Film deposition method, sputtering device, and rotary target

The sputtering apparatus with a rotary target system addresses the challenge of depositing highly crystalline semiconductor films on large substrates by controlling film thickness and composition, enabling efficient production of advanced semiconductor devices on amorphous substrates.

WO2024219132A1PCT designated stage expired Publication Date: 2024-10-24JAPAN DISPLAY INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010481
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-03-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current sputtering methods face challenges in efficiently depositing highly crystalline semiconductor films on large substrates, limiting the production of advanced semiconductor devices like light emitting diodes and transistors.

Method used

A sputtering apparatus with a rotary target system, where multiple rotary targets with different radii and compositions are arranged parallel to each other, allowing for precise control of film thickness and composition by adjusting the substrate movement and plasma distribution, enabling the deposition of films with varying thicknesses and compositions.

Benefits of technology

This approach allows for the precise formation of films with a wide range of thicknesses, from ultra-thin to thick, facilitating the production of high-quality semiconductor devices without the need for high-temperature processes, suitable for large amorphous substrates like glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010481_24102024_PF_FP_ABST
    Figure JP2024010481_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This film deposition method includes subjecting a plurality of rotary targets, arranged so that the rotation axes are parallel with each other, to sputtering while moving a substrate in a direction perpendicular to the rotation axes. All of the plurality of rotary targets are disposed on one side of the substrate. The plurality of rotary targets comprise a first rotary target and a second rotary target that has a smaller radius than the first rotary target. The plurality of rotary targets may be arranged so that a maximum distance between two selected from among the plurality of rotary targets is longer than the length in the longitudinal direction of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Film formation method, sputtering apparatus, and rotary target

[0001] One embodiment of the present invention relates to a film formation method using a sputtering method, or to a sputtering apparatus and a rotary target for implementing the film formation method.

[0002] Transistors, capacitors, and other components of semiconductor devices are constructed by laminating multiple appropriately patterned thin films of conductors, insulators, and semiconductors. One of the most common methods for fabricating these thin films is sputtering. In recent years, it has been discovered that highly crystalline thin films can be fabricated by sputtering nitrides of Group 13 elements, such as gallium nitride (GaN) and indium nitride (InN), which are expected to be wide-gap semiconductors (see, for example, Patent Documents 1 to 5).

[0003] International Publication No. 2020 / 075599 Japanese Patent Application Laid-Open No. 2008-270749 Japanese Patent Application Laid-Open No. 2019-147976 International Publication No. 2022 / 070922 Japanese Patent Application Laid-Open No. 2017-179529

[0004] An object of one embodiment of the present invention is to provide a novel film formation method using a sputtering method, and to provide a sputtering apparatus and a rotary target for realizing this film formation method. Alternatively, an object of one embodiment of the present invention is to provide a method for efficiently depositing a highly crystalline semiconductor film on a large substrate by a sputtering method, and to provide a sputtering apparatus and a rotary target for realizing this method.

[0005] One embodiment of the present invention is a film deposition method. The film deposition method includes sputtering a substrate while moving the substrate in a direction perpendicular to a rotation axis of a plurality of rotary targets arranged so that the rotation axes are parallel to each other. The plurality of rotary targets are all arranged on one side of the substrate. The plurality of rotary targets includes a first rotary target and a second rotary target having a radius smaller than that of the first rotary target.

[0006] One embodiment of the present invention is a sputtering apparatus. The sputtering apparatus includes a chamber, a substrate stage disposed within the chamber, multiple target holders, and a movement mechanism. The multiple target holders each hold a rotary target, are all disposed on one side of the substrate stage, and are arranged so that the rotation axes of the rotary targets are parallel to each other. The multiple target holders include a first target holder and a second target holder. The movement mechanism is configured to move the substrate stage in a direction perpendicular to the rotation axis. The radius of the rotary target held by the second target holder is smaller than the radius of the rotary target held by the first target holder.

[0007] One embodiment of the present invention is a rotary target. The rotary target includes a backing tube and a coating material covering the backing tube. The coating material has n 1 / n tube sections arranged to surround the backing tube. The 1 / n tube sections include different materials, where n is a natural number of 2 or greater.

[0008] 1 is a schematic diagram of a sputtering apparatus according to one embodiment of the present invention; 2 is a schematic side view of a portion of a sputtering apparatus according to one embodiment of the present invention; 3 is a schematic end view of a portion of a sputtering apparatus according to one embodiment of the present invention; 4 is a schematic end view of a rotary target according to one embodiment of the present invention; 5 is a schematic end view of a rotary target according to one embodiment of the present invention; 6 is a schematic end view of a rotary target according to one embodiment of the present invention; 7 is a schematic end view of a rotary target according to one embodiment of the present invention; 8 is a schematic end view of a substrate and a rotary target in a sputtering apparatus according to one embodiment of the present invention; 9 is a schematic top view of a substrate and a rotary target in a sputtering apparatus according to one embodiment of the present invention; 10 is a schematic end view of a substrate and a rotary target in a sputtering apparatus according to one embodiment of the present invention; 11 is a schematic top view of a substrate and a rotary target in a sputtering apparatus according to one embodiment of the present invention; 12 is a schematic end view of a laminate formed by a film formation method according to one embodiment of the present invention; 13 is a schematic end view illustrating a film formation method according to one embodiment of the present invention; 1 is a schematic end view illustrating a film formation method according to one embodiment of the present invention. 2 is a schematic view illustrating a film formation method according to one embodiment of the present invention. 3 is a schematic view illustrating a film formation method according to one embodiment of the present invention. 4 is a schematic view illustrating a film formation method according to one embodiment of the present invention. 5 is a schematic end view of a light-emitting element manufactured using a sputtering apparatus according to one embodiment of the present invention. 6 is a schematic end view of a transistor manufactured using a sputtering apparatus according to one embodiment of the present invention. 7 is a schematic end view of a transistor manufactured using a sputtering apparatus according to one embodiment of the present invention.

[0009] Hereinafter, various embodiments of the present invention will be described with reference to the drawings, etc. However, the present invention can be embodied in various forms without departing from the spirit of the present invention, and should not be construed as being limited to the description of the embodiments exemplified below.

[0010] In order to clarify the description, the drawings may show the width, thickness, shape, etc. of each part schematically compared to the actual embodiment, but these are merely examples and do not limit the interpretation of the present invention. In this specification and each drawing, elements having the same function as those described in the previous drawings may be given the same reference numerals, and duplicated explanations may be omitted. This reference numeral is used to collectively represent multiple identical or similar structures, and when these are individually represented, a hyphen and a natural number are added after the reference numeral.

[0011] In this specification and claims, when expressing an aspect of placing another structure on top of a certain structure, the term "on top" is used, unless otherwise specified, to include both a case in which another structure is placed directly on top of a certain structure so as to be in contact with the certain structure, and a case in which another structure is placed above a certain structure via yet another structure.

[0012] In this specification and claims, the expression "a structure exposed from another structure" means a state in which a part of a structure is not covered by another structure, and includes a state in which the part not covered by another structure is covered by yet another structure. The state expressed by this expression also includes a state in which a structure is not in contact with another structure.

[0013] The sputtering apparatus, rotary target, and film formation method using the sputtering apparatus and rotary target according to this embodiment will be described below.

[0014] 1. Sputtering Apparatus (1) Overall Configuration Figure 1 shows a schematic diagram including an end face of a sputtering apparatus 100 according to this embodiment. The sputtering apparatus 100 is a film formation apparatus that functions to form a thin or ultra-thin conductive film, semiconductor film, or insulating film on a substrate 150 by sputtering. The sputtering apparatus 100 has a chamber 102, which provides a field for collision of high-speed ions with a sputtering target and deposition of the target atoms generated during the collision. The chamber 102 is provided with one or more load lock doors 104, and the substrate 150 is introduced into the chamber 102 and removed from the chamber 102 via the load lock door 104.

[0015] The substrate 150 that can be used in the sputtering apparatus 100 is not limited, and the substrate 150 may be a single-crystal substrate or an amorphous substrate. For example, a silicon substrate, a sapphire substrate, a quartz substrate, a glass substrate, or a plastic substrate can be used as the substrate 150. For example, a large rectangular amorphous glass substrate, also known as mother glass, can also be used as the substrate 150. Specifically, a glass substrate called eighth-generation mother glass having a size of 2160 mm x 2460 mm, a glass substrate called ninth-generation mother glass having a size of 2400 mm x 2800 mm, a glass substrate called tenth-generation mother glass having a size of 2880 mm x 3130 mm, or even larger glass substrates may be used. Examples of materials that can be used in plastic substrates include polymers such as polyimide, polyamide, and polycarbonate. The substrate 150 may be flexible.

[0016] A plurality of target holders 120 are provided in the upper part of the chamber 102, each for holding a rotary target 130. The target holders 120 are arranged so that the rotation axes of the rotary targets 130 are parallel to one another. There is no restriction on the number of target holders 120, and the number may be, for example, between two and ten. A substrate stage 108 for placing a substrate 150 on which a thin film is to be formed, and a movement mechanism 106 for moving the substrate stage 108 are provided in the lower part of the chamber 102. The movement mechanism 106 is configured to move the substrate stage 108 in a direction perpendicular to the rotation axis of the target holder 120 and reversibly along this direction. This allows the substrate 150 placed on the substrate stage 108 to be moved relative to the plurality of rotary targets 130. There are no restrictions on the configuration of the movement mechanism 106, and the movement mechanism 106 may be, for example, a combination of one or more rails and wheels mounted on the rails, or a combination of a rack and pinion gear, a combination of a belt and multiple pulleys, or a combination of a chain and gears. For convenience, the direction in which the substrate 150 is moved by the moving mechanism 106 will be referred to as the x-direction, the vertical direction as the z-direction, and the direction perpendicular to the x-direction and z-direction as the y-direction (i.e., the direction in which the rotation axis of the rotary target extends).

[0017] Although not shown, the chamber 102 is connected to an exhaust system for reducing the pressure inside the chamber 102, one or more gas inlet pipes for introducing sputtering gases such as argon, nitrogen, oxygen, and hydrogen into the chamber 102, and the like. The sputtering apparatus 100 is also provided with a plasma generation power supply connected to the substrate stage 108 and the rotary target 130. This plasma generation power supply may be a high-frequency power supply, a DC power supply, or a pulse power supply. The sputtering apparatus 100 may also be provided with an electrostatic chuck for fixing the substrate 150 on the substrate stage 108, a power supply for the electrostatic chuck, a heater power supply for heating the substrate stage 108, a controller for controlling the temperature of the cooling medium circulated within the substrate stage 108, and the like.

[0018] 1, multiple target holders 120 are arranged above the substrate stage 108, but the configuration of the sputtering apparatus 100 is not limited to this. For example, the substrate stage 108 may be arranged above the multiple target holders 120, or the substrate stage 108 may be set so that the normal to the substrate 150 is horizontal, and multiple target holders 120 may be arranged above and below it. In either configuration, all of the multiple target holders 120 are arranged on one side of the substrate stage 108 and the substrate 150.

[0019] (2) Target Holder Schematic side and end views of the rotary target 130 and the target holder 120 are shown in Figures 2A and 2B, respectively. As can be seen from these figures, the target holder 120 includes a control unit 124 that rotates the rotary target 130 around its rotation axis and connects the rotary target 130 to a plasma generation power supply to control the potential supplied to the rotary target 130, and a bearing 122. The rotary target 130 is attached and held between the control unit 124 and the bearing 122. As an optional configuration, the sputtering apparatus 100 may include an adhesion shield 126 to prevent contamination by material sputtered from the coating material 134 in an unintended direction.

[0020] (3) Rotary Target The rotary target 130 basically comprises a tubular backing tube 132 and a coating material 134 covering the backing tube 132. Although not shown, the rotary target 130 may optionally include a binder between the backing tube 132 and the coating material 134 to reinforce the bond therebetween. There are no restrictions on the length (length in the direction of the rotation axis) of the rotary target 130, but it is preferably longer than one side or the shortest diameter of the substrate 150 or the substrate stage 108. When a rectangular glass substrate is used as the substrate 150, it is preferable that the length of the rotary target 130 be longer than the short side of the substrate 150 or the substrate stage 108. This allows a film of the material contained in the coating material 134 to be formed over the entire surface of the substrate 150, as described below.

[0021] The backing tube 132 is electrically conductive and is connected to a plasma generation power supply via the control unit 124 to receive a voltage. A magnet 128, such as a permanent magnet, connected to the control unit 124 is disposed inside the backing tube 132. The control unit 124 applies a voltage to the backing tube 132, and a rotation mechanism (not shown) included in the control unit 124 rotates the backing tube 132, thereby rotating the coating material 134. However, the magnet 128 is independent of the rotation of the backing tube 132 and is positioned closer to the substrate stage 108 than the rotation axis while the backing tube 132 is rotating. This allows plasma generated by the plasma generation power supply to be constantly distributed on the substrate stage 108 side of the coating material 134, and the portion of the coating material 134 exposed to the plasma is sputtered. The direction of travel (scattering angle) of the material ejected by sputtering can be adjusted as desired by adjusting the magnetic force of the magnet 128 to control the region where plasma is generated.

[0022] The coating material 134 includes a material that constitutes the film formed on the substrate 150. Ions of the sputtering gas collide with the coating material 134 at high speed, expelling the material contained in the coating material 134, and the material is deposited on the substrate 150 to form a film. There are no limitations on the material contained in the coating material 134, and examples include metals (zero-valent metals) such as aluminum, cobalt, chromium, molybdenum, niobium, titanium, tungsten, zinc, silver, gold, iron, and iridium, or alloys thereof; oxides such as aluminum oxide, copper oxide, chromium oxide, cesium oxide, magnesium oxide, titanium oxide, tungsten oxide, and strontium titanate; nitrides such as aluminum nitride, chromium nitride, and silicon nitride; non-metallic elements such as silicon, boron, carbon, and germanium; and compound semiconductors. The oxide may be a conductive oxide that transmits visible light, such as indium-tin mixed oxide (ITO) or indium-zinc mixed oxide (IZO). Examples of compound semiconductors include gallium nitride-based compound semiconductors such as gallium nitride, aluminum gallium nitride, and indium gallium nitride, as well as gallium phosphide-based compound semiconductors such as gallium phosphide, aluminum indium gallium phosphide, and indium gallium arsenide phosphide, indium-based compound semiconductors such as indium phosphide, silicon carbide, etc. The coating material 134 may contain dopants such as silicon, germanium, magnesium, zinc, cadmium, and beryllium.

[0023] In each rotary target 130, the coating material 134 may contain one or more types of material. That is, the coating material 134 may have multiple regions with different compositions. For example, as shown in FIG. 3A , the coating material 134 of a rotary target 130 according to one embodiment of the present invention may have two half-tube sections (a first half-tube section 134-1 and a second half-tube section 134-2) facing each other with the backing tube 132 sandwiched therebetween. The first half-tube section 134-1 and the second half-tube section 134-2 contain materials with different compositions. For example, if the coating material 134 contains a gallium nitride-based compound semiconductor, the first half-tube section 134-1 and the second half-tube section 134-2 may each contain a gallium nitride-based compound semiconductor with a different composition (e.g., gallium nitride and indium gallium nitride). In this way, when the coating material 134 has multiple regions with different compositions, the magnet 128 can be used to unevenly distribute the plasma between the rotary target 130 and the substrate 150, so that the first half-tube portion 134-1 and the second half-tube portion 134-2 can be alternately exposed to the plasma as the rotary target 130 rotates (FIG. 3B). As a result, materials with different compositions can be alternately scattered from the single rotary target 130, making it possible to produce an alternating laminate of films with different compositions.

[0024] The number of regions with different compositions included in the coating material 134 is not limited to two and may be three or more. For example, as shown in FIG. 4 , the coating material 134 may have three 1 / 3 tube sections 134-3 to 136-5 arranged to surround the backing tube 132 and having different compositions. Generally speaking, the coating material 134 of the rotary target 130 according to one embodiment of the present invention may have n 1 / n tube sections arranged to surround the backing tube 132 and having different compositions, and first to nth films with different compositions can be formed in sequence and repeatedly by rotating the rotary target 130. Here, n is a natural number greater than or equal to two.

[0025] (4) Arrangement of Rotary Target and Substrate The arrangement relationship between the rotary target 130 and the substrate 150 will be explained using the schematic end view and top view shown in Figures 5A and 5B, respectively. As described above, the multiple rotary targets 130 are all longer than the short side of the substrate 150 and are arranged on one side of the substrate 150 or the substrate stage 108 so that their rotation axes are parallel to each other. In addition, the multiple rotary targets 130 are arranged so that the maximum distance between any two selected from these targets (distance D in Figure 5B) is 1 ) is greater than the longitudinal length L of the substrate 150. By employing such an arrangement and sputtering the coating material 134 while moving the substrate 150 in the x direction, it is possible to deposit material over the entire surface of the substrate 150. Furthermore, by appropriately selecting the materials contained in the coating materials 134 of the multiple rotary targets 130, it is possible to deposit multiple layers containing different materials.

[0026] 6A and 6B, the radii of the rotary targets 130 (or the outer diameter of the coating material 134; the same applies hereinafter) do not necessarily have to be the same, and the radius of at least one rotary target 130 may be different from the radii of the other rotary targets 130. In the example shown in FIGS. 6A and 6B, a rotary target 130-3 having the largest radius, a rotary target 130-2 having the smallest radius, and a rotary target 130-1 having a radius larger than the radius of the rotary target 130-2 and smaller than the radius of the rotary target 130-3 are arranged.

[0027] When using multiple rotary targets 130 with different radii, the distance D from the substrate stage 108 or the substrate 150 to the rotation axis of the rotary target 130 is 2 More specifically, the larger the radius of the rotary target 130, the shorter the distance D from the substrate 150 or the substrate stage 108 to the rotation axis. 2 The rotary targets 130 are arranged so that the distance D 2The plurality of rotary targets 130 are arranged so that the number of rotary targets 130 increases in the order of rotary target 130-2, rotary target 130-1, and rotary target 130-3.

[0028] The distance D from the substrate 150 or the substrate stage 108 to the surface of the coating material 134 3 may be substantially the same or different between the rotary targets 130. In the latter case, as shown in FIG. 7, the larger the radius of the rotary target 130, the larger the distance D from the substrate 150 or the substrate stage 108 to the surface of the coating material 134. 3 It is preferable to arrange the multiple rotary targets 130 so that the radius of the target holders 120 is large. In this case, the multiple target holders 120 may also be configured so that the distance from the substrate 150 or the substrate stage 108 varies depending on the radius of the rotary targets 130, or so that the distance from the rotation axis of the rotation mechanism of the control unit 124 to the substrate stage 108 or the substrate 150 varies. As will be described later, by employing such an arrangement, not only a film having a large thickness but also an ultra-thin film whose thickness is precisely controlled can be formed.

[0029] 2. Film Formation Method A method for depositing multiple films on a substrate 150 using the sputtering apparatus 100 will be described below. Here, a stack 152 including films 152-1 to 152-6 shown in FIG. 8A is used as an example. The stack 152 is fabricated by sequentially depositing films 152-1 to 152-6 on the substrate 150. In the stack 152, films 152-2 to 152-5, each having a thickness smaller than that of films 152-1 and 152-6, are stacked between the films 152-1 and 152-6, which contain different materials. Furthermore, the materials contained in films 152-2 to 152-5 are different from the materials contained in films 152-1 and 152-6. The materials contained in films 152-2 and 152-4 are the same, and the materials contained in films 152-3 and 152-5 are also the same. However, the materials contained in films 152-2 and 152-4 are different from the materials contained in films 152-3 and 152-5. That is, the laminate 152 is made up of four different types of materials.

[0030] (1) Film Forming Method 1: When Rotary Targets of Different Radii are Used When rotary targets 130 of different radii are used, as shown in FIG. 8B , rotary targets 130-1 to 130-6 in which the material contained in the films 152-1 to 152-6 is contained in the coating material 134 are arranged in order. Furthermore, rotary targets 130-2 to 130-5 for forming thin films are selected so that their radii are smaller than those of rotary targets 130-1 and 130-6 for forming thick films. Therefore, the distance D from the rotation axis of rotary targets 130-2 to 130-5 to the substrate 150 is 2 is the distance D from the rotation axes of the rotary targets 130-1 and 130-6 to the substrate 150. 2 8B, the rotary targets 130-1 to 130-6 are arranged so that the distance D from the surface of the coating material 134 to the substrate 150 is smaller than 3 is the same among the rotary targets 130-1 to 130-6, but the smaller the radius of the rotary target 130, the greater the distance D 3 The rotary target 130 may be arranged so that

[0031] In this state, the chamber 102 is depressurized, and a potential difference is created between the rotary target 130 and the substrate 150 using the plasma generation power supply while supplying sputtering gas. Furthermore, the substrate stage 108 is moved at a constant speed from the rotary target 130-1 side to the rotary target 130-6 side using the movement mechanism 106. The scattering angle of the material ejected from the rotary target 130 is controlled by the magnet 128. Therefore, as shown by the dotted lines in FIG. 8B , the area (film formation area) where the material ejected from each rotary target 130 is deposited can be limited to a certain range. In other words, the film formation area 154 of each rotary target 130 is limited to a certain width centered on the area overlapping with each rotary target 130, rather than covering the entire substrate 150.

[0032] Furthermore, as described above, the rotation axes of the rotary targets 130-2 to 130-5 for forming the thin films 152-2 to 152-5 are positioned closer to the substrate 150 than the rotation axes of the rotary targets 130-1 and 130-6 for forming the thick films 152-1 and 152-6. Therefore, when the scattering angles of the material ejected from the rotary targets 130-1 to 130-6 are the same, the deposition zones of the rotary targets 130-2 to 130-5 (e.g., deposition zone 154-2 in FIG. 5B ) have a smaller width (length in the x-direction) than the deposition zones 154-1 and 154-6 of the rotary targets 130-1 and 130-6. Because the substrate 150 is moved at a constant speed, the time it takes for the substrate 150 to pass through the deposition zones 154-1 and 154-6 is longer than the time it takes for the substrate 150 to pass through the deposition zone 154-2. As a result, when focusing on a certain point on the substrate 150, a film 152-1 is formed with a large thickness while passing through the film formation region 154-1, and then a film 152-2 is formed with a small thickness while passing through the film formation region 154-2. This point then passes through the film formation regions of the rotary targets 130-3 to 130-5 in order, so that films 152-3 to 152-5 with smaller thicknesses are deposited in order. Finally, this point passes through the film formation region 154-6, which has a relatively large width, so that film 152-6 with a large thickness is deposited. As a result, a stack 152 having multiple films 152-1 to 152-6 with different thicknesses can be produced.

[0033] The thickness of each of the films 152-1 to 152-6 varies depending on the moving speed of the substrate 150 and the distance D from the rotation axis of the rotary target 130 to the substrate 150. 2 , the distance D between the surface of the coating material 134 and the substrate 150 3 , can be controlled by appropriately adjusting the rotation speed of the rotary target 130. For example, the distance D 2 and / or distance D 3 By reducing the distance D, the film formation area is reduced, making it possible to form an extremely thin film. 2 and / or distance D 3Increasing the magnet size increases the deposition area, making it possible to form extremely thick films. Furthermore, the thicknesses of the multiple films 152-1 to 152-6 may be controlled by appropriately adjusting the size of the magnet 128 or the range of magnetic force, thereby controlling the area where plasma is generated and adjusting the deposition area 154. For example, the scattering angle may be reduced by relatively reducing the area where plasma is generated on the surface of the rotary target 130 that produces thin films 152-2 to 152-5. Conversely, the scattering angle may be increased by relatively increasing the area where plasma is generated on the surface of the rotary target 130 that produces thick films 152-1 and 152-6. This allows the time the substrate 150 takes to pass through the deposition area 154 to be appropriately adjusted, thereby controlling the thicknesses of the multiple films 152-1 to 152-6.

[0034] In this method, it is not necessary to simultaneously form the films 152-1 to 152-6. For example, first, while moving the substrate 150 in one direction (forward direction), a potential is supplied from the plasma generation power supply only to the rotary target 130-1, thereby forming the film 152-1 over the entire surface of the substrate 150. Thereafter, while moving the substrate 150 in the reverse direction, or while returning the substrate 150 to the position before film 152-1 was formed and then moving it in the forward direction, a potential is supplied to the rotary targets 130-2 to 130-5, thereby forming the films 152-2 to 152-5. Thereafter, while moving the substrate 150 in the reverse direction, or while returning the substrate 150 to the position before film 152-1 was formed and then moving it in the forward direction, a potential may be supplied to the rotary target 130-6, thereby forming the film 152-6. In this case, it is not necessary to use the same number of rotary targets 130 as the number of films included in the stack 152; for example, one rotary target 130-2 may be used to form films 152-2 and 152-4, and one rotary target 130-3 may be used to form films 152-3 and 152-5, and the substrate 150 may be moved back and forth in the x direction.

[0035] The above-described method can be used to fabricate ultrathin films with thicknesses of, for example, several nanometers or thick films with thicknesses of up to several hundred nanometers, which makes it possible to precisely form, for example, quantum well structures used in electroluminescent devices and extremely thin active layers in thin film transistors.

[0036] (2) Film Formation Method 2: Using Rotary Targets with Multiple Different Compositions A rotary target 130 having coating materials 134 each having multiple different compositions, as described above, may be used as a target for forming a structure in which multiple thin films are repeatedly deposited (here, a stack of films 152-2 to 152-5). For example, as shown in FIG. 8C , a rotary target 130-1 for forming film 152-1, a rotary target 130-7 for forming films 152-2 and 152-3, a rotary target 130-8 for forming films 152-4 and 152-5, and a rotary target 130-6 for forming film 152-6 are arranged in this order. In this case, the radii of the rotary targets 130-7 and 130-8 may be the same as or smaller than the radii of the rotary targets 130-1 and 130-6. Furthermore, the distance D 2 and distance D 3 Regarding the rotary targets 130-7 and 130-8, the rotary targets 130-7 and 130-8 may be smaller than the rotary targets 130-1 and 130-6.

[0037] In this state, the pressure inside the chamber 102 is reduced, and a potential difference is created between the rotary target 130 and the substrate 150 using the plasma generation power supply while supplying sputtering gas. Furthermore, the substrate stage 108 is moved at a constant speed from the rotary target 130-1 side to the rotary target 130-6 side using the movement mechanism 106. This allows films 152-1 to 152-6 to be deposited sequentially on the substrate 150, as in film formation method 1. Furthermore, by appropriately adjusting the rotation speeds of the rotary targets 130-7 and 130-8, the period during which the first half-tube portion 134-1 and the second half-tube portion 134-2 are exposed to plasma can be controlled, thereby adjusting the thicknesses of the films 152-2 to 152-5.

[0038] In this film formation method 2, it is not necessary to supply plasma generation power to all rotary targets 130 at the same time to simultaneously form films 152-1 to 152-6. As in film formation method 1, film 152-1 may be formed over the entire surface of substrate 150, followed by formation of films 152-2 to 152-5, and then formation of film 152-6.

[0039] (3) Film Forming Method 3: When Rotary Targets of the Same Radius are Used The film forming method according to the embodiment of the present invention can also be applied when multiple rotary targets 130 having the same or substantially the same radius are used as targets for providing films 152-1 to 152-6, respectively. In this case, as shown in FIG. 9A, the rotary targets 130-1, 130-9 to 130-12, and 130-6 for providing films 152-1 to 152-6, respectively, are arranged in this order. At this time, the distance D between the substrate 150 and the rotation axis of the rotary targets 130 is 2 may be the same for all rotary targets 130, or may be different for some rotary targets 130. For example, the distance D between the rotation axes of the rotary targets 130-9 to 130-12 and the substrate 150 is 2 The width of the film formation region may be reduced by making the width of the rotary target 130 smaller than that of the rotary target 130-1 or 130-6.

[0040] In this state, the pressure inside the chamber 102 is reduced, and a potential difference is created between the rotary target 130 and the substrate 150 using the plasma generation power supply while supplying sputtering gas. Furthermore, the substrate stage 108 is moved at a constant speed from the rotary target 130-1 side to the rotary target 130-6 side using the movement mechanism 106. This allows films 152-1 to 152-6 to be deposited in order on the substrate 150, similar to film formation methods 1 and 2.

[0041] However, if the distances from the rotation axes of all rotary targets 130 to the substrate 150 are the same or substantially the same, the widths of the film formation regions will be substantially the same, and as a result, the thicknesses of the films 152-1 to 152-6 may be approximately the same. For this reason, in this method, the time for which a potential is supplied from the plasma generation power supply to the rotary targets 130 is controlled. Specifically, a potential is supplied for the longest period to the rotary targets 130-1 and 130-6 for forming the thick films 152-1 and 152-6. For example, when the plasma generation power supply is a DC power supply, a potential is supplied continuously to the rotary targets 130-1 and 130-6, as shown in FIG. 9B . In contrast, a potential is supplied intermittently to the rotary targets 130-9 to 130-12 for forming the thin films 152-2 to 152-5, respectively, and the potential supply time is adjusted to be shorter than that of the rotary targets 130-1 and 130-6. A potential is alternately supplied to the rotary targets 130-9 and 130-11 for forming the films 152-2 and 152-4, and to the rotary targets 130-10 and 130-12 for forming the films 152-3 and 152-5. The time for supplying the potential to the rotary targets 130 may be set appropriately taking into consideration the moving speed of the substrate 150, etc.

[0042] When the plasma generation power supply is a high-frequency power supply, as shown in FIG. 10A, a steady potential is supplied to the rotary targets 130-1 and 130-6 for forming the thick films 152-1 and 152-6 while periodically changing the polarity. In contrast, as shown in FIGS. 10B and 10C, a potential is supplied intermittently to the rotary targets 130-9 to 130-12 for forming the thin films 152-2 to 152-5 while periodically changing the polarity. A potential is also supplied alternately to the pair of rotary targets 130-9 and 130-11 and the pair of rotary targets 130-10 and 130-12. Even in this case, the time for supplying the potential to the rotary target 130 can be appropriately set taking into account the movement speed of the substrate 150, etc. This allows the sputtering time for the multiple rotary targets 130 to be adjusted, thereby controlling the thickness of the multiple films 152-1 to 152-6.

[0043] In this film formation method 3, it is not necessary to form the films 152-1 to 152-6 simultaneously. As in film formation methods 1 and 2, the film 152-1 may be formed over the entire surface of the substrate 150, and then the films 152-2 to 152-5 may be formed, and then the film 152-6 may be formed.

[0044] The above-described film formation methods 1 to 3 can be combined as appropriate. For example, in film formation method 1, rotary targets 130-2 to 130-5 having smaller radii than the rotary targets 130-1 and 130-6 for forming thick films 152-1 and 152-6 may be used to form thin films 152-2 to 152-5, and the coating material 134 of the rotary targets 130-2 to 130-5 may be provided with n 1 / n tube portions having different compositions. Alternatively, the potential supply time may be controlled in film formation method 1. For example, as in film formation method 3, the potential supply time for rotary targets 130-2 to 130-5 for forming thin films may be shorter than that for rotary targets 130-1 and 130-6 for forming thick films. Alternatively, in the film forming method 3, rotary targets 130-9 to 130-12 having a smaller radius than the radius of rotary targets 130-1 and 130-6 for forming thick films 152-1 and 152-6 may be used for forming thin films 152-2 to 152-5.

[0045] Similarly, in film formation method 2, the thicknesses of the films 152-1 to 152-6 may be controlled by adjusting the time for which a potential is supplied from the plasma generation power supply. Specifically, the time for which a potential is supplied to the rotary targets 130-7 and 130-8 is shorter than that for the rotary targets 130-1 and 130-6. For example, a potential is supplied intermittently to the rotary targets 130-7 and 130-8, and a potential is supplied continuously to the rotary targets 130-1 and 130-6. This allows the sputtering time for the multiple rotary targets 130 to be adjusted, thereby controlling the thicknesses of the films 152-1 to 152-6. Furthermore, pulse sputtering is performed on the rotary targets 130-7 and 130-8, thereby improving the crystallinity of the resulting films 152-2 to 152-5.

[0046] As described above, by using the sputtering apparatus 100 and applying the above-described film formation method, films of a wide range of thicknesses can be deposited in any order and with precisely controlled thicknesses. Furthermore, because high temperatures are not necessarily required for film formation by sputtering, a large amorphous substrate (e.g., a glass substrate or a plastic substrate) can be used as the substrate 150 used for film formation. Therefore, by applying the embodiments of the present invention, it becomes possible to supply a variety of semiconductor devices at low cost.

[0047] 3. Applications The sputtering apparatus 100 and the film formation method using the same described above can be applied to the manufacture of various semiconductor devices, such as light-emitting diodes and transistors.

[0048] (1) Light-Emitting Diode FIG. 11 shows a schematic end view of an example of a light-emitting diode 200 manufactured using the sputtering apparatus 100. The light-emitting diode 200 includes a substrate 202 and further includes an n-type cladding layer 220 on the substrate 202 with a buffer layer 210 interposed therebetween. The light-emitting diode 200 further includes a stacked structure including a p-type cladding layer 224 on the n-type cladding layer 220 and a light-emitting layer 222 sandwiched between the n-type cladding layer 220 and the p-type cladding layer 224. The light-emitting diode 200 further includes an anode 226 and a cathode 228 provided on the p-type cladding layer 224 and the n-type cladding layer 220, respectively. The light-emitting diode 200 may further include optional components such as an overcoat 204 between the substrate 202 and the buffer layer 210, an undercoat 206 under the substrate 202, and a protective film 230 on the anode 226 and the cathode 228. By applying a potential difference between the anode 226 and the cathode 228 that is equal to or greater than the light emission threshold voltage, holes and electrons are injected from the anode 226 and the cathode 228, respectively, and the holes and electrons recombine in the light emitting layer 222, resulting in light emission.

[0049] The substrate 202 is a structure that supports each component provided thereon, and may be made of not only quartz, single crystal silicon, or single crystal sapphire, but also amorphous glass such as alkali-free glass.

[0050] The optional overcoat 204 is provided on the substrate 202 so as to contact the substrate 202. The overcoat 204 prevents diffusion of impurities, such as alkali metal ions, contained in the substrate 202. The overcoat 204 may be a single film or a laminate of multiple films containing a silicon-containing inorganic compound, such as silicon oxide or silicon nitride. The undercoat 206 suppresses desorption of water and other impurities from the substrate 202 under high-temperature conditions during the manufacture of the light-emitting diode 200, prevents the incorporation of oxygen-containing impurities into the n-type cladding layer 220, the light-emitting layer 222, the p-type cladding layer 224, and the like, and prevents warping of the substrate 202 due to differences in the thermal expansion coefficients between the substrate 202 and the n-type cladding layer 220. A film containing aluminum nitride, a film containing aluminum oxide, or a laminate thereof may be used as the undercoat 206.

[0051] The buffer layer 210 improves the adhesion between the substrate 202 and the n-type cladding layer 220, thereby preventing deformation (warping) of the substrate 202 under high-temperature conditions during the manufacture of the light-emitting diode 200. Furthermore, the buffer layer 210 contributes to promoting crystallization in the c-axis direction of the n-type cladding layer 220 formed thereon. This improves the crystallinity of the n-type cladding layer 220 and the layers formed thereon. This makes it possible to provide a light-emitting diode 200 with excellent characteristics. The buffer layer 210 can be configured to include titanium nitride, aluminum nitride, aluminum oxide, aluminum oxynitride, or the like. The buffer layer 210 may have a single-layer structure or a multilayer structure.

[0052] The n-type cladding layer 220, the light-emitting layer 222, and the p-type cladding layer 224 are configured to emit visible light by recombination of holes and electrons injected from the anode 226 and the cathode 228, respectively. The n-type cladding layer 220, the light-emitting layer 222, and the p-type cladding layer 224 may each have a single-layer structure or a laminated structure in which multiple layers are stacked. For example, the n-type cladding layer 220 may be a laminated layer of a layer containing undoped gallium nitride without a dopant and a layer containing n-type gallium nitride containing a dopant that imparts n-type conductivity, such as silicon or germanium. In the example shown in FIG. 11 , the n-type cladding layer 220, the light-emitting layer 222, and the p-type cladding layer 224 are stacked in this order from the substrate 202 side, but the reverse order may also be used.

[0053] The n-type cladding layer 220, the light-emitting layer 222, and the p-type cladding layer 224 are semiconductor layers containing Group 13 and Group 15 elements, respectively. Specifically, these layers contain semiconductors containing aluminum, gallium, and / or indium, as well as nitrogen, phosphorus, and / or arsenic. Typical semiconductors include gallium-based materials. Examples include gallium nitride-based materials such as gallium nitride, aluminum gallium nitride (AlGaN), and indium gallium nitride (InGaN), and gallium phosphide-based materials such as gallium phosphide (GaP) and aluminum indium gallium phosphide (AlGaInP). The n-type cladding layer 220 and the p-type cladding layer 224 may further contain the dopants described above. Adding dopants allows for control of the valence electrons of each layer and also allows for bandgap control.

[0054] The light-emitting layer 222 may have, for example, a single layer structure of indium gallium nitride, or may have a quantum well structure as shown in Fig. 11. A quantum well structure is a structure in which a plurality of thin films having different bandgaps and extremely small thicknesses of about 1 to 5 nm are alternately stacked, and examples thereof include an alternating stack of indium gallium nitride and gallium nitride, an alternating stack of indium gallium arsenide phosphide (GaInAsP) and indium phosphide (InP), and an alternating stack of aluminum indium arsenide (AlInAs) and indium gallium arsenide (InGaAs).

[0055] The anode 226 and the cathode 228 inject holes and electrons into the p-type cladding layer 224 and the n-type cladding layer 220, respectively. The anode 226 can be made of, for example, a metal such as palladium or gold, an alloy thereof, or a thin film of a conductive oxide that transmits visible light, such as indium-tin mixed oxide (ITO) or indium-zinc mixed oxide (IZO). The cathode 228 can be made of a metal such as aluminum, titanium, gold, silver, or indium, or an alloy thereof. Both the anode 226 and the cathode 228 can have a single-layer structure or can be a laminate of multiple films having different compositions.

[0056] Protective film 230 is configured to prevent impurities such as oxygen and water from entering light-emitting diode 200, and is composed of one or more films containing a silicon-containing inorganic compound such as silicon oxide or silicon nitride. Openings are provided in protective film 230 to expose anode 226 and cathode 228, and wiring (not shown) is electrically connected to anode 226 and cathode 228 using these openings.

[0057] The films of the various materials that make up the light-emitting diode 200 may be formed using chemical vapor deposition (CVD), or they may be formed by sputtering using the sputtering apparatus 100 and film formation method described above. The use of sputtering eliminates the need for high-temperature film formation, which is required for epitaxial growth using CVD methods such as metalorganic chemical vapor deposition (MOCVD). Therefore, even when using a substrate 202 containing amorphous glass, the n-type cladding layer 220, p-type cladding layer 224, and light-emitting layer 222 can be formed without deformation or damage to the substrate 202. In this case, a rotary target 130 containing the materials to be contained in the films to be formed is used. By using the sputtering apparatus 100, it is possible to precisely form not only the n-type cladding layer 220 and p-type cladding layer 224, but also a quantum well structure to achieve high light-emitting efficiency in the light-emitting layer 222. For example, in the example shown in Figure 8A, the n-type cladding layer 220 corresponds to the film 152-1 shown in Figure 8A, the light-emitting layer 222 corresponds to the films 152-2 to 152-5 shown in Figure 8A, and the p-type cladding layer 224 corresponds to the film 152-6 shown in Figure 8A. By forming the light-emitting layer 222, which has an extremely small thickness, using the sputtering apparatus 100 and film formation method described above, the thicknesses of these layers can be precisely controlled. This makes it possible to mass-produce light-emitting diodes 200 with excellent characteristics.

[0058] (2) Transistor FIG. 12A shows a schematic end view of an example of a transistor 250 fabricated using the sputtering apparatus 100. The transistor 250 shown in FIG. 12A is a high-electron-mobility field-effect transistor and includes a substrate 252, a buffer layer 260, and an active layer (also referred to as an electron transit layer) 262 on the substrate 252. The transistor 250 further includes an electron supply layer 264 on the active layer 262, a gate electrode 270 located on the active layer 262 and electrically connected to the active layer 262 and the electron supply layer 264, and a pair of terminals (a first terminal 266 and a second terminal 268). The first terminal 266 and the second terminal 268 may be in contact with the active layer 262, or may be in contact with the active layer 262 via the electron supply layer 264, as shown in FIG. 12A. These structures will be described below, but the structures of the substrate 252, the overcoat 254, the undercoat 256, and the buffer layer 260 are similar to the corresponding structures of the light-emitting diode 200 described above, and therefore will not be described again.

[0059] The stack of the active layer 262 and the electron supply layer 264 forms a path for source / drain current when the transistor 250 is operating. The active layer 262 and the electron supply layer 264 contain a Group 13 element and a Group 15 element. For example, the active layer 262 and the electron supply layer 264 may each contain a gallium nitride or gallium arsenide-based compound semiconductor. For example, the active layer 262 may be configured to contain undoped gallium nitride, and the electron supply layer 264 may be configured to include a first electron supply layer 264-1 containing undoped aluminum gallium nitride, a second electron supply layer 264-2 containing undoped gallium nitride, and a third electron supply layer 264-3 containing p-type indium gallium nitride.

[0060] The buffer layer 260, active layer 262, and electron supply layer 264 can be formed using a sputtering method in the sputtering apparatus 100 described above. Therefore, the high temperature required for epitaxial growth using the MOCVD method is not required, and even when a substrate 252 containing amorphous glass is used, these layers can be formed without deformation or damage to the substrate 252. Furthermore, the buffer layer 260, which serves as a base, promotes crystallization of the active layer 262 and the electron supply layer 264 in the c-axis direction. Even when the active layer 262 and the electron supply layer 264 are formed using a sputtering method, it is possible to achieve high c-axis orientation in these layers. As a result, a transistor with high field mobility can be provided.

[0061] The first terminal 266, the second terminal 268, and the gate electrode 270 contain a metal such as aluminum, gold, silver, tantalum, molybdenum, titanium, or copper, or an alloy containing one or more of the above metals. Although not shown, a gate insulating film may be provided as an optional configuration between the electron supply layer 264 and the gate electrode 270. The gate insulating film may contain, for example, a silicon-containing inorganic compound such as silicon oxide or silicon nitride, or a so-called high-k material such as hafnium silicate, zirconium silicate, hafnium oxide, or zirconium oxide. These configurations may also be formed by vacuum evaporation, electron beam evaporation, or CVD, but can also be formed by sputtering using the sputtering apparatus 100.

[0062] By forming each component of the transistor 250, particularly the extremely thin electron supply layer 264, the active layer 262, and the buffer layer 260, using the sputtering apparatus 100 and film formation method described above, it is possible to precisely control their thicknesses. For example, focusing on the configuration shown in FIG. 12A , the active layer 262 corresponds to film 152-1 or film 152-6 shown in FIG. 8A, and the layers constituting the electron supply layer 264 correspond to films 152-2 to 152-5. By forming each layer constituting the extremely thin electron supply layer 264 using the sputtering apparatus 100 and film formation method described above, it is possible to precisely control their thicknesses. This enables efficient mass production of transistors 250 with excellent characteristics.

[0063] The transistor manufactured using the sputtering apparatus 100 is not limited to the transistor structure shown in FIG. 12A . For example, the active layer 262 may have a two-layer structure, as in the transistor 280 shown in FIG. 12B . In this case, the active layer 262 may be composed of, for example, a first active layer 262-1 containing undoped gallium nitride and a second active layer 262-2 containing undoped aluminum gallium nitride. The configuration of the electron supply layer 264 is also not limited. For example, the electron supply layer 264 may be composed of a stack of a first electron supply layer 264-1 containing undoped gallium nitride, a second electron supply layer 264-2 containing n-type gallium nitride, and a third electron supply layer 264-3 containing undoped gallium nitride. A gate insulating film 272 is provided between the active layer 262 and the gate electrode 270. The gate insulating film 272 may be configured to contain, in addition to aluminum oxide, the silicon-containing inorganic compound or high-k material described above.

[0064] In the transistor 280, not only the buffer layer 260, the gate insulating film 272, the gate electrode 270, the first terminal 266, and the second terminal 268, but also the extremely thin active layer 262, which determines the characteristics of the transistor 280, can be formed by sputtering using the sputtering apparatus 100. For example, focusing on the configuration shown in FIG. 12B, the layers constituting the active layer 262 correspond to the films 152-1 or 152-6 shown in FIG. 8A, and the layers constituting the electron supply layer 264 correspond to the films 152-2 to 152-5. By forming the layers constituting the electron supply layer 264, which has a particularly small thickness, using the sputtering apparatus 100 and film formation method described above, the thicknesses of these layers can be precisely controlled. This allows these components to be precisely formed, enabling mass production of transistors 280 with highly controlled characteristics.

[0065] Although not explained here, the sputtering apparatus 100 and the film formation method using the same can be used not only to manufacture the semiconductor device, but also to form various structures such as wiring, terminals, capacitance elements, and electrodes necessary for driving the semiconductor device.

[0066] The above-described embodiments of the present invention can be combined as appropriate as long as they are not mutually inconsistent. Furthermore, even if a person skilled in the art appropriately adds or deletes components or modifies the design of a display device of each embodiment, or adds or omits processes or modifies conditions, such a display device is included in the scope of the present invention as long as it includes the gist of the present invention.

[0067] Even if there are other effects and advantages different from those brought about by the aspects of each of the above-mentioned embodiments, those that are clear from the description in this specification or that can be easily predicted by a person skilled in the art are naturally understood to be brought about by the present invention.

[0068] 100: sputtering apparatus, 102: chamber, 104: load lock door, 106: moving mechanism, 108: substrate stage, 120: target holder, 122: bearing, 124: control unit, 126: adhesion prevention plate, 128: magnet, 130: rotary target, 132: backing tube, 134: coating material, 134-1: first half tube section, 134-2: second half tube section, 134-3: 1 / 3 tube section, 134-4: 1 / 3 tube section, 134-5: 1 / 3 tube section, 150: substrate, 152: laminate, 152-1: film, 152-2: film, 152-3: film, 152-4: film, 152-5: film, 152-6: film, 154: film formation area, 200: generation Photodiode, 202: substrate, 204: overcoat, 206: undercoat, 210: buffer layer, 220: n-type cladding layer, 222: light-emitting layer, 224: p-type cladding layer, 226: anode, 228: cathode, 230: protective film, 250: transistor, 252: substrate, 254: overcoat, 256: undercoat, 260: buffer layer, 262: active layer, 262-1: first active layer, 262-2: second active layer, 264: electron supply layer, 264-1: first electron supply layer, 264-2: second electron supply layer, 264-3: third electron supply layer, 266: first terminal, 268: second terminal, 270: gate electrode, 272: gate insulating film, 280: transistor

Claims

1. A film formation method comprising: performing sputtering on a substrate while moving the substrate in a direction perpendicular to a rotation axis of a plurality of rotary targets arranged so that the rotation axes of the rotary targets are parallel to each other; the plurality of rotary targets are all arranged on one side of the substrate; and the plurality of rotary targets includes a first rotary target and a second rotary target having a smaller radius than the first rotary target.

2. The film formation method according to claim 1, wherein the plurality of rotary targets are arranged such that the maximum distance between any two selected from the plurality of rotary targets is greater than the longitudinal length of the substrate.

3. The film forming method described in claim 1, wherein the first rotary target and the second rotary target are positioned so that the distance from the rotation axis of the second rotary target to the substrate is smaller than the distance from the rotation axis of the first rotary target to the substrate.

4. The film forming method according to claim 1, wherein each of the plurality of rotary targets has a backing tube and a tubular coating material covering the backing tube, and the coating materials of the first rotary target and the second rotary target are different from each other.

5. The film forming method of claim 1, wherein each of the plurality of rotary targets has a backing tube to which an electric potential is supplied and a tubular coating material covering the backing tube, and a time for supplying an electric potential to the backing tube of the first rotary target is longer than that for the backing tube of the second rotary target.

6. The film forming method according to claim 1, wherein each of the plurality of rotary targets has a backing tube to which an electric potential is supplied and a tubular coating material covering the backing tube, and the electric potential is alternately supplied to the backing tubes of two adjacent rotary targets.

7. The film formation method described in claim 1, wherein each of the first rotary target and the second rotary target has a backing tube to which an electric potential is supplied and a tubular coating material covering the backing tube, and the coating material of the first rotary target and the second rotary target includes a gallium nitride compound semiconductor.

8. The film formation method of claim 1, wherein the plurality of rotary targets further includes a third rotary target adjacent to the second rotary target, the third rotary target having a radius smaller than the radius of the first rotary target, the second rotary target and the third rotary target each having a backing tube to which an electric potential is supplied and a tubular coating material covering the backing tube, and the coating materials of the second rotary target and the third rotary target each including a gallium nitride compound semiconductor having a composition different from each other.

9. The film forming method of claim 1, wherein each of the plurality of rotary targets has a backing tube and a tubular coating material covering the backing tube, and the coating material of at least one of the plurality of rotary targets has a first half tube portion and a second half tube portion comprising different materials.

10. The method of forming a film according to claim 1, wherein the sputtering is performed while reversibly moving the substrate.

11. A sputtering apparatus comprising: a chamber; a substrate stage within the chamber; a plurality of target holders disposed within the chamber, each configured to hold a rotary target; and a moving mechanism within the chamber, wherein the plurality of target holders are all disposed on one side of the substrate stage and are disposed such that the rotation axes of the rotary targets are parallel to each other, the moving mechanism is configured to move the substrate stage in a direction perpendicular to the rotation axis, the plurality of target holders include a first target holder and a second target holder, and a radius of the rotary target held by the second target holder is smaller than a radius of the rotary target held by the first target holder.

12. A sputtering apparatus as recited in claim 11, wherein the plurality of target holders are arranged such that the maximum distance between any two selected from the plurality of target holders is greater than the length of the substrate stage in the direction.

13. A sputtering apparatus as described in claim 11, wherein the first target holder and the second target holder are arranged such that the distance from the rotation axis of the rotary target held by the second target holder to the substrate stage is smaller than the distance from the rotation axis of the rotary target held by the first target holder to the substrate stage.

14. The sputtering apparatus of claim 11, wherein the movement mechanism is configured to reversibly move the substrate stage.

15. A rotary target comprising: a backing tube; and a coating material covering the backing tube, the coating material having n 1 / n tube sections arranged to surround the backing tube, the 1 / n tube sections including materials different from each other, and n being a natural number greater than or equal to 2.

16. The rotary target according to claim 15, wherein the coating material includes a gallium nitride compound semiconductor.

Citation Information

Patent Citations

  • Electronic cyclotron resonance plasma sputtering device, and manufacture of thin film

    JP2000199060A

  • Film deposition apparatus

    JP2015157985A

  • Apparatus with Adjacent Sputter Cathodes and Method of Operation

    JP2016507656A

  • Sputter device, and film deposition method

    JP2017036466A

  • Sputtering film deposition apparatus and sputtering film deposition method

    JP2019116644A