P4, and the fifth measurement point P5 are set to (18.75, 0), (0, 18.75), (-18.75, 0), and (0, -18.75), respectively. Here, for a GaAs single crystal substrate with a diameter of 75 mm, measurement target A1 will overlap with measurement target A2, measurement target A3, measurement target A4, and measurement target A5 in some regions. However, this overlap is acceptable because it does not pose a problem from the perspective of evaluating the uniformity of the main surface of the GaAs single crystal substrate.

[0111] 5 , in the GaAs single crystal substrate according to the second embodiment, in addition to the first through fifth measurement points P1 through P5 set on the GaAs single crystal substrate according to the first embodiment, four measurement points, namely, a sixth measurement point P6, a seventh measurement point P7, an eighth measurement point P8, and a ninth measurement point P9, are set at equal intervals on a circumference located 10 mm inward from the outer periphery of the GaAs single crystal substrate and further outward from the second, third, fourth, and fifth measurement points P2, P3, P4, and P5. Furthermore, measurement targets A6, A7, A8, and A9 are set as circular regions with a diameter of 20 mm centered on the sixth, seventh, eighth, and ninth measurement points P8 and P9, respectively.

[0112] 5 is a GaAs single crystal substrate having a diameter of 150 mm, the coordinates (X, Y) of the second measurement point P2, the third measurement point P3, the fourth measurement point P4, and the fifth measurement point P5 are set to (37.5, 0), (0, 37.5), (-37.5, 0), and (0, 37.5), respectively. Furthermore, the coordinates (X, Y) of the sixth measurement point P6, the seventh measurement point P7, the eighth measurement point P8, and the ninth measurement point P9 are set to (65, 0), (0, 65), (-65, 0), and (0, -65), respectively.

[0113] <Epitaxial Film> The GaAs single crystal substrate preferably has an epitaxial film disposed on the main surface. In this case, the maximum surface haze of the epitaxial film is preferably 100 ppm or less, and the average surface haze of the epitaxial film is preferably 2.5 ppm or less. The maximum surface haze of the epitaxial film is more preferably 20 ppm or less, and the average surface haze of the epitaxial film is more preferably 2.0 ppm or less. The lower limits of the maximum and average surface haze of the epitaxial film are ideal values ​​of 0.

[0114] The epitaxial film is, for example, Al 1-y-z Ga y In zIn this embodiment, the epitaxial film formed on the main surface of the GaAs single crystal substrate is a compound film made of AlAs, and the y is 0 or more and 1 or less, the z is 0 or more and 1 or less, and the sum of the y and the z is 0 or more and 1 or less. 1-y-z Ga y In z A compound film made of As (0≦y≦1, 0≦z≦1, 0≦y+z≦1) can be applied. x Ga 1-x N (0≦x≦1) or Al x Ga 1-x It may also be a compound film of As (0≦x≦1).

[0115] The epitaxial film is formed to have a thickness of, for example, 0.5 to 10 μm. When the thickness of the epitaxial film is within the above range, the GaAs single crystal substrate can be used in a wide range of applications. It is more preferable that the epitaxial film has a thickness of 1 to 5 μm.

[0116] The haze value of the epitaxial film disposed on the main surface of the GaAs single crystal substrate can be determined by a conventional surface foreign matter inspection device (for example, product name "Surfscan 6420" manufactured by KLA-Tencor Corporation). The device targets the entire surface of the epitaxial film (excluding the region 2 mm inside from the outer periphery of the substrate) and measures the haze within 1 cm of the surface. 2 The haze value (quantity of scattered light (ppm)) per unit area can be measured. Based on the results of such measurements, the maximum and average haze values ​​on the surface of the epitaxial film can be determined.

[0117] [Method for Manufacturing Gallium Arsenide Single Crystal Substrate] The method for manufacturing a gallium arsenide single crystal substrate (GaAs single crystal substrate) according to this embodiment is preferably a method for manufacturing the GaAs single crystal substrate described above. For example, the manufacturing method includes a step of preparing a gallium arsenide single crystal substrate precursor (hereinafter also referred to as "GaAs single crystal substrate precursor") having a circular surface (preparation step), and a cleaning step for obtaining the GaAs single crystal substrate from the GaAs single crystal substrate precursor. The cleaning step includes a step of polishing the surface of the GaAs single crystal substrate precursor to form a polished surface (surface polishing step), a step of cleaning the polished surface with a first alkaline cleaning solution to form an alkali-cleaned surface (first alkaline cleaning step), a step of cleaning the alkali-cleaned surface with an acid cleaning solution containing 0.3 mass ppm to 0.5 mass % acid to form the alkali-cleaned surface (acid cleaning step), and a step of rotating the acid-cleaned surface at a speed of 1000 rpm or more in the circumferential direction. The method includes a step of cleaning the acid-washed surface by supplying a second alkaline cleaning solution to the acid-washed surface at a flow rate of 0.1 L / min to 5 L / min for 30 seconds to 5 minutes while rotating the substrate at a rotational speed (second alkaline cleaning step), thereby converting the acid-washed surface into a second alkaline-washed surface; and a step of heat-treating the second alkaline-washed surface in an inert gas atmosphere under conditions of 1.1 atm to 3 atm and 150°C to 300°C, thereby converting the second alkaline-washed surface into the main surface (heat treatment step). The first alkaline cleaning solution contains 0.1 mass% to 10 mass% of a first base. The first base contains at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide. The second alkaline cleaning solution contains 0.3 mass ppm to 0.5 mass% of a second base. The second base contains at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide.

[0118] The manufacturing method having these features can provide a GaAs single crystal substrate having an oxide film on the main surface that can be effectively removed by wet etching. The manufacturing method preferably includes a step of forming an epitaxial film on the main surface (epitaxial film formation step). This allows for the production of a GaAs single crystal substrate having an epitaxial film with a reduced haze value formed on the main surface.

[0119] In this specification, the term "gallium arsenide single crystal substrate precursor (GaAs single crystal substrate precursor)" refers to a GaAs single crystal substrate having a circular surface that is cut out from a gallium arsenide single crystal (hereinafter also referred to as "GaAs single crystal") manufactured using a conventionally known manufacturing method such as the vertical boat method, and in particular refers to a GaAs single crystal substrate that is the object on which each of the steps included in the above-mentioned cleaning step is performed.

[0120] Based on the findings obtained from the above-mentioned synchrotron XPS analysis, the inventors focused on improving the conventional cleaning process for obtaining the GaAs single crystal substrate. It is known that the oxide film on the GaAs single crystal substrate is formed by oxidation of the surface during the acid cleaning process, which removes impurities in the alkaline cleaning agent adhering to the surface of the GaAs single crystal substrate precursor after alkaline cleaning. Therefore, the inventors focused on performing a process after the acid cleaning process to enrich the oxide film and the interface between the oxide film and the GaAs layer of the GaAs single crystal substrate with gallium (gallium oxide, hereinafter also referred to as "Ga oxide") after the acid cleaning process. Specifically, the surface of the GaAs single crystal substrate precursor was cleaned in the alkaline cleaning process and the acid cleaning process, respectively, and then a second alkaline cleaning process, in which an alkaline cleaning solution was supplied to the surface while the surface was rotating, thereby suppressing the progress of oxidation of the oxide film. Furthermore, the surface after the second alkaline cleaning step was subjected to a heat treatment to modify the composition of the oxide film so that it was primarily composed of Ga oxide. It was discovered that this resulted in a Ga oxide-rich composition in the oxide film and in the vicinity of the interface between the oxide film and the GaAs layer of the GaAs single crystal substrate. GaAs single crystal substrates that have undergone this cleaning method have an oxide film with good wettability formed on their major surfaces, making it possible to effectively remove the oxide film using wet etching. Thus, the inventors have arrived at a method for producing GaAs single crystal substrates that can produce GaAs single crystal substrates with highly specular major surfaces and on which epitaxial films with reduced haze can be formed.

[0121] Each step included in the method for manufacturing a GaAs single crystal substrate according to this embodiment will now be described in detail with reference to Fig. 6. Fig. 6 is a flow chart showing the method for manufacturing a GaAs single crystal substrate according to this embodiment.

[0122] <Preparation Step S100> The method for producing the GaAs single crystal substrate includes a step (preparation step S100) of preparing a GaAs single crystal substrate precursor having a circular surface. In preparation step S100, a GaAs single crystal substrate precursor necessary for performing the cleaning step is prepared. Preparation step S100 can include a step of performing a conventionally known method for producing a GaAs single crystal substrate precursor. That is, preparation step S100 can include a step of producing a GaAs single crystal using a conventionally known production method, such as the vertical boat method, and cutting out a GaAs single crystal substrate precursor having a circular surface from the GaAs single crystal. For example, when producing a GaAs single crystal substrate precursor having a (100) plane as its main surface, it can be obtained by cutting out a GaAs single crystal grown in the <100> direction so that the (100) plane is the main surface. The preparation step S100 may also include a step of processing the GaAs single crystal substrate precursor cut from the GaAs single crystal into a desired size (for example, a disk shape having a diameter of 2 to 8 inches and a thickness of 250 to 1500 μm). As a processing method, a conventionally known method such as slicing or chamfering can be used.

[0123] <Cleaning Step S200> The method for producing a GaAs single crystal substrate includes a cleaning step S200 for obtaining the GaAs single crystal substrate from the GaAs single crystal substrate precursor. This cleaning step S200 allows a GaAs single crystal substrate having an oxide film on its main surface that can be effectively removed by wet etching to be obtained from the GaAs single crystal substrate precursor. The cleaning step S200 includes the steps of: polishing the surface of the GaAs single crystal substrate precursor to form a polished surface (surface polishing step S210); cleaning the polished surface with a first alkaline cleaning solution to form an alkali-cleaned surface (first alkaline cleaning step S220); cleaning the alkali-cleaned surface with an acid cleaning solution containing 0.3 mass ppm to 0.5 mass % acid to form an acid-cleaned surface (acid cleaning step S230); and rotating the acid-cleaned surface circumferentially at 1000 rpm. and a step (heat treatment step S250) of converting the second alkali-cleaned surface into the main surface by heating the second alkali-cleaned surface in an inert gas atmosphere under conditions of 1.1 to 3 atmospheres and 150° C. to 300° C. Each step included in the cleaning step S200 will be described in detail below.

[0124] (Surface Polishing Step S210) The surface polishing step S210 is a step of polishing the surface of the GaAs single crystal substrate precursor to form a polished surface. The surface polishing step S210 turns the surface of the GaAs single crystal substrate precursor into a mirror-finished polished surface. For example, the surface polishing step S210 can turn the surface of the GaAs single crystal substrate precursor into a polished surface having a surface roughness, expressed as an arithmetic mean roughness Ra, of 0.3 nm or less. As the polishing method in the surface polishing step S210, various polishing methods such as conventionally known mechanical polishing and chemical-mechanical polishing can be used.

[0125] (First Alkaline Cleaning Step S220) The first alkaline cleaning step S220 is a step of converting the polished surface into an alkaline-cleaned surface by cleaning the polished surface with a first alkaline cleaning solution. In the first alkaline cleaning step S220, foreign matter, impurities, etc. adhering to the polished surface of the GaAs single crystal substrate precursor can be removed using the first alkaline cleaning solution. The first alkaline cleaning solution is not particularly limited, but is preferably an aqueous solution containing 0.1 to 10 mass % of an organic alkaline compound that does not contain a metal element that affects electrical properties, such as choline, a quaternary ammonium hydroxide such as tetramethylammonium hydroxide (TMAH), or a quaternary pyridinium hydroxide.

[0126] (Acid Cleaning Step S230) The acid cleaning step S230 converts the alkali-cleaned surface into an acid-cleaned surface by cleaning the alkali-cleaned surface with an acid cleaning solution containing 0.3 mass ppm to 0.5 mass % of acid. This acid cleaning step S230 removes impurities in the first alkaline cleaning solution adhering to the alkali-cleaned surface of the GaAs single crystal substrate precursor through an oxidation reaction (etching of the alkali-cleaned surface) caused by the acid cleaning solution. In particular, the acid cleaning step S230 cleans the alkali-cleaned surface with an acid cleaning solution containing 0.3 mass ppm to 0.5 mass % of acid. This optimizes the ratio of Ga atoms to As atoms on the main surface and suppresses the formation of excess oxide film, allowing the oxide film to be efficiently removed by wet etching. In the acid cleaning step S230, the alkali-cleaned surface is preferably cleaned with an acid cleaning solution containing 0.3 mass ppm to 0.1 mass % of acid.

[0127] If the acid concentration of the acid in the pickling solution is less than 0.3 ppm by mass, the modifying effect on the alkali-cleaned surface is reduced. On the other hand, the influence of carbon dioxide (CO2) gas dissolved in the pickling solution from the atmosphere is increased, causing variations in the chemical composition of the pickled surface after the pickling step S230. If the acid concentration of the acid in the pickling solution is greater than 0.5% by mass, the acid action increases the deviation from stoichiometry of the pickled surface, which tends to result in variations in the chemical composition of the pickled surface (and ultimately the main surface in downstream processes). Here, "stoichiometry" means that when a certain compound exists, the ratio (composition) of the numbers of atoms constituting that compound exists according to the chemical formula.

[0128] The acid contained in the pickling solution is not particularly limited, but it is preferable that it has high detergency, does not contain elements that affect electrical properties (e.g., metal elements, sulfur, etc.), and is unlikely to cause serious secondary contamination or equipment degradation when droplets of the acid evaporate along with the water when the acid is dispersed within the equipment. For example, the acid contained in the pickling solution preferably contains at least one inorganic acid selected from the group consisting of hydrofluoric acid (HF), hydrochloric acid (HCl), nitric acid (HNO), and nitrous acid (HNO). Organic acids such as acetic acid, citric acid, and malic acid can also be used. Two or more of these acids can also be used in combination, for example, a combination of hydrochloric acid and nitric acid.

[0129] From the viewpoint of cleaning performance, the pickling solution preferably contains 0.3 mass ppm to 0.3 mass % hydrogen peroxide (HO). If the concentration of HO is less than 0.3 mass ppm, the effect of dissolved oxygen in the pickling solution may be increased, reducing the effectiveness of promoting impurity removal. If the concentration of HO is greater than 0.3 mass %, the etching rate may become too high, potentially causing etching steps on the pickled surface.

[0130] In the acid cleaning step S230, the GaAs single crystal substrate precursor is held so that its surface is horizontal and rotated in the circumferential direction at 100 to 800 rpm while the acid cleaning solution is supplied to the alkaline-cleaned surface. This allows for efficient acid cleaning while forming a film of the acid cleaning solution on the alkaline-cleaned surface and suppressing excessive oxidation of the alkaline-cleaned surface. If the rotation speed of the GaAs single crystal substrate precursor is lower than 100 rpm, the cleaning efficiency may not be improved, while if the rotation speed is higher than 800 rpm, the acid cleaning solution may not be able to form a film, reducing the effect of suppressing oxidation.

[0131] Furthermore, after the acid cleaning step S230, preferably immediately after the acid cleaning step S230, the acid-cleaned surface of the GaAs single crystal substrate precursor is preferably cleaned with pure water. While there are no particular limitations on the cleaning method using pure water, it is preferable to clean the acid-cleaned surface of the GaAs single crystal substrate precursor with pure water having a dissolved oxygen concentration (DO) of 100 ppb or less for 5 minutes or less. This prevents excessive oxidation of the acid-cleaned surface. To further prevent excessive oxidation, the dissolved oxygen concentration of the pure water is preferably 50 ppb or less. To minimize impurities, the total organic carbon (TOC) of the pure water is preferably 40 ppb or less. The cleaning method using pure water can also be performed by supplying the above-described pure water to the acid-cleaned surface while rotating the GaAs single crystal substrate precursor circumferentially at 100 to 800 rpm with its main surface held horizontally.

[0132] (Second Alkali Cleaning Step S240) The second alkaline cleaning step S240 involves rotating the acid-cleaned surface in the circumferential direction at a speed of 1000 rpm or more while supplying a second alkaline cleaning solution to the acid-cleaned surface at a flow rate of 0.1 L / min to 5 L / min for 30 seconds to 5 minutes to clean the acid-cleaned surface, converting it into a second alkaline cleaned surface. The second alkaline cleaning step S240 prevents excessive GaAs oxidation on the acid-cleaned surface, thereby preventing the acid-cleaned surface from becoming rich in As oxides. This allows the oxide film to be efficiently modified to a Ga oxide-rich composition in the heat treatment step S250, which will be described later.

[0133] In particular, the second alkaline cleaning solution contains a base in a range of 0.3 mass ppm to 0.5 mass %. The base is an organic alkaline compound that does not contain metal elements that affect electrical properties. Examples of such organic alkaline compounds include, but are not limited to, choline, quaternary ammonium hydroxides such as tetramethylammonium hydroxide (TMAH), and quaternary pyridinium hydroxide. This can suppress excessive GaAs oxidation on the acid-cleaned surface. If the base concentration in the second alkaline cleaning solution is less than 0.3 mass ppm, the effect of suppressing excessive oxidation on the acid-cleaned surface is reduced. On the other hand, if the base concentration in the second alkaline cleaning solution exceeds 0.5 mass %, dissolution of the acid-cleaned surface may occur, resulting in loss of surface flatness. The base concentration in the second alkaline cleaning solution is preferably 0.3 mass ppm to 0.1 mass %.

[0134] As described above, the first alkaline cleaning solution used in the first alkaline cleaning step S220 may be, for example, an aqueous solution containing 0.1 to 10 mass % of choline, a quaternary ammonium hydroxide such as tetramethylammonium hydroxide (TMAH), or a quaternary pyridinium hydroxide. The first alkaline cleaning solution and the second alkaline cleaning solution may contain at least one base selected from the group consisting of quaternary ammonium hydroxides and quaternary pyridinium hydroxides, and the first alkaline cleaning solution may contain the same type of base as the second alkaline cleaning solution. The first alkaline cleaning solution and the second alkaline cleaning solution may contain at least one base selected from the group consisting of quaternary ammonium hydroxides and quaternary pyridinium hydroxides, and the first alkaline cleaning solution may contain a different type of base from the second alkaline cleaning solution. That is, the first alkaline cleaning solution and the second alkaline cleaning solution contain at least one base selected from the group consisting of quaternary ammonium hydroxides and quaternary pyridinium hydroxides, and the first alkaline cleaning solution may contain the same or a different type of base as the second alkaline cleaning solution.

[0135] In the second alkaline cleaning step S240, the acid-cleaned surface is preferably rotated in the circumferential direction at a rotation speed of 1500 rpm or more. The upper limit of the rotation speed at which the acid-cleaned surface is rotated in the circumferential direction is not particularly limited, but is preferably 2000 rpm. The flow rate at which the second alkaline cleaning solution is supplied to the acid-cleaned surface is preferably 0.5 L / min or more and 3 L / min or less. The time for which the second alkaline cleaning solution is supplied to the acid-cleaned surface is preferably 30 seconds or more and 3 minutes or less. This more effectively suppresses excessive oxidation of GaAs on the acid-cleaned surface.

[0136] Furthermore, after the second alkaline cleaning step S240, preferably immediately after the second alkaline cleaning step S240, the second alkaline-cleaned surface can be cleaned with pure water for an extremely short time that does not adversely affect the GaAs single crystal substrate precursor. In this cleaning method using pure water, the second alkaline-cleaned surface of the GaAs single crystal substrate precursor is preferably cleaned with pure water having a dissolved oxygen concentration (DO) of 100 ppb or less for 30 seconds or less. This allows impurities adhering to the second alkaline-cleaned surface to be removed. Here, the dissolved oxygen concentration of the pure water is more preferably 50 ppb or less from the viewpoint of further suppressing the progression of excessive oxidation. In terms of minimizing impurities, the total organic carbon (TOC) of the pure water is preferably 40 ppb or less. The cleaning method using pure water can also be performed by supplying the above-described pure water to the second alkaline-cleaned surface while rotating the GaAs single crystal substrate precursor at 100 to 800 rpm with its main surface held horizontally.

[0137] (Heat Treatment Step S250) The heat treatment step S250 is a step of converting the second alkali-cleaned surface into the main surface by heat-treating the second alkali-cleaned surface in an inert gas atmosphere under conditions of 1.1 to 3 atmospheres and 150 to 300°C. The heat treatment step S250 can modify the oxide film on the second alkali-cleaned surface so that its composition is primarily composed of Ga oxide. This allows the oxide film and the vicinity of the interface between the oxide film and the GaAs layer of the GaAs single crystal substrate to have a composition rich in Ga oxide. Therefore, the GaAs single crystal substrate has an oxide film with good surface wettability, which allows the oxide film to be effectively removed by wet etching.

[0138] In the heat treatment step S250, the second alkali-cleaned surface is heat-treated in an inert gas atmosphere under conditions of 1.1 to 3 atmospheres and 150 to 300°C. The type of inert gas is not particularly limited, but argon or nitrogen is preferred. Furthermore, the heat treatment temperature is preferably 175 to 275°C. The heat treatment pressure is preferably 1.5 to 2.5 atmospheres. By performing the heat treatment under the above conditions, the oxide film can be appropriately enriched in gallium. If the heat treatment temperature is less than 150°C or the heat treatment pressure is 1.1 atmospheres, the oxide film tends to be insufficiently modified. If the heat treatment temperature exceeds 300°C or the heat treatment pressure exceeds 3 atmospheres, excessive heating may adversely affect the GaAs single crystal substrate. The heat treatment time is preferably 1 to 30 minutes.

[0139] <Wet Etching Step> As described above, the method for manufacturing a GaAs single crystal substrate according to this embodiment can provide a GaAs single crystal substrate having a main surface including an oxide film with the following characteristics: The oxide film has a Ga oxide-rich composition both within the oxide film and near the interface between the oxide film and the GaAs layer of the GaAs single crystal substrate. Even when such a GaAs single crystal substrate is subjected to a wet etching step under conventional conditions (e.g., washing with sulfuric acid (HSO:H2O:H2O) = 7:1:1) for one minute, followed by running water and drying), the oxide film has good wettability on the surface, allowing the oxide film to be effectively removed.

[0140] <Epitaxial Film Forming Step S300> The GaAs single crystal substrate manufacturing method according to this embodiment preferably includes a step of forming an epitaxial film on the main surface (epitaxial film forming step S300). The epitaxial film forming step S300 makes it possible to obtain a GaAs single crystal substrate having an epitaxial film with a reduced haze value formed on the main surface. For example, the maximum haze value on the surface of the epitaxial film can be 100 ppm or less, and the average haze value on the surface can be 2.5 ppm or less, thereby improving device characteristics.

[0141] In the epitaxial film formation step S300, a conventionally known method can be used to form an epitaxial film on the main surface of the GaAs single crystal substrate. The characteristics of the epitaxial film obtained in this step are as explained above in the section <Epitaxial Film>, and therefore will not be described again. The GaAs single crystal substrate having the epitaxial film formed on its main surface has a sufficiently small haze value, and therefore can be used in devices such as field-effect transistors, microwave diodes, and other integrated circuits.

[0142] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these. GaAs single crystal substrates of Samples 1 to 6 described below are examples, and GaAs single crystal substrates of Samples 11 to 13 are comparative examples.

[0143] [Manufacturing of GaAs Single Crystal Substrates] <Sample 1> (Preparation Step) A semi-insulating GaAs single crystal doped with carbon (C) atoms, grown by the Vertical Bridgman (VB) method, was sliced ​​and chamfered to prepare a plurality of GaAs single crystal substrate precursors, each 6 inches (150 mm) in diameter and 675 μm in thickness.

[0144] The surface of the GaAs single crystal substrate precursor was subjected to conventional mechanical polishing and chemical mechanical polishing to produce a GaAs single crystal substrate precursor having a polished surface with an arithmetic mean roughness Ra of 0.3 nm or less as specified in JIS B0601:2001 and an off-angle of 2° relative to the (100) plane.

[0145] (First alkaline cleaning step) The polished surface of the GaAs single crystal substrate precursor was immersed in an aqueous solution containing 0.5 mass % of tetramethylammonium hydroxide (first alkaline cleaning solution) at room temperature (25°C) for 10 minutes using a vertical batch system. The GaAs single crystal substrate precursor was then rinsed for 3 minutes with ultrapure water (electrical resistivity (specific resistance) of 18 MΩ cm or more, TOC (total organic carbon) of less than 10 μg / L, and particulate count of less than 100 particles / L; the same applies hereinafter).

[0146] (Acid Cleaning Step) The alkali-cleaned surface of the GaAs single crystal substrate precursor was subjected to acid cleaning using a vertical batch method using an acid cleaning solution. In the acid cleaning, the alkali-cleaned surface of the GaAs single crystal substrate precursor was immersed for 2 minutes in a hydrochloric acid aqueous solution containing 0.3 mass ppm of hydrochloric acid at room temperature (25°C). The GaAs single crystal substrate precursor was then rinsed for 3 minutes with the same ultrapure water as used in the alkali cleaning step. This converted the alkali-cleaned surface into an acid-cleaned surface.

[0147] (Second Alkali Cleaning Step) The acid-cleaned surface of the GaAs single crystal substrate precursor was subjected to alkaline cleaning by spin cleaning using a second alkaline cleaning solution. Specifically, an aqueous solution containing 0.3 mass ppm of tetramethylammonium hydroxide as a base was supplied to the acid-cleaned surface of the GaAs single crystal substrate precursor, which was rotating in the circumferential direction at 1500 rpm, at a flow rate of 3 L / min for 3 minutes. The GaAs single crystal substrate precursor was then rinsed for 3 minutes with the same ultrapure water as used in the acid cleaning step. This resulted in the acid-cleaned surface being the second alkaline-cleaned surface.

[0148] (Heat Treatment Step) The second alkali-cleaned surface of the GaAs single crystal substrate precursor was subjected to heat treatment under conditions of argon gas atmosphere, 3 atmospheres, 300°C, and 5 minutes. This resulted in the second alkali-cleaned surface being a major surface provided with a predetermined oxide film. In this manner, the required number of GaAs single crystal substrates of Sample 1 were obtained. The GaAs single crystal substrates maintained the diameter and thickness of the GaAs single crystal substrate precursor.

[0149] (Epitaxial film formation process) The GaAs single crystal substrates were washed with sulfuric acid water (H2SO4:H2O2:H2O = 7:1:1) for 1 minute, then wet-etched under running water and dried. Furthermore, one of the GaAs single crystal substrates that had undergone the wet etching was coated on its main surface with a 1 μm thick Al film as an epitaxial layer. 0.5 Ga 0.5 (Hereinafter, a GaAs single crystal substrate having an epitaxial layer grown on its main surface will also be referred to as an "epitaxial substrate.") In this way, the epitaxial substrate of Sample 1 was obtained. When growing the epitaxial layer, the GaAs single crystal substrate was heated to 550°C.

[0150] <Sample 2> The required number of GaAs single crystal substrates for Sample 2 were obtained in the same manner as Sample 1, except that in the second alkaline cleaning step, an aqueous solution containing 0.1 mass % tetramethylammonium hydroxide as a base was supplied at a flow rate of 0.5 L / min for 30 seconds to the acid-cleaned surface of the GaAs single crystal substrate precursor, which was rotating in the circumferential direction at 1500 rpm, and in the heat treatment step, the heat treatment was carried out under conditions of 1.1 atmospheres, 150°C, and 1 minute. Furthermore, a 1 μm-thick Al epitaxial layer was formed on the main surface of one of the GaAs single crystal substrates in the same manner as Sample 1. 0.5 Ga 0.5 An As layer was grown.

[0151] <Sample 11> The required number of GaAs single crystal substrates for Sample 11 were obtained in the same manner as Sample 1, except that the second alkaline cleaning step and the heat treatment step were not performed. Furthermore, one of the GaAs single crystal substrates was subjected to the same procedure as Sample 1 to form an Al epitaxial layer with a thickness of 1 μm on its main surface. 0.5 Ga 0.5 An As layer was grown.

[0152] <Sample 12> The required number of GaAs single crystal substrates for Sample 12 were obtained in the same manner as Sample 1, except that the second alkaline cleaning step was not performed. Furthermore, one of the GaAs single crystal substrates was subjected to the same procedure as Sample 1 to form an epitaxial layer of 1 μm thick Al on its main surface. 0.5 Ga 0.5 An As layer was grown.

[0153] [Sample 13] The required number of GaAs single crystal substrates for Sample 13 were obtained in the same manner as Sample 1, except that the heat treatment step was not performed. Furthermore, one of the GaAs single crystal substrates was subjected to the same procedure as Sample 1 to form an epitaxial layer of 1 μm thick Al on its main surface. 0.5 Ga 0.5 An As layer was grown.

[0154] [First Test] <Analysis of GaAs Single Crystal Substrates Using X-ray Photoelectron Spectroscopy> X-rays with an energy of 600 eV were prepared by utilizing "BL17," one of the beamlines dedicated to Sumitomo Electric Industries, Ltd., at the Kyushu Synchrotron Light Research Center in Saga Prefecture. Analysis using X-ray photoelectron spectroscopy was performed by irradiating the centers of the main surfaces of the GaAs single crystal substrates of Samples 1 to 2 and Samples 11 to 13 with these X-rays. Note that, since the GaAs single crystal substrates of Samples 1 to 2 and Samples 11 to 13 could not be placed entirely on the sample stage, test pieces were cut out from the GaAs single crystal substrates of Samples 1 to 2 and Samples 11 to 13, and these test pieces were analyzed.

[0155] The analysis conditions were as follows: Condition 1: X-ray incident energy 600 eV and photoelectron take-off angle 30° Condition 2: X-ray incident energy 600 eV and photoelectron take-off angle 45° Condition 3: X-ray incident energy 600 eV and photoelectron take-off angle 85° Size of test piece under each condition: 10 mm × 10 mm Pressure around test piece under each condition: 4 × 10 -7 Pa High-resolution XPS analyzer used under each condition (trade name: "R3000", manufactured by Scienta Omicron) Energy resolution E / ΔE: 3480 Plot interval of binding energy: 0.02 eV Accumulation time and number of accumulations at each energy value: 100 ms, 50 times.

[0156] Based on the Ga 3d spectrum and As 3d spectrum obtained by XPS analysis under the above conditions (conditions 1 to 3), the Ga + and the integrated intensity of Ga 3+ The sum of the integrated intensity of Ga—As and the integrated intensity of Ga—As is 5+ and the integral intensity of As 3+ The first integrated intensity ratio (In1) and the second integrated intensity ratio (In2), which are the ratios of the sum of the integrated intensity of As—Ga, the integrated intensity of As, and the integrated intensity of metallic As, were calculated. Furthermore, based on the Ga 3d spectrum and the As 3d spectrum obtained by the analysis under each of the above conditions (conditions 1 to 3), the Ga 3d spectrum and the As 3d spectrum in samples 1 to 2 and samples 11 to 13 were calculated. + and the integrated intensity of Ga 3+ As for the sum of the integrated intensity of 5+ and the integral intensity of As 3+ The third integrated intensity ratio (In3), fourth integrated intensity ratio (In4), and fifth integrated intensity ratio (In5), which are the ratios of the sum of the integrated intensities of the first and second integrated intensity ratios In1 and In2, respectively, were calculated. The ratios (In1 / In2) of the first integrated intensity ratio (In1) to the second integrated intensity ratio (In2) for Samples 1 to 2 and Samples 11 to 13 were also calculated. The results are shown in Table 1. Table 1 shows the Ga 3d spectrum and As 3d spectrum obtained from the XPS analysis under Condition 2. + and the integrated intensity of Ga 3+The sum of the integrated intensity of Ga—As and the integrated intensity of Ga—As is 5+ and the integral intensity of As 3+ The ratio of the integrated intensity of As-Ga to the integrated intensity of metallic As is also shown. + and the integrated intensity of Ga 3+ The "total As" means the sum of the integrated intensity of Ga—As and the integrated intensity of Ga—As. 5+ and the integral intensity of As 3+ The integral intensity of As—Ga is the sum of the integral intensity of As—Ga and the integral intensity of metal As.

[0157] <Maximum and average haze values ​​on the surface of the epitaxial film> The maximum and average haze values ​​on the surface of the epitaxial film on the epitaxial substrates of Samples 1 to 2 and Samples 11 to 13 were determined using a surface foreign matter inspection device (product name: "Surfscan 6420", manufactured by KLA-Tencor Corporation). The results are shown in Table 1.

[0158] Furthermore, based on the maximum and average values ​​of haze on the surface of the epitaxial film, the quality of the epitaxial substrates of Samples 1 and 2 and Samples 11 to 13 was judged according to the following criteria. The results are shown in Table 1. A: The maximum haze value is 20 ppm or less, and the average haze value is 2.0 ppm or less. B: The maximum haze value is more than 20 ppm and 100 ppm or less, and the average haze value is more than 2.0 ppm and 2.5 ppm or less. C: At least the maximum haze value exceeds 100 ppm, or the average haze value exceeds 2.5 ppm.

[0159] <Wettability (Contact Angle)> At room temperature (20 to 25°C) and a relative humidity of 40 to 60%, 2 μL of distilled water was dropped onto the center of the main surface of each of the GaAs single crystal substrates of Samples 1 to 2 and Samples 11 to 13, and the contact angle of the distilled water droplet formed on the main surface was measured using the θ / 2 method. A contact angle meter (for example, product name (product number) "Drop Master 500", manufactured by Kyowa Interface Science Co., Ltd.) was used to observe the droplet. The results are shown in Table 1.

[0160]

[0161] <Discussion> According to Table 1 above, the epitaxial substrates of Samples 1 and 2, which all satisfied the relationships that the second integrated intensity ratio was 0.9 or more and 1.05 or less, the third integrated intensity ratio and the fourth integrated intensity ratio were 1.0 or less, the fifth integrated intensity ratio was 0.8 or less, and the ratio of the first integrated intensity ratio to the second integrated intensity ratio was 0.5 or more and 1 or less, were judged to be of quality A or B. In contrast, the epitaxial substrates of Samples 11 to 13, which did not satisfy at least one of the above relationships, were judged to be of quality C.

[0162] [Second Test] <Production of GaAs Single Crystal Substrate> (Sample 3) A GaAs single crystal substrate of Sample 3 was obtained in the same manner as Sample 1, except that in the above preparation step, a semi-insulating GaAs single crystal doped with carbon (C) atoms was sliced ​​and chamfered to prepare a GaAs single crystal substrate precursor having a diameter of 3 inches (76 mm) and a thickness of 350 μm.

[0163] (Sample 4) In the above preparation step, a GaAs single crystal substrate of Sample 4 was obtained in the same manner as Sample 1, except that a semi-insulating GaAs single crystal doped with carbon (C) atoms was sliced ​​and chamfered to prepare a GaAs single crystal substrate precursor having a diameter of 4 inches (100 mm) and a thickness of 350 μm.

[0164] (Sample 5) In the above preparation step, a GaAs single crystal substrate of Sample 5 was obtained in the same manner as Sample 1, except that a semi-insulating GaAs single crystal doped with carbon (C) atoms was sliced ​​and chamfered to prepare a GaAs single crystal substrate precursor having a diameter of 6 inches (150 mm) and a thickness of 675 μm.

[0165] (Sample 6) In the above preparation step, a GaAs single crystal substrate of Sample 6 was obtained in the same manner as Sample 1, except that a semi-insulating GaAs single crystal doped with carbon (C) atoms was sliced ​​and chamfered to prepare a GaAs single crystal substrate precursor having a diameter of 8 inches (200 mm) and a thickness of 675 μm.

[0166] <Uniformity analysis of the main surface of GaAs single crystal substrate> (Sample 3 and Sample 4) Five test pieces cut out from each main surface of the GaAs single crystal substrate of Sample 3 and Sample 4 were analyzed in the same manner as in the first test [Analysis of GaAs single crystal substrate using X-ray photoelectron spectroscopy]. + and the integrated intensity of Ga 3+ The sum of the integrated intensity of Ga—As and the integrated intensity of Ga—As is 5+ and the integral intensity of As 3+ The sixth integrated intensity ratio (In6) was calculated, which is the ratio of the sum of the integrated intensity of As—Ga, the integrated intensity of metal As, and the integrated intensity of Ga. + and the integrated intensity of Ga 3+ As for the sum of the integrated intensity of 5+ and the integral intensity of As 3+ The seventh integrated intensity ratio (In7) was calculated as the ratio of the sum of the integrated intensities of the seventh integrated intensity ratio (In7) and the sixth integrated intensity ratio (In6). Furthermore, the ratio (In7 / In6) of the seventh integrated intensity ratio (In7) to the sixth integrated intensity ratio (In6) was calculated. Subsequently, the standard deviation and average value of In7 / In6 were calculated to determine their standard deviation / average value.

[0167] The five test pieces each include the first measurement point P1, the second measurement point P2, the third measurement point P3, the fourth measurement point P4, and the fifth measurement point P5 shown in FIG. 4 . Furthermore, the five test pieces were placed in a high-resolution XPS analyzer so that X-rays were irradiated onto the first measurement point P1, the second measurement point P2, the third measurement point P3, the fourth measurement point P4, and the fifth measurement point P5, respectively. The results are shown in Tables 2 and 3. Table 2 shows the In7 / In6 ratios, as well as their standard deviations and average values, for the GaAs single crystal substrate of Sample 3. Table 3 shows the In7 / In6 ratios, as well as their standard deviations and average values, for the GaAs single crystal substrate of Sample 4. The smaller the standard deviation / average values ​​shown in Tables 2 and 3, the more uniform the characteristics of the GaAs single crystal substrate within the plane of the main surface.

[0168] (Sample 5 and Sample 6) Nine test pieces cut out from each main surface of the GaAs single crystal substrate of Sample 5 and Sample 6 were analyzed in the same manner as in the first test [Analysis of GaAs single crystal substrate using X-ray photoelectron spectroscopy].+ and the integrated intensity of Ga 3+ The sum of the integrated intensity of Ga—As and the integrated intensity of Ga—As is 5+ and the integral intensity of As 3+ The eighth integrated intensity ratio (In8) was calculated, which is the ratio of the sum of the integrated intensity of As—Ga, the integrated intensity of metal As, and the integrated intensity of Ga. + and the integrated intensity of Ga 3+ As for the sum of the integrated intensity of 5+ and the integral intensity of As 3+ The ninth integrated intensity ratio (In9) was calculated as the ratio of the sum of the integrated intensities of the first and second integrated intensities. Furthermore, the ratio (In9 / In8) of the ninth integrated intensity ratio (In9) to the eighth integrated intensity ratio (In8) was calculated. Subsequently, the standard deviation and average value of In9 / In8 were calculated to determine the standard deviation / average value.

[0169] The nine test pieces each include the first measurement point P1, the second measurement point P2, the third measurement point P3, the fourth measurement point P4, the fifth measurement point P5, the sixth measurement point P6, the seventh measurement point P7, the eighth measurement point P8, and the ninth measurement point P9, as shown in FIG. 5 . Furthermore, the nine test pieces were placed in a high-resolution XPS analyzer so that X-rays were irradiated onto the first measurement point P1, the second measurement point P2, the third measurement point P3, the fourth measurement point P4, the fifth measurement point P5, the sixth measurement point P6, the seventh measurement point P7, the eighth measurement point P8, and the ninth measurement point P9, respectively. The results are shown in Tables 4 and 5. Table 4 shows the In9 / In8 ratios for the GaAs single crystal substrate of Sample 5, as well as their standard deviations and average values. Table 5 shows the In9 / In8 ratios for the GaAs single crystal substrate of Sample 6, as well as their standard deviations and average values. The smaller the standard deviation / average value shown in Tables 4 and 5, the more uniform the characteristics of the GaAs single crystal substrate are within the plane of the main surface.

[0170]

[0171]

[0172]

[0173]

[0174] <Discussion> According to Tables 2 and 3, in the GaAs single crystal substrates of Samples 3 and 4, the standard deviation and average value of the ratio (In7 / In6) of the seventh integrated intensity ratio (In7) to the sixth integrated intensity ratio (In6) satisfy the relationship of standard deviation / average value ≦ 0.039. According to Tables 4 and 5, in the GaAs single crystal substrates of Samples 5 and 6, the standard deviation and average value of the ratio (In9 / In8) of the ninth integrated intensity ratio (In9) to the eighth integrated intensity ratio (In8) satisfy the relationship of standard deviation / average value ≦ 0.022. In other words, it can be seen that the characteristics of the GaAs single crystal substrates of Samples 3 to 6 are sufficiently uniform within the plane of their main surfaces. Therefore, it is expected that the GaAs single crystal substrates of Samples 3 to 6 have high specularity over the entire main surfaces, and thus can form epitaxial films with reduced haze values.

[0175] Although the embodiments and examples of the present disclosure have been described above, it is also planned from the beginning that the configurations of the above-described embodiments and examples may be appropriately combined.

[0176] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the embodiments and examples described above, and is intended to include meanings equivalent to the claims and all modifications within the scope of the claims.

[0177] 1 GaAs single crystal substrate, 1m main surface, 10 X-ray generating equipment, 11 X-ray source, 12, 14 slit, 13 grating, 20 vacuum vessel, 30 electron spectrometer, 50 notch, 100 analysis system, LA As3d spectrum, LG Ga3d spectrum, L1 Ga 3+ Spectrum, L2 Ga + spectrum, L3 Ga-As spectrum, L4 As 5+ Spectrum, L5 As 3+spectrum, L6 metallic As spectrum, L7 As-Ga spectrum, P1 first measurement point, P2 second measurement point, P3 third measurement point, P4 fourth measurement point, P5 fifth measurement point, P6 sixth measurement point, P7 seventh measurement point, P8 eighth measurement point, P9 ninth measurement point, A1 to A9 measurement object, S100 preparation step, S200 cleaning step, S210 surface polishing step, S220 first alkaline cleaning step, S230 acid cleaning step, S240 second alkaline cleaning step, S250 heat treatment step, S300 epitaxial film formation step.

Claims

1. A gallium arsenide single crystal substrate having a circular main surface, the gallium arsenide single crystal substrate having a first integrated intensity ratio, a second integrated intensity ratio, a third integrated intensity ratio, a fourth integrated intensity ratio, and a fifth integrated intensity ratio, the first integrated intensity ratio and the third integrated intensity ratio being obtained by determining a spectrum of the detection intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which X-rays are irradiated onto the center of the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 30°, the second integrated intensity ratio and the fifth integrated intensity ratio are obtained by determining a spectrum of detection intensity of gallium and arsenic 3d electrons versus binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which X-rays are irradiated to the center of the main surface under conditions of X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°, and the fourth integrated intensity ratio is obtained by determining a spectrum of detection intensity of gallium and arsenic 3d electrons versus binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which X-rays are irradiated to the center of the main surface under conditions of X-ray incident energy of 600 eV and a photoelectron take-off angle of 45°, the first integrated intensity ratio and the second integrated intensity ratio are a ratio of a sum of an integrated intensity of an arsenic element present as diarsenic pentaoxide, an integrated intensity of an arsenic element present as diarsenic trioxide, an integrated intensity of an arsenic element present as gallium arsenide, and an integrated intensity of an arsenic element present as metallic arsenic to a sum of an integrated intensity of an arsenic element present as digallium monoxide, an integrated intensity of an arsenic element present as digallium trioxide, and an integrated intensity of an arsenic element present as gallium arsenide; the third integrated intensity ratio, the fourth integrated intensity ratio, and the fifth integrated intensity ratio are a ratio of a sum of an integrated intensity of an arsenic element present as diarsenic pentaoxide and an integrated intensity of an arsenic element present as diarsenic trioxide to a sum of an integrated intensity of an arsenic element present as digallium monoxide and an integrated intensity of an arsenic element present as digallium trioxide;a gallium arsenide single crystal substrate, wherein the second integrated intensity ratio is 0.9 or more and 1.05 or less, the third integrated intensity ratio and the fourth integrated intensity ratio are 1.0 or less, the fifth integrated intensity ratio is 0.8 or less, and a ratio of the first integrated intensity ratio to the second integrated intensity ratio is 0.5 or more and 1 or less.

2. The gallium arsenide single crystal substrate according to claim 1, wherein the second integrated intensity ratio is equal to or greater than 0.9 and less than 1.

04.

3. The gallium arsenide single crystal substrate according to claim 1 or 2, wherein the gallium arsenide single crystal substrate has an oxide film having a thickness of 2 nm or less on the main surface.

4. The gallium arsenide single crystal substrate according to claim 3, wherein the contact angle of said oxide film is 20 degrees or less.

5. The gallium arsenide single crystal substrate according to any one of claims 1 to 4, wherein the gallium arsenide single crystal substrate has a diameter of 75 mm or more and 205 mm or less.

6. The gallium arsenide single crystal substrate has a diameter of 75 mm or more and less than 150 mm, and the gallium arsenide single crystal substrate has a sixth integrated intensity ratio and a seventh integrated intensity ratio, and the sixth integrated intensity ratio and the seventh integrated intensity ratio are obtained by determining a spectrum of the detection intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which X-rays are irradiated to five measurement points on the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°, the sixth integrated intensity ratio is a ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentaoxide, the integrated intensity of the arsenic element present as diarsenic trioxide, the integrated intensity of the arsenic element present as gallium arsenide, and the integrated intensity of the arsenic element present as metallic arsenic to the sum of the integrated intensity of the gallium element present as digallium monoxide, the integrated intensity of the gallium element present as digallium trioxide, and the integrated intensity of the gallium element present as gallium arsenide; the seventh integrated intensity ratio is a ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentaoxide and the integrated intensity of the arsenic element present as diarsenic trioxide to the sum of the integrated intensity of the gallium element present as digallium monoxide and the integrated intensity of the gallium element present as digallium trioxide; and the standard deviation and average value of the ratio of the seventh integrated intensity ratio to the sixth integrated intensity ratio satisfy a relationship of standard deviation / average value≦0.

039.

6. The gallium arsenide single crystal substrate according to claim 1, wherein the diameter is represented by D, and two mutually orthogonal axes on the main surface passing through the center of the main surface are represented by X-axis and Y-axis. The X-axis and Y-axis coordinates (X, Y) of the five measurement points are (0, 0), (D / 4, 0), (0, D / 4), (-D / 4, 0), and (0, -D / 4), and the units of D and X and Y in the coordinates (X, Y) are mm.

7. The gallium arsenide single crystal substrate has a diameter of 150 mm or more and 205 mm or less, and the gallium arsenide single crystal substrate has an eighth integrated intensity ratio and a ninth integrated intensity ratio, and the eighth integrated intensity ratio and the ninth integrated intensity ratio are obtained by determining a spectrum of the detection intensity of gallium and arsenic 3d electrons versus the binding energy of photoelectrons emitted outside the gallium arsenide single crystal substrate based on X-ray photoelectron spectroscopy in which X-rays are irradiated to nine measurement points on the main surface under conditions of an X-ray incident energy of 600 eV and a photoelectron take-off angle of 85°, the eighth integrated intensity ratio is a ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentaoxide, the integrated intensity of the arsenic element present as diarsenic trioxide, the integrated intensity of the arsenic element present as gallium arsenide, and the integrated intensity of the arsenic element present as metallic arsenic to the sum of the integrated intensity of the gallium element present as digallium monoxide, the integrated intensity of the gallium element present as digallium trioxide, and the integrated intensity of the gallium element present as gallium arsenide; the ninth integrated intensity ratio is a ratio of the sum of the integrated intensity of the arsenic element present as diarsenic pentaoxide and the integrated intensity of the arsenic element present as diarsenic trioxide to the sum of the integrated intensity of the gallium element present as digallium monoxide and the integrated intensity of the gallium element present as digallium trioxide; and the standard deviation and average value of the ratio of the ninth integrated intensity ratio to the eighth integrated intensity ratio satisfy a relationship of standard deviation / average value≦0.022, When the diameter is represented by D and two mutually orthogonal axes on the main surface passing through the center of the main surface are the X-axis and the Y-axis, the X-axis and Y-axis coordinates (X, Y) of the nine measurement points are (0, 0), (D / 4, 0), (0, D / 4), (-D / 4, 0), (0, -D / 4), (D / 2-10, 0), (0, D / 2-10), (- (D / 2-10), 0), and (0, - (D / 2-10)), and the units of X and Y in the D and the coordinates (X, Y) are mm. The gallium arsenide single crystal substrate according to any one of claims 1 to 5.

8. The gallium arsenide single crystal substrate according to any one of claims 1 to 7, wherein the gallium arsenide single crystal substrate has an epitaxial film disposed on the main surface, the maximum haze value of the surface of the epitaxial film being 100 ppm or less, and the average haze value of the surface of the epitaxial film being 2.5 ppm or less.

9. A method for producing a gallium arsenide single crystal substrate having a circular main surface, the method comprising the steps of: preparing a gallium arsenide single crystal substrate precursor having a circular surface; and a cleaning step for obtaining the gallium arsenide single crystal substrate from the gallium arsenide single crystal substrate precursor, the cleaning step comprising: polishing the surface of the gallium arsenide single crystal substrate precursor to make the surface a polished surface; cleaning the polished surface with a first alkaline cleaning solution to make the polished surface an alkaline-cleaned surface; cleaning the alkaline-cleaned surface with an acid cleaning solution containing an acid of 0.3 mass ppm or more and 0.5 mass % or less to make the alkaline-cleaned surface an acid-cleaned surface; and supplying a second alkaline cleaning solution to the acid-cleaned surface at a flow rate of 0.1 L / min to 5 L / min for 30 seconds to 5 minutes while rotating the acid-cleaned surface in a circumferential direction at a rotation speed of 1000 rpm or more, thereby cleaning the acid-cleaned surface and making the acid-cleaned surface a second alkaline-cleaned surface. and heat-treating the second alkaline-washed surface in an inert gas atmosphere under conditions of 1.1 atm to 3 atm and 150°C to 300°C, thereby converting the second alkaline-washed surface into the main surface. The first alkaline cleaning solution contains 0.1 mass % to 10 mass % of a first base, the first base containing at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide, the second alkaline cleaning solution contains 0.3 mass ppm to 0.5 mass % of a second base, and the second base containing at least one of a quaternary ammonium hydroxide and a quaternary pyridinium hydroxide.

10. The method for producing a gallium arsenide single crystal substrate according to claim 9, further comprising the step of forming an epitaxial film on said main surface.

11. The gallium arsenide single crystal substrate according to claim 2, wherein said gallium arsenide single crystal substrate has an oxide film on said main surface having a thickness of 2 nm or less, and said oxide film has a contact angle of 20 degrees or less.

Citation Information

Patent Citations

  • Gaas wafer surface processing method

    JP1995283209A

  • GaAs SEMICONDUCTOR SUBSTRATE AND ITS MANUFACTURING METHOD

    JP2008300747A

  • Gallium arsenide substrate, epitaxial substrate, manufacturing method of gallium arsenide substrate, and manufacturing method of epitaxial substrate

    JP2020177970A

  • GaAs SUBSTRATE CLEANING METHOD, GaAs SUBSTRATE MANUFACTURING METHOD, EPITAXIAL SUBSTRATE MANUFACTURING METHOD AND GaAs WAFER