Organic hydride production device and organic hydride production method

The use of a high entropy alloy as the anode catalyst in organic hydride production equipment addresses durability and cost issues, enhancing catalyst longevity and production efficiency by employing base metal elements, thus overcoming limitations in conventional noble metal-based systems.

WO2024219065A1PCT designated stage expired Publication Date: 2024-10-24ENEOS CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/004583
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-02-09
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional organic hydride production equipment has limitations in durability and efficiency due to the use of noble metals like Ir, which are costly and prone to degradation from hydride and organic hydride leakage, leading to increased electrolytic voltage and reduced catalyst activity over time.

Method used

The use of a high entropy alloy containing base metal elements as the anode catalyst, which improves durability and maintains catalytic activity, combined with a cathode catalyst layer and electrolyte membrane for efficient electrochemical reduction of hydrides to produce organic hydrides.

Benefits of technology

This solution enhances the durability and cost-effectiveness of the anode catalyst, maintaining activity over time and improving production efficiency while reducing equipment costs by using cheaper base metal elements in the high entropy alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024004583_24102024_PF_FP_ABST
    Figure JP2024004583_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This organic hydride production device 2 comprises, as an anode catalyst 11, an anode electrode 10 having a high entropy alloy containing a base metal element, a cathode electrode 8, and an electrolyte membrane 12 positioned between the anode electrode 10 and the cathode electrode 8. The anode electrode 10 oxidizes water or hydroxide ions. The cathode electrode 8 electrochemically reduces a hydride to generate an organic hydride.
Need to check novelty before this filing date? Find Prior Art

Description

Organic hydride production apparatus and organic hydride production method

[0001] The present invention relates to an organic hydride manufacturing apparatus and an organic hydride manufacturing method.

[0002] Patent Document 1 describes a water electrolysis device that includes a high-entropy alloy as a catalyst for the oxygen generation reaction.

[0003] International Publication No. 2022 / 080142

[0004] In recent years, organic hydrides have attracted attention as an energy carrier for the large-scale transport and storage of hydrogen derived from renewable energy. Regarding the production of organic hydrides, an organic hydride production apparatus is known that generates protons from water at an anode electrode and hydrogenates a substance to be hydrided with the protons at a cathode electrode to produce an organic hydride.

[0005] As in the case of water electrolysis, the anode catalyst of an organic hydride manufacturing apparatus is required to have oxygen evolution reaction (OER) activity, acid resistance, oxidation potential resistance, electrical conductivity, etc., as well as resistance to the substances to be hydrided and organic hydrides that cross leak from the cathode electrode side. In conventional organic hydride manufacturing apparatuses, Ir or the like has generally been used as the anode catalyst, but the present inventors, after extensive research, have come to recognize that there is room for improving the durability of the anode catalyst in conventional organic hydride manufacturing apparatuses.

[0006] The present invention has been made in view of the above circumstances, and one of its objects is to improve the durability of an anode catalyst used in an organic hydride manufacturing apparatus.

[0007] One aspect of the present invention is an apparatus for producing organic hydrides. The apparatus includes an anode electrode having a high-entropy alloy containing a base metal element as an anode catalyst, a cathode electrode, and an electrolyte membrane positioned between the anode electrode and the cathode electrode. The anode electrode oxidizes water or hydroxide ions. The cathode electrode electrochemically reduces a substance to be hydrided to produce an organic hydride.

[0008] Another aspect of the present invention is a method for producing an organic hydride using an organic hydride production apparatus including an anode electrode having a high-entropy alloy containing a base metal element as an anode catalyst, a cathode electrode, and an electrolyte membrane located between the anode electrode and the cathode electrode. This production method includes oxidizing water or hydroxide ions at the anode electrode and electrochemically reducing a substance to be hydrided at the cathode electrode to produce an organic hydride.

[0009] Any combination of the above components, and conversion of the expression of the present disclosure into a method, device, system, etc., are also valid aspects of the present disclosure.

[0010] According to the present invention, it is possible to improve the durability of the anode catalyst used in an organic hydride manufacturing apparatus.

[0011] 5A is a schematic diagram of an organic hydride production system including an organic hydride production apparatus according to an embodiment. FIG. 6A is a diagram showing the current density of each cell in a toluene poisoning test. FIG. 6B is a diagram showing by-products generated by constant-potential electrolysis. FIG. 4A is a diagram showing the results of FT-IR analysis of the working electrode of Example 1 after a toluene poisoning test. FIG. 4B is a diagram showing the results of FT-IR analysis of the working electrode of Comparative Example 1 after a toluene poisoning test. FIG. 5A is a diagram showing the current density of the cell of Example 1 in a toluene oxidation product poisoning test. FIG. 5B is a diagram showing the current density of the cell of Comparative Example 1 in a toluene oxidation product poisoning test. FIG. 6A is a diagram showing the results of FT-IR analysis of the working electrode of Example 1 after a toluene oxidation product poisoning test. FIG. 6B is a diagram showing the results of FT-IR analysis of the working electrode of Comparative Example 1 after a toluene oxidation product poisoning test.

[0012] The present invention will be described below with reference to the drawings, based on preferred embodiments. The embodiments are merely illustrative and do not limit the technical scope of the present invention. Not all features or combinations thereof described in the embodiments are necessarily essential to the invention. Therefore, many design modifications, such as changes, additions, or deletions of components, are possible within the scope of the invention as defined in the claims. A new embodiment incorporating design modifications will combine the effects of the combined embodiments and modifications. In the embodiments, design modifications that are possible are emphasized by using terms such as "in this embodiment" or "in this embodiment." However, design modifications are also permitted even in areas without such notation. Any combination of the components described in the embodiments is also valid as an aspect of the present invention. Identical or equivalent components, members, and processes shown in each drawing are designated by the same reference numerals, and redundant descriptions are omitted where appropriate. Furthermore, the scale and shape of each part shown in each drawing are set for convenience and should not be construed as limiting unless otherwise specified. Furthermore, when terms such as "first" and "second" are used in this specification or claims, these terms do not represent any order or importance, but are used to distinguish one configuration from another. Furthermore, in each drawing, some members that are not important for explaining the embodiments are omitted.

[0013] FIG. 1 is a schematic diagram of an organic hydride production system 1 including an organic hydride production apparatus 2 according to an embodiment. The organic hydride production system 1, as an example, includes an organic hydride production apparatus 2, a cathode fluid tank 4, and an anode fluid tank 6. Although FIG. 1 illustrates only one organic hydride production apparatus 2, the organic hydride production system 1 may include a plurality of organic hydride production apparatuses 2. In this case, the organic hydride production apparatuses 2 are stacked and oriented in the same direction, for example, so that the cathode electrodes 8 and anode electrodes 10 are aligned in the same order, and are electrically connected in series. The organic hydride production apparatuses 2 may be connected in parallel, or a combination of series and parallel connections may be used. The configuration of the organic hydride production system 1 is not limited to that described below, and the configuration of each component may be modified as appropriate.

[0014] The organic hydride production apparatus 2 is an electrolysis cell that produces organic hydride by hydrogenating a material to be hydrogenated, which is a dehydrogenated form of organic hydride, through an electrochemical reduction reaction. The organic hydride production apparatus 2 includes a cathode electrode 8 (negative electrode), an anode electrode 10 (positive electrode), an electrolyte membrane 12, a pair of plate members 14a, 14b, and a pair of gaskets 16a, 16b. The cathode electrode 8, the anode electrode 10, and the electrolyte membrane 12 constitute a membrane electrode assembly. While the present embodiment will be described using a membrane electrode assembly as an example, the organic hydride production apparatus 2 may have a so-called zero-gap electrode structure in which an electrode, formed by applying an anode catalyst to a solid support substrate, is in physical contact with the electrolyte membrane.

[0015] The cathode electrode 8 electrochemically reduces the material to be hydrided to produce an organic hydride. In this embodiment, "electrochemical" means that the reaction proceeds when a voltage or current is applied from outside the organic hydride manufacturing apparatus 2. The cathode electrode 8 has a cathode catalyst 9. For example, the cathode catalyst 9 is contained in a cathode catalyst layer. The cathode catalyst 9 includes a noble metal such as Pt (platinum), Ru (ruthenium), or Pd (palladium), or a base metal such as Ni (nickel). In the cathode catalyst layer, the cathode catalyst 9 can be supported by a porous catalyst support. The catalyst support is made of an electron-conductive material such as porous carbon, porous metal, or porous metal oxide.

[0016] When the electrolyte membrane 12 has proton conductivity, the cathode catalyst 9 is coated with a cation exchange ionomer. For example, a catalyst support supporting the cathode catalyst 9 is coated with the ionomer. Examples of cation exchange ionomers include perfluorosulfonic acid polymers such as Nafion (registered trademark), Flemion (registered trademark), Aquivion (registered trademark), and Aciplex (registered trademark), and hydrocarbon-based sulfonic acid polymers. The ionomer preferably partially coats the cathode catalyst 9. Preferably, 10% or more of the surface of each cathode catalyst 9 is coated with the ionomer. This allows the three elements necessary for the electrochemical reaction at the cathode electrode 8, i.e., the substance to be hydrided, protons, and electrons, to be efficiently supplied to the reaction field.

[0017] When the electrolyte membrane 12 has anion conductivity, the cathode catalyst 9 is coated with an anion exchange ionomer. For example, a catalyst support supporting the cathode catalyst 9 is coated with the ionomer. An example of an anion exchange ionomer is a polymer such as Fumion (registered trademark). It is preferable that the ionomer partially coats the cathode catalyst 9. Preferably, 10% or more of the surface of each cathode catalyst 9 is coated with the ionomer. This allows the three elements necessary for the electrochemical reaction at the cathode electrode 8, i.e., the substance to be hydrided, water, and electrons, to be efficiently supplied to the reaction field.

[0018] The cathode electrode 8 may be provided with a cathode diffusion layer. As an example, the cathode catalyst layer is disposed so as to be in contact with one main surface of the electrolyte membrane 12. The cathode diffusion layer is disposed so as to be in contact with the main surface of the cathode catalyst layer opposite the electrolyte membrane 12. The cathode diffusion layer uniformly diffuses the substance to be hydrogenated, which is supplied from the outside, into the cathode catalyst layer. The organic hydride generated in the cathode catalyst layer is discharged to the outside of the cathode electrode 8 through the cathode diffusion layer. The cathode diffusion layer is made of a conductive material such as carbon or metal. The cathode diffusion layer is also a porous body such as a sintered body of fibers or particles, or a foam molded body. Examples of materials that can be used to form the cathode diffusion layer include woven carbon fabric (carbon cloth), nonwoven carbon fabric, and carbon paper. The cathode diffusion layer may be omitted in some cases.

[0019] The anode electrode 10 oxidizes water or hydroxide ions. If the electrolyte membrane 12 has proton conductivity, the anode electrode 10 oxidizes water to produce protons. If the electrolyte membrane 12 has anion conductivity, the anode electrode 10 oxidizes hydroxide ions to produce oxygen. The anode electrode 10 has an anode catalyst 11. For example, the anode catalyst 11 is contained in an anode catalyst layer. In the anode catalyst layer, the anode catalyst 11 may be dispersed and supported on or coated on an electronically conductive substrate. The substrate is made of a material whose main component is a metal such as Ti (titanium) or SUS (stainless steel). Examples of the form of the substrate include a woven or nonwoven sheet, a mesh, a porous sintered body, a foam, and an expanded metal.

[0020] The anode electrode 10 of this embodiment has a high-entropy alloy (HEA) containing a base metal element as the anode catalyst 11. A high-entropy alloy is a solid solution alloy in which the atomic composition ratios of five or more constituent elements are substantially equal. The entropy of mixing is increased when the atomic composition ratios of five or more constituent elements are substantially equal. In this embodiment, "substantially equal" means that the atomic composition ratios of the elements are equal to an extent that the entropy is high, and differences of the order of manufacturing error are allowed. For example, the atomic composition ratio of the element with the highest atomic composition ratio among the five or more constituent elements is C max The atomic composition ratio of the element with the lowest atomic composition ratio is C min When this is done, (C max -C min ) / (C max +C min )≦0.2, and (C max -C min ) / (C max +C min )≦0.1 is preferable. The atomic composition ratio of each metal element in the solid solution alloy is preferably 4 atm % or more and 24 atm % or less, and more preferably 5 atm % or more and 20 atm % or less.

[0021] As described above, it is known to use a high-entropy alloy for an oxygen generating electrode in water electrolysis. However, a person skilled in the art would not easily have conceived of using a high-entropy alloy containing a base metal element as the anode catalyst 11 of the organic hydride manufacturing apparatus 2 as in the present embodiment.

[0022] This is because, firstly, in the organic hydride manufacturing apparatus 2, the material to be hydrided and the organic hydride may leak from the cathode electrode 8 side to the anode electrode 10 side. For this reason, in the organic hydride manufacturing apparatus 2, the OER overvoltage at the anode electrode 10 tends to be larger than in the case of water electrolysis. Therefore, those skilled in the art believe that a high-entropy alloy containing a base metal element that has a lower OER activity than a noble metal such as Ir is useless as the anode catalyst 11.

[0023] Second, the operating temperature of the organic hydride production apparatus 2 is set lower than that for water electrolysis so as not to exceed the boiling points of the material to be hydrided and the organic hydride. The electrolysis voltage of the organic hydride production apparatus 2 is highly dependent on temperature, with the electrolysis voltage increasing as the temperature decreases. Therefore, those skilled in the art believe that high-entropy alloys containing base metal elements, which are expected to increase the electrolysis voltage due to their low OER activity, are useless as the anode catalyst 11.

[0024] Third, it is common technical knowledge that high-entropy alloys containing base metals as constituent elements are considered to be less durable than noble metals such as Ir. Also, as mentioned in the first reason, the anode catalyst 11 is prone to deterioration because the material to be hydrided and the organic hydride may leak in the organic hydride production apparatus 2. Therefore, those skilled in the art would consider that high-entropy alloys containing base metal elements, which are less durable, are useless as the anode catalyst 11.

[0025] Thus, it is natural that one would not normally think of using a high-entropy alloy containing a base metal element as the anode catalyst 11 for producing organic hydrides. However, as a result of intensive research, the present inventors have discovered that, contrary to expectations, a high-entropy alloy containing a base metal element has high durability against substances to be hydrided. This finding should not be considered as something that a person skilled in the art could easily arrive at.

[0026] Therefore, by using a high-entropy alloy as the anode catalyst 11, the durability of the anode catalyst 11 can be improved. This allows the activity of the anode catalyst 11 to be maintained for a long period of time, thereby improving the production efficiency of organic hydrides. Furthermore, since high-entropy alloys containing base metal elements are cheaper than noble metals such as Ir, the costs associated with producing organic hydrides can also be reduced. Furthermore, it is preferable that all of the constituent elements of a high-entropy alloy containing a base metal element are base metal elements. Note that although Cu has a smaller ionization tendency than hydrogen and a standard electrode potential that is positive relative to a hydrogen standard electrode, it is treated as a base metal in this application.

[0027] Preferably, the high-entropy alloy contains at least one element selected from the group consisting of Mn, Fe, Co, Ni, Cr, Ti, Zr, Nb, Mo, and Cu. More preferably, the high-entropy alloy contains at least one element selected from the group consisting of Mn, Fe, Co, and Ni (hereinafter referred to as the first group) and at least one element selected from the group consisting of Cr, Ti, Zr, Nb, Mo, and Cu (hereinafter referred to as the second group).

[0028] The elements of the first group have higher catalytic activity than the elements of the second group. Meanwhile, the elements of the second group have higher durability against the anolyte LA than the elements of the first group. Therefore, by including elements of the first group and elements of the second group in the high-entropy alloy, it is possible to achieve both improved catalytic performance and improved durability of the anode catalyst 11. The average particle size D50 of the high-entropy alloy is, for example, 1 nm or more and 100 μm or less.

[0029] Furthermore, the anode catalyst 11 preferably has a elution rate of elements contained in the high-entropy alloy of 60 μg / h or less per 1 g of anode catalyst when a rated current, i.e., a current during rated electrolysis in the organic hydride production apparatus 2, is applied, or when a rated voltage, i.e., a voltage during rated electrolysis in the organic hydride production apparatus 2, is applied, or when the anode catalyst 11 is immersed in an acidic solution with a pH of 4.0 or less, the elution rate of elements contained in the high-entropy alloy is 60 μg / h or less per 1 g of anode catalyst. In this way, by keeping the high-entropy alloy in a stable state, elution of the constituent elements of the high-entropy alloy from the anode catalyst 11 during operation of the organic hydride production system 1 can be suppressed.

[0030] The stable state of the high-entropy alloy can be achieved by subjecting the anode catalyst 11 to a prior aging treatment. The aging treatment includes at least one of electrolysis of an electrolyte using the anode catalyst 11 and immersion of the anode catalyst 11 in an acidic solution having a pH of 4.0 or less. In the present embodiment, "prior" means before organic hydride production is carried out in the organic hydride production apparatus 2. For example, "pre-aging" means immersing the anode electrode 10 alone in an electrolyte such as a sulfuric acid aqueous solution and applying an electrolytic current or an electrolytic voltage. Furthermore, "pre-aging" means immersing the anode electrode 10 alone in an acidic solution having a pH of 4.0 or less.

[0031] The anode electrode 10 may be provided with an anode diffusion layer. For example, the anode catalyst layer is disposed so as to be in contact with the other main surface of the electrolyte membrane 12. The anode diffusion layer is disposed so as to be in contact with the main surface of the anode catalyst layer opposite the electrolyte membrane 12. The anode diffusion layer may have a structure similar to that of the cathode diffusion layer.

[0032] The electrolyte membrane 12 is located between the cathode electrode 8 and the anode electrode 10. As an example, the electrolyte membrane 12 has proton conductivity. In this case, the electrolyte membrane 12 moves protons from the anode electrode 10 to the cathode electrode 8. As an example, the electrolyte membrane 12 is made of a proton-conductive polymer electrolyte membrane (PEM). Examples of PEMs include fluorine-based ion exchange membranes having sulfonic acid groups, such as Nafion (registered trademark), and hydrocarbon-based ion exchange membranes, such as Fumasep (registered trademark).

[0033] 1 illustrates an electrolyte membrane 12 having proton conductivity, but is not limited to this configuration, and the electrolyte membrane 12 may also have anion conductivity. In this case, the electrolyte membrane 12 moves hydroxide ions from the cathode electrode 8 to the anode electrode 10. As an example, the electrolyte membrane 12 is formed of a solid polymer electrolyte membrane (AEM) having anion conductivity. Examples of AEM include known anion exchange membranes such as Fumasep (registered trademark), Pension, and Sustainion (registered trademark).

[0034] The plate members 14a and 14b are made of metal such as SUS or Ti. The plate member 14a is stacked on the membrane electrode assembly from the cathode electrode 8 side. The plate member 14b is stacked on the membrane electrode assembly from the anode electrode 10 side. Therefore, the membrane electrode assembly is sandwiched between the pair of plate members 14a and 14b. The gap between the plate member 14a and the membrane electrode assembly is sealed by a gasket 16a. The gap between the plate member 14b and the membrane electrode assembly is sealed by a gasket 16b. When the organic hydride production system 1 includes only one organic hydride production apparatus 2, the pair of plate members 14a and 14b can correspond to so-called end plates. When the organic hydride production system 1 includes multiple organic hydride production apparatuses 2 and another organic hydride production apparatus 2 is arranged next to the plate member 14a or the plate member 14b, the plate member can correspond to so-called separators.

[0035] A cathode flow path 18 is connected to the cathode electrode 8. The cathode flow path 18 supplies and discharges the cathode fluid LC to the cathode electrode 8. Note that a groove may be provided on the main surface of the plate member 14a facing the cathode electrode 8, and this groove may constitute the cathode flow path 18.

[0036] An anode flow path 20 is connected to the anode electrode 10. The anode flow path 20 supplies and discharges the anolyte LA to and from the anode electrode 10. A groove may be provided in a main surface of the plate member 14b facing the anode electrode 10, and this groove may constitute the anode flow path 20.

[0037] The cathode fluid tank 4 is connected to the cathode flow path 18 via a first cathode pipe 24 and a second cathode pipe 26. The cathode fluid tank 4 stores cathode fluid LC. One end of the first cathode pipe 24 is connected to the cathode fluid tank 4, and the other end of the first cathode pipe 24 is connected to the inlet of the cathode flow path 18. A cathode pump 28 is provided midway along the first cathode pipe 24. The cathode pump 28 can be a known pump such as a gear pump or a cylinder pump. Note that the circulation of the cathode fluid LC may be achieved by a liquid delivery device other than a pump. One end of the second cathode pipe 26 is connected to the outlet of the cathode flow path 18, and the other end of the second cathode pipe 26 is connected to the cathode fluid tank 4.

[0038] The catholyte LC contains a hydrogenation target substance, which is an organic hydride raw material. As an example, the catholyte LC does not contain any organic hydride before the organic hydride production system 1 starts operating, and after the start of operation, the catholyte LC becomes a mixed liquid of the target substance and organic hydride as a result of the organic hydride produced by electrolysis being mixed in. The target substance and organic hydride are preferably liquids at 20°C and 1 atmosphere.

[0039] The material to be hydrogenated and the organic hydride are not particularly limited as long as they are organic compounds that can add / desorb hydrogen by reversibly causing a hydrogenation reaction / dehydrogenation reaction. The material to be hydrogenated and the organic hydride used in this embodiment can be a wide variety of materials such as acetone-isopropanol, benzoquinone-hydroquinone, and aromatic hydrocarbons. Among these, aromatic hydrocarbons are preferred from the viewpoint of transportability during energy transportation.

[0040] The aromatic hydrocarbon compound used as the compound to be hydrogenated is a compound containing at least one aromatic ring. Examples of aromatic hydrocarbon compounds include benzene, alkylbenzene, naphthalene, alkylnaphthalene, anthracene, diphenylethane, and tetralin. Alkylbenzenes include compounds in which one to four hydrogen atoms on the aromatic ring are substituted with a linear or branched alkyl group having one to six carbon atoms. Examples of such compounds include toluene, xylene, mesitylene, ethylbenzene, and diethylbenzene. Alkylnaphthalenes include compounds in which one to four hydrogen atoms on the aromatic ring are substituted with a linear or branched alkyl group having one to six carbon atoms. Examples of such compounds include methylnaphthalene. These compounds may be used alone or in combination.

[0041] The substance to be hydrogenated is preferably at least one selected from the group consisting of toluene, benzene, and xylene. Nitrogen-containing heterocyclic aromatic compounds such as quinoline, isoquinoline, N-alkylpyrrole, N-alkylindole, and N-alkyldibenzopyrrole can also be used as the substance to be hydrogenated. Organic hydrides are the hydrogenated versions of the above-mentioned substances to be hydrogenated, and examples include cyclohexane, methylcyclohexane, dimethylcyclohexane, and decahydroquinoline.

[0042] The cathode pump 28 drives the cathode fluid LC in the cathode fluid tank 4 to flow into the cathode electrode 8 via the first cathode pipe 24. The cathode fluid LC that has flowed into the cathode electrode 8 is used for an electrode reaction at the cathode electrode 8. The cathode fluid LC in the cathode electrode 8 returns to the cathode fluid tank 4 via the second cathode pipe 26. As an example, the cathode fluid tank 4 also functions as a gas-liquid separator. Hydrogen gas may be generated at the cathode electrode 8 due to a side reaction. Therefore, the cathode fluid LC discharged from the cathode electrode 8 may contain hydrogen gas. The cathode fluid tank 4 separates the hydrogen gas in the cathode fluid LC from the cathode fluid LC and discharges it to the outside of the system.

[0043] A gas-liquid separator may be provided separately from the cathode fluid tank 4. The organic hydride manufacturing system 1 may also be provided with an oil-water separator for separating water from the cathode fluid LC, as necessary. Alternatively, the cathode fluid tank 4 may function as the oil-water separator. In the organic hydride manufacturing system 1 of this embodiment, the cathode fluid LC is circulated between the cathode electrode 8 and the cathode fluid tank 4. However, the present invention is not limited to this configuration, and the cathode fluid LC may be sent from the cathode electrode 8 to the outside of the system without being returned to the cathode fluid tank 4.

[0044] An anode fluid tank 6 is connected to the anode flow path 20 via a first anode pipe 30 and a second anode pipe 32. The anode fluid tank 6 stores anode fluid LA. One end of the first anode pipe 30 is connected to the anode fluid tank 6, and the other end of the first anode pipe 30 is connected to an inlet of the anode flow path 20. An anode pump 34 is provided midway along the first anode pipe 30. The anode pump 34 may be a known pump such as a gear pump or a cylinder pump. The flow of the anode fluid LA may be achieved by a fluid delivery device other than a pump. One end of the second anode pipe 32 is connected to an outlet of the anode flow path 20, and the other end of the second anode pipe 32 is connected to the anode fluid tank 6.

[0045] The anolyte LA contains water. When the electrolyte membrane 12 has proton conductivity, examples of the anolyte LA include acidic solutions such as an aqueous sulfuric acid solution, an aqueous nitric acid solution, and an aqueous hydrochloric acid solution; pure water; and ion-exchanged water. Preferably, the pH of the anolyte LA is 8 or less. When the electrolyte membrane 12 has anion conductivity, examples of the anolyte LA include alkaline solutions such as an aqueous potassium hydroxide solution; ion-exchanged water; and aqueous solutions containing inorganic electrolytes such as potassium sulfate. Preferably, the pH of the anolyte LA is 6 or more.

[0046] The anode pump 34 drives the anode fluid LA in the anode fluid tank 6 to flow into the anode electrode 10 via the first anode pipe 30. If the electrolyte membrane 12 has proton conductivity, the water in the anode fluid LA that has flowed into the anode electrode 10 is used for the electrode reaction at the anode electrode 10. If the electrolyte membrane 12 has anion conductivity, the water in the anode fluid LA that has flowed into the anode electrode 10 diffuses through the electrolyte membrane 12 to the cathode electrode 8 side and is used for the electrode reaction at the cathode electrode 8. The anode fluid LA in the anode electrode 10 is returned to the anode fluid tank 6 via the second anode pipe 32. For example, the anode fluid tank 6 also functions as a gas-liquid separator. Oxygen gas is generated by the electrode reaction at the anode electrode 10. Therefore, oxygen gas is mixed into the anode fluid LA discharged from the anode electrode 10. The anolyte tank 6 separates the oxygen gas in the anolyte LA from the anolyte LA and discharges it to the outside of the system.

[0047] A gas-liquid separator may be provided separately from the anode fluid tank 6. In the organic hydride manufacturing system 1 of the present embodiment, the anode fluid LA is circulated between the anode electrode 10 and the anode fluid tank 6. However, the present invention is not limited to this configuration, and the anode fluid LA may be sent from the anode electrode 10 to the outside of the system without being returned to the anode fluid tank 6.

[0048] Electric power is supplied to the organic hydride manufacturing apparatus 2 from a power source 22. The supply of electric power from the power source 22 applies a predetermined electrolysis voltage between the cathode electrode 8 and the anode electrode 10, causing an electrolysis current to flow. The power source 22 sends electric power supplied from an external power supply device 38 to the organic hydride manufacturing apparatus 2. The power supply device 38 can be configured as a power generation device that generates electric power using renewable energy, such as a wind power generation device 40 or a solar power generation device 42. Note that the power supply device 38 is not limited to a power generation device that uses renewable energy, and may be a system power source, or a power storage device that stores electric power from a renewable energy power generation device or a system power source. Alternatively, two or more of these may be combined.

[0049] When the electrolyte membrane 12 has proton conductivity, the reaction that occurs in the organic hydride production apparatus 2 is as follows. In the following reaction, toluene (TL) is shown as an example of the substance to be hydrogenated. When toluene is used as the substance to be hydrogenated, the organic hydride obtained is methylcyclohexane (MCH). <Electrode reaction at the anode electrode> 3H 2 O → 3 / 2O 2 +6H + +6e - <Electrode reaction at the cathode electrode> TL+6H + +6e - →MCH

[0050] That is, the electrode reaction at the anode electrode 10 and the electrode reaction at the cathode electrode 8 proceed in parallel. At the anode electrode 10, a water oxidation reaction occurs, producing oxygen, protons, and electrons. The produced protons pass through the electrolyte membrane 12 and move to the cathode electrode 8. The electrons are sent to the cathode electrode 8 via the power supply 22. The oxygen is discharged from the anode flow path 20 to the outside of the organic hydride manufacturing apparatus 2. At the cathode electrode 8, the toluene contained in the cathode fluid LC reacts with the protons that have moved from the anode electrode 10 side, electrochemically hydrogenating (reducing) the toluene to produce methylcyclohexane. The produced methylcyclohexane is discharged from the cathode flow path 18 to the outside of the organic hydride manufacturing apparatus 2.

[0051] When the electrolyte membrane 12 has anion conductivity, the reaction that occurs in the organic hydride manufacturing apparatus 2 is as follows. In the following reaction, toluene is used as an example of the substance to be hydrogenated. <Electrode reaction at the cathode electrode> TL + 6H 2 O+6e - →MCH+6OH - <Electrode reaction at the anode electrode> 6OH - →3 / 20 2 +3H 2 O+6e -

[0052] That is, the electrode reaction at the cathode electrode 8 and the electrode reaction at the anode electrode 10 proceed in parallel. At the cathode electrode 8, the toluene contained in the cathode fluid LC reacts with water diffusing from the anode electrode 10, resulting in electrochemical hydrogenation (reduction) of the toluene, producing methylcyclohexane and hydroxide ions. The methylcyclohexane is discharged from the cathode flow path 18 to the outside of the organic hydride manufacturing apparatus 2. The hydroxide ions pass through the electrolyte membrane 12 and move to the anode electrode 10. At the anode electrode 10, an oxidation reaction of the hydroxide ions migrated from the cathode electrode 8 occurs, producing oxygen, water, and electrons. The electrons are supplied to the cathode electrode 8 via the power source 22 and are used in the electrode reaction at the cathode electrode 8. The oxygen and water are discharged from the anode flow path 20 to the outside of the organic hydride manufacturing apparatus 2.

[0053] Therefore, according to the organic hydride manufacturing apparatus 2 of this embodiment, the electrolysis of water and the hydrogenation reaction of the material to be hydrogenated can be carried out in one step. Alternatively, the oxidation reaction of hydroxide ions and the hydrogenation reaction of the material to be hydrogenated can be carried out in one step. This improves the efficiency of organic hydride manufacturing compared to conventional techniques that manufacture organic hydrides using a two-stage process consisting of a process for producing hydrogen by water electrolysis or the like and a process for chemically hydrogenating the material to be hydrogenated in a reactor of a plant or the like. Furthermore, since a reactor for chemical hydrogenation and a high-pressure vessel for storing hydrogen produced by water electrolysis or the like are not required, a significant reduction in facility costs can be achieved.

[0054] In the organic hydride manufacturing apparatus 2 according to the present embodiment, when 200 ppm or more of a substance to be hydrided or an organic hydride is added to the anolyte LA supplied to the anode electrode 10 in predetermined constant-voltage electrolysis, the current decrease rate after 10 hours is 1% or less, or when 200 ppm or more of a substance to be hydrided or an organic hydride is added to the anolyte LA in predetermined constant-current electrolysis, the voltage increase rate after 10 hours is 1% or less.

[0055] By keeping the current decrease rate after 10 hours at 1% or less, it is possible to prevent a significant decrease in current over the lifetime of the organic hydride manufacturing apparatus 2. This makes it possible to maintain the equipment utilization rate of the organic hydride manufacturing system 1 and improve operating costs. Furthermore, by keeping the voltage increase rate after 10 hours at 1% or less, it is possible to suppress an increase in the electricity cost required to operate the organic hydride manufacturing system 1 and improve operating costs.

[0056] Furthermore, in the organic hydride manufacturing apparatus 2 according to the present embodiment, when 200 ppm or more of a material to be hydrided or an organic hydride is added to the anolyte LA supplied to the anode electrode 10 and electrolysis is performed for 50 hours, the Faradaic efficiency of formation of at least one selected from the group consisting of a product in which a hydroxy group is bonded to the material to be hydrided or the organic hydride (hereinafter referred to as oxidation product I as appropriate), a product in which an aldehyde group is bonded to the material to be hydrided or the organic hydride or a part of the material to be hydrided or the organic hydride has been converted to an aldehyde group (hereinafter referred to as oxidation product II as appropriate), and a product in which a carboxy group is bonded to the material to be hydrided or the organic hydride or a part of the material to be hydrided or the organic hydride has been converted to a carboxy group (hereinafter referred to as oxidation product III as appropriate).

[0057] This makes it possible to reduce the cost of removing the oxidation products I to III from the anolyte LA, thereby improving the operating cost of the organic hydride production system 1.

[0058] Furthermore, the organic hydride manufacturing apparatus 2 according to this embodiment allows the reaction to proceed at each electrode at a pressure of 1 atmosphere or more and 3 atmospheres or less and a temperature of 20° C. or more and 70° C. or less. The reaction temperature is more preferably 20° C. or more and 60° C. or less. The potential of the anode electrode 10 is preferably 0 to 2.07 V vs. RHE.

[0059] The embodiments may be specified by the following items: [Item 1] An organic hydride manufacturing apparatus (2) comprising: an anode electrode (10) having a high-entropy alloy containing a base metal element as an anode catalyst (11); a cathode electrode (8); and an electrolyte membrane (12) located between the anode electrode (10) and the cathode electrode (8), wherein the anode electrode (10) oxidizes water or hydroxide ions, and the cathode electrode (8) electrochemically reduces a substance to be hydrided to produce an organic hydride. [Item 2] The organic hydride manufacturing apparatus (2) according to Item 1, wherein the high-entropy alloy contains at least one element selected from the group consisting of Mn, Fe, Co, Ni, Cr, Ti, Zr, Nb, Mo, and Cu. [Item 3] The organic hydride manufacturing apparatus (2) according to Item 2, wherein the high-entropy alloy contains at least one element selected from the group consisting of Mn, Fe, Co, and Ni, and at least one element selected from the group consisting of Cr, Ti, Zr, Nb, Mo, and Cu. [Item 4] The organic hydride manufacturing apparatus (2) according to any one of Items 1 to 3, wherein all constituent elements of the high-entropy alloy are base metal elements. [Item 5] The organic hydride manufacturing apparatus (2) according to any one of Items 1 to 4, wherein, when 200 ppm or more of a substance to be hydrided or an organic hydride is added to the anolyte (LA) supplied to the anode electrode (10) in predetermined constant-voltage electrolysis, the rate of decrease in current after 10 hours is 1% or less, or, when 200 ppm or more of a substance to be hydrided or an organic hydride is added to the anolyte (LA) in predetermined constant-current electrolysis, the rate of increase in voltage after 10 hours is 1% or less.[Item 6] The organic hydride manufacturing apparatus (2) according to any one of Items 1 to 5, wherein, when 200 ppm or more of a material to be hydrided or an organic hydride is added to the anolyte (LA) supplied to the anode electrode (10) and electrolysis is performed for 50 hours, the Faraday efficiency of formation of at least one selected from the group consisting of a product in which a hydroxy group is bonded to the material to be hydrided or the organic hydride, a product in which an aldehyde group is bonded to the material to be hydrided or the organic hydride or a part of the material to be hydrided or the organic hydride has been converted to an aldehyde group, and a product in which a carboxy group is bonded to the material to be hydrided or the organic hydride or a part of the material to be hydrided or the organic hydride has been converted to a carboxy group is 0.1% or less. [Item 7] The organic hydride manufacturing apparatus (2) according to any one of Items 1 to 6, wherein the anode catalyst (11) has a dissolution rate of elements contained in the high-entropy alloy of 60 μg / h or less per 1 g of the anode catalyst (11) when a rated current or a rated voltage is applied, or has a dissolution rate of elements contained in the high-entropy alloy of 60 μg / h or less per 1 g of the anode catalyst (11) when immersed in an acidic solution with a pH of 4.0 or less. [Item 8] The organic hydride manufacturing apparatus (2) according to any one of Items 1 to 7, wherein a reaction is allowed to proceed at each electrode (8, 10) at a pressure of 1 atmosphere or more and 3 atmospheres or less and at a temperature of 20°C or more and 70°C or less. [Item 9] A method for producing an organic hydride using an organic hydride production apparatus (2) including an anode electrode (10) having a high-entropy alloy containing a base metal element as an anode catalyst (11), a cathode electrode (8), and an electrolyte membrane (12) located between the anode electrode (10) and the cathode electrode (8), the method comprising: oxidizing water or hydroxide ions at the anode electrode (10); and electrochemically reducing a substance to be hydrided at the cathode electrode (8) to produce an organic hydride. [Item 10] The method for producing an organic hydride according to item 9, further comprising subjecting the anode catalyst (11) to a prior aging treatment, the aging treatment comprising at least one of electrolysis of an electrolyte using the anode catalyst (11) and immersion of the anode catalyst (11) in an acidic solution having a pH of 4.0 or less.

[0060] Examples of the present invention will be described below, but these examples are merely illustrative examples for suitably explaining the present invention and do not limit the present invention in any way.

[0061] [Fabrication of Anode Electrode] (Example 1) Ingots of Mn, Fe, Co, Ni, Cr, Ti, Zr, Nb, and Mo were charged into an arc melting furnace. The amount of each ingot charged was adjusted so that the composition ratio of each metal in the high-entropy alloy was 11.1 atm%. Then, arc melting was performed in a pure Ar atmosphere. In the arc melting process, the base material was completely melted, and then the ingot was rotated and remelted. This operation was repeated six or more times to uniformly mix the metals. The resulting ingot of high-entropy alloy (9eHEA) was formed into a sheet with a predetermined area to obtain the anode electrode of Example 1.

[0062] Example 2 An anode electrode according to Example 2 made of a high-entropy alloy (10eHEA) was fabricated in the same manner as in Example 1, except that Cu was added to the nine metals used in Example 1 to use 10 metals. The amount of each ingot added was adjusted so that the composition ratio of each metal in the high-entropy alloy was 10 atm %.

[0063] (Comparative Example 1) IrO was deposited on a Ti film by cyclic voltammetry according to the paper by Zhao et al., Electrochimica Acta 391, 2021. X was deposited to prepare an anode electrode according to Comparative Example 1.

[0064] [Fabrication of Organic Hydride Production Apparatus] An H-shaped cell was prepared, which was divided into two spaces by a proton exchange membrane, Nafion 117, fixed in the center. The anode electrode of Example 1, Example 2, or Comparative Example 1 was inserted as a working electrode into one space of the H-shaped cell. A reference electrode and a stirrer were also inserted into this space. A Pt mesh was inserted as a counter electrode into the other space of the H-shaped cell. Then, 15 mL of a 0.5 mol / L aqueous sulfuric acid solution was poured into each space, and an organic hydride production apparatus (hereinafter referred to as a cell, as appropriate) according to each Example and Comparative Example was fabricated.

[0065] [Toluene Poisoning Test] A 1 / 4-inch PTFE tube was inserted into the working electrode side of each cell. The PTFE tube was inserted until its tip reached near the center of the aqueous solution in the cell. While stirring the aqueous solution on the working electrode side, constant-potential electrolysis was performed at a potential such that the potential of the working electrode was 2.0 V vs. RHE. In addition, the current in each cell was measured, and the current density was calculated. After the current stabilized, a sufficient amount of toluene was dripped from the top of the tube while continuing electrolysis. This formed a two-layer structure of sulfuric acid aqueous solution and toluene within the tube. As a result, toluene was saturated in the sulfuric acid aqueous solution, and a state was achieved in which undissolved toluene did not adhere to the surface of the working electrode. Constant-potential electrolysis was continued in this state.

[0066] FIG. 2 shows the current density of each cell in the toluene poisoning test. As shown in FIG. 2, in Comparative Example 1, a rapid decrease in current density was observed after the addition of toluene. On the other hand, in Examples 1 and 2, the decrease in current density was gradual even after the addition of toluene. This confirmed that high-entropy alloys have higher durability against substances to be hydrided than Ir. Therefore, it was demonstrated that the durability of the anode catalyst is improved by using a high-entropy alloy as the anode catalyst.

[0067] After the test, the sulfuric acid aqueous solution on the working electrode side in each example and comparative example was collected. Then, each sulfuric acid aqueous solution was mixed with ether, and the by-products in each sulfuric acid aqueous solution were extracted into ether. This ether was measured using a gas chromatograph mass spectrometer (GC / MS: JMS-T100 GCV, manufactured by JEOL) to analyze the components of the by-products. Furthermore, component analysis of the by-products was also performed when constant-potential electrolysis was performed at a potential of 1.6 V vs. RHE at the working electrode and when constant-potential electrolysis was performed at a potential of 1.8 V vs. RHE at the working electrode. The results are shown in Figure 3.

[0068] Figure 3 shows by-products generated by constant-potential electrolysis. As shown in Figure 3, in Comparative Example 1, benzaldehyde, benzyl alcohol, and benzoic acid, which are oxidation products of toluene, were detected at a potential of 2.0 V vs. RHE. Also, benzaldehyde and benzyl alcohol were detected at potentials of 1.6 V vs. RHE and 1.8 V vs. RHE. On the other hand, in Example 1, only benzaldehyde was detected at both potentials. Also, in Example 2, benzaldehyde and benzoic acid were detected at a potential of 2.0 V vs. RHE, and benzaldehyde was detected at a potential of 1.8 V vs. RHE. No oxidation products of toluene were detected at a potential of 1.6 V vs. RHE.

[0069] Benzaldehyde corresponds to part of the product to be hydrogenated, i.e., the product in which the methyl group of toluene is converted to an aldehyde group. Benzyl alcohol corresponds to the product in which a hydroxy group is bonded to toluene, which is also the product to be hydrogenated. Benzoic acid corresponds to part of the product to be hydrogenated, i.e., the product in which the methyl group of toluene is converted to a carboxy group.

[0070] After the test, the working electrodes of Example 1 and Comparative Example 1 were removed and subjected to FT-IR analysis using a Fourier transform infrared spectrophotometer (FT-IR: IRTracer-100, manufactured by Shimadzu Corporation). The removed working electrodes were then immersed in ethanol for 5 days to clean them. Subsequently, each of the cleaned working electrodes was vacuum dried for 24 hours. After that, FT-IR analysis was performed on each of the cleaned working electrodes using the FT-IR. The results are shown in Figures 4(A) and 4(B).

[0071] 4(A) is a diagram showing the results of FT-IR analysis of the working electrode of Example 1 after the toluene poisoning test. FIG. 4(B) is a diagram showing the results of FT-IR analysis of the working electrode of Comparative Example 1 after the toluene poisoning test. In FIGS. 4(A) and 4(B), the results before cleaning are shown by a solid line, and the results after cleaning are shown by a dashed line. As shown in FIG. 4(B), in Comparative Example 1, peaks derived from toluene polymers and polymerization products of oxidation products, i.e., CH 2 and CH 3A peak due to the high entropy alloy was observed. On the other hand, as shown in Figure 4(A), in Example 1, this peak was not observed either before or after cleaning. This confirmed that the surface of the anode electrode containing a high entropy alloy is less susceptible to polymerization of the substances to be hydrided and their oxidation products, and is therefore less susceptible to poisoning by the substances to be hydrided, etc. This demonstrates that the durability of the anode catalyst is improved by using a high entropy alloy as the anode catalyst.

[0072] [Toluene Oxidation Product Poisoning Test] Using the cell of Example 1 described above, constant-potential electrolysis was performed at a potential where the working electrode potential was 2.0 V vs. RHE. Furthermore, using the cell of Comparative Example 1 described above, constant-potential electrolysis was performed at a potential where the working electrode potential was 1.6 V vs. RHE. Furthermore, the current in each cell was measured, and the current density was calculated. After constant-potential electrolysis was performed for 2 hours while stirring the aqueous solution on the working electrode side, 0.2 mmol of benzyl alcohol, benzaldehyde, or benzoic acid was added to the aqueous solution on the working electrode side of each cell while continuing electrolysis.

[0073] FIG. 5(A) shows the current density of the cell of Example 1 in a toluene oxidation product poisoning test. FIG. 5(B) shows the current density of the cell of Comparative Example 1 in a toluene oxidation product poisoning test. As shown in FIG. 5(B), in Comparative Example 1, a significant decrease in current density was observed after the addition of all of benzyl alcohol, benzaldehyde, and benzoic acid. In particular, the current density decreased rapidly immediately after the addition of benzyl alcohol and benzoic acid. On the other hand, as shown in FIG. 5(A), in Example 1, the decrease in current density was more gradual for all of benzyl alcohol, benzaldehyde, and benzoic acid compared to Comparative Example 1. In particular, the current density was maintained more remarkably for benzyl alcohol and benzaldehyde than for benzoic acid.

[0074] This confirmed that high-entropy alloys have higher durability against oxidation products of the substance to be hydrided than Ir. Therefore, it was demonstrated that the durability of the anode catalyst is improved by using a high-entropy alloy as the anode catalyst. Furthermore, since benzoic acid was not produced in Example 1 (see FIG. 3 ), it was demonstrated that the anode electrode of Example 1 has even higher durability than the anode electrode of Example 2. Furthermore, since benzoic acid was not produced at potentials of 1.8 V vs. RHE or less in Examples 1 and 2 (see FIG. 3 ), it was demonstrated that it is preferable to perform constant-potential electrolysis at a potential at which the anode electrode potential is 1.8 V vs. RHE or less.

[0075] After the test, the working electrode of each cell was removed and immersed in ethanol for five days to clean it. The cleaned working electrodes were then vacuum dried for 24 hours. FT-IR analysis was then performed on each cleaned working electrode using an FT-IR spectrometer. The results are shown in Figures 6(A) and 6(B). For reference, Figures 6(A) and 6(B) also include the FT-IR analysis results shown in Figures 4(A) and 4(B).

[0076] 6(A) is a diagram showing the results of FT-IR analysis of the working electrode of Example 1 after a toluene oxidation product poisoning test. FIG. 6(B) is a diagram showing the results of FT-IR analysis of the working electrode of Comparative Example 1 after a toluene oxidation product poisoning test. As shown in FIG. 6(B), when benzyl alcohol and benzoic acid were added in Comparative Example 1, a peak derived from a polymer of oxidation products, i.e., CH 2 and CH 3 A peak due to the oxidation product was observed. On the other hand, as shown in Figure 6(A), no such peak was observed in Example 1 when any of the oxidation products was added. This confirmed that the oxidation products of the substance to be hydrided are unlikely to polymerize on the surface of the anode electrode containing a high-entropy alloy, and therefore the surface is unlikely to be poisoned by the substance to be hydrided, etc. This demonstrates that the durability of the anode catalyst is improved by using a high-entropy alloy as the anode catalyst.

[0077] The present invention can be used in an organic hydride manufacturing apparatus and an organic hydride manufacturing method.

[0078] 2 organic hydride production apparatus, 8 cathode electrode, 9 cathode catalyst, 10 anode electrode, 11 anode catalyst, 12 electrolyte membrane

Claims

1. An organic hydride manufacturing apparatus comprising: an anode electrode having a high-entropy alloy containing a base metal element as an anode catalyst; a cathode electrode; and an electrolyte membrane located between the anode electrode and the cathode electrode, wherein the anode electrode oxidizes water or hydroxide ions, and the cathode electrode electrochemically reduces a substance to be hydrided to produce an organic hydride.

2. The organic hydride manufacturing apparatus according to claim 1, wherein the high entropy alloy contains at least one element selected from the group consisting of Mn, Fe, Co, Ni, Cr, Ti, Zr, Nb, Mo and Cu.

3. The organic hydride manufacturing apparatus according to claim 2, wherein the high entropy alloy contains at least one element selected from the group consisting of Mn, Fe, Co, and Ni, and at least one element selected from the group consisting of Cr, Ti, Zr, Nb, Mo, and Cu.

4. The organic hydride manufacturing apparatus according to claim 1, wherein all of the constituent elements of the high entropy alloy are base metal elements.

5. An organic hydride manufacturing apparatus as claimed in any one of claims 1 to 4, wherein when 200 ppm or more of a substance to be hydrided or an organic hydride is added to the anolyte supplied to the anode electrode in a prescribed constant voltage electrolysis, the current drop rate after 10 hours is 1% or less, or when 200 ppm or more of a substance to be hydrided or an organic hydride is added to the anolyte in a prescribed constant current electrolysis, the voltage rise rate after 10 hours is 1% or less.

6. An organic hydride manufacturing apparatus according to any one of claims 1 to 4, wherein, when 200 ppm or more of a material to be hydrogenated or an organic hydride is added to the anolyte supplied to the anode electrode and electrolysis is performed for 50 hours, the Faraday efficiency of formation of at least one selected from the group consisting of a product in which a hydroxyl group is bonded to the material to be hydrogenated or the organic hydride, a product in which an aldehyde group is bonded to the material to be hydrogenated or the organic hydride or a part of the material to be hydrogenated or the organic hydride has been converted to an aldehyde group, and a product in which a carboxyl group is bonded to the material to be hydrogenated or the organic hydride or a part of the material to be hydrogenated or the organic hydride has been converted to a carboxyl group is 0.1% or less.

7. An organic hydride manufacturing apparatus as described in any one of claims 1 to 4, wherein the anode catalyst has a dissolution rate of elements contained in the high entropy alloy of 60 μg / h or less per 1 gram of the anode catalyst when a rated current or a rated voltage is applied, or the dissolution rate of elements contained in the high entropy alloy when immersed in an acidic solution of pH 4.0 or less is 60 μg / h or less per 1 gram of the anode catalyst.

8. An organic hydride manufacturing apparatus according to any one of claims 1 to 4, wherein the reaction at each electrode is carried out at a pressure of 1 to 3 atmospheres and a temperature of 20°C to 70°C.

9. A method for producing an organic hydride using an organic hydride production apparatus comprising an anode electrode having a high-entropy alloy containing a base metal element as an anode catalyst, a cathode electrode, and an electrolyte membrane located between the anode electrode and the cathode electrode, the method comprising: oxidizing water or hydroxide ions at the anode electrode; and electrochemically reducing a substance to be hydrided at the cathode electrode to produce an organic hydride.

10. The method for producing an organic hydride according to claim 9, further comprising subjecting the anode catalyst to a prior aging treatment, the aging treatment including at least one of electrolysis of an electrolyte using the anode catalyst and immersion of the anode catalyst in an acidic solution having a pH of 4.0 or less.

Citation Information

Patent Citations

  • High-entropy amorphous anode oxygen evolution electrode material and preparation method thereof

    CN113862722A

  • Low-temperature synthesis supported high-entropy alloy catalyst as well as preparation method and application thereof

    CN115672340A

  • Organic hydride production device

    WO2018216356A1

  • Method for controlling organic hydride generation system, and organic hydride generation system

    WO2021054445A1

  • Electrode, method for producing same, water electrolyzer, and fuel cell

    WO2022080142A1