Multilayer ceramic capacitor

The multilayer ceramic capacitor design addresses crack propagation issues by dispersing stress through specific electrode configurations and layer arrangements, improving mechanical strength and reliability in miniaturized forms.

WO2024219030A1PCT designated stage expired Publication Date: 2024-10-24MURATA MFG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/001184
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-01-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Multilayer ceramic capacitors face issues with cracks extending from the tips of external electrodes into the internal structure due to stress concentration, particularly in miniaturized devices where the thickness of external electrodes becomes significant, leading to potential failures.

Method used

The design incorporates a multilayer ceramic capacitor with specific electrode configurations and layer arrangements, including alternately laminated internal electrode layers and external electrodes with unique length ratios and orientations, which disperses stress and reduces the likelihood of crack propagation by concentrating stress on the exterior surfaces.

Benefits of technology

This configuration effectively suppresses crack extension from the external electrodes into the internal structure, enhancing the mechanical strength and reliability of the multilayer ceramic capacitors, especially in compact designs where stress concentration is a concern.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024001184_24102024_PF_FP_ABST
    Figure JP2024001184_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a multilayer ceramic capacitor in which the extension of a crack from the tip of an external electrode to the inside of the multilayer ceramic capacitor can be suppressed. In a multilayer ceramic capacitor 10 according to the present invention, a first external electrode 24a and a second external electrode 24b respectively have first main surface electrode parts 26a1, 26b1, second main surface electrode parts 26a2, 26b2, third main surface electrode parts 26a3, 26b3, and fourth main surface electrode parts 26a4, 26b4 which are disposed on a first main surface 12a. On the first main surface 12a, when the length of the first main surface electrode parts 26a1, 26b1 is denoted by length A, the length of the second main surface electrode parts 26a2, 26b2 is denoted by length B, the length of the third main surface electrode parts 26a3, 26b3 is denoted by length C, and the length of the fourth main surface electrode parts 26a4, 26b4 is denoted by length D, a relationship of length A > length B > length C > length D is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer ceramic capacitors

[0001] The present invention relates to a multilayer ceramic capacitor.

[0002] In recent years, as electronic devices incorporating multilayer ceramic capacitors become smaller in size, there has been a demand for multilayer ceramic capacitors with a lower height.

[0003] For example, Patent Document 1 discloses a multilayer ceramic capacitor in which the dimension of the ceramic layers in the stacking direction is less than 0.3 mm. The multilayer ceramic capacitor described in Patent Document 1 has external electrodes configured with a base film made of a sintered metal film and a plating film disposed thereon.

[0004] Japanese Patent Application Laid-Open No. 2020-136363

[0005] However, in the multilayer ceramic capacitor described in Patent Document 1, the thickness of the external electrodes becomes large in the stacking direction of the ceramic layers, and the end portions of the films constituting the external electrodes near the center of the laminate are sometimes covered by the respective films, which may cause cracks to extend from the tips of the external electrodes into the interior of the multilayer ceramic capacitor.

[0006] Therefore, a primary object of the present invention is to provide a multilayer ceramic capacitor that can prevent cracks from propagating from the tips of the external electrodes into the interior of the multilayer ceramic capacitor.

[0007] The multilayer ceramic capacitor according to the present invention comprises a laminate including a plurality of laminated ceramic layers, the laminate including first and second main surfaces opposing each other in the lamination direction of the plurality of ceramic layers, first and second side surfaces opposing each other in a width direction perpendicular to the lamination direction, first end surfaces and second end surfaces opposing each other in a length direction perpendicular to the lamination direction and the width direction, first internal electrode layers alternately laminated with the plurality of ceramic layers and exposed at the first end surfaces, and second internal electrode layers alternately laminated with the plurality of ceramic layers and exposed at the second end surfaces, a first external electrode covering a portion of the first main surface and at least a portion of the first end surfaces of the laminate, and a second external electrode covering a portion of the first main surface and at least a portion of the second end surfaces of the laminate, Each of the first and second external electrodes has a first main-surface electrode portion disposed on the first main surface, a second main-surface electrode portion disposed on a portion of the first main-surface electrode portion, a third main-surface electrode portion disposed on a portion of the second main-surface electrode portion, and a fourth main-surface electrode portion disposed on a portion of the third main-surface electrode portion, and the multilayer ceramic capacitor has a structure in which, on the first main surface, the length of the first main-surface electrode portion in a direction connecting the center of the laminate to either a surface of the first internal electrode layer or a surface of the second internal electrode layer exposed on the surface of the laminate is length A, the length of the second main-surface electrode portion in the same direction as length A is length B, the length of the third main-surface electrode portion in the same direction as length A is length C, and the length of the fourth main-surface electrode portion in the same direction as length A is length D, such that length A > length B > length C > length D.

[0008] According to this invention, it is possible to distribute the locations where stress occurs, thereby preventing cracks from propagating from the tips of the external electrodes into the interior of the multilayer ceramic capacitor.

[0009] The above and other objects, features and advantages of the present invention will become more apparent from the following detailed description of the preferred embodiments of the present invention, which proceeds with reference to the accompanying drawings.

[0010] 1 is an external perspective view showing a multilayer ceramic capacitor as an example of a multilayer ceramic capacitor according to a first embodiment of the present invention; FIG. 2 is a front view showing a multilayer ceramic capacitor as an example of a multilayer ceramic capacitor according to the first embodiment of the present invention; FIG. 3 is a plan view showing a multilayer ceramic capacitor as an example of a multilayer ceramic capacitor according to the first embodiment of the present invention; FIG. 4 is a cross-sectional schematic view taken along line IV-IV in FIG. 1; FIG. 5 is a cross-sectional schematic view taken along line V-V in FIG. 1; FIG. 6 is a cross-sectional schematic view taken along line VI-VI in FIG. 1; FIG. 7 is a cross-sectional schematic view showing a multilayer ceramic capacitor as an example of a multilayer ceramic capacitor according to a modification of the first embodiment of the present invention; FIG. 8 is a cross-sectional schematic view showing a multilayer ceramic capacitor as an example of a multilayer ceramic capacitor according to a modification of the first embodiment of the present invention; FIG. 9 is a cross-sectional schematic view showing a multilayer ceramic capacitor as an example of a multilayer ceramic capacitor according to a modification of the first embodiment of the present invention; 11 is a cross-sectional view taken along line XII-XII in Fig. 11, illustrating the structure of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a second embodiment of the present invention. 12 is a cross-sectional view taken along line XIII-XIII in Fig. 11, illustrating the structure of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a second embodiment of the present invention. 13 is a cross-sectional view taken along line XIV-XIV in Fig. 11, illustrating the structure of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a second embodiment of the present invention. 14 is a cross-sectional view taken along line XV-XV in Fig. 11, illustrating the structure of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a second embodiment of the present invention.11 is a cross-sectional view taken along line XVI-XVI in FIG. 11 , illustrating the structure of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a second embodiment of the present invention. 12 is an exploded perspective view of the laminate shown in FIG. 11 . 13 is an external perspective view of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a third embodiment of the present invention. 14 is a cross-sectional view taken along line XV-XV in FIG. 11 , illustrating the structure of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a third embodiment of the present invention. 15 is a cross-sectional view taken along line XX-XX in FIG. 11 , illustrating the structure of a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a third embodiment of the present invention.

[0011] As an example of the present invention, a multilayer ceramic capacitor will be described below in this embodiment.

[0012] A. First Embodiment 1. Multilayer Ceramic Capacitor A multilayer ceramic capacitor 10, which is an example of a multilayer ceramic capacitor according to an embodiment of the present invention, will be described. FIG. 1 is an external perspective view showing a multilayer ceramic capacitor, which is an example of a multilayer ceramic capacitor according to the first embodiment of the present invention. FIG. 2 is a front view showing a multilayer ceramic capacitor, which is an example of a multilayer ceramic capacitor according to the first embodiment of the present invention. FIG. 3 is a plan view showing a multilayer ceramic capacitor, which is an example of a multilayer ceramic capacitor according to the first embodiment of the present invention. FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 1. FIG. 5 is a cross-sectional view taken along line V-V in FIG. 1. FIG. 6 is a cross-sectional view taken along line VI-VI in FIG. 1.

[0013] The multilayer ceramic capacitor 10 has a laminate 12 and external electrodes 24. The configuration of each will be described below in the order of the laminate 12 and the external electrodes 24.

[0014] (Laminate) The laminate 12 includes a plurality of stacked ceramic layers 14 and a plurality of internal electrode layers 16. The laminate 12 further includes a first main surface 12a and a second main surface 12b that face in a height direction x, which is the stacking direction of the plurality of ceramic layers 14, a first side surface 12c and a second side surface 12d that face in a width direction y that is perpendicular to the height direction x, and a first end surface 12e and a second end surface 12f that face in a length direction z that is perpendicular to the height direction x and the width direction y. The corners and ridges of the laminate 12 are rounded. The corners refer to the intersections of three adjacent surfaces of the laminate 12, and the ridges refer to the intersections of two adjacent surfaces of the laminate 12. Furthermore, unevenness may be formed on part or all of the first main surface 12a and the second main surface 12b, the first side surface 12c and the second side surface 12d, and the first end surface 12e and the second end surface 12f.

[0015] As shown in Figures 4 and 5, the laminate 12 has, in the height direction x connecting the first main surface 12a and the second main surface 12b, an effective layer portion 15a in which a plurality of internal electrode layers 16 face each other, a first outer layer portion 15b1 formed from a plurality of ceramic layers 14 located between the first main surface 12a and the internal electrode layer 16 located closest to the first main surface 12a, and a second outer layer portion 15b2 formed from a plurality of ceramic layers 14 located between the second main surface 12b and the internal electrode layer 16 located closest to the second main surface 12b.

[0016] The first outer layer portion 15b1 is located on the first main surface 12a side of the laminate 12 and is an assembly of multiple ceramic layers 14 located between the first main surface 12a and the internal electrode layer 16 closest to the first main surface 12a.

[0017] The second outer layer portion 15b2 is located on the second main surface 12b side of the laminate 12 and is an assembly of multiple ceramic layers 14 located between the second main surface 12b and the internal electrode layer 16 closest to the second main surface 12b.

[0018] The area sandwiched between the first outer layer portion 15b1 and the second outer layer portion 15b2 is the effective layer portion 15a.

[0019] The laminate 12 includes side portions 22a (W gaps) of the laminate 12 located between the effective layer portion 15a and the first side surface 12c and between the effective layer portion 15a and the second side surface 12d. Furthermore, the laminate 12 includes end portions 22b (L gaps) of the laminate 12 located between the effective layer portion 15a and the first end surface 12e and between the effective layer portion 15a and the second end surface 12f and including lead electrodes of either the first internal electrode layer 16a or the second internal electrode layer 16b described below.

[0020] The number of ceramic layers 14 to be laminated is not particularly limited, but is preferably 3 to 1000, including first outer layer portion 15b1 and second outer layer portion 15b2. The thickness of ceramic layer 14 is preferably 2.0 μm to 80 μm.

[0021] The ceramic layer 14 may be formed from, for example, a dielectric material. Examples of the dielectric material include dielectric ceramics primarily composed of BaTiO3, CaTiO3, SrTiO3, or CaZrO3. Depending on the desired properties of the laminate, a material containing a minor component, such as a manganese compound, an iron compound, a chromium compound, a cobalt compound, or a nickel compound, may be added.

[0022] The ceramic layer 14 may have a plurality of crystal grains containing a perovskite-type compound having a basic structure of BaTiO3.

[0023] The thinner the ceramic layer 14, the greater the capacitance of the capacitor, so the crystal grain size is preferably 1 μm or less.

[0024] Here, the multiple inner ceramic layers 14 constituting the effective layer portion 15a are formed so as to be sandwiched between the first internal electrode layer 16a and the second internal electrode layer 16b of the multiple internal electrode layers 16. The inner ceramic layers 14 are composed of dielectric ceramic particles having a perovskite structure, with a perovskite-type compound containing, for example, Ba and Ti as the main component. Furthermore, at least one of Si, Mg, Ba, and Mn may be added as an additive to these main components. The additive is present between the ceramic particles.

[0025] The ceramic layers 14 for the outer layers constituting the first outer layer portion 15b1 and the second outer layer portion 15b2 are formed from the same dielectric ceramic material as the ceramic layers 14 for the inner layers. The ceramic layers 14 for the outer layers may be formed from a different material from the ceramic layers 14 for the inner layers. When the ceramic layers 14 for the first outer layer portion 15b1 and the second outer layer portion 15b2 each have a multi-layer structure, it is preferable that the segregated Si portions of the ceramic layers 14 for the other outer layers are greater than the segregated Si portions of the ceramic layers 14 located closest to the first internal electrode layer 16a and the second internal electrode layer 16b. This improves the flexural strength of the multilayer ceramic capacitor from the height direction x. The ceramic layers 14 for the first outer layer portion 15b1 and the second outer layer portion 15b2 may each have a multi-layer structure or a single-layer structure.

[0026] (Internal Electrode Layers) As shown in Fig. 4 and Fig. 5, the internal electrode layers 16 include first internal electrode layers 16a and second internal electrode layers 16b. The first internal electrode layers 16a and the second internal electrode layers 16b are alternately stacked with the ceramic layers 14 interposed therebetween.

[0027] The first internal electrode layer 16a is disposed on the surface of the ceramic layer 14. The first internal electrode layer 16a has a first opposing electrode portion 18a that faces the second internal electrode layer 16b, and a first lead electrode portion 20a that is located on one end side of the first internal electrode layer 16a and extends from the first opposing electrode portion 18a to the first end face 12e of the laminate 12. The end of the first lead electrode portion 20a is led out to and exposed at the first end face 12e.

[0028] The shape of the first opposing electrode portion 18a of the first internal electrode layer 16a is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the first opposing electrode portion 18a may be tapered in plan view, with a slope increasing in either direction.

[0029] The shape of the first lead electrode portion 20a of the first internal electrode layer 16a is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the first lead electrode portion 20a may be tapered in plan view, with a slope increasing in either direction.

[0030] The width of the first opposing electrode portion 18a of the first internal electrode layer 16a and the width of the first extraction electrode portion 20a of the first internal electrode layer 16a may be formed to be the same width, or one of them may be formed to be narrower in width.

[0031] The second internal electrode layer 16b is arranged on a surface of a ceramic layer 14 different from the ceramic layer 14 on which the first internal electrode layer 16a is arranged. The second internal electrode layer 16b has a second opposing electrode portion 18b facing the first internal electrode layer 16a, and a second extraction electrode portion 20b located on one end side of the second internal electrode layer 16b and extending from the second opposing electrode portion 18b to a second end face 12f of the laminate 12. The second extraction electrode portion 20b has an end portion extended to and exposed at the second end face 12f.

[0032] The shape of the second opposing electrode portion 18b of the second internal electrode layer 16b is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the second opposing electrode portion 18b may be tapered in plan view, with a slope increasing in either direction.

[0033] The shape of the second extraction electrode portion 20b of the second internal electrode layer 16b is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the second extraction electrode portion 20b may be tapered in plan view, with a slope increasing in either direction.

[0034] The width of the second opposing electrode portion 18b of the second internal electrode layer 16b and the width of the second extraction electrode portion 20b of the second internal electrode layer 16b may be formed to be the same width, or one of them may be formed to be narrower in width.

[0035] The first internal electrode layer 16a and the second internal electrode layer 16b can be made of an appropriate conductive material, for example, metals such as Ni, Cu, Ag, Pd, Au, etc., or alloys containing at least one of these metals, such as an Ag-Pd alloy, but are not limited thereto. In this embodiment, the first opposing electrode portion 18a of the first internal electrode layer 16a and the second opposing electrode portion 18b of the second internal electrode layer 16b face each other via the ceramic layer 14, thereby forming capacitance and exhibiting capacitor characteristics.

[0036] (External Electrodes) As shown in FIGS. 1 to 6, external electrodes 24 are disposed on the first end face 12e side and the second end face 12f side of the laminate 12.

[0037] The external electrode 24 includes a base electrode layer 26 and a plating layer 28 formed to cover the base electrode layer 26 .

[0038] The external electrode 24 includes a first external electrode 24a and a second external electrode 24b.

[0039] The first external electrode 24a is disposed on the first end face 12e and part of the first main surface 12a of the laminate 12. In this case, the first external electrode 24a is electrically connected to the first extraction electrode portion 20a of the first internal electrode layer 16a. Note that the first external electrode 24a may extend slightly around to part of the first side face 12c and part of the second side face 12d.

[0040] The second external electrode 24b is disposed on the second end face 12f and part of the first main surface 12a of the laminate 12. In this case, the second external electrode 24b is electrically connected to the second extraction electrode portion 20b of the second internal electrode layer 16b. The second external electrode 24b may extend slightly around part of the first side face 12c and part of the second side face 12d.

[0041] The thickness of the first external electrode 24a and the second external electrode 24b is preferably, for example, about 0.5 μm or more and 12 μm or less.

[0042] (Underlying Electrode Layer) The underlying electrode layer 26 includes a first underlying electrode layer 26a and a second underlying electrode layer 26b.

[0043] The first base electrode layer 26 a is formed to cover a portion of the first main surface 12 a on the side of the first end face 12 e of the laminate 12 and the first end face 12 e of the laminate 12 .

[0044] The second base electrode layer 26 b is formed to cover a portion of the first main surface 12 a on the second end face 12 f side of the laminate 12 and the second end face 12 f of the laminate 12 .

[0045] The first and second base electrode layers 26a and 26b each have a first, second, third, and fourth principal surface electrode portion. Specifically, the first base electrode layer 26a has a configuration in which a first, second, third, and fourth principal surface electrode portion 26a1, 26a2, 26a3, and 26a4 are stacked. The second base electrode layer 26b has a configuration in which a first, second, third, and fourth principal surface electrode portion 26b1, 26b2, 26b3, and 26b4 are stacked.

[0046] (Principal surface electrode portion) As shown in FIG. 4, the first principal surface electrode portion 26a1 is arranged on the surface of the laminate 12, the second principal surface electrode portion 26a2 is arranged on the surface of the first principal surface electrode portion 26a1, the third principal surface electrode portion 26a3 is arranged on the surface of the second principal surface electrode portion 26a2, and the fourth principal surface electrode portion 26a4 is arranged on the surface of the third principal surface electrode portion 26a3.

[0047] Here, a direction on the first main surface 12a connecting an end of the first main-surface electrode portion of the first base electrode layer toward the center of the laminate to a surface at which the first internal electrode layer is exposed on the surface of the laminate is defined, specifically, a direction connecting a first end 26a1t of the first main-surface electrode portion 26a1 of the first base electrode layer 26a toward the center of the laminate 12 to a first end surface 12e of the laminate 12 at which the first extraction electrode portion 20a of the first internal electrode layer 16a is exposed (hereinafter referred to as a first reference direction). When the length of the first main-surface electrode portion 26a1 in the first reference direction is length A, the length of the second main-surface electrode portion 26a2 in the same direction as length A is length B, the length of the third main-surface electrode portion 26a3 in the same direction as length A is length C, and the length of the fourth main-surface electrode portion 26a4 in the same direction as length A is length D, the relationship is length A > length B > length C > length D.

[0048] As a result, on the first main surface 12a, the first main surface electrode portion 26a1, the second main surface electrode portion 26a2, the third main surface electrode portion 26a3, and the fourth main surface electrode portion 26a4 of the first underlying electrode layer 26a have first end portions 26a1t, second end portions 26a2t, third end portions 26a3t, and fourth end portions 26a4t on the central side of the laminate 12 that are not aligned with each other, so that the stress of the external electrode 24 toward the central side of the laminate 12 that occurs when the solder shrinks can be dispersed.

[0049] Furthermore, a direction on the first main surface 12a connecting an end portion of the first main-surface electrode portion of the second base electrode layer toward the center of the laminate to a surface at which the second internal electrode layer is exposed on the surface of the laminate, specifically, a direction connecting a first end portion 26b1t of the first main-surface electrode portion 26b1 of the second base electrode layer 26b toward the center of the laminate 12 to a second end surface 12f of the laminate 12 at which the second extraction electrode portion 20b of the second internal electrode layer 16b is exposed (hereinafter, a second reference direction) is defined. When the length of the first main-surface electrode portion 26b1 in the second reference direction is length A, the length of the second main-surface electrode portion 26b2 in the same direction as length A is length B, the length of the third main-surface electrode portion 26b3 in the same direction as length A is length C, and the length of the fourth main-surface electrode portion 26b4 in the same direction as length A is length D, the relationship is length A > length B > length C > length D.

[0050] As a result, on the first main surface 12a, the first main surface electrode portion 26b1, the second main surface electrode portion 26b2, the third main surface electrode portion 26b3, and the fourth main surface electrode portion 26b4 of the second base electrode layer 26b have their first end 26b1t, second end 26b2t, third end 26b3t, and fourth end 26b4t on the central side of the laminate 12 that are not aligned with each other, so that the stress of the external electrode 24 toward the central side of the laminate 12 that occurs when the solder shrinks can be dispersed.

[0051] Furthermore, as shown in FIG. 4, in the first reference direction, it is preferable that the first end 26a1t of the first principal surface electrode portion 26a1 is not covered by the second principal surface electrode portion 26a2, the second end 26a2t of the second principal surface electrode portion 26a2 is not covered by the third principal surface electrode portion 26a3, and the third end 26a3t of the third principal surface electrode portion 26a3 is not covered by the fourth principal surface electrode portion 26a4.

[0052] This allows the stress acting on the first end 26a1t to the fourth end 26a4t of each of the first principal surface electrode portion 26a1 to the fourth principal surface electrode portion 26a4 to be concentrated outside the laminate 12 (towards the first end face 12e) rather than at these ends, thereby dispersing the stress and improving the mechanical strength.

[0053] Similarly, in the second reference direction, it is preferable that the first end 26b1t of the first principal surface electrode portion 26b1 is not covered by the second principal surface electrode portion 26b2, the second end 26b2t of the second principal surface electrode portion 26b2 is not covered by the third principal surface electrode portion 26b3, and the third end 26b3t of the third principal surface electrode portion 26b3 is not covered by the fourth principal surface electrode portion 26b4.

[0054] This allows the stress acting on the first end 26b1t to the fourth end 26b4t of each of the first to fourth principal surface electrode portions 26b1 to 26b4 to be concentrated outside the laminate 12 (towards the second end face 12f) rather than at these ends, thereby dispersing the stress and improving the mechanical strength.

[0055] Next, the first to fourth main surface electrode portions constituting the base electrode layer 26 can be formed by a thin film forming method such as sputtering or vapor deposition, or by screen printing.

[0056] (In the case of thin film formation method) When each of the first to fourth principal surface electrode portions is formed by a thin film formation method, they can be made of a metal such as Cu, Cr, Au, Pt, Ag, Sn, Ti, or Ni.

[0057] The first to fourth principal surface electrode portions can be configured in consideration of their respective functions. For example, the first principal surface electrode portions 26a1 and 26b1 can be made of NiCr or the like in consideration of adhesion to ceramic.

[0058] In this case, the thickness of each of the first to fourth principal surface electrode portions in the direction connecting the first principal surface 12 a and the second principal surface 12 b of the laminate 12 is 10 μm or less, which allows the dimension of the multilayer ceramic capacitor 10 in the lamination direction to be sufficiently small, thereby enabling a low profile.

[0059] Furthermore, each of the first to fourth principal surface electrode portions may be disposed on at least one of the first principal surface 12a or the second principal surface 12b of the laminate 12. In other words, when each of the first to fourth principal surface electrode portions is disposed only on the first principal surface 12a, a direct plating layer (described later) is not disposed on the second principal surface 12b, or even if it is disposed on the second principal surface 12b, it is preferable that the amount of the direct plating layer that wraps around onto the first principal surface 12a is greater than the amount of the direct plating layer that wraps around onto the second principal surface 12b.

[0060] The thickness of each of the first to fourth principal-surface electrode portions can be changed by changing the sputtering distance. For example, the thickness can be increased by shortening the sputtering distance to the area where the principal-surface electrode portion is to be formed.

[0061] (Screen Printing) When each of the first to fourth principal surface electrode portions is formed by screen printing, it contains a ceramic component and a metal.

[0062] The metal includes at least one of Cu, Ni, Ag, Pd, an Ag—Pd alloy, and Au.

[0063] Furthermore, each of the first principal-surface electrode portions 26a1 and 26b1 may contain the same main component as the ceramic layer 14. For example, when the ceramic layer 14 is made of BaTiO3, each of the first principal-surface electrode portions 26a1 and 26b1 preferably contains at least a portion of BaTiO3, thereby improving the adhesion between the laminate 12 and each of the first principal-surface electrode portions 26a1 and 26b1.

[0064] Furthermore, when each of the first principal-surface electrode portions 26a1 and 26b1 contains the same main component as the ceramic layer 14, the adhesion can be further improved by simultaneously firing the laminate 12 and each of the first principal-surface electrode portions 26a1 and 26b1. In this case, the metal component is preferably Ni, Cu, or the like, but can be changed as appropriate depending on the metal component of the internal electrode layer 16.

[0065] The thickness of the portion of each of the first to fourth principal surface electrode portions that is disposed on the first principal surface 12a is preferably 0.5 μm or more and 3.0 μm or less.

[0066] (Plating Layer) The plating layer 28 includes a first plating layer 28a and a second plating layer 28b.

[0067] The first plating layer 28a is disposed so as to cover the first principal surface electrode portion 26a1 to the fourth principal surface electrode portion 26a4 as the first base electrode layer 26a.

[0068] The second plating layer 28b is disposed so as to cover the first to fourth principal surface electrode portions 26b1 to 26b4 as the second base electrode layer 26b.

[0069] The plating layer 28 is formed of multiple layers. That is, the plating layer 28 has an underplating layer 30 and a top plating layer 32. The underplating layer 30 includes a first underplating layer 30a included in the first plating layer 28a and a second underplating layer 30b included in the second plating layer 28b. The top plating layer 32 includes a first top plating layer 32a included in the first plating layer 28a and a second top plating layer 32b included in the second plating layer 28b.

[0070] The first underplating layer 30a of the underplating layer 30 is disposed so as to cover the fourth principal surface electrode portion 26a4 of the first base electrode layer 26a.

[0071] The second underplating layer 30b of the underplating layer 30 is disposed so as to cover the fourth main surface electrode portion 26b4 of the second base electrode layer 26b.

[0072] The underplating layer 30 preferably contains at least one metal selected from Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, Zn, etc., or an alloy containing such a metal. In particular, in this embodiment, the underplating layer 30 is preferably a Cu plating layer.

[0073] The surface plating layer 32 may be formed of multiple layers. In this embodiment, the surface plating layer 32 has a two-layer structure including a middle plating layer 34 that is a Ni plating layer and a top plating layer 36 that is a Sn plating layer.

[0074] In the top plating layer 32, the first intermediate plating layer 34a covers the first under plating layer 30a, and the first upper plating layer 36a covers the first intermediate plating layer 34a. The second intermediate plating layer 34b covers the second under plating layer 30b, and the second upper plating layer 36b covers the second intermediate plating layer 34b.

[0075] The middle plating layer 34, which is a Ni plating layer, can prevent the lower plating layer 30 from being eroded by solder when mounting the multilayer ceramic capacitor 10. Furthermore, the upper plating layer 36, which is a Sn plating layer, improves the wettability of the solder when mounting the multilayer ceramic capacitor 10, facilitating mounting. When the plating layer 28 has a three-layer structure, in addition to the above, it is preferable that the layers are laminated in the order of Sn plating layer, Ni plating layer, and Sn plating layer.

[0076] The metal content per unit volume of the plating layer 28 is preferably 99% by volume or more.

[0077] The thickness of each of the plating layers 28 is preferably 0.5 μm or more and 6.0 μm or less.

[0078] The dimension in the length direction z of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 24a, and the second external electrode 24b is defined as dimension L, the dimension in the height direction x of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 24a, and the second external electrode 24b is defined as dimension T, and the dimension in the width direction y of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 24a, and the second external electrode 24b is defined as dimension W.

[0079] The dimensions of the multilayer ceramic capacitor 10 are preferably such that the L dimension in the length direction z is 0.2 mm to 3.2 mm, the T dimension in the height direction x is 0.04 mm to 2.5 mm, and the W dimension in the width direction y is 0.1 mm to 2.5 mm.

[0080] In the multilayer ceramic capacitor 10 shown in FIG. 1, the first base electrode layer 26a is configured by laminating a first principal surface electrode portion 26a1, a second principal surface electrode portion 26a2, a third principal surface electrode portion 26a3, and a fourth principal surface electrode portion 26a4, and the second base electrode layer 26b is configured by laminating a first principal surface electrode portion 26b1, a second principal surface electrode portion 26b2, a third principal surface electrode portion 26b3, and a fourth principal surface electrode portion 26b4.

[0081] On the first main surface 12a, when the length of the first main surface electrode portion 26a1 in a first reference direction connecting the end portion of the first main surface electrode portion of the first base electrode layer toward the center of the laminate 12 to the surface at which the first internal electrode layer is exposed on the surface of the laminate 12, specifically, connecting the first end portion 26a1t of the first main surface electrode portion 26a1 of the first base electrode layer 26a toward the center of the laminate 12 to the first end surface 12e of the laminate 12 at which the first extraction electrode portion 20a of the first internal electrode layer 16a is exposed, is length A, the length of the second main surface electrode portion 26a2 in the same direction as length A is length B, the length of the third main surface electrode portion 26a3 in the same direction as length A is length C, and the length of the fourth main surface electrode portion 26a4 in the same direction as length A is length D, then length A > length B > length C > length D.

[0082] On the first main surface 12a, when the length of the first main surface electrode portion 26b1 in a direction connecting the end portion of the first main surface electrode portion of the second base electrode layer toward the center of the laminate 12 to the surface at which the second internal electrode layer is exposed on the surface of the laminate 12, specifically, a second reference direction connecting the first end portion 26b1t of the first main surface electrode portion 26b1 of the second base electrode layer 26b toward the center of the laminate 12 to the second end face 12f of the laminate 12 at which the second extraction electrode portion 20b of the second internal electrode layer 16b is exposed, is length A, the length of the second main surface electrode portion 26b2 in the same direction as length A is length B, the length of the third main surface electrode portion 26b3 in the same direction as length A is length C, and the length of the fourth main surface electrode portion 26b4 in the same direction as length A is length D, then length A > length B > length C > length D.

[0083] As a result, the first end 26a1t, second end 26a2t, third end 26a3t, and fourth end 26a4t of each of the first principal surface electrode portions 26a1 to 26a4 of the first base electrode layer 26a are not aligned with one another on the central side of the laminate 12, and the first end 26b1t, second end 26b2t, third end 26b3t, and fourth end 26b4t of each of the first principal surface electrode portions 26b1 to 26b4 of the second base electrode layer 26b are not aligned with one another on the central side of the laminate 12, so that stress on the central side of the external electrode 24 of the laminate 12 that occurs during solder contraction can be dispersed.

[0084] The effect of the present invention is more pronounced when the T dimension of the multilayer ceramic capacitor 10 is 150 μm or less. Furthermore, when the T dimension is 50 μm or less, the multilayer ceramic capacitor 10 is thinned, and reliability in mechanical strength becomes more important, so the effect of the present invention is more pronounced.

[0085] In addition, in the multilayer ceramic capacitor 10 shown in FIG. 1, the first to fourth principal surface electrode portions 26a1 to 26a4 of the first base electrode layer 26a and the first to fourth principal surface electrode portions 26b1 to 26b4 of the second base electrode layer 26b are each formed to extend around to the first end face 12e and the second end face 12f, which are surfaces perpendicular to the first principal surface 12a.

[0086] As a result, the points (ridges, seams) where the first main surface 12a intersects with the first end face 12e and the second end face 12f are continuously covered with the first base electrode layer 26a and the second base electrode layer 26b, respectively, thereby improving moisture resistance.

[0087] At this time, it is preferable to form the first to fourth principal surface electrode portions 26a1 to 26a4 and the first to fourth principal surface electrode portions 26b1 to 26b4 of each of the external electrodes 24 by a sputtering method. This makes it possible to form the first external electrode 24a and the second external electrode 24b, which are the external electrodes 24, with a thickness of 10 μm or less on each of the first end face 12e and the second end face 12f that are orthogonal to the first main face 12a, and therefore makes it possible to reduce the dimensions of the multilayer ceramic capacitor 10 in the length direction z and the width direction y.

[0088] The lengths A, B, C, and D of the first to fourth principal surface electrode portions 26a1 to 26a4 of the first base electrode layer 26a and the first to fourth principal surface electrode portions 26b1 to 26b4 of the second base electrode layer 26b can be measured by the following measurement method.

[0089] For example, in the width direction y connecting the first side surface 12c and the second side surface 12d of the laminate 12, the cross section is polished to 1 / 2 of the W dimension in the width direction y. The polished cross section is then observed using a VHX. Note that, if the first lead electrode portion 20a of the first internal electrode layer 16a or the second lead electrode portion 20b of the second internal electrode layer 16b is not present in the cross section, for example, it is also possible to observe the principal surface electrode portion directly above the first lead electrode portion 20a of the first internal electrode layer 16a or the second lead electrode portion 20b of the second internal electrode layer 16b by further polishing to 1 / 4 of the W dimension in the width direction y.

[0090] At this time, if the first to fourth principal-surface electrode portions 26a1 to 26a4 and the first to fourth principal-surface electrode portions 26b1 to 26b4 of the second base electrode layer 26b are formed by a method such as sputtering, it is also possible to observe the differences in the components of each principal-surface electrode portion using WDX or EDX using a TEM. For example, if the thickness of each layer of the principal-surface electrode portion is about 1 μm, the composition of each layer can be confirmed by exposing a cross section (¼ LT cross section) of the center of the external electrode 24 and performing composition analysis using WDX. Furthermore, if the thickness of each layer of the principal-surface electrode portion is 1 μm or less, the detailed structure can be confirmed using EDX using a TEM.

[0091] When a TEM is used, the field of view is about 1 μm, and the magnification is 20k.

[0092] When the ridge portions of the laminate 12 are rounded, each of the lengths A, B, C, and D is defined by the straight-line distance between a perpendicular line drawn from the exposed portion of the lead electrode portion closest to the first main surface 12a, of the first lead electrode portion 20a of the first internal electrode layer 16a or the second lead electrode portion 20b of the second internal electrode layer 16b, toward the mounting surface or the first main surface 12a of the multilayer ceramic capacitor 10, and a desired one of the first end 26a1t to the fourth end 26a4t and the first end 26b1t to the fourth end 26b4t of the first main surface electrode portion 26a1 to the fourth main surface electrode portion 26a4 and the first main surface electrode portion 26b1 to the fourth main surface electrode portion 26b4 of the second base electrode layer 26b.

[0093] (1) First Modification Next, a description will be given of a multilayer ceramic capacitor 110 according to a first modification of the first embodiment of the present invention. Fig. 7 is a schematic cross-sectional view showing a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a first modification of the first embodiment of the present invention. However, the same components as those in Figs. 1 to 6 are designated by the same reference numerals, and detailed description thereof will be omitted.

[0094] As shown in FIG. 7 , in the multilayer ceramic capacitor 110 according to the first modified example, the plating layer 28 of the external electrode 24 has two plating layers, namely, an underplating layer 30 and a top plating layer 32, and the top plating layer 32 is formed from a single layer.

[0095] As in the first embodiment, the underplating layer 30 preferably contains at least one metal selected from, for example, Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, or Zn, or an alloy containing such a metal.

[0096] The surface plating layer 32 is preferably formed as a Sn plating layer, which improves the wettability of the solder when mounting the multilayer ceramic capacitor 10, making it easier to mount.

[0097] The multilayer ceramic capacitor 210 according to the first modified example shown in FIG. 7 has the same effects as the multilayer ceramic capacitor 10 shown in FIG.

[0098] (2) Second Modification Next, a multilayer ceramic capacitor 210 according to a second modification of the first embodiment of the present invention will be described. Fig. 8 is a schematic cross-sectional view showing a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to the second modification of the first embodiment of the present invention. However, the same components as those in Figs. 1 to 6 are designated by the same reference numerals, and detailed description thereof will be omitted.

[0099] As shown in FIG. 8, in a multilayer ceramic capacitor 210 according to the second modification, the plating layer 28 of the external electrode 24 is formed of a single plating layer.

[0100] The plating layer 28 is preferably formed as a Sn plating layer, which improves the wettability of the solder when mounting the multilayer ceramic capacitor 210, making it easier to mount.

[0101] The multilayer ceramic capacitor 210 according to the second modified example shown in FIG. 8 has the same effects as the multilayer ceramic capacitor 10 shown in FIG.

[0102] (3) Third Modification Next, a multilayer ceramic capacitor 310 according to a third modification of the first embodiment of the present invention will be described. Fig. 9 is a schematic cross-sectional view showing a multilayer ceramic capacitor that is an example of a multilayer ceramic capacitor according to a second modification of the first embodiment of the present invention. However, the same components as those in Figs. 1 to 6 are designated by the same reference numerals, and detailed description thereof will be omitted.

[0103] 9 , in the first external electrode 24a, the first base electrode layer 26a is disposed only on a portion of the first main surface 12a of the laminate 12, and the first plating layer 28a covers the first base electrode layer 26a and is disposed on the surface of the first end face 12e and a portion of the first main surface 12a of the laminate 12. In this case, the first external electrode 24a is electrically connected to the first lead electrode portion 20a of the first internal electrode layer 16a via the first plating layer 28a.

[0104] Similarly, in the second external electrode 24b, the second base electrode layer 26b is disposed only on a portion of the first main surface 12a of the laminate 12, and the second plating layer 28b covers the second base electrode layer 26b and is disposed on the surface of the second end face 12f and on a portion of the first main surface 12a of the laminate 12. In this case, the second external electrode 24b is electrically connected to the second extraction electrode portion 20b of the second internal electrode layer 16b via the second plating layer 28b.

[0105] That is, in this modification, the plating layer 28 is a direct plating layer formed directly on the surface of the laminate 12 .

[0106] In this modified example, similar to the multilayer ceramic capacitor 10 of FIG. 1, the plating layer 28 as a direct plating layer has a lower plating layer 30 and a top plating layer 32, and the top plating layer 32 further has a two-layer structure of a middle plating layer 34 and a top plating layer 36.

[0107] In such a case, a catalyst may be applied to the surface of the laminate 12 as a pretreatment, and then the plating layer 28 may be directly formed as a plating layer.

[0108] The plating layer 28 as a direct plating layer preferably contains at least one metal selected from, for example, Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, Zn, etc., or an alloy containing such a metal. For example, when the first internal electrode layer 16a and the second internal electrode layer 16b are formed using Ni, in the plating layer 28 as a direct plating layer, the first under plating layer 30a and the second under plating layer 30b of the under plating layer 30 directly connected to the first lead electrode portion 20a of the first internal electrode layer 16a and the second lead electrode portion 20b of the second internal electrode layer 16b are preferably formed using Cu, which has good bonding properties with Ni.

[0109] The top plating layer 32 preferably has a two-layer structure of a middle plating layer 34 which is a Ni plating layer and a top plating layer 36 which is a Sn plating layer, similar to the multilayer ceramic capacitor 10 of FIG.

[0110] The thickness of each of the directly plated layers 28 is preferably 1 μm or more and 6 μm or less.

[0111] Each of the directly plated layers 28 preferably does not contain glass, and the metal content per unit volume of the plated layer is preferably 99% by volume or more.

[0112] 9 provides the following effect in addition to the same effect as that of the multilayer ceramic capacitor 10 of FIG. 1. That is, since the first end face 12 e and the second end face 12 f are not provided with the first principal surface electrode portion 26 a1, the second principal surface electrode portion 26 a2, the third principal surface electrode portion 26 a3, and the fourth principal surface electrode portion 26 a4 of the first base electrode layer 26 a, and the first principal surface electrode portion 26 b1, the second principal surface electrode portion 26 b2, the third principal surface electrode portion 26 b3, and the fourth principal surface electrode portion 26 b4 of the second base electrode layer 26 b, the size of the L dimension in the longitudinal direction z can be reduced, thereby making it possible to reduce the size of the multilayer ceramic capacitor.

[0113] (4) Fourth Modification Next, a multilayer ceramic capacitor 410 according to a fourth modification of the first embodiment of the present invention will be described. Fig. 10 is a cross-sectional schematic diagram showing a multilayer ceramic capacitor as an example of the multilayer ceramic capacitor according to the fourth modification of the first embodiment of the present invention. However, the same components as those in Figs. 1 to 6 are designated by the same reference numerals, and detailed description thereof will be omitted.

[0114] As shown in FIG. 10 , a multilayer ceramic capacitor 410 according to the fourth modified example has the same configuration as the multilayer ceramic capacitor 10 of FIG. 1 , except that the first external electrode 24 a does not include a plating layer and includes only the first to fourth principal surface electrode portions 26 a 1 to 26 a 4, and the second external electrode 24 b does not include a plating layer and includes only the first to fourth principal surface electrode portions 26 b 1 to 26 b 4.

[0115] 10 , the multilayer ceramic capacitor 310 according to the fourth modification example has the following effect in addition to the same effect as that of the multilayer ceramic capacitor 10 shown in FIG. 1. That is, no plating layer is formed, and the external electrodes 24 are formed only by the first to fourth principal-surface electrode portions 26 a 1 to 26 a 4 and the first to fourth principal-surface electrode portions 26 b 1 to 26 b 4, which are base electrode layers. This reduces the T dimension in the height direction x and the L dimension in the length direction z, thereby making it possible to reduce the size of the multilayer ceramic capacitor.

[0116] Furthermore, in the multilayer ceramic capacitor 310 according to the fourth modified example shown in FIG. 10 , the fourth principal surface electrode portion 26 a4 of the first base electrode layer 26 a and the fourth principal surface electrode portion 26 b4 of the second base electrode layer 26 b are exposed on the surface of the multilayer ceramic capacitor 10 as the outermost layers, respectively. Therefore, if the fourth principal surface electrode portion 26 a4 and the fourth principal surface electrode portion 26 b4 are oxidized while they are exposed on the surface, the solder will not wet up to the fourth end portion 26 a4 t and the fourth end portion 26 b4 t on the central side of the laminate 12 when the multilayer ceramic capacitor 10 is mounted, thereby suppressing short-circuit defects.

[0117] 2. Method for Manufacturing the Multilayer Ceramic Capacitor A method for manufacturing the multilayer ceramic capacitor, which is an example of the multilayer ceramic capacitor according to the first embodiment, will now be described.

[0118] First, a dielectric sheet and a conductive paste for the internal electrodes are prepared. The dielectric sheet and the conductive paste for the internal electrode layers contain a binder (for example, a known organic binder) and an organic solvent (for example, a known organic binder).

[0119] Next, a conductive paste for the internal electrodes is printed in a predetermined pattern on the dielectric sheet by, for example, screen printing or gravure printing to form an internal electrode pattern. Regarding the dielectric sheet, an outer layer dielectric sheet on which no internal electrode pattern is printed is also produced.

[0120] A predetermined number of dielectric sheets for outer layers on which no internal electrode pattern is formed are stacked, and then dielectric sheets on which an internal electrode pattern corresponding to the first internal electrode layer 16a and a dielectric sheet on which an internal electrode pattern corresponding to the second internal electrode layer 16b are formed are alternately stacked on top of these, and then a predetermined number of dielectric sheets for outer layers on which no internal electrode pattern is formed are stacked on top of these to produce a laminated sheet.

[0121] Furthermore, the laminated sheets are pressed in the lamination direction by means of a hydrostatic press or the like to produce a laminated block.

[0122] The laminated block is then cut to a predetermined size to cut out laminated chips, which may then be wet-barreled to round the corners and ridges of the laminated chips.

[0123] Next, the laminated chip is fired to produce the laminate 12. The firing temperature depends on the ceramic and the materials of the internal electrode layers 16, but is preferably 900°C or higher and 1400°C or lower.

[0124] Next, a base electrode layer 26 having first to fourth main surface electrode portions is formed on the first end face 12e and second end face 12f of the laminate 12, as well as on a portion of the first main surface 12a and a portion of the second main surface 12b.

[0125] Each of the first to fourth principal surface electrode portions is formed by sputtering or screen printing.

[0126] When each of the first to fourth principal surface electrode portions is formed by sputtering, the following steps are performed.

[0127] (1-1) A sputtered film is formed on the entire surface of the laminate 12.

[0128] (1-2) Next, the portions of the sputtered film that are to be left as the first principal surface electrode portion 26a1 and the first principal surface electrode portion 26b1 of the first principal surface electrode portion, specifically, a portion of the first principal surface 12a of the laminate 12 and the first end surface 12e and the second end surface 12f, are covered with a resin mask.

[0129] (1-3) Next, the sputtered film is dissolved using an etching solution, thereby removing the sputtered film from the laminate 12 except for the portion covered with the resin mask.

[0130] (1-4) Next, the resin mask is dissolved in an organic solvent, leaving only the sputtered film in the areas corresponding to the resin mask on the laminate 12. This sputtered film forms the first principal-surface electrode portion 26a1 and the first principal-surface electrode portion 26b1 of the first principal-surface electrode portion.

[0131] (1-5) Next, on the first main surface 12a of the laminate 12, the exposed portions of the first main surface electrode portion between the first main surface electrode portion 26a1 and the first main surface electrode portion 26b1 and the portions of the first main surface electrode portion 26a1 and the first main surface electrode portion 26b1 formed in the above step (1-4) that correspond to the first ends 26a1t and the first ends 26b1t on the first main surface 12a are covered with a resin mask.

[0132] (1-6) Next, as the surface of the laminate 12, a further sputtered film is formed on the sputtered film obtained in the above step (1-4) and the surface of the mask obtained in the above step (1-5).

[0133] (1-7) Next, the portions of the sputtered film obtained in the above step (1-6) that are to be left as second principal-surface electrode portion 26a2 and second principal-surface electrode portion 26b2, specifically, portions corresponding to part of first principal surface 12a and first end face 12e and second end face 12f of laminate 12, are covered with a resin mask. Note that the mask in this step is formed so that the length along the direction connecting the end of the first principal-surface electrode portion of the base electrode layer of laminate 12 toward the center of the laminate to the surface of the first internal electrode layer exposed on the surface of laminate 12 is shorter than that formed in the above step (1-2).

[0134] (1-8) Next, the sputtered film obtained in the above step (1-6) is dissolved using an etching solution, thereby removing the sputtered film from the laminate 12 except for the portion covered with the resin mask.

[0135] (1-9) Next, the resin masks obtained in steps (1-5) and (1-7) are dissolved in an organic solvent, leaving only the sputtered film in the areas corresponding to the resin masks on the laminate 12. This sputtered film forms the second principal surface electrode portions 26a2 and 26b2.

[0136] (1-10) Thereafter, the third principal surface electrode portion and the fourth principal surface electrode portion are sequentially formed by repeating the steps (1-5) through (1-9). Note that the mask used in step (1-5) when sequentially forming the third principal surface electrode portion and the fourth principal surface electrode portion is formed so that the length along the direction connecting the end of the first principal surface electrode portion of the base electrode layer of the laminate 12 on the central side of the laminate to the surface of the first internal electrode layer exposed on the surface of the laminate 12 is longer than that formed in the previous step (1-5).

[0137] 4 , when the length of the first principal-surface electrode portion 26a1 is length A, the length of the second principal-surface electrode portion 26a2 is length B, the length of the third principal-surface electrode portion 26a3 is length C, and the length of the fourth principal-surface electrode portion 26a4 is length D, a relationship of length A > length B > length C > length D is obtained. Similarly, when the length of the first principal-surface electrode portion 26b1 is length A, the length of the second principal-surface electrode portion 26b2 is length B, the length of the third principal-surface electrode portion 26b3 is length C, and the length of the fourth principal-surface electrode portion 26b4 is length D, a relationship of length A > length B > length C > length D is obtained.

[0138] In addition, when the base electrode layer 26 having the first, second, third, and fourth principal surface electrode portions is formed only on the first principal surface 12 a, as in the multilayer ceramic capacitor 310 shown in FIG. 9 , the resin masks obtained in the above steps (1-2) and (1-7) are formed so as not to cover the sides of the first end face 12 e and the second end face 12 f of the laminate 12.

[0139] When each of the first to fourth principal surface electrode portions is formed by screen printing, the following process is performed: a different printing plate is used for each principal surface electrode of each layer, and a printing pattern corresponding to the desired shape of the principal surface electrode portion is formed at a desired position on the laminate 12.

[0140] At this time, the opposing distance between a pair of printed patterns formed on the first main surface 12a of the laminate 12 is formed so that the length along the direction connecting the end of the first main surface electrode portion of the base electrode layer toward the center of the laminate to the surface of the first internal electrode layer exposed on the surface of the laminate 12 is longer for the one formed earlier than the one formed later for each of the formation of the first main surface electrode portion, the formation of the second main surface electrode portion, the formation of the third main surface electrode portion, and the formation of the fourth main surface electrode portion.

[0141] As a result, similar to the case where they are formed by sputtering, the configuration of each of the first to fourth main surface electrode portions such as the multilayer ceramic capacitor 10 shown in FIG. 4 is obtained.

[0142] Thereafter, a plating layer 28 is formed on the surface of the fourth principal-surface electrode portion of the base electrode layer 26. The plating layer 28 is formed, for example, by barrel plating. When the plating layer 28 has an under plating layer 30 and a top plating layer 32 as in the multilayer ceramic capacitor 10 shown in FIG. 4 , each plating layer is formed sequentially, for example, by barrel plating.

[0143] When the plating layer 28 is formed directly as a plating layer, as in the case of a multilayer ceramic capacitor 310 shown in FIG. 9, the following procedure is carried out.

[0144] That is, the first end face 12e and the second end face 12f of the laminate 12 are plated to form a plating film directly on the exposed portions of the first lead electrode portion 20a and the second lead electrode portion 20b of the internal electrode layer 16. While either electrolytic plating or electroless plating may be used for the plating process, electroless plating has the disadvantage of requiring pretreatment using a catalyst or the like to improve the plating deposition rate, which complicates the process. Therefore, electrolytic plating is usually preferred. Barrel plating is preferred as the plating method. If necessary, the plating layer 28 as the direct plating layer may be formed as a multilayer layer, as in the multilayer ceramic capacitor 10 shown in FIG. 9 , or an upper-layer plated electrode may be formed on the surface of a lower-layer plated electrode in the same manner.

[0145] In this manner, the multilayer ceramic capacitor 10 shown in FIG. 1 can be manufactured.

[0146] According to the method for manufacturing a multilayer ceramic capacitor according to the present embodiment described above, the ends of the first to fourth main-surface electrode portions formed on the first main surface of the laminate are arranged so as not to align, thereby dispersing the locations where stress occurs and making it possible to prevent cracks from propagating from the tips of the external electrodes into the interior of the multilayer ceramic capacitor.

[0147] B. Second Embodiment 1. Multilayer Ceramic Capacitor Next, a multilayer ceramic capacitor according to a second embodiment of the present invention will be described. FIG. 11 is an external perspective view showing a multilayer ceramic capacitor, which is an example of a multilayer ceramic electronic component according to the second embodiment of the present invention. FIG. 12 is a cross-sectional view taken along line XII-XII in FIG. 11. FIG. 13 is a cross-sectional view taken along line XIII-XIII in FIG. 11. FIG. 14 is a cross-sectional view taken along line XIV-XIV in FIG. 11. FIG. 15 is a cross-sectional view taken along line XV-XV in FIG. 11. FIG. 16 is a cross-sectional view taken along line XVI-XVI in FIG. 11. FIG. 17 is an exploded perspective view of the laminate shown in FIG. 1.

[0148] The multilayer ceramic capacitor 510 includes a laminate 512 and external electrodes 524 and 525 .

[0149] (Laminate) The laminate 512 includes a plurality of ceramic layers 514 and a plurality of internal electrode layers 516. The laminate 512 has a first main surface 512a and a second main surface 512b that face each other in a height direction x, a first side surface 512c and a second side surface 512d that face each other in a width direction y that is perpendicular to the height direction x, and a third side surface 512e and a fourth side surface 512f that face each other in a length direction z that is perpendicular to the height direction x and the width direction y. The first main surface 512a and the second main surface 512b extend along the width direction y and the length direction z, respectively. The first side surface 512c and the second side surface 512d extend along the height direction x and the length direction z, respectively. The third side surface 512e and the fourth side surface 512f extend along the height direction x and the width direction y, respectively. Therefore, the height direction x is the direction connecting the first main surface 512a and the second main surface 512b, the width direction y is the direction connecting the first side surface 512c and the second side surface 512d, and the length direction z is the direction connecting the third side surface 512e and the fourth side surface 512f.

[0150] Furthermore, it is preferable that the corners and ridges of the laminate 512 are rounded. Here, a corner is a portion where three surfaces of the laminate 512 intersect, and a ridge is a portion where two surfaces of the laminate 512 intersect.

[0151] As shown in Figures 14 and 15, the laminate 512 has, in the height direction x connecting the first main surface 512a and the second main surface 512b, an effective layer portion 515a in which a plurality of internal electrode layers 516 face each other, a first outer layer portion 515b1 formed from a plurality of ceramic layers 514 located between the first main surface 512a and the internal electrode layer 516 located closest to the first main surface 512a, and a second outer layer portion 515b2 formed from a plurality of ceramic layers 514 located between the second main surface 512b and the internal electrode layer 516 located closest to the second main surface 512b.

[0152] The first outer layer portion 515b1 is located on the first main surface 512a side of the laminate 512, and is an assembly of multiple ceramic layers 514 located between the first main surface 512a and the internal electrode layer 516 closest to the first main surface 512a.

[0153] The second outer layer portion 515b2 is located on the second main surface 512b side of the laminate 512 and is an assembly of multiple ceramic layers 514 located between the second main surface 512b and the internal electrode layer 516 closest to the second main surface 512b.

[0154] The area sandwiched between the first outer layer portion 515b1 and the second outer layer portion 515b2 is the effective layer portion 515a.

[0155] The ceramic layer 514 may be formed from, for example, a dielectric material. Examples of the dielectric material include dielectric ceramics primarily composed of BaTiO3, CaTiO3, SrTiO3, or CaZrO3. Depending on the desired properties of the laminate, a material containing a minor component such as a manganese compound, an iron compound, a chromium compound, a cobalt compound, or a nickel compound in a smaller amount than the major component may be used.

[0156] The ceramic layer 514 may have a plurality of crystal grains containing a perovskite-type compound having a basic structure of BaTiO3.

[0157] The thinner the ceramic layer 514, the greater the capacitance of the capacitor, so the crystal grain size is preferably 1 μm or less.

[0158] 12 to 17, the internal electrode layer 516 has a plurality of first internal electrode layers 516a and a plurality of second internal electrode layers 516b. The first internal electrode layers 516a and the second internal electrode layers 516b are alternately stacked with the ceramic layers 514 interposed therebetween.

[0159] The first internal electrode layer 516a is disposed on the surface of the ceramic layer 514. The first internal electrode layer 516a faces the first main surface 512a and the second main surface 512b, has a first opposing electrode portion 518a facing the second internal electrode layer 516b, and is laminated in the direction connecting the first main surface 512a and the second main surface 512b.

[0160] The second internal electrode layer 516b is disposed on a surface of a ceramic layer 514 different from the ceramic layer 514 on which the first internal electrode layer 516a is disposed. The second internal electrode layer 516b has a second opposing electrode portion 518b opposing the first main surface 512a and the second main surface 512b, and is laminated in a direction connecting the first main surface 512a and the second main surface 512b.

[0161] 12 to 17 , the first internal electrode layer 516a is extended by a first extension electrode portion 520a to the first side surface 512c and the third side surface 512e of the laminate 512, and is extended by a second extension electrode portion 520b to the second side surface 512d and the fourth side surface 512f of the laminate 512. The width of the first extension electrode portion 520a extended to the first side surface 512c may be approximately equal to the width of the first extension electrode portion 520a extended to the third side surface 512e, and the width of the second extension electrode portion 520b extended to the second side surface 512d may be approximately equal to the width of the second extension electrode portion 520b extended to the fourth side surface 512f.

[0162] That is, the first extraction electrode portion 520a is extracted to the third side surface 512e side of the laminate 512, and the second extraction electrode portion 520b is extracted to the fourth side surface 512f side of the laminate 512. Note that the first extraction electrode portion 520a may be extracted only to the third side surface 512e, and the second extraction electrode portion 520b may be extracted only to the fourth side surface 512f.

[0163] The second internal electrode layer 516b is extended by a third extension electrode portion 521a to the first side surface 512c and the fourth side surface 512f of the laminate 512, and is extended by a fourth extension electrode portion 521b to the second side surface 512d and the third side surface 512e of the laminate 512. The width of the third extension electrode portion 521a extended to the first side surface 512c may be approximately equal to the width of the third extension electrode portion 521a extended to the fourth side surface 512f, and the width of the fourth extension electrode portion 521b extended to the second side surface 512d may be approximately equal to the width of the fourth extension electrode portion 521b extended to the third side surface 512e.

[0164] That is, the third extraction electrode portion 521a is extracted to the fourth side surface 512f side of the laminate 512, and the fourth extraction electrode portion 521b is extracted to the third side surface 512e side of the laminate 512. Note that the third extraction electrode portion 521a may be extracted only to the fourth side surface 512f, and the fourth extraction electrode portion 521b may be extracted only to the third side surface 512e.

[0165] Furthermore, when the multilayer ceramic capacitor 510 is viewed from the stacking direction, it is preferable that a straight line connecting the first extraction electrode portion 520a and the second extraction electrode portion 520b of the first internal electrode layer 516a intersects with a straight line connecting the third extraction electrode portion 521a and the fourth extraction electrode portion 521b of the second internal electrode layer 516b.

[0166] Furthermore, on the first side surface 512c, the second side surface 512d, the third side surface 512e and the fourth side surface 512f of the laminate 512, it is preferable that the first extraction electrode portion 520a of the first internal electrode layer 516a and the fourth extraction electrode portion 521b of the second internal electrode layer 516b are extracted to opposing positions, and that the second extraction electrode portion 520b of the first internal electrode layer 516a and the third extraction electrode portion 521a of the second internal electrode layer 516b are extracted to opposing positions.

[0167] As shown in FIG. 16, the laminate 512 also includes a side portion (W gap) 522a of the laminate 512 formed between one end in the width direction y of the first opposing electrode portion 518a and the first side surface 512c, and between the other end in the width direction y of the second opposing electrode portion 518b and the second side surface 512d.

[0168] Furthermore, as shown in FIG. 16, the laminate 512 includes a side portion (L gap) 522b of the laminate 512 formed between one end in the longitudinal direction z of the first opposing electrode portion 518a and the third side surface 512e, and between the other end in the longitudinal direction z of the second opposing electrode portion 518b and the fourth side surface 512f.

[0169] The internal electrode layer 516 can be made of an appropriate conductive material, such as, for example, metals such as Ni, Cu, Ag, Pd, Au, or alloys containing at least one of these metals, such as Ag-Pd alloys, but is not limited to these.

[0170] (External Electrodes) As shown in FIGS. 11 to 16, external electrodes 524 and 525 are disposed on the laminate 512.

[0171] The external electrode 524 includes a base electrode layer 526 and a plating layer 528 formed to cover the base electrode layer 526 .

[0172] The external electrode 525 includes a base electrode layer 527 and a plating layer 529 formed to cover the base electrode layer 527 .

[0173] The external electrode 524 includes a first external electrode 524a and a second external electrode 524b.

[0174] The first external electrode 524a is disposed so as to cover the first lead electrode portion 520a on the first side surface 512c and the third side surface 512e, and is disposed so as to cover a part of the first main surface 512a. The first external electrode 524a is electrically connected to the first lead electrode portion 520a of the first internal electrode layer 516a.

[0175] The second external electrode 524b is disposed so as to cover the second lead electrode portion 520b on the second side surface 512d and the fourth side surface 512f, and is disposed so as to cover a part of the first main surface 512a. The second external electrode 524b is electrically connected to the second lead electrode portion 520b of the first internal electrode layer 516a.

[0176] The external electrode 525 includes a third external electrode 525a and a fourth external electrode 525b.

[0177] The third external electrode 525a is disposed so as to cover the third lead electrode portion 521a on the first side surface 512c and the fourth side surface 512f, and is disposed so as to cover a part of the first main surface 512a. The third external electrode 525a is electrically connected to the third lead electrode portion 521a of the second internal electrode layer 516b.

[0178] The fourth external electrode 525b is disposed so as to cover the fourth lead electrode portion 521b on the second side surface 512d and the third side surface 512e, and is disposed so as to cover a part of the first main surface 512a. The fourth external electrode 525b is electrically connected to the fourth lead electrode portion 521b of the second internal electrode layer 516b.

[0179] In the laminate 512, a capacitance is formed by the first opposing electrode portion 518a of the first internal electrode layer 516a and the second opposing electrode portion 518b of the second internal electrode layer 516b facing each other via the ceramic layer 514. Therefore, a capacitance can be obtained between the first external electrode 524a and the second external electrode 524b to which the first internal electrode layer 516a is connected and the third external electrode 525a and the fourth external electrode 525b to which the second internal electrode layer 516b is connected, and the characteristics of a capacitor are exhibited.

[0180] (Base Electrode Layer) The base electrode layer 526 has a first base electrode layer 526a and a second base electrode layer 526b.

[0181] The base electrode layer 527 includes a third base electrode layer 527a and a fourth base electrode layer 527b.

[0182] The first base electrode layer 526a, the second base electrode layer 526b, the third base electrode layer 527a, and the fourth base electrode layer 527b each have a first principal surface electrode portion, a second principal surface electrode portion, a third principal surface electrode portion, and a fourth principal surface electrode portion. Specifically, the first base electrode layer 526a has a configuration in which a first principal surface electrode portion 526a1, a second principal surface electrode portion 526a2, a third principal surface electrode portion 526a3, and a fourth principal surface electrode portion 526a4 are stacked. The second base electrode layer 526b has a configuration in which a first principal surface electrode portion 526b1, a second principal surface electrode portion 526b2, a third principal surface electrode portion 526b3, and a fourth principal surface electrode portion 526b4 are stacked. The third base electrode layer 527a has a configuration in which a first principal surface electrode portion 527a1, a second principal surface electrode portion 527a2, a third principal surface electrode portion 527a3, and a fourth principal surface electrode portion 527a4 are stacked. The fourth base electrode layer 527b has a configuration in which a first principal surface electrode portion 527b1, a second principal surface electrode portion 527b2, a third principal surface electrode portion 527b3, and a fourth principal surface electrode portion 527b4 are stacked.

[0183] (Principal surface electrode portion) As shown in Figures 12 and 14, the first principal surface electrode portion 526a1 is arranged on the surface of the laminate 512, the second principal surface electrode portion 526a2 is arranged on the surface of the first principal surface electrode portion 526a1, the third principal surface electrode portion 526a3 is arranged on the surface of the second principal surface electrode portion 526a2, and the fourth principal surface electrode portion 526a4 is arranged on the surface of the third principal surface electrode portion 526a3.

[0184] Here, as shown in Figure 14, on the first main surface 512a, a direction is defined that connects the end of the first main surface electrode portion of the first base electrode layer toward the center of the laminate to the surface at which the first internal electrode layer is exposed on the surface of the laminate, specifically, a direction that connects the first end 526a1t toward the center of the laminate 512 of the first main surface electrode portion 526a1 of the first base electrode layer 526a to the first side surface 512c of the laminate 512 at which the first extraction electrode portion 520a of the first internal electrode layer 516a is exposed (hereinafter referred to as the third reference direction). Then, when the length of the first principal surface electrode portion 526a1 in the third reference direction is length A, the length of the second principal surface electrode portion 526a2 in the same direction as length A is length B, the length of the third principal surface electrode portion 526a3 in the same direction as length A is length C, and the length of the fourth principal surface electrode portion 526a4 in the same direction as length A is length D, then length A > length B > length C > length D.

[0185] Although not shown, the relationship between the lengths of the first main surface electrode portion 526a1, the second main surface electrode portion 526a2, the third main surface electrode portion 526a3, and the fourth main surface electrode portion 526a4 of the first base electrode layer 526a is the same as the above-mentioned configuration shown in Figure 14 even when viewed in the LT cross section.

[0186] As a result, on the first main surface 512a, the first main surface electrode portion 526a1, the second main surface electrode portion 526a2, the third main surface electrode portion 526a3, and the fourth main surface electrode portion 526a4 of the first base electrode layer 526a have first end portions 526a1t, second end portions 526a2t, third end portions 526a3t, and fourth end portions 526a4t on the central side of the laminate 512 that are not aligned with each other, so that the stress of the first external electrode 524a toward the central side of the laminate 512 that occurs when the solder shrinks can be dispersed.

[0187] Furthermore, on the first main surface 512a, a direction is determined that connects the end portion of the first main surface electrode portion of the fourth base electrode layer toward the center of the laminate to the surface at which the second internal electrode layer is exposed on the surface of the laminate, specifically, a direction that connects the first end portion 527b1t toward the center of the laminate 512 of the first main surface electrode portion 527b1 of the fourth base electrode layer 527b to the third side surface 512e of the laminate 512 at which the second extraction electrode portion 520b of the second internal electrode layer 516b is exposed (hereinafter, the fourth reference direction). Then, when the length of the first principal surface electrode portion 527b1 in the fourth reference direction is length A, the length of the second principal surface electrode portion 527b2 in the same direction as length A is length B, the length of the third principal surface electrode portion 527b3 in the same direction as length A is length C, and the length of the fourth principal surface electrode portion 527b4 in the same direction as length A is length D, then length A > length B > length C > length D.

[0188] Although not shown, the relationship between the lengths of the first main surface electrode portion 527b1, the second main surface electrode portion 527b2, the third main surface electrode portion 527b3, and the fourth main surface electrode portion 527b4 of the fourth base electrode layer 527b is the same as the above-mentioned configuration shown in Figure 14 even when viewed in the LT cross section.

[0189] As a result, on the first main surface 512a, the first main surface electrode portion 527b1, the second main surface electrode portion 527b2, the third main surface electrode portion 527b3 and the fourth main surface electrode portion 527b4 of the fourth base electrode layer 527b have first end 527b1t, second end 527b2t, third end 527b3t and fourth end 527b4t on the central side of the laminate 512 that are not aligned with each other, so that the stress of the third external electrode 525a toward the central side of the laminate 512 that occurs when the solder shrinks can be dispersed.

[0190] Furthermore, as shown in Figure 15, on the first main surface 512a, a direction is determined that connects the end of the first main surface electrode portion of the second base electrode layer toward the center of the laminate to the surface at which the first internal electrode layer is exposed on the surface of the laminate, specifically, a direction that connects the first end 526b1t toward the center of the laminate 512 of the first main surface electrode portion 526b1 of the second base electrode layer 526b to the fourth side surface 512f of the laminate 512 at which the first extraction electrode portion 520a of the first internal electrode layer 516a is exposed (hereinafter, this is referred to as the fifth reference direction). Then, when the length of the first principal surface electrode portion 526b1 in the fifth reference direction is length A, the length of the second principal surface electrode portion 526b2 in the same direction as length A is length B, the length of the third principal surface electrode portion 526b3 in the same direction as length A is length C, and the length of the fourth principal surface electrode portion 526b4 in the same direction as length A is length D, then length A > length B > length C > length D.

[0191] Although not shown, the relationship between the lengths of the first main surface electrode portion 526b1, the second main surface electrode portion 526b2, the third main surface electrode portion 526b3, and the fourth main surface electrode portion 526b4 of the second base electrode layer 526b is the same as the above-mentioned configuration shown in Figure 15 even when viewed in the LT cross section.

[0192] As a result, on the first main surface 512a, the first main surface electrode portion 526b1, the second main surface electrode portion 526b2, the third main surface electrode portion 526b3, and the fourth main surface electrode portion 526b4 of the second base electrode layer 526b have first end portions 526b1t, second end portions 526b2t, third end portions 526b3t, and fourth end portions 526b4t on the central side of the laminate 512 that are not aligned with each other, so that the stress of the second external electrode 524b toward the central side of the laminate 512 that occurs when the solder shrinks can be dispersed.

[0193] Furthermore, on the first main surface 512a, a direction connecting the end portion of the first main surface electrode portion of the third base electrode layer toward the center of the laminate to the surface at which the second internal electrode layer is exposed on the surface of the laminate is determined, specifically, a direction connecting the first end portion 527a1t toward the center of the laminate 512 of the first main surface electrode portion 527a1 of the third base electrode layer 527a to the third side surface 512e of the laminate 512 at which the third extraction electrode portion 521a of the second internal electrode layer 516b is exposed (hereinafter, referred to as the sixth reference direction). Then, when the length of the first principal surface electrode portion 527a1 in the sixth reference direction is length A, the length of the second principal surface electrode portion 527a2 in the same direction as length A is length B, the length of the third principal surface electrode portion 527a3 in the same direction as length A is length C, and the length of the fourth principal surface electrode portion 527a4 in the same direction as length A is length D, then length A > length B > length C > length D.

[0194] Although not shown, the relationship between the lengths of the first main surface electrode portion 527a1, the second main surface electrode portion 527a2, the third main surface electrode portion 527a3, and the fourth main surface electrode portion 527a4 of the third base electrode layer 527a is the same as the above-mentioned configuration shown in Figure 15 even when viewed in the LT cross section.

[0195] As a result, on the first main surface 512a, the first main surface electrode portion 527a1, the second main surface electrode portion 527a2, the third main surface electrode portion 527a3, and the fourth main surface electrode portion 527a4 of the third base electrode layer 527a have first end 526a1t, second end 526a2t, third end 526a3t, and fourth end 526a4t on the central side of the laminate 512 that are not aligned with each other, so that the stress of the fourth external electrode 525b toward the central side of the laminate 512 that occurs when the solder shrinks can be dispersed.

[0196] Furthermore, in the third reference direction and in a direction perpendicular to the third reference direction around the height direction x, it is preferable that the first end 526a1t of the first principal surface electrode portion 526a1 is not covered by the second principal surface electrode portion 526a2, the second end 526a2t of the second principal surface electrode portion 526a2 is not covered by the third principal surface electrode portion 526a3, and the third end 526a3t of the third principal surface electrode portion 526a3 is not covered by the fourth principal surface electrode portion 526a4.

[0197] This allows the stress acting on the first end 526a1t to the fourth end 526a4t of each of the first to fourth principal surface electrode portions 526a1 to 526a4 to be concentrated outside the laminate 512 (towards the first side surface 512c and the third side surface 512e) rather than at these ends, thereby dispersing the stress and improving the mechanical strength.

[0198] Similarly, in the fourth reference direction and in a direction perpendicular to the fourth reference direction around the height direction x, it is preferable that the first end 527b1t of the first principal surface electrode portion 527b1 is not covered by the second principal surface electrode portion 527b2, the second end 527b2t of the second principal surface electrode portion 527b2 is not covered by the third principal surface electrode portion 527b3, and the third end 527b3t of the third principal surface electrode portion 527b3 is not covered by the fourth principal surface electrode portion 527b4.

[0199] This allows the stress acting on the first end 527b1t to the fourth end 527b4t of each of the first to fourth principal surface electrode portions 527b1 to 527b4 to be concentrated outside the laminate 512 (towards the second side surface 512d and the third side surface 512e) rather than at these ends, thereby dispersing the stress and improving the mechanical strength.

[0200] Furthermore, in the fifth reference direction and in a direction perpendicular to the fifth reference direction around the height direction x, it is preferable that the first end 527a1t of the first principal surface electrode portion 527a1 is not covered by the second principal surface electrode portion 527a2, the second end 527a2t of the second principal surface electrode portion 527a2 is not covered by the third principal surface electrode portion 527a3, and the third end 527a3t of the third principal surface electrode portion 527a3 is not covered by the fourth principal surface electrode portion 527a4.

[0201] This allows the stress acting on the first end 527a1t to the fourth end 527a4t of each of the first to fourth principal surface electrode portions 527a1 to 527a4 to be concentrated outside the laminate 512 (towards the first side surface 512c and the fourth side surface 512f) rather than at these ends, thereby dispersing the stress and improving the mechanical strength.

[0202] Similarly, in the sixth reference direction and in a direction perpendicular to the sixth reference direction around the height direction x, it is preferable that the first end 526b1t of the first principal surface electrode portion 526b1 is not covered by the second principal surface electrode portion 526b2, the second end 526b2t of the second principal surface electrode portion 526b2 is not covered by the third principal surface electrode portion 526b3, and the third end 526b3t of the third principal surface electrode portion 526b3 is not covered by the fourth principal surface electrode portion 526b4.

[0203] This allows the stress acting on the first end 526b1t to the fourth end 526b4t of each of the first to fourth principal surface electrode portions 526b1 to 526b4 to be concentrated outside the laminate 512 (towards the second side surface 512d and the fourth side surface 512f) rather than at these ends, thereby dispersing the stress and improving the mechanical strength.

[0204] In addition, the fourth principal surface electrode portion 526a4 of the first base electrode layer 526a, the fourth principal surface electrode portion 526b4 of the second base electrode layer 526b, the fourth principal surface electrode portion 527a4 of the third base electrode layer 527a, and the fourth principal surface electrode portion 527b4 of the fourth base electrode layer 527b may each be exposed on the surface of the multilayer ceramic capacitor 110 as the outermost layer. If the fourth main surface electrode portion 526a4, the fourth main surface electrode portion 526b4, the fourth main surface electrode portion 527a4, and the fourth main surface electrode portion 527b4 are exposed on the surface and are oxidized, for example, the solder will not wet up to the fourth ends 526a4t, 526b4t, 527a4t, and 527b4t on the central side of the laminate 512 when the multilayer ceramic capacitor 110 is mounted, thereby suppressing short circuit defects.

[0205] In addition, the fourth principal surface electrode portion 526a4, the fourth principal surface electrode portion 526b4, the fourth principal surface electrode portion 527a4, and the fourth principal surface electrode portion 527b4 may be covered with a plating layer, as in the examples shown in Figures 12 to 15.

[0206] Next, the first to fourth principal surface electrode portions constituting the base electrode layers 526 and 527 can be formed by a thin film formation method such as sputtering or vapor deposition, or by screen printing. However, the details of these methods are the same as those in the first embodiment, and detailed explanations thereof will be omitted.

[0207] (Plating Layer) The plating layer 528 includes a first plating layer 528a and a second plating layer 528b.

[0208] The first plating layer 528a is disposed so as to cover the first principal surface electrode portion 526a1 to the fourth principal surface electrode portion 526a4 as the first base electrode layer 526a.

[0209] The second plating layer 528b is disposed so as to cover the first to fourth principal surface electrode portions 526b1 to 526b4 serving as the second base electrode layer 526b.

[0210] The plating layer 528 is formed of multiple layers. That is, the plating layer 528 has an underplating layer 530 and a top plating layer 532. The underplating layer 530 includes a first underplating layer 530a included in the first plating layer 528a and a second underplating layer 530b included in the second plating layer 528b. The top plating layer 532 includes a first top plating layer 532a included in the first plating layer 528a and a second top plating layer 532b included in the second plating layer 528b.

[0211] The first underplating layer 530a of the underplating layer 530 is disposed so as to cover the fourth principal surface electrode portion 526a4 of the first base electrode layer 526a.

[0212] The second underplating layer 530b of the underplating layer 530 is disposed so as to cover the fourth principal surface electrode portion 526b4 of the second base electrode layer 526b.

[0213] The surface plating layer 532 may be formed of multiple layers. In this embodiment, the surface plating layer 532 has a two-layer structure including a middle plating layer 534 that is a Ni plating layer and an upper plating layer 536 that is a Sn plating layer.

[0214] In the top plating layer 532, the first intermediate plating layer 534a covers the first lower plating layer 530a, and the first upper plating layer 536a covers the first intermediate plating layer 534a. The second intermediate plating layer 534b covers the second lower plating layer 530b, and the second upper plating layer 536b covers the second intermediate plating layer 534b.

[0215] The plating layer 529 includes a third plating layer 529a and a fourth plating layer 529b.

[0216] The plating layer 529 is formed of multiple layers. That is, the plating layer 529 has an underplating layer 531 and a top plating layer 533. The underplating layer 531 includes a first underplating layer 531a included in the third plating layer 529a and a second underplating layer 531b included in the fourth plating layer 529b. The top plating layer 533 includes a first top plating layer 533a included in the third plating layer 529a and a second top plating layer 533b included in the fourth plating layer 529b.

[0217] The first underplating layer 531a of the underplating layer 531 is disposed so as to cover the fourth principal surface electrode portion 527a4 of the third base electrode layer 527a.

[0218] The second lower plating layer 531b of the lower plating layer 531 is disposed so as to cover the fourth principal surface electrode portion 527b4 of the fourth base electrode layer 527b.

[0219] The surface plating layer 533 may be formed of multiple layers. In this embodiment, the surface plating layer 533 has a two-layer structure including a middle plating layer 535 that is a Ni plating layer and an upper plating layer 537 that is a Sn plating layer.

[0220] In the top plating layer 533, the first intermediate plating layer 535a covers the first lower plating layer 531a, and the first upper plating layer 537a covers the first intermediate plating layer 535a. The second intermediate plating layer 535b covers the second lower plating layer 531b, and the second upper plating layer 537b covers the second intermediate plating layer 535b.

[0221] The under-plating layers 530 and 531 preferably contain at least one metal selected from Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, Zn, etc., or an alloy containing such a metal. In particular, in this embodiment, the under-plating layers 530 and 531 are preferably Cu plating layers.

[0222] The middle plating layers 534, 535 as Ni plating layers can prevent the lower plating layers 530, 531 from being eroded by solder when mounting the multilayer ceramic capacitor 110. Furthermore, the upper plating layers 536, 537 as Sn plating layers can improve the wettability of the solder when mounting the multilayer ceramic capacitor 110, facilitating mounting. When the plating layers 528, 529 have a three-layer structure, in addition to the above, it is preferable that the layers are laminated in the order of Sn plating layer, Ni plating layer, and Sn plating layer.

[0223] It is preferable that the ratio of the W dimension to the L dimension of the multilayer ceramic capacitor 510 is 0.85 or more and 1.00 or less, but the ratio of the W dimension to the L dimension may take any other value.

[0224] The multilayer ceramic capacitor 510 shown in Fig. 11 having the above-described configuration exhibits the same effects as the multilayer ceramic capacitor 10 of the first embodiment. As with the first embodiment, the effects of the present invention are more pronounced when the T dimension of the multilayer ceramic capacitor 510 is 150 µm or less. Furthermore, when the T dimension is 50 µm or less, the multilayer ceramic capacitor 10 is thinned, and reliability in mechanical strength becomes even more important, so the effects of the present invention are more pronounced.

[0225] In addition, in the multilayer ceramic capacitor according to the second embodiment of the present invention, it is preferable that the external electrodes 524 and 525 of the multilayer ceramic capacitor 510 have the first to fourth modified examples similar to the external electrodes 24 of the first to fourth modified examples of the multilayer ceramic capacitor 10 according to the first embodiment.

[0226] 2. Method for Manufacturing a Multilayer Ceramic Capacitor A method for manufacturing a multilayer ceramic capacitor, which is an example of a multilayer ceramic capacitor according to the second embodiment, will now be described.

[0227] First, a dielectric sheet and a conductive paste for the internal electrodes are prepared. The dielectric sheet and the conductive paste for the internal electrode layers contain a binder (for example, a known organic binder) and a solvent (for example, a known organic binder).

[0228] Next, a conductive paste for the internal electrodes is printed in a predetermined pattern on the dielectric sheet by, for example, screen printing or gravure printing, to form an internal electrode pattern. Specifically, a conductive paste layer is formed by applying a paste made of a conductive material to the dielectric sheet by a method such as the printing method described above. The conductive paste is, for example, a paste made of a metal powder to which an organic binder and an organic solvent have been added. Regarding the dielectric sheets, outer layer dielectric sheets on which no internal electrode patterns are printed are also produced.

[0229] As a result, a dielectric sheet on which an internal electrode pattern corresponding to the first internal electrode layer 516a is formed and a dielectric sheet on which an internal electrode pattern corresponding to the second internal electrode layer 516b is formed are prepared.

[0230] More specifically, a screen plate for printing the first internal electrode layer 516a and a screen plate for printing the second internal electrode layer 516b are prepared separately, and the internal electrode layers of the present invention can be printed using a printer that can print the two types of screen plates separately.

[0231] A laminate sheet is produced using the dielectric sheets on which these internal electrode patterns are formed. That is, a predetermined number of dielectric sheets for outer layers on which no internal electrode patterns are formed are stacked to form a portion that will become the first outer layer portion 515b1 on the first main surface 512a side. On top of that, dielectric sheets on which internal electrode patterns corresponding to the first internal electrode layer 516a are formed and dielectric sheets on which internal electrode patterns corresponding to the second internal electrode layer 516b are formed are alternately stacked to form a portion that will become the effective layer portion 515a, and further on top of that, a predetermined number of dielectric sheets for outer layers on which no internal electrode patterns are formed are stacked to form a portion that will become the second outer layer portion 515b2. In this way, the laminate sheet is produced.

[0232] Furthermore, the laminated sheets are pressed in the lamination direction by means of a hydrostatic press or the like to produce a laminated block.

[0233] The laminated block is then cut to a predetermined size to cut out laminated chips, which are then wet-barreled to round the corners and ridges of the laminated chips.

[0234] Next, the laminated chip is fired to produce laminate 512. The firing temperature depends on the ceramic and internal electrode materials, but is preferably 900° C. or higher and 1400° C. or lower.

[0235] Next, base electrode layers 526, 527 consisting of a first principal surface electrode portion, a second principal surface electrode portion, a third principal surface electrode portion, and a fourth principal surface electrode portion are formed on parts of the first principal surface 512a and the second principal surface 512b, and the first side surface 512c, the second side surface 512d, the third side surface 512e, and the fourth side surface 512f of the laminate 512.

[0236] The first to fourth main surface electrode portions are formed by sputtering or screen printing, as in the first embodiment.

[0237] When each of the first to fourth principal surface electrode portions is formed by sputtering, the following steps are performed.

[0238] (2-1) A sputtered film is formed on the entire surface of the laminate 512.

[0239] (2-2) Next, the portions of the sputtered film that are to be left as first principal surface electrode portion 526a1 and first principal surface electrode portion 526b1 of base electrode layer 526 and first principal surface electrode portion 527a1 and first principal surface electrode portion 527b1 of base electrode layer 527, specifically, a portion of first principal surface 512a of laminate 512 and portions of each of first side surface 512c, second side surface 512d, third side surface 512e and fourth side surface 512f, are covered with a resin mask.

[0240] (2-3) Next, the sputtered film is dissolved using an etching solution, thereby removing the sputtered film from the laminate 512 except for the portion covered with the resin mask.

[0241] (2-4) Next, the resin mask is dissolved in an organic solvent, leaving only the sputtered film in the areas corresponding to the resin mask on the laminate 512. This sputtered film forms the first principal-surface electrode portions 526a1 and 526b1 of the base electrode layer 526 and the first principal-surface electrode portions 527a1 and 527b1 of the base electrode layer 527.

[0242] (2-5) Next, on first main surface 512a of laminate 512, exposed portions between first main surface electrode portion 526a1, first main surface electrode portion 526b1, first main surface electrode portion 527a1, and first main surface electrode portion 526b1, and portions of first main surface electrode portion 526a1, first main surface electrode portion 526b1, first main surface electrode portion 527a1, and first main surface electrode portion 527b1 formed in the above step (2-4) that correspond to first ends 526a1t, 526b1t, 527a1t, and 527b1t on first main surface 512a, respectively, are covered with a resin mask.

[0243] (2-6) Next, as the surface of the laminate 512, a further sputtered film is formed on the sputtered film obtained in the above step (2-4) and the surface of the mask obtained in the above step (2-5).

[0244] (2-7) Next, on the sputtered film obtained in the above step (2-6), portions to be left as the second principal-surface electrode portions 526a2 and 526b2 and the second principal-surface electrode portions 527a2 and 527b2, specifically portions corresponding to a part of the first principal surface 512a of the laminate 512 and parts of each of the first side surface 512c, the second side surface 512d, the third side surface 512e, and the fourth side surface 512f, are covered with a resin mask. Note that the mask in this step is formed so that the length along the direction connecting the end of the first principal-surface electrode portion of the base electrode layer of the laminate 512 toward the center of the laminate 512 to the surface of the first internal electrode layer 516a and the second internal electrode layer 516b exposed on the surface of the laminate 512 is shorter than that formed in the previous step (2-2).

[0245] (2-8) Next, the sputtered film obtained in the above step (2-6) is dissolved using an etching solution, thereby removing the sputtered film from the laminate 512 except for the portion covered with the resin mask.

[0246] (2-9) Next, the resin masks obtained in steps (2-5) and (2-7) are dissolved in an organic solvent, leaving only the sputtered film in the areas corresponding to the resin masks on laminate 512. This sputtered film forms second principal-surface electrode portions 526a2 and 526b2 of base electrode layer 526 and second principal-surface electrode portions 527a2 and 527b2 of base electrode layer 527.

[0247] (2-10) Thereafter, the third and fourth principal surface electrode portions are sequentially formed by repeating the steps (2-5) through (2-9). Note that the mask used in step (2-5) when sequentially forming the third and fourth principal surface electrode portions is formed so that the length along the direction connecting the end of the first principal surface electrode portion of the base electrode layer of the laminate 512 on the central side of the laminate 512 to the surfaces of the first internal electrode layer 516 a and the second internal electrode layer 516 b exposed on the surface of the laminate 512 is longer than that formed in the previous step (2-5).

[0248] As a result, as shown in Figure 14, when the length of the first principal surface electrode portion 526a1 is length A, the length of the second principal surface electrode portion 526a2 is length B, the length of the third principal surface electrode portion 526a3 is length C, and the length of the fourth principal surface electrode portion 526a4 is length D, the relationship of length A > length B > length C > length D is obtained.

[0249] Similarly, when the length of the first principal surface electrode portion 527b1 is length A, the length of the second principal surface electrode portion 527b2 is length B, the length of the third principal surface electrode portion 527b3 is length C, and the length of the fourth principal surface electrode portion 527b4 is length D, the relationship length A > length B > length C > length D is obtained.

[0250] Furthermore, as shown in FIG. 15, when the length of the first principal surface electrode portion 526b1 is length A, the length of the second principal surface electrode portion 526b2 is length B, the length of the third principal surface electrode portion 526b3 is length C, and the length of the fourth principal surface electrode portion 526b4 is length D, the relationship length A > length B > length C > length D is obtained.

[0251] Similarly, when the length of the first principal surface electrode portion 527a1 is length A, the length of the second principal surface electrode portion 527a2 is length B, the length of the third principal surface electrode portion 527a3 is length C, and the length of the fourth principal surface electrode portion 527a4 is length D, the relationship length A > length B > length C > length D is obtained.

[0252] In addition, when the base electrode layers 526, 527 having the first, second, third, and fourth principal surface electrode portions are formed only on the first principal surface 512a, as in the multilayer ceramic capacitor 310 shown in Figure 9, the resin masks obtained in the above steps (2-2) and (2-7) are formed so as not to cover the first side surface 512c, the second side surface 512d, the third side surface 512e, and the fourth side surface 512f of the laminate 512.

[0253] Next, when forming by screen printing, the following process is performed: That is, a printing plate is changed for each principal surface electrode of each layer, and a printing pattern corresponding to the desired shape of the principal surface electrode portion is formed at a desired position on the laminate 512.

[0254] At this time, the opposing distance between a pair of printed patterns in each of the width direction y and length direction z formed on the first main surface 512a of the laminate 512 is such that the length along the direction connecting the end of the first main surface electrode portion of the base electrode layer toward the center of the laminate to the surface of the first internal electrode layer exposed on the surface of the laminate 512 is longer for the one formed earlier than the one formed later for each of the formation of the first main surface electrode portion, the second main surface electrode portion, the third main surface electrode portion, and the fourth main surface electrode portion.

[0255] As a result, similar to the case where they are formed by sputtering, the configuration of each of the first to fourth main surface electrode portions such as the multilayer ceramic capacitor 510 shown in FIGS. 14 and 15 is obtained.

[0256] Thereafter, plating layers 528, 529 are formed on the surfaces of the fourth principal-surface electrode portions of the base electrode layers 526, 527. The plating layers 528, 529 are formed, for example, by barrel plating. When the plating layers 528, 529 have lower plating layers 530, 531 and upper plating layers 532, 533 as in the multilayer ceramic capacitor 510 shown in FIGS. 12 to 15 , the respective plating layers are formed sequentially, for example, by barrel plating.

[0257] When the plating layer 528 is directly formed as a plating layer, the following procedure is carried out.

[0258] That is, the first side surface 512c to the fourth side surface 512f of the laminate 512 are plated to form a plating film directly on the exposed portions of the first lead electrode portion 520a and the second lead electrode portion 520b of the internal electrode layer 516. While either electrolytic plating or electroless plating may be used for the plating process, electroless plating has the disadvantage of requiring pretreatment using a catalyst or the like to improve the plating deposition rate, which complicates the process. Therefore, electrolytic plating is usually preferred. Barrel plating is preferred as the plating method. If necessary, the plating layer 528 as the direct plating layer may be formed as a multilayer layer, as in the multilayer ceramic capacitor 310 shown in FIG. 9 , or an upper-layer plated electrode may be formed on the surface of a lower-layer plated electrode in the same manner.

[0259] In this manner, the multilayer ceramic capacitor 510 shown in FIG. 11 can be manufactured.

[0260] According to the method for manufacturing a multilayer ceramic capacitor according to the present embodiment described above, the ends of the first to fourth main-surface electrode portions formed on the first main surface of the laminate are arranged so as not to align, thereby dispersing the locations where stress occurs and making it possible to prevent cracks from propagating from the tips of the external electrodes into the interior of the multilayer ceramic capacitor.

[0261] C. Third Embodiment 1. Multilayer Ceramic Capacitor Next, a multilayer ceramic capacitor according to a third embodiment of the present invention will be described. FIG. 18 is an external perspective view showing a multilayer ceramic capacitor, which is an example of a multilayer ceramic electronic component according to the third embodiment of the present invention. FIG. 19 is a schematic cross-sectional view taken along line XIX-XIX in FIG. 18. FIG. 20 is a schematic cross-sectional view taken along line XX-XX in FIG. 18. However, components that are the same as or equivalent to those in the multilayer ceramic capacitor 10 of the first embodiment shown in FIGS. 1 to 10 are designated by the same reference numerals, and detailed description thereof will be omitted.

[0262] The multilayer ceramic capacitor 610 according to the third embodiment of the present invention has a laminate 12 and external electrodes 24 having the same configuration as the multilayer ceramic capacitor 10 according to the first embodiment. However, the multilayer ceramic capacitor 610 has the L dimension and the W dimension reversed compared to the multilayer ceramic capacitor 10 according to the first embodiment.

[0263] Specifically, it is preferable that the dimensions of the multilayer ceramic capacitor 610 are such that the L dimension in the length direction z is 0.1 mm or more and 2.5 mm or less, the T dimension in the height direction x is 0.04 mm or more and 2.5 mm or less, and the W dimension in the width direction y is 0.2 mm or more and 3.2 mm or less.

[0264] The multilayer ceramic capacitor 610 shown in FIG. 18 having the above-described configuration exhibits the same effects as the multilayer ceramic capacitor 10 of the first embodiment.

[0265] In addition, in the multilayer ceramic capacitor according to the third embodiment of the present invention, it is preferable that the external electrodes 24 of the multilayer ceramic capacitor 610 have the first to fourth modified examples similar to the external electrodes 24 of the first to fourth modified examples of the multilayer ceramic capacitor 10 according to the first embodiment.

[0266] 2. Method for Manufacturing the Multilayer Ceramic Capacitor A method for manufacturing the multilayer ceramic capacitor, which is an example of the multilayer ceramic capacitor according to the third embodiment, will now be described.

[0267] The method for manufacturing the multilayer ceramic capacitor according to the third embodiment is the same as the method for manufacturing the multilayer ceramic capacitor according to the first embodiment, except that the L dimension and the W dimension are interchanged with respect to the multilayer ceramic capacitor 10 according to the first embodiment.

[0268] In this manner, the multilayer ceramic capacitor 610 shown in FIG. 18 can be manufactured.

[0269] According to the method for manufacturing a multilayer ceramic capacitor according to the present embodiment described above, the ends of the first to fourth main-surface electrode portions formed on the first main surface of the laminate are arranged so as not to align, thereby dispersing the locations where stress occurs and making it possible to prevent cracks from propagating from the tips of the external electrodes into the interior of the multilayer ceramic capacitor.

[0270] As described above, the embodiment of the present invention has been disclosed in the above description, but the present invention is not limited to this.

[0271] In other words, various modifications can be made to the above-described embodiments and variants in terms of mechanism, shape, material, quantity, position, arrangement, etc., without departing from the scope of the technical idea and purpose of the present invention, and these modifications are included in the present invention.

[0272] <1> A laminate including a plurality of stacked ceramic layers, the laminate including first and second main surfaces opposing each other in a stacking direction of the plurality of ceramic layers, first and second side surfaces opposing each other in a width direction perpendicular to the stacking direction, first end surfaces and second end surfaces opposing each other in a length direction perpendicular to the stacking direction and the width direction, first internal electrode layers stacked alternately with the plurality of ceramic layers and exposed at the first end surfaces, and second internal electrode layers stacked alternately with the plurality of ceramic layers and exposed at the second end surfaces; a first external electrode covering a portion of the first main surface and at least a portion of the first end surfaces of the laminate; and a second external electrode covering a portion of the first main surface and at least a portion of the second end surfaces of the laminate, each of the first external electrode and the second external electrode comprising: a first main surface electrode portion disposed on the first main surface; and a second main surface electrode portion disposed on a portion of the first main surface electrode portion. a third main surface electrode portion disposed on a portion of the second main surface electrode portion; and a fourth main surface electrode portion disposed on a portion of the third main surface electrode portion, wherein, on the first main surface, when the length of the first main surface electrode portion in a direction connecting a center of the laminate to either a surface of the first internal electrode layer or a surface of the second internal electrode layer exposed on the surface of the laminate is length A, the length of the second main surface electrode portion in the same direction as length A is length B, the length of the third main surface electrode portion in the same direction as length A is length C, and the length of the fourth main surface electrode portion in the same direction as length A is length D, the relationship of length A > length B > length C > length D is satisfied.

[0273] <2> The multilayer ceramic capacitor according to <1>, wherein, in a direction connecting a center of the laminate and either a surface of the first internal electrode layer or the second internal electrode layer exposed on a surface of the laminate, an end of the first principal surface electrode portion on the center side of the laminate is not covered by the second principal surface electrode portion, an end of the second principal surface electrode portion on the center side of the laminate is not covered by the third principal surface electrode portion, and an end of the third principal surface electrode portion on the center side of the laminate is not covered by the fourth principal surface electrode portion.

[0274] <3> The multilayer ceramic capacitor according to <1> or <2>, wherein, in a direction connecting the first principal surface and the second principal surface, the first principal surface electrode portion has a thickness of 10 μm or less, the second principal surface electrode portion has a thickness of 10 μm or less, the third principal surface electrode portion has a thickness of 10 μm or less, and the fourth principal surface electrode portion has a thickness of 10 μm or less.

[0275] <4> The multilayer ceramic capacitor according to any one of <1> to <3>, wherein the first principal surface electrode portion contains a component similar to a main component of the ceramic layer.

[0276] <5> The multilayer ceramic capacitor according to <4>, wherein the second principal surface electrode portion includes a component similar to a main component of the ceramic layer, the third principal surface electrode portion includes a component similar to a main component of the ceramic layer, and the fourth principal surface electrode portion includes a component similar to a main component of the ceramic layer.

[0277] <6> The multilayer ceramic capacitor according to any one of <1> to <5>, wherein the first principal surface electrode portion is arranged so as to wrap around a plane orthogonal to the first principal surface, the second principal surface electrode portion is arranged so as to wrap around a plane orthogonal to the first principal surface, the third principal surface electrode portion is arranged so as to wrap around a plane orthogonal to the first principal surface, and the fourth principal surface electrode portion is arranged so as to wrap around a plane orthogonal to the first principal surface.

[0278] <7> The multilayer ceramic capacitor according to any one of <1> to <6>, wherein the thickness of the laminate is 150 μm or less in a direction connecting the first main surface and the second main surface.

[0279] <8> The multilayer ceramic capacitor according to any one of <1> to <6>, wherein the thickness of the laminate is 50 μm or less in a direction connecting the first main surface and the second main surface.

[0280] <9> The multilayer ceramic capacitor according to any one of <1> to <8>, wherein the fourth principal surface electrode portion is an outermost layer.

[0281] <10> The multilayer ceramic capacitor according to any one of <1> to <9>, wherein the dimension in the length direction is greater than the dimension in the width direction.

[0282] <11> The multilayer ceramic capacitor according to any one of <1> to <9>, wherein the dimension in the width direction is greater than the dimension in the length direction.

[0283] <12> A laminate including a plurality of stacked ceramic layers, the laminate including first and second main surfaces opposing each other in a stacking direction of the plurality of ceramic layers, first and second side surfaces opposing each other in a width direction perpendicular to the stacking direction, third and fourth side surfaces opposing each other in a length direction perpendicular to the stacking direction and the width direction, first internal electrode layers alternately stacked with the plurality of ceramic layers and exposed at least on the third and fourth side surfaces, and second internal electrode layers alternately stacked with the plurality of ceramic layers and exposed at least on the fourth and third side surfaces; a first external electrode covering a portion of the first main surface and at least a portion of the third side surface of the laminate; a second external electrode covering a portion of the first main surface and at least a portion of the fourth side surface of the laminate; and a third external electrode covering a portion of the first main surface and at least a portion of the fourth side surface of the laminate. and a fourth external electrode covering a portion of the first main surface of the laminate and at least a portion of the third side surface, wherein each of the first external electrode, the second external electrode, the third external electrode, and the fourth external electrode has: a first main surface electrode portion arranged on the first main surface; a second main surface electrode portion arranged on a portion of the first main surface electrode portion; a third main surface electrode portion arranged on a portion of the second main surface electrode portion; and a fourth main surface electrode portion arranged on a portion of the third main surface electrode portion, wherein on the first main surface, a length of the first main surface electrode portion in a direction connecting a center of the laminate to a surface of either the first internal electrode layer or the second internal electrode layer exposed on the surface of the laminate is defined as length A, a length of the second main surface electrode portion in the same direction as length A is length B, a length of the third main surface electrode portion in the same direction as length A is length C, When the length of the fourth principal surface electrode portion in the same direction as length A is length D, the multilayer ceramic capacitor satisfies the relationship length A>length B>length C>length D.

[0284] <13> The multilayer ceramic capacitor according to <12>, wherein a ratio of the dimension in the width direction to the dimension in the length direction is 0.85 or more and 1.00 or less.

[0285] 10, 110, 210, 310, 410, 510, 610 Multilayer ceramic capacitor 12, 512 Laminate 12a, 512a First main surface 12b, 512b Second main surface 12c, 512c First side surface 12d, 512d Second side surface 12e First end surface 12f Second end surface 14, 514 Ceramic layer 15a, 515a Effective layer portion 15b1, 515b1 First outer layer portion 15b2, 515b2 Second outer layer portion 16, 516 Internal electrode layer 16a, 516a First internal electrode layer 16b, 516b Second internal electrode layer 18a, 518a First opposing electrode portion 18b, 518b Second opposing electrode portion 20a, 520a First lead electrode portion 20b, 520b Second lead electrode portion 22a, 522a, 522b Side portion 22b End portion 24, 524, 525 External electrode 24a, 524a First external electrode 24b, 524b Second external electrode 26, 526, 527 Base electrode layer 26a, 526a First base electrode layer 26b, 526b Second base electrode layer 26a1, 26b1, 526a1, 526b1, 527a1, 527b1 First principal surface electrode portion 26a2, 26b2, 526a2, 526b2, 527a2, 527b2 Second principal surface electrode portion 26a3, 26b3, 526a3, 526b3, 527a3, 527b3 Third principal surface electrode portion 26a4, 26b4, 526a4, 526b4, 527a4, 527b4 Fourth principal surface electrode portion 26a1t, 26b1t, 526a1t, 526b1t, 527a1t, 527b1t First end portion 26a2t, 26b2t, 526a2t, 526b2t, 527a2t, 527b2t Second end portion 26a3t, 26b3t, 526a3t, 526b3t, 527a3t, 527b3t Third end portion 26a4t, 26b4t, 526a4t, 526b4t, 527a4t, 527b4t Fourth end 28, 528, 529 Plating layer 28a, 528a First plating layer 28b, 528b Second plating layer 30, 530, 531 Underplating layer 30a, 530a, 531a First underplating layer 30b, 530b, 531b Second underplating layer 32, 532, 533 Top plating layer 32a, 532a, 533a First top plating layer32b, 532b, 533b Second top plating layer 34, 534, 535 Intermediate plating layer 34a, 534a, 535a First intermediate plating layer 34b, 534b, 535b Second intermediate plating layer 36, 536, 537 Top plating layer 36a, 536a, 537a First top plating layer 36b, 536b, 537b Second top plating layer 512e Third side surface 512f Fourth side surface 521a Third lead electrode portion 521b Fourth lead electrode portion 525a Third external electrode 525b Fourth external electrode 527a Third base electrode layer 527b Fourth base electrode layer 529a Third plating layer 529b Fourth plating layer

Claims

1. A laminate including a plurality of ceramic layers stacked together, the laminate including first and second main surfaces facing each other in a stacking direction of the plurality of ceramic layers, first and second side surfaces facing each other in a width direction perpendicular to the stacking direction, first end faces and second end faces facing each other in a length direction perpendicular to the stacking direction and the width direction, first internal electrode layers stacked alternately with the plurality of ceramic layers and exposed at the first end faces, and second internal electrode layers stacked alternately with the plurality of ceramic layers and exposed at the second end faces; a first external electrode covering a portion of the first main surface and at least a portion of the first end faces of the laminate; and a second external electrode covering a portion of the first main surface and at least a portion of the second end faces of the laminate, each of the first external electrode and the second external electrode comprising: a first main surface electrode portion disposed on the first main surface; and a second main surface electrode portion disposed on a portion of the first main surface electrode portion. a third main surface electrode portion disposed on a portion of the second main surface electrode portion; and a fourth main surface electrode portion disposed on a portion of the third main surface electrode portion, wherein, on the first main surface, when a length of the first main surface electrode portion in a direction connecting a center of the laminate to either a surface of the first internal electrode layer or a surface of the second internal electrode layer exposed on a surface of the laminate is defined as length A, a length of the second main surface electrode portion in the same direction as length A is length B, a length of the third main surface electrode portion in the same direction as length A is length C, and a length of the fourth main surface electrode portion in the same direction as length A is length D, the relationship of length A > length B > length C > length D is satisfied.

2. The multilayer ceramic capacitor according to claim 1, wherein, in a direction connecting the center of the laminate to either a surface of the laminate where the first internal electrode layer or the second internal electrode layer is exposed, an end of the first principal surface electrode portion toward the center of the laminate is not covered by the second principal surface electrode portion, an end of the second principal surface electrode portion toward the center of the laminate is not covered by the third principal surface electrode portion, and an end of the third principal surface electrode portion toward the center of the laminate is not covered by the fourth principal surface electrode portion.

3. A multilayer ceramic capacitor as described in claim 1 or 2, wherein, in a direction connecting the first main surface and the second main surface, the first main surface electrode portion has a thickness of 10 μm or less, the second main surface electrode portion has a thickness of 10 μm or less, the third main surface electrode portion has a thickness of 10 μm or less, and the fourth main surface electrode portion has a thickness of 10 μm or less.

4. The multilayer ceramic capacitor according to claim 1, wherein the first principal surface electrode portion contains a component similar to the main component of the ceramic layers.

5. The multilayer ceramic capacitor according to claim 4, wherein the second principal surface electrode portion contains a component similar to a main component of the ceramic layer, the third principal surface electrode portion contains a component similar to a main component of the ceramic layer, and the fourth principal surface electrode portion contains a component similar to a main component of the ceramic layer.

6. A multilayer ceramic capacitor as claimed in any one of claims 1 to 5, wherein the first principal surface electrode portion is arranged so as to wrap around a plane perpendicular to the first principal surface, the second principal surface electrode portion is arranged so as to wrap around a plane perpendicular to the first principal surface, the third principal surface electrode portion is arranged so as to wrap around a plane perpendicular to the first principal surface, and the fourth principal surface electrode portion is arranged so as to wrap around a plane perpendicular to the first principal surface.

7. The multilayer ceramic capacitor according to claim 1, wherein the thickness of the laminate in the direction connecting the first main surface and the second main surface is 150 μm or less.

8. The multilayer ceramic capacitor according to claim 1, wherein the thickness of the laminate in the direction connecting the first main surface and the second main surface is 50 μm or less.

9. The multilayer ceramic capacitor according to claim 1, wherein the fourth principal surface electrode portion is the outermost layer.

10. The multilayer ceramic capacitor according to claim 1, wherein the dimension in the length direction is greater than the dimension in the width direction.

11. The multilayer ceramic capacitor according to claim 1, wherein the dimension in the width direction is greater than the dimension in the length direction.

12. A laminate including a plurality of stacked ceramic layers, the laminate including a first main surface and a second main surface facing each other in a stacking direction of the plurality of ceramic layers, a first side surface and a second side surface facing each other in a width direction perpendicular to the stacking direction, a third side surface and a fourth side surface facing each other in a length direction perpendicular to the stacking direction and the width direction, a first internal electrode layer stacked alternately with the plurality of ceramic layers and exposed at least on the third side surface and the fourth side surface, and a second internal electrode layer stacked alternately with the plurality of ceramic layers and exposed at least on the fourth side surface and the third side surface; a first external electrode covering a portion of the first main surface and at least a portion of the third side surface of the laminate; a second external electrode covering a portion of the first main surface and at least a portion of the fourth side surface of the laminate; and a third external electrode covering a portion of the first main surface and at least a portion of the fourth side surface of the laminate. and a fourth external electrode covering a portion of the first main surface of the laminate and at least a portion of the third side surface, wherein each of the first external electrode, the second external electrode, the third external electrode, and the fourth external electrode has a first main surface electrode portion arranged on the first main surface, a second main surface electrode portion arranged on a portion of the first main surface electrode portion, a third main surface electrode portion arranged on a portion of the second main surface electrode portion, and a fourth main surface electrode portion arranged on a portion of the third main surface electrode portion, and on the first main surface, A multilayer ceramic capacitor, wherein, when the length of the fourth principal surface electrode portion in the same direction as length A is length D, length A>length B>length C>length D.

13. The multilayer ceramic capacitor according to claim 12, wherein the ratio of the dimension in the width direction to the dimension in the length direction is 0.85 or more and 1.00 or less.

Citation Information

Patent Citations

  • Multilayer ceramic capacitor

    JP2017199847A

  • Multilayer ceramic electronic component, manufacturing method thereof, and electronic component built-in substrate

    JP2020017557A

  • Ceramic electronic component and method for manufacturing same

    WO2008001542A1