Temporary fixing member
The temporary fixing material with a composite modulus of 30 to 900 MPa, adjusted by polyfunctional acrylate and isocyanate blending, addresses the challenge of stable adhesion and easy removability during semiconductor wafer processing, improving productivity by ensuring easy and residue-free peeling.
Patent Information
- Application Number
- PCT/JP2024/012184
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-24
AI Technical Summary
Existing temporary fixing materials for semiconductor wafers fail to provide stable adhesion during processing and easy removability after heat-resistant processes, often leaving adhesive residue or requiring excessive peeling force.
A temporary fixing material with an adhesive layer having a composite modulus of 30 to 900 MPa, adjusted by blending polyfunctional acrylate and isocyanate crosslinking agents, which can be easily peeled off after curing, ensuring sufficient adhesion during processing without leaving residue.
The material allows for stable processing of thin wafers through various methods without damaging functional layers, enhancing productivity and yield in semiconductor manufacturing by ensuring easy and residue-free peeling.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Temporary fixing material
[0001] The present invention relates to a temporary fixing material used when processing workpieces such as semiconductor wafers. In particular, the present invention relates to a temporary fixing material that protects semiconductor wafers in order to perform wafer processing such as grinding, etching, and film formation on the backside of the semiconductor wafer. More specifically, the present invention relates to a temporary fixing material used in a wafer processing method in which the semiconductor wafer is processed using a system (wafer support system) in which the semiconductor wafer is fixed by a support substrate.
[0002] Prior art documents related to heat-resistant tapes for protecting semiconductor wafers include Patent Document 1, which discloses controlling the post-curing modulus of elasticity by photo- or thermal curing as a solution for achieving sufficient adhesive strength during wafer processing and enabling removal of the support substrate after the wafer processing process without damaging the wafer or leaving adhesive residue. Meanwhile, Patent Document 2 discloses that controlling either the composite modulus of elasticity or the indentation hardness measured by nanoindentation testing within a preferred range can enable the design of a suitable dicing tape (Patent Document 2) and a tape for backgrinding hard and brittle substrates (Patent Document 3). However, no suitable design for a temporary fixing material applicable to heat-resistant processes is known. The same is true for Patent Documents 3 to 6.
[0003] Japanese Patent Application Laid-Open No. 2015-29105 International Publication No. 2014-142193 Japanese Patent Application Laid-Open No. 2021-028392 International Publication No. 2020-162330 Japanese Patent Application Laid-Open No. 2021-73365 Japanese Patent Application Laid-Open No. 2017-132940
[0004] The above-mentioned temporary fixing material is required to reliably fix a wafer during a wafer processing step and to be easily removable after the backside process involving heating is completed. In view of the above technical background, an object of the present invention is to provide a temporary fixing material having an adhesive layer and used for processing a workpiece such as a semiconductor wafer, which can be stably separated from the wafer (workpiece) after the processing of the workpiece such as a semiconductor wafer and is also applicable to heat-resistant processes. Another object of the present invention is to provide a method for manufacturing a final wafer product using the temporary fixing material.
[0005] The inventors conducted an investigation using a wafer coated with polyimide (PI), which is often used as an insulating film on patterned wafers. As shown in Comparative Example 1, even when the overall elastic modulus of the cured adhesive was set within the preferred range specified in Patent Document 1, peeling was difficult and difficult after heat treatment. As a result of their investigation, the inventors discovered that it is important to appropriately control the surface elastic modulus after curing (composite elastic modulus measured by nanoindentation testing). The inventors discovered that controlling the composite elastic modulus and hardness of the cured temporary fixing tape device adhesive, as measured by nanoindentation testing, can suppress adhesion enhancement due to heat treatment and design a tape that can be easily peeled without leaving any adhesive residue. Specifically, they found that controlling the type and amount of multifunctional acrylate allowed them to control the composite elastic modulus and ensure easy peeling even after heat treatment (Examples 1 to 6). Without the addition of a multifunctional acrylate, peeling was difficult and difficult (Comparative Example 1). It was also found that using too much multifunctional acrylate resulted in an excessively high composite elastic modulus after curing, making peeling difficult (Comparative Examples 2 and 3).
[0006] That is, the present invention provides: [1] a temporary fixing material having a pressure-sensitive adhesive layer and used for processing a workpiece, wherein the pressure-sensitive adhesive layer in contact with the workpiece has a composite elastic modulus of 30 to 900 MPa as measured by a nanoindentation test after being cured by heating or light irradiation under the following conditions: (Heating condition) Heating at 140°C for 30 minutes (Irradiation condition) 1000 mJ / cm 2 Regarding.
[0007] Hereinafter, [2] to
[14] are all preferred aspects or embodiments of the present invention. [2] The temporary fixing material according to [1], wherein the temporary fixing material is a single-sided tape. [3] The temporary fixing material according to [1] or [2], wherein the temporary fixing material is for use in a wafer support system. [4] The temporary fixing material according to any one of [1] to [3], wherein the temporary fixing material is a double-sided tape. [5] The temporary fixing material according to any one of [1] to [4], wherein the temporary fixing material is a liquid temporary fixing material. [6] The temporary fixing material according to any one of [1] to [5], wherein the pressure-sensitive adhesive layer, after curing under the above conditions, has an indentation hardness of 4 to 80 MPa as measured by a nanoindentation test. [7] The temporary fixing material according to any one of [1] to [6], wherein the pressure-sensitive adhesive layer contains an acrylic polymer. [8] The temporary fixing material according to any one of [1] to [7], wherein the pressure-sensitive adhesive layer further contains 0.01 to 8 parts by mass of an isocyanate crosslinking agent relative to 100 parts by mass of the acrylic polymer. [9] The temporary fixing material according to any one of [1] to [8], wherein the pressure-sensitive adhesive layer further contains 0.1 to 3.0 parts by mass of an organic peroxide relative to 100 parts by mass of the acrylic polymer.
[10] The temporary fixing material according to any one of [1] to [9], wherein the pressure-sensitive adhesive layer further contains 10 to 100 parts by mass of a bifunctional and / or trifunctional acrylate relative to 100 parts by mass of the acrylic polymer.
[11] A method for producing a final wafer product, comprising: (a) a step of forming a laminate including a wafer, a temporary fixing material, and a support; (b) a step of curing a pressure-sensitive adhesive layer included in the temporary fixing material by heating or ultraviolet light irradiation; (c) a step of subjecting the wafer to a heat treatment, a mechanical processing treatment, a chemical treatment, a physical treatment, a laser processing treatment, and / or a film-forming treatment after the step (b); (d) a step of removing the support from the laminate after the step (c); and (e) a step of removing the temporary fixing material from the laminate including the wafer and the temporary fixing material after the step (d), wherein the pressure-sensitive adhesive layer has a composite elastic modulus of 30 to 900 MPa as measured by a nanoindentation test after being cured by heating or light irradiation under the following conditions: (heating condition) heating at 140°C for 30 minutes; and (irradiation condition) 1000 mJ / cm.2
[12] The manufacturing method according to
[11] , wherein the pressure-sensitive adhesive layer, after curing under the conditions, has an indentation hardness of 4 to 80 MPa as measured by a nanoindentation test.
[13] The manufacturing method according to
[11] or
[12] , wherein the step (b) cures the pressure-sensitive adhesive layer by heating at 120 to 160°C for 5 to 40 minutes or by irradiating with light at an integrated illuminance of 500 mJ or more and 10,000 mJ or less.
[14] The manufacturing method according to any one of
[11] to
[12] , wherein the step (d) removes the support from the laminate by laser peeling or mechanical peeling.
[0008] The temporary fixing material having a pressure-sensitive adhesive layer used in the present invention improves the handleability of thin or fragile wafers, enables stable processing of wafers in a wide variety of processing processes, and also enables stable removal of the pressure-sensitive adhesive layer from the wafer after the wafer processing. This makes it possible to perform multiple and / or diverse processes on the wafer with high productivity and yield without damaging electronic components such as functional layers formed on the wafer, and greatly contributes to improving the productivity of electronic components such as electronic devices.
[0009] The present invention provides a temporary fixing material having a pressure-sensitive adhesive layer and used for processing a workpiece, wherein the pressure-sensitive adhesive layer in contact with the workpiece has a composite elastic modulus of 30 to 900 MPa as measured by a nanoindentation test after being cured by heating or light irradiation under the following conditions: (Heating condition) Heating at 140°C for 30 minutes (Irradiation condition) 1000 mJ / cm 2 is.
[0010] The adhesive layer used in the present invention is used to temporarily fix a workpiece such as a wafer. In particular, it is an adhesive layer that comes into contact with a workpiece such as a wafer. The adhesive layer used in the present invention is easily peeled off from the wafer after wafer processing, and has a composite elastic modulus of 30 to 900 MPa as measured by a nanoindentation test after being cured by heating or light irradiation under the following conditions: (heating condition) heating at 140°C for 30 minutes; (irradiation condition) 1000 mJ / cm 2When the composite elastic modulus is within this range, the adhesive layer has sufficient adhesive strength to fix the wafer to the support, but has sufficiently low adhesive strength to allow peeling. The mechanism by which the composite elastic modulus achieves the above-mentioned easy peelability from the wafer is not necessarily clear, but it is presumed that there is some relationship between the composite elastic modulus satisfying this range and providing the adhesive layer with appropriate flexibility during peeling and appropriate dissipation of the force required for peeling. The nanoindentation test conditions will be explained in the examples below.
[0011] The composite elastic modulus may be preferably 32 to 780 MPa. The composite elastic modulus can be adjusted by the types and amounts of the components described below.
[0012] The pressure-sensitive adhesive layer used in the present invention, after being cured under the above conditions, preferably has an indentation hardness measured by a nanoindentation test of 4 to 80 MPa, more preferably 5 to 75 MPa.
[0013] Examples of the adhesive component used in the adhesive layer used in the present invention include those containing rubber-based, acrylic-based, epoxy-based, urethane-based, allyl-based, silicone-based, fluorine-based and polyimide-based adhesive components. The adhesive layer used in the present invention preferably contains an acrylic polymer because it has heat resistance and allows easy adjustment of the adhesive strength and adhesion.
[0014] The adhesive component is preferably a curable adhesive component because, by curing it before wafer processing, voids are less likely to occur during high-temperature processes in the wafer manufacturing process, and adhesion buildup due to high temperatures in the high-temperature processes is suppressed, allowing for easy peeling without leaving any adhesive residue. Examples of the curable adhesive component include photocurable adhesive components that crosslink and harden when irradiated with light, and thermosetting adhesive components that crosslink and harden when heated. In particular, examples of thermosetting adhesive components include thermosetting adhesive components that contain, as curing components, monomers, oligomers, or polymers such as acrylic, epoxy, urethane acrylate, epoxy acrylate, silicone acrylate, or polyester acrylate, and that contain a thermal polymerization initiator.
[0015] Of the above, the acrylic polymer can be obtained, for example, by synthesizing in advance a (meth)acrylic polymer having a functional group in the molecule (hereinafter referred to as a functional group-containing (meth)acrylic polymer), and then reacting it with a compound having in the molecule a functional group reactive with the functional group and a radically polymerizable unsaturated bond (hereinafter referred to as a functional group-containing unsaturated compound).
[0016] The functional group-containing (meth)acrylic polymer is obtained by copolymerizing, in a conventional manner, an alkyl acrylate and / or alkyl methacrylate ester, whose alkyl group typically has 2 to 18 carbon atoms, with a functional group-containing monomer and, if necessary, with other modifying monomers copolymerizable therewith. The weight-average molecular weight of the functional group-containing (meth)acrylic polymer is typically about 200,000 to 2,000,000.
[0017] Examples of the functional group-containing monomer include carboxyl group-containing monomers such as acrylic acid and methacrylic acid, hydroxyl group-containing monomers such as hydroxyethyl acrylate and hydroxyethyl methacrylate, epoxy group-containing monomers such as glycidyl acrylate and glycidyl methacrylate, isocyanate group-containing monomers such as isocyanate ethyl acrylate and isocyanate ethyl methacrylate, and amino group-containing monomers such as aminoethyl acrylate and aminoethyl methacrylate.
[0018] Examples of the other copolymerizable modifying monomers include various monomers used in general (meth)acrylic polymers, such as vinyl acetate, acrylonitrile, and styrene.
[0019] The functional group-containing unsaturated compound to be reacted with the functional group-containing (meth)acrylic polymer can be the same as the functional group-containing monomer described above, depending on the functional group of the functional group-containing (meth)acrylic polymer. For example, when the functional group of the functional group-containing (meth)acrylic polymer is a carboxyl group, an epoxy group-containing monomer or an isocyanate group-containing monomer is used. When the functional group is a hydroxyl group, an isocyanate group-containing monomer is used. When the functional group is an epoxy group, a carboxyl group-containing monomer or an amide group-containing monomer such as acrylamide is used. When the functional group is an amino group, an epoxy group-containing monomer is used.
[0020] Organic Peroxide In one embodiment, the pressure-sensitive adhesive layer used in the present invention may contain a curable adhesive component. In this case, an organic peroxide may be contained as a thermal polymerization initiator. Examples of organic peroxides include those that decompose when heated to generate active radicals that initiate polymerization and curing. Specific examples include t-butylperoxy-2-ethyl hexanoate, bis(4-methylbenzoyl)peroxide, benzoyl peroxide, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-bis-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarboxylate, t-butylperoxyacetate, 2,2-bis-( t-butylperoxy)butane, 4,4-bis-(t-butylperoxy)n-butyl pentanoate, bis-t-hexyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, bis(2-t-butylperoxyisopropyl)benzene, t-butylcumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne, and diisopropylbenzene hydroperoxide.
[0021] Among these thermal polymerization initiators, commercially available ones are not particularly limited, but suitable examples include Perbutyl O, Niper BMT, Niper BW, Perhexa HC, Perhexa C, Pertetra A, Perhexyl I, Perbutyl A, Perhexa 22, Perhexa V, Perhexyl D, Percumyl D, Perhexa 25B, Perbutyl P, Perbutyl C, Perhexyne 25B, Percumyl P (all manufactured by NOF Corporation), Perkadox 12XL25 (manufactured by Nouryon Chemical Co., Ltd.), etc. These thermal polymerization initiators may be used alone or in combination of two or more.
[0022] The amount of the organic peroxide is preferably 0.1 to 3.0 parts by mass relative to 100 parts by mass of the acrylic polymer. The amount is more preferably 0.1 to 1.0 part by mass. When the amount of the organic peroxide is within this range, it can function sufficiently as a thermal polymerization initiator.
[0023] Polyfunctional Acrylate The pressure-sensitive adhesive layer used in the present invention may contain, as a curing component, for example, a monomer, oligomer, or polymer such as acrylic, epoxy, urethane acrylate, epoxy acrylate, silicone acrylate, or polyester acrylate. The oligomer or monomer as the curing component generally has a molecular weight of 10,000 or less and has 1 to 40 radically polymerizable unsaturated bonds in the molecule. From the viewpoint of three-dimensional reticulation, the number of radically polymerizable unsaturated bonds is preferably 2 or more.
[0024] Examples of the oligomer or monomer as the curing component include trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol monohydroxypentaacrylate, dipentaerythritol hexaacrylate, and the same methacrylates as above. Other examples include 1,4-butylene glycol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, commercially available oligoester acrylates, urethane acrylates, and the same methacrylates as above. These polyfunctional oligomers or monomers may be used alone or in combination of two or more.
[0025] In one embodiment, the adhesive layer used in the present invention can contain a polyfunctional acrylate as a curing component. The polyfunctional acrylate is preferably a bifunctional or trifunctional acrylate. The elastic modulus of the adhesive layer after curing is thought to depend on the polyfunctional acrylate, and the use of a bifunctional or trifunctional acrylate allows the adhesive layer to be easily peeled off without leaving any adhesive residue after wafer processing. Examples of bifunctional or trifunctional acrylates include trimethylolpropane triacrylate, trimethylolpropane PO-modified triacrylate, and polyester acrylate.
[0026] The amount of the bifunctional and / or trifunctional acrylate blended is preferably 10 to 100 parts by mass relative to 100 parts by mass of the acrylic polymer. The blended amount is more preferably 30 to 60 parts by mass. When the amount of the polyfunctional acrylate blended is 10 parts by mass or more, sufficient adhesive strength is exerted to temporarily fix the wafer and the support, preventing unintended peeling during the wafer processing step. When the amount of the polyfunctional acrylate blended is 100 parts by mass or less, adhesive residue due to excessive adhesive strength can be prevented.
[0027] Isocyanate Crosslinking Agent The pressure-sensitive adhesive layer used in the present invention may contain an isocyanate crosslinking agent. As the isocyanate crosslinking agent, a HDI (hexamethylene diisocyanate)-based isocyanate crosslinking agent is preferred. Commercially available HDI-based isocyanate crosslinking agents include, for example, D170N (manufactured by Mitsui Chemicals, Inc.) and Coronate HX (manufactured by Tosoh Corporation).
[0028] The amount of the isocyanate crosslinking agent is preferably 0.01 to 8 parts by mass relative to 100 parts by mass of the acrylic polymer. The amount is more preferably 3 to 6 parts by mass. When the amount of the isocyanate crosslinking agent is within this range, the agent can function sufficiently as a crosslinking agent.
[0029] When the pressure-sensitive adhesive layer used in the present invention contains an acrylic polymer, it may further contain at least two or more of: (a) 0.01 to 8 parts by mass of an isocyanate crosslinking agent, (b) 0.1 to 3.0 parts by mass of an organic peroxide, and (c) 10 to 100 parts by mass of a difunctional and / or trifunctional acrylate, relative to 100 parts by mass of the acrylic polymer. That is, as long as the blending amount relative to the acrylic polymer is within the above range, the pressure-sensitive adhesive layer may contain a combination of (a) an isocyanate crosslinking agent and (b) an organic peroxide, (a) an isocyanate crosslinking agent and (c) a difunctional and / or trifunctional acrylate, and (b) an organic peroxide and (c) a difunctional and / or trifunctional acrylate, or may contain all of (a) an isocyanate crosslinking agent, (b) an organic peroxide, and (c) a difunctional and / or trifunctional acrylate.
[0030] The pressure-sensitive adhesive layer used in the present invention may contain, if desired, known additives such as an acrylic polymer having no unsaturated double bond, various thermal crosslinking agents such as a melamine compound or an epoxy compound, a release agent, a plasticizer, a resin, a surfactant, a wax, or a fine particle filler.
[0031] The release agent is not particularly limited as long as it generally exhibits a release effect. Examples include hydrocarbon compounds, silicone compounds, fluorine compounds, and polyethylene waxes, carnauba wax, montanic acid, and stearic acid, which are known as release agents for plastic materials. Among these, silicone and fluorine compounds are preferred, and silicone and fluorine compounds having functional groups crosslinkable with the curable adhesive are more preferred. Silicone compounds, in particular, have excellent heat resistance, preventing scorching of the adhesive layer even after treatment involving heating at 200°C or higher, and bleed out to the adherend interface during peeling, facilitating peeling. Since the silicone compound has functional groups crosslinkable with the curable adhesive, it chemically reacts with the curable adhesive upon light irradiation or heating and is incorporated into the curable adhesive, preventing the silicone compound from adhering to the adherend and causing contamination. The inclusion of a silicone compound also exhibits the effect of preventing adhesive residue on semiconductor chips. Other examples of the release agent include plasticizers. Plasticizers are not particularly limited as long as they generally reduce the adhesive strength of the adhesive layer to the adherend. Examples of plasticizers include trimellitic acid ester, pyromellitic acid ester, phthalic acid ester, and adipic acid ester.
[0032] The amount of release agent added is not particularly limited, but is appropriately determined so as to obtain a release effect. On the other hand, the amount added is controlled so as not to be excessive so as not to significantly impair the adhesive function of the pressure-sensitive adhesive layer used in the present invention. For example, it is desirable to adjust the amount added according to the peel force, with an amount of usually 0.1 to 5 parts by mass, preferably 0.1 to 3 parts by mass, and more preferably 0.1 to 1 part by mass, based on 100 parts by mass of the entire pressure-sensitive adhesive layer.
[0033] When a plasticizer is added, it is desirable to adjust the amount of addition according to the peel strength, typically about 5 to 50 parts by mass, preferably about 10 to 50 parts by mass, and more preferably about 20 to 40 parts by mass. In this embodiment, these release agents can be used alone or in combination.
[0034] The thickness of the adhesive layer used in the present invention is not particularly limited, but the preferred lower limit is 5 μm and the preferred upper limit is 250 μm, and the more preferred lower limit of the adhesive layer thickness is 10 μm and the more preferred upper limit is 200 μm. When the adhesive layer thickness is within this range, it can absorb the unevenness of the wafer and can be temporarily fixed to the support with sufficient strength, and when peeling off the adhesive layer, the peel force can be easily adjusted to a preferred range.
[0035] The present invention provides a temporary fixing material having the above-described adhesive layer. The temporary fixing material may be a single-sided tape. The single-sided tape may include a substrate such as a film and a device-side adhesive layer (wafer-side adhesive layer). The adhesive layer of the single-sided tape may be a single layer or a laminate of multiple adhesive layers. The temporary fixing material of the present invention may be used in a wafer support system. The temporary fixing material for use in a wafer support system may be a double-sided tape such as a double-sided adhesive tape. In the double-sided tape, the temporary fixing material may include a substrate, a first adhesive layer on one side of the substrate, and a second adhesive layer (support-side adhesive layer) on the other side (opposite side) of the substrate, where the first adhesive layer is the adhesive layer that contacts the workpiece, and the second adhesive layer may include the same adhesive layer as the adhesive layer that contacts the workpiece. In this embodiment, the adhesive strength of the support can be appropriately adjusted, allowing the support to be easily removed after wafer processing. The substrate film can be designed from the perspective of the mechanical strength and handleability of the entire laminate, which is particularly advantageous from the perspective of optimizing the performance of the tape. While there are no particular limitations on the material of the substrate film, it is preferable to use a plastic film, such as a film, sheet, sheet with a mesh structure, or sheet with holes made of acrylic, olefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), nylon, urethane, polyether ether ketone (PEEK), liquid crystal polymer (LCP), or polyimide. From the perspective of handling, PET, PEN, or polyimide film is preferred.
[0036] In one embodiment of the present invention, the temporary fixing material used in the wafer support system can be a liquid temporary fixing material. In this liquid temporary fixing material, the adhesive layer can contain a liquid adhesive. Here, the liquid adhesive refers to an adhesive that is liquid or semi-liquid at room temperature, and includes, for example, a liquid curable adhesive that hardens upon heating. According to the liquid adhesive material of the present invention, the liquid adhesive is applied to either or both of the wafer and the support by spin coating or the like to form a laminate of wafer / adhesive layer or adhesive layer / support, and then the adhesive layers of both are bonded together to produce a laminate consisting of support / adhesive layer / wafer.
[0037] Workpieces to be processed using the temporary fixing material of the present invention are not particularly limited, and examples thereof include semiconductor wafers. For example, there are no particular limitations on the wafers to be temporarily fixed to a support and processed using the temporary fixing material of the present invention, and any wafer generally used in semiconductor manufacturing processes can be used. Among these, wafers that require careful handling during processing due to their thinness and fragility are preferably used, and therefore require temporary fixing. Here, the thinness and fragility of the wafer are assumed to be, for example, cases in which the thickness temporarily thins during processing, causing handling problems. The temporary fixing material of the present invention is used to temporarily fix such wafers to a support. Examples of cases in which a wafer is temporarily thinned include cases in which a thin wafer is processed as a starting point, cases in which a relatively thick wafer is thinned during a process, and cases in which the thinned wafer is further processed. The thickness of the temporarily thinned wafer is usually 1 to 200 μm. For example, in a case where a semiconductor wafer on which processing of a functional layer has been completed is temporarily fixed to a support via a temporary fixing material so that the functional layer faces the support, the surface opposite to the functional layer (back surface) is thinly ground, ions are implanted on the back surface, annealing is performed, and an electrode is formed, and the semiconductor wafer in the process is separated from the support, the semiconductor wafer corresponds to the workpiece. As described above, wafers temporarily fixed using the temporary fixing material of the present invention also include those whose state changes during the process.
[0038] As described above, there are no particular limitations on the wafers that can be temporarily fixed using the temporary fixing material of the present invention, but more specific examples include semiconductor wafers such as silicon wafers, compound semiconductor wafers of SiC, AlSb, AlAs, AlN, AlP, BN, BP, BAs, GaSb, GaAs, GaN, GaP, InSb, InAs, InN, or InP, quartz wafers, sapphire, glass, mold wafers, etc. The silicon wafers and compound semiconductor wafers may be doped.
[0039] Electrical / electronic functional layers may be formed on or within the wafer. Examples of suitable functional layers include electronic circuits, capacitors, transistors, resistors, electrodes, optical elements, and MEMS, but other microdevices may also be used. The surfaces of these functional layers may have structures, typically electrodes, formed from one or more of the following materials: silicon, polysilicon, silicon dioxide, (oxy)silicon nitride, metals (e.g., copper, aluminum, gold, tungsten, and tantalum), low-k dielectrics, polymer dielectrics, and various metal nitrides and metal silicides. The surface of the wafer on which the functional layer is formed (the functional layer surface) may have raised structures such as solder bumps, metal posts, and pillars. The wafer surface may also be covered with an oxide or nitride film for the formation of the functional layer or for protection of the functional layer. The wafer surface may also be covered with a passivation film for wafer protection.
[0040] In one aspect, the present invention provides the following manufacturing method for a final wafer product, comprising: (a) a step of forming a laminate including a wafer, a temporary fixing material, and a support; (b) a step of curing a pressure-sensitive adhesive layer included in the temporary fixing material by heating or ultraviolet light irradiation; (c) a step of subjecting the wafer to a heat treatment, a mechanical processing treatment, a chemical treatment, a physical treatment, a laser processing treatment, and / or a film-forming treatment after the step (b); (d) a step of removing the support from the laminate after the step (c); and (e) a step of removing the temporary fixing material from the laminate including the wafer and the temporary fixing material after the step (d), wherein the pressure-sensitive adhesive layer has a composite elastic modulus of 30 to 900 MPa as measured by a nanoindentation test after being cured by heating or light irradiation under the following conditions: (heating condition) heating at 140°C for 30 minutes; and (irradiation condition) 1000 mJ / cm. 2 .
[0041] Step (a) is a step of forming a laminate including a wafer, a temporary fixing material, and a support. That is, this is a step of laminating the wafer and the support so as to temporarily fix them via the temporary fixing material. The temporary fixing material may be the same as that described above.
[0042] The adhesive layer contained in the temporary fixing material may be any of those described above. In addition, instead of the adhesive layer having the thermosetting adhesive component described above, an adhesive layer having a photocurable adhesive component that is crosslinked and cured by light irradiation may be used.
[0043] Examples of the photocurable adhesive component include a photocurable adhesive component containing a monomer, oligomer, or polymer such as acrylic, epoxy, urethane acrylate, epoxy acrylate, silicone acrylate, or polyester acrylate as a curable component, and containing a photopolymerization initiator.
[0044] Examples of the photopolymerization initiator include those that are activated by irradiation with light having a wavelength of 250 to 800 nm. Examples of such photopolymerization initiators include acetophenone derivative compounds such as methoxyacetophenone, benzoin ether compounds such as benzoin propyl ether and benzoin isobutyl ether, ketal derivative compounds such as benzyl dimethyl ketal and acetophenone diethyl ketal, phosphine oxide derivative compounds, bis(η5-cyclopentadienyl)titanocene derivative compounds, benzophenone, Michler's ketone, chlorothioxanthone, todecylthioxanthone, dimethylthioxanthone, diethylthioxanthone, α-hydroxycyclohexylphenyl ketone, and 2-hydroxymethylphenylpropane. These photopolymerization initiators may be used alone or in combination of two or more.
[0045] Wafer The wafer can be the same as the wafer shown in the specific example of the workpiece described above.
[0046] The support preferably has sufficient strength and rigidity and excellent heat resistance and chemical resistance. By using such a support, even if the wafer is thin-ground in a subsequent process, the wafer can be stably handled, and the wafer can be subjected to multiple and / or diverse processes without bending or the like. For example, a wafer on which an electronic circuit is formed can be subjected to various processes required for manufacturing an electronic device having a structure in which semiconductor chips are stacked, such as TSV connection.
[0047] Materials preferably used for the support include silicon, sapphire, quartz, metals (e.g., aluminum, copper, steel), and various glasses and ceramics. The support may be composed of a single material, or may be composed of multiple materials, or may include other materials deposited on the substrate. For example, a silicon wafer may have a vapor-deposited layer such as silicon nitride on it. The support may be surface-treated, for example, by providing a release layer.
[0048] Depending on the temperature of the process to which the laminate is subjected, the support may be made of plastic. For example, a sheet made of plastic such as polyimide, acrylic, polyolefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), nylon, or urethane can be preferably used as the support. Polyimide can be used because it has a certain degree of heat resistance.
[0049] To obtain uniformity in the thickness of the wafer after grinding, etc., it is desirable for the thickness of the support to be uniform. For example, to thin a silicon wafer to 50 μm or less and maintain the uniformity at ±10% or less, the variation in the thickness of the support should be kept to ±2 μm or less. There are no particular restrictions on the thickness of the support, but from the viewpoint of effectively preventing wafer curvature, it is preferably 300 μm or more, and more preferably 500 μm or more. From the viewpoint of reducing the total weight during handling or reducing the stress required for mechanical peeling, it is preferably 1500 μm or less, and more preferably 1000 μm or less.
[0050] In the step (a), a laminate including a wafer, a temporary fixing material, and a support can be obtained. By curing the pressure-sensitive adhesive layer of the laminate in the step (b) described below, the laminate has sufficient strength and rigidity, and can be used in various semiconductor manufacturing processes while preventing bending and breakage.
[0051] As a method for forming the laminate, the support, the temporary fixing material, and the wafer can be laminated in this order. The order of lamination is not particularly limited, and these layers may be laminated at once or sequentially.
[0052] When the adhesive layer is supplied as a liquid curable adhesive material or the like, the liquid curable adhesive material or the like is applied to either or both of the wafer and the support by spin coating or the like to form a laminate of wafer / adhesive layer or adhesive layer / support, and then the other of the support or wafer is bonded to the laminate under reduced pressure, thereby making it possible to prepare a laminate consisting of support / adhesive layer / wafer.
[0053] When the pressure-sensitive adhesive layer is supplied as a solid tape (film), the solid tape (film) is attached to either the wafer or the support, and then the other is attached thereto under reduced pressure, thereby producing a laminate consisting of the support / pressure-sensitive adhesive layer / wafer.
[0054] Step (b) Step (b) is a step of curing the pressure-sensitive adhesive layer contained in the temporary fixing material by heating or ultraviolet irradiation, and is a step of curing the pressure-sensitive adhesive layer in the laminate obtained in step (a).
[0055] The curable adhesive component that has been crosslinked and cured by irradiation with light or heat has dramatically improved chemical resistance, and can prevent the adhesive from dissolving in a chemical solution, even when a chemical solution is applied to the backside of the wafer during a wafer processing step. Furthermore, the crosslinked and cured curable adhesive component has an increased elastic modulus, so that adhesion is less likely to increase even at high temperatures, and peeling is relatively easy.
[0056] For example, when a photocurable adhesive component containing a polymer having an unsaturated double bond such as a vinyl group in a side chain and a photopolymerization initiator activated at a wavelength of 250 to 800 nm is used as the photocurable adhesive component in which the adhesive layer is crosslinked and cured by irradiation with light, such a photocurable adhesive component is preferably irradiated at an illuminance of 5 mW or more, more preferably 10 mW or more, even more preferably 20 mW or more, and particularly preferably 50 mW or more. Furthermore, irradiation is preferably at an integrated illuminance of 300 mJ or more, more preferably 500 mJ to 10,000 mJ, even more preferably 500 mJ to 7,500 mJ, and particularly preferably 1,000 mJ to 5,000 mJ.
[0057]
[0046] In addition, for example, when a pressure-sensitive adhesive layer containing a polymer having an unsaturated double bond such as a vinyl group in a side chain and a thermal polymerization initiator that is activated by heating at about 50 to 200°C is used as the thermosetting pressure-sensitive adhesive component that crosslinks and cures when heated, the pressure-sensitive adhesive layer can be crosslinked and cured by heating at a temperature of about 50 to 200°C for 5 to 40 minutes.
[0058] In one embodiment of the present invention, in step (b), the pressure-sensitive adhesive layer may be cured by heating at 120 to 160°C for 5 to 40 minutes. Heating at 120°C or higher for 5 minutes or longer can sufficiently cure the pressure-sensitive adhesive layer. Furthermore, it is sufficient to cure the pressure-sensitive adhesive layer to an extent that the laminate can withstand the wafer processing step, and it is preferable from the viewpoint of cost to set the heating conditions to 160°C or 40 minutes or shorter.
[0059] Step (c) is a step of subjecting the wafer to heat treatment, mechanical processing, chemical treatment, physical treatment, laser processing, and / or film formation treatment after step (b). The stack formed through steps (a) and (b) can be subjected to at least one wafer treatment selected from heat treatment (including treatment involving heat generation; the same applies below), mechanical processing, chemical treatment, physical treatment, laser processing, and film formation treatment. In addition, the stack formed through steps (a) and (b) can also be subjected to processing required for TSV processing and for forming a structure in which TSV-processed semiconductor chips are stacked.
[0060] Examples of the heat treatment include, but are not limited to, thermal curing of the resin composition, heat drying of the resin composition, baking of the resin composition, reflow, resin sealing, and the like.
[0061] The above-mentioned machining processes typically include polishing, grinding, drilling, and cutting of the wafer, but are not limited to these and also include singulation. When grinding or polishing a wafer having electrodes formed on its surface, the surface on which the electrodes are not formed (back surface) is ground or polished. The thickness of the wafer after back surface grinding and polishing varies depending on the electronic device in which the obtained electronic device is used, but is usually set to 1 μm or more and 200 μm or less, preferably 5 μm or more and 100 μm or less, and more preferably 5 μm or more and 50 μm or less. This allows the obtained electronic device to be made thinner, thereby realizing the miniaturization of electronic devices using such electronic devices.
[0062] In this embodiment, when grinding or polishing a wafer, by laminating the wafer to a rigid support via the adhesive layer, the wafer can be ground or polished with higher processing accuracy, and after grinding or polishing, the wafer can be subjected to a further processing step or the wafer can be easily separated from the adhesive layer without damaging the wafer.
[0063] The chemical treatment is, for example, a polishing treatment such as CMP, a treatment using an acid, an alkali, or an organic solvent, and examples thereof include plating treatments such as electrolytic plating and electroless plating, wet etching treatments using hydrofluoric acid, an aqueous solution of tetramethylammonium hydroxide (TMAH), or the like, a resist stripping process using N-methyl-2-pyrrolidone, monoethanolamine, DMSO, or the like, and a cleaning process using concentrated sulfuric acid, aqueous ammonia, aqueous hydrogen peroxide, or the like, but is not limited to these.
[0064] Examples of the physical treatment include, but are not limited to, plasma treatment, ion implantation, and laser annealing.
[0065] Examples of the laser processing include, but are not limited to, annealing, via processing, circuit formation processing by direct writing, and pre-processing for separation from the support.
[0066] Examples of the film formation process include, but are not limited to, coating processes such as spin coating, inkjet printing, and screen printing, sputtering, vapor deposition, etching, chemical vapor deposition (CVD), physical vapor deposition (PVD), resist coating / patterning, heat lamination of a resin composition film, and back metal.
[0067] As described above, in this embodiment, although the wafer is subjected to heat treatment, mechanical processing treatment, chemical treatment, physical treatment, laser processing treatment, and film formation treatment in the wafer processing step, sufficient adhesive strength is maintained during the wafer processing, and after the wafer processing step is completed, in the step of peeling the wafer from the laminate, the wafer can be peeled from the pressure-sensitive adhesive layer without being damaged or leaving adhesive residue.
[0068] Furthermore, after the treatment of step (c), chip bonding, wire bonding, flip chip bonding, surface activation direct bonding, etc. may be performed. Furthermore, a dicing tape may be attached to the treated surface (preferably the ground surface) of the wafer. By attaching the dicing tape in advance, dicing can be performed quickly after peeling off the support and the adhesive layer.
[0069] Step (d) Step (d) is a step of removing the support from the laminate after step (c). In step (d), the method for removing the support from the laminate is not particularly limited, but laser peeling or mechanical peeling is preferred because it is cost-effective and can simplify the equipment. Note that pre-peeling treatment may be performed in advance, and a method such as swelling or dissolution of the pressure-sensitive adhesive layer with a solvent may be appropriately adopted as the pre-peeling treatment.
[0070] Step (e) Step (e) is a step of removing the temporary fixing material from a laminate including a wafer and a temporary fixing material after step (d). Because the support is removed from the laminate through step (d), the temporary fixing material can be separated from the wafer without applying excessive stress to the wafer, thereby minimizing the risk of damaging functional layers formed on the wafer. There are no particular limitations on the method for removing the temporary fixing material, but considering the ease of peeling of the temporary fixing material, for example, peeling tape can be attached to the temporary fixing material and the temporary fixing material can be peeled off from the wafer together with the peeling tape. This is also advantageous in terms of cost because no special equipment is required.
[0071] According to the temporary fixing material and the wafer processing method used in the present invention, the wafer can be stably processed and then subjected to subsequent processes to manufacture a final wafer product. When a functional layer is formed on the wafer, the final product can be manufactured by carrying out processes such as dicing, bonding, packaging, and sealing that are commonly used in the manufacture of electronic devices such as semiconductor devices.
[0072] The present invention will be specifically described below, but the present invention is not limited in any way by the following examples.
[0073] Details of the materials and ingredients used in the examples and comparative examples are as follows.
[0074] Separator: The following silicone release-treated PET film (polyethylene terephthalate film) was used: Mitsui Chemicals Tocello Co., Ltd., product name: T15, thickness: 38 μm
[0075] Substrate Film The non-corona treated side of a PEN film (polyethylene naphthalate film, manufactured by Toyobo Co., Ltd., trade name: Teonex Q83C, thickness: 50 μm, corona treated on one side) was subjected to corona treatment to obtain a substrate film corona treated on both sides.
[0076] Substrate film with primer: An aqueous urethane resin liquid (manufactured by DIC Corporation, product name: Hydran AP-40N) was diluted with distilled water to obtain a coating liquid. This coating liquid was applied to a substrate film (polyethylene naphthalate film) using a wire bar and dried at 130°C for 5 minutes. Similarly, a primer was laid on the back surface to obtain a substrate film with primer.
[0077] Resins for forming adhesive layers: (Meth)acrylic resin solution N: 49 parts by mass of ethyl acrylate, 20 parts by mass of 2-ethylhexyl acrylate, 21 parts by mass of methyl acrylate, 10 parts by mass of glycidyl methacrylate, and 0.5 parts by mass of a benzoyl peroxide-based polymerization initiator were reacted in a solvent consisting of 65 parts by mass of toluene and 50 parts by mass of ethyl acetate at 80°C for 10 hours. After completion of the reaction, the resulting solution was cooled, and 25 parts by mass of xylene, 5 parts by mass of acrylic acid, and 0.5 parts by mass of tetradecyldimethylbenzylammonium chloride were added to the cooled solution. The reaction was carried out at 85°C for 32 hours while blowing air into the solution, yielding (meth)acrylic resin solution N. The solids concentration was 39%. (Meth)acrylic resin solution SA591: Mitsui Chemicals, Inc., product name: Bindceram SA591
[0078] Compounds for forming adhesive layer: Polyfunctional isocyanate D-170N manufactured by Mitsui Chemicals, Inc., trade name: Takenate D-170N; Polyfunctional acrylate M309 manufactured by Toagosei Co., Ltd., trade name: Aronix M309; Polyfunctional acrylate M402 manufactured by Toagosei Co., Ltd., trade name: Aronix M402; Organic peroxide 12XL25 manufactured by Kayaku Nouryon Co., Ltd., trade name: Perkadox 12XL25; Chemical name: 2,2-Di(4,4-di(t-butylperoxy)cyclohexyl)propane; 1-minute half-life temperature: 145°C; Mold release agent BYK-UV3500 manufactured by BYK Japan KK, trade name: BYK-UV3500
[0079] The adhesive tape described in Example 1 was prepared as follows. Other Examples and Comparative Examples were also prepared in the same manner based on the Example Table.
[0080] Adhesive Intermediate Layer Coating: (Meth)acrylic resin solution N (75 parts by weight as solids), (meth)acrylic resin solution SA591 (25 parts by weight as solids), organic peroxide 12XL25 (0.5 parts by weight as solids), polyfunctional isocyanate D-170N (0.1 parts by weight as solids), and ethyl acetate were mixed to obtain a coating solution for the intermediate layer (solids concentration: 35%). This coating solution was applied to the release surface of the separator using an applicator and dried in a hot air oven at 100°C for 10 minutes to form a 40 μm thick adhesive layer. This was then bonded to the primer-coated substrate film side to obtain a separator / intermediate layer (40 μm) / primer-coated substrate.
[0081] Adhesive Surface Coating and Adhesive Tape: (Meth)acrylic Resin Solution N (75 parts by weight in terms of solids), (Meth)acrylic Resin Solution SA591 (25 parts by weight in terms of solids), Organic Peroxide 12XL25 (0.5 parts by weight in terms of solids), Polyfunctional Isocyanate D-170N (5.68 parts by weight in terms of solids), and ethyl acetate were mixed to obtain a surface coating solution (solids concentration: 30%). This coating solution was applied to the release surface of a separator using an applicator and dried in a hot air oven at 100°C for 10 minutes to form a 10 μm thick adhesive layer. This was then bonded to the separator / intermediate layer (40 μm) / primer-attached substrate film from which the separator had been peeled, to obtain a laminate consisting of separator / surface layer (10 μm) / intermediate layer (40 μm) / primer-attached substrate film. Subsequently, this laminate was aged by heating in an oven at 50° C. for 5 days to obtain an adhesive tape.
[0082] A sample for the surface layer tensile test described in Example 2 was prepared as follows.
[0083] Surface Layer for Tensile Test Evaluation (Meth)acrylic Resin Solution N (100 parts by mass as solids), Organic Peroxide 12XL25 (0.5 parts by mass as solids), Polyfunctional Isocyanate D-170N (5.68 parts by mass as solids), and ethyl acetate were mixed to obtain a coating solution for the surface layer (solids concentration: 35%). This coating solution was applied to the release surface of a separator using an applicator and dried in a hot air oven at 100°C for 10 minutes to form a 50 μm-thick adhesive layer. Two such adhesive layers were formed and bonded together to prepare an adhesive layer (100 μm) with separators on both sides. This was then heat-aged in a hot air oven at 50°C for 5 days. Next, the separator on one side was peeled off, and the adhesive layers were repeatedly bonded together to obtain a surface layer (1 mm) for tensile test evaluation with separators on both sides.
[0084] <Evaluation Method> (1) Tensile Test of Cured Pressure-Sensitive Adhesive A pressure-sensitive adhesive (1 mm) with separators on both sides was heated in a nitrogen atmosphere at 140°C for 30 minutes to obtain a cured product. The obtained cured product was heated at 50°C for 30 minutes and punched into a strip shape (10 mm wide). The separators on both sides were peeled off from the obtained test piece, and a tensile test was performed using a tensile tester (Shimadzu Corporation, AGX-V) (23°C, tensile speed: 10 mm / min, grip distance: 20 mm) to measure the Young's modulus.
[0085] (2) Nanoindentation Method of Adhesive Tape (Cured Product) The separator was peeled off from the adhesive tape, and the adhesive material was pre-dried at 100°C. After being attached to a silicon wafer, the tape was cured by heating at 140°C for 30 minutes using a hot plate. The tape was peeled off from the silicon wafer to obtain an adhesive tape (cured product). Using instant adhesive (manufactured by Konishi Co., Ltd., product name: Aron Alpha EXTRA Quick Action Multipurpose), the substrate (primer) side of the adhesive tape (cured product) was attached to a sample disk with the adhesive surface facing up. Next, the sample disk with the adhesive tape (cured product) attached was fixed to the stage of the nanoindenter using correction fluid. The displacement-load curve obtained by pressing the probe against this adhesive surface was numerically processed using the software provided with the measurement device to obtain the composite elastic modulus and hardness (indentation hardness). Measurements were performed at three different locations, and the average value was used as the measured value.
[0086] <Measurement conditions> Apparatus: Bruker Japan Co., Ltd., product name: Hysitron TI Premier Probe: Bruker Japan Co., Ltd., diamond Berkovich type, product number: TI-0039 Measurement method: single indentation, depth control (measurement depth: 500 nm) Measurement temperature: 23°C Loading time: loading 5 seconds → holding 2 seconds → unloading 5 seconds
[0087] (3) Adhesive Strength (without heat treatment) After peeling off the separator from an adhesive tape (25 mm wide), the adhesive tape was attached to a silicon wafer with a PI (polyimide) film (Seiren KST Corporation, film thickness after baking: 5 μm). After one hour, the load was read using a universal testing machine (Toyo Seiki Seisaku-sho, Strograph E-S) to measure the adhesive strength (tensile speed: 300 mm / min, measurement temperature: 23°C).
[0088] (4) Adhesive Strength (After 140°C / 30 minutes → 200°C / 30 minutes) The separator was peeled off from an adhesive tape (25 mm wide), and the adhesive was pre-dried at 100°C. The adhesive tape was attached to a silicon wafer with a PI (polyimide) film (Seiren KST Co., Ltd., film thickness after baking: 5 μm). Next, the tape was heated at 140°C / 30 minutes using a hot plate to harden it. Subsequently, a heat treatment was performed at 200°C / 30 minutes using a hot plate. After one hour, the load was read using a universal testing machine (Toyo Seiki Seisakusho Co., Ltd., Strograph E-S) to measure the adhesive strength (tensile speed: 300 mm / min, measurement temperature: 23°C).
[0089] The formulations of each Example / Comparative Example and the results of each test are shown in Table 1.
[0090]
[0091] From the results in Table 1, in the Examples, the adhesive material (adhesive layer) was cured by heating at 140°C for 30 minutes, and then the composite elastic modulus measured by the nanoindentation test was 30 to 800 MPa, and the adhesive strength (PI film-attached wafer (after 140°C / 30 minutes → 200°C / 30 minutes)) was good (10 N / 25 mm or less). In contrast, in the Comparative Examples, in which the composite elastic modulus was outside the range of 30 to 800 MPa, the adhesive strength was rated as x, and adhesive residue remained, peeling was impossible, or the peeling force was large.
[0092] The temporary fixing material of the present invention allows a large number and / or a wide variety of processes to be carried out on wafers with high productivity and yield without damaging electronic components such as functional layers formed on the wafers, and therefore contributes greatly to improving the productivity of electronic devices, and has high applicability in various fields of industries such as the electronic component industry, including the semiconductor process industry, the electrical and electronics industry that uses electronic components, the transportation machinery industry, the information and communications industry, and the precision equipment industry.
Claims
1. A temporary fixing material having a pressure-sensitive adhesive layer and used for processing a workpiece, wherein the pressure-sensitive adhesive layer in contact with the workpiece is cured under the following conditions by heating or light irradiation, and then has a composite elastic modulus of 30 to 900 MPa as measured by a nanoindentation test: (Heating conditions) Heat at 140°C for 30 minutes (Irradiation conditions) 1000 mJ / cm 2 .
2. The temporary fixing material according to claim 1, wherein the temporary fixing material is a single-sided tape.
3. The temporary fixation material of claim 1, wherein said temporary fixation material is for use in a wafer support system.
4. The temporary fixing material according to claim 3, wherein the temporary fixing material is a double-sided tape.
5. The temporary fixing material according to claim 3, wherein the temporary fixing material is a liquid temporary fixing material.
6. The temporary fixing material according to claim 1, wherein the adhesive layer has an indentation hardness of 4 to 80 MPa as measured by a nanoindentation test after curing under the above conditions.
7. The temporary fixing material according to claim 1, wherein the adhesive layer comprises an acrylic polymer.
8. The temporary fixing material according to claim 1, wherein the adhesive layer further comprises: 0.01 to 8 parts by mass of an isocyanate crosslinking agent relative to 100 parts by mass of the acrylic polymer.
9. The temporary fixing material according to claim 1, wherein the adhesive layer further comprises: an organic peroxide: 0.1 to 3.0 parts by mass per 100 parts by mass of the acrylic polymer.
10. The temporary fixing material according to claim 1, wherein the adhesive layer further comprises: 10 to 100 parts by mass of a bifunctional and / or trifunctional acrylate, relative to 100 parts by mass of the acrylic polymer.
11. A method for producing a final wafer product, comprising: (a) forming a laminate including a wafer, a temporary fixing material, and a support; (b) curing a pressure-sensitive adhesive layer included in the temporary fixing material by heating or ultraviolet light irradiation; (c) subjecting the wafer to a heat treatment, a mechanical processing treatment, a chemical treatment, a physical treatment, a laser processing treatment, and / or a film formation treatment after step (b); (d) removing the support from the laminate after step (c); and (e) removing the temporary fixing material from the laminate including the wafer and the temporary fixing material after step (d), wherein the pressure-sensitive adhesive layer has a composite elastic modulus of 30 to 900 MPa as measured by a nanoindentation test after being cured by heating or light irradiation under the following conditions: (heating conditions) heating at 140°C for 30 minutes; (irradiation conditions) 1000 mJ / cm 2 .
12. The manufacturing method according to claim 11, wherein the pressure-sensitive adhesive layer, after curing under the above conditions, has an indentation hardness of 4 to 80 MPa as measured by a nanoindentation test.
13. The method according to claim 11 or 12, wherein in step (b), the pressure-sensitive adhesive layer is cured by heating at 120 to 160° C. for 5 to 40 minutes, or by irradiating with light at an integrated illuminance of 500 mJ or more and 10,000 mJ or less.
14. The method of claim 11 or 12, wherein step (d) removes the support from the laminate by laser peeling or mechanical peeling.
Citation Information
Patent Citations
Active ray curing releasable adhesive composition
JP2003171622A
Protective film, and production method for semiconductor device using protective film
WO2015152010A1
Cited By
Workpiece processing method
JPWO2022202659A1