Sealing method, sealing structure, and sealing material
By compressing band-shaped sealing materials with an adhesive layer and foam to align ends perpendicularly, the method addresses the challenges of material loss and water-stopping effectiveness, achieving robust sealing and efficient material use.
Patent Information
- Application Number
- PCT/JP2024/013860
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional sealing methods using foam-based materials face challenges in achieving high water-stopping properties and efficient material utilization, particularly when processing band-shaped sealing materials, which often result in material loss and compromised sealing effectiveness.
A band-shaped sealing material with an adhesive layer and foam is compressed perpendicularly to align the ends in a direction perpendicular to the main surface, satisfying the condition (w1 - w0) / (t * w0) ≤ 0.15mm^-1, allowing for effective sealing while minimizing material loss and optimizing water-stopping properties.
This method achieves high water-stopping properties, meeting IPX7 standards and reducing material waste, thereby enhancing the yield and effectiveness of the sealing process.
Smart Images

Figure JP2024013860_24102024_PF_FP_ABST
Abstract
Description
Sealing method, sealing structure, and sealing material
[0001] The present invention relates to a sealing method, a sealing structure, and a sealing material.
[0002] BACKGROUND ART Conventionally, it is known to use a sealing material containing a foam to seal a space surrounded by the sealing material so as to be waterproof.
[0003] For example, Patent Document 1 describes a waterproof sealant having a layer of a predetermined pressure-sensitive adhesive composition on at least one surface of a foam structure having closed cells. This waterproof sealant is processed into a doughnut shape to obtain a sample, which is sandwiched between an acrylic plate and an acrylic molded body, and the compressibility of the sample in the thickness direction is adjusted to examine whether it is waterproof.
[0004] Japanese Patent Application Publication No. 10-77463
[0005] In the technology described in Patent Document 1, the waterproof sealant is processed into a doughnut shape, and it is thought that processing such as cutting out a circle in the center of the sheet-shaped waterproof sealant is necessary. In this case, it is thought that a lot of material will be wasted. For this reason, it is thought that a sealing method that involves processing such as cutting out the waterproof sealant will make it difficult to increase the yield of products to which the sealing method is applied.
[0006] For example, it is conceivable to surround a specific space with a strip-shaped sealing material to seal the space in a waterproof manner, but in this case, it is thought to be difficult to improve the waterproofing properties.
[0007] In view of the above circumstances, the present invention provides a sealing method that uses a strip-shaped sealing material and is advantageous from the viewpoint of high water-stopping properties.
[0008] The present invention includes a method of sealing a space surrounded by a strip-shaped sealing material, the strip-shaped sealing material having a pressure-sensitive adhesive layer and a foam that form one main surface, in such a state that one end and the other end in the length direction of the strip-shaped sealing material are overlapped so that the one end and the other end are aligned in a direction perpendicular to the main surface, and compressing the sealing material in a direction perpendicular to the main surface, and sealing the space surrounded by the sealing material in a waterproof manner, wherein (w1-w0) / (t*w0)≦0.15 mm -1The following condition is satisfied: w1 is the width of the sealing material after compression at the overlapping portion of the one end and the other end; w0 is the width of the sealing material before compression; and t is the thickness of the sealing material before compression.
[0009] The present invention also provides a strip-shaped sealing material having a foam and an adhesive layer forming one main surface, wherein one end and the other end in the length direction of the sealing material are overlapped so that the one end and the other end are aligned in a direction perpendicular to the main surface, the sealing material is compressed in the direction perpendicular to the main surface, and a space surrounded by the sealing material is sealed in a waterproof manner, and (w1-w0) / (t*w0)≦0.15 mm -1 The following condition is satisfied: w1 is the width of the sealing material after compression at the overlapping portion of the one end and the other end; w0 is the width of the sealing material before compression; and t is the thickness of the sealing material before compression.
[0010] Furthermore, the present invention provides a strip-shaped sealing material comprising an adhesive layer forming one main surface and a foam, wherein when one end and the other end in the length direction of the sealing material are overlapped so that the one end and the other end are aligned in a direction perpendicular to the main surface, and the sealing material is compressed in a direction perpendicular to the main surface to seal a space surrounded by the sealing material in a waterproof manner, (w1-w0) / (t*w0)≦0.15 mm -1 The present invention provides a sealing material that can satisfy the following condition, wherein: w1 is the width of the sealing material after compression at the overlapping portion of the one end and the other end; w0 is the width of the sealing material before compression; and t is the thickness of the sealing material before compression.
[0011] The above sealing method is advantageous from the viewpoint of high water-stopping property while using a strip-shaped sealing material.
[0012] FIG. 1 is a diagram schematically showing an example of a water-stopping method according to the present invention. FIG. 2 is a cross-sectional view of a sealing material taken along line II-II in FIG. 1. FIG. 3 is a cross-sectional view of a sealing material taken along line III-III in FIG. 1. FIG. 4 is a diagram schematically showing a water-stopping method according to a reference example. FIG. 5 is a diagram schematically showing another example of a water-stopping method according to the present invention. FIG. 6 is a diagram schematically showing yet another example of a water-stopping method according to the present invention. FIG. 7 is a diagram schematically showing yet another example of a water-stopping method according to the present invention. FIG. 8 is a diagram schematically showing yet another example of a water-stopping method according to the present invention.
[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments.
[0014] As shown in FIG. 1 , the sealing method of this embodiment includes sealing a space 5 surrounded by a strip-shaped sealing material 10 in a waterproof manner. In this sealing method, one end 11 and the other end 12 of the strip-shaped sealing material 10 in the longitudinal direction are overlapped so that the one end 11 and the other end 12 are aligned in a direction perpendicular to one of the main surfaces F1 of the sealing material 10, and the sealing material 10 is compressed in a direction perpendicular to the main surface F1. In this sealing method, the condition of the following formula (1) is satisfied. In the condition of formula (1), as shown in FIGS. 1 and 3 , w1 is the width of the sealing material 10 after compression at the overlapping portion 15 of the one end 11 and the other end 12 of the sealing material 10, w0 is the width of the sealing material 10 before compression, and t is the thickness of the sealing material 10 before compression. (w1 - w0) / (t * w0)≦0.15 mm -1 Formula (1)
[0015] 2, the sealing material 10 includes an adhesive layer 10p and a foam 10f. The adhesive layer 10p forms one of the main surfaces F1.
[0016] The above sealing method can provide a seal structure 1 including a seal material 10. In the seal structure 1, one end 11 and the other end 12 of the seal material 10 in the length direction are overlapped so that they are aligned in a direction perpendicular to the main surface F1. The seal material 10 is also compressed in a direction perpendicular to the main surface F1, thereby sealing the space surrounded by the seal material 10 in a watertight manner. Furthermore, in the seal structure 1, the condition of the above formula (1) is satisfied.
[0017] According to the above-described sealing method and sealing structure 1, the space 5 can be sealed waterproofly using the strip-shaped sealing material 10, which tends to reduce material waste compared to, for example, a sealing method using an annular sealing material obtained by cutting out a sheet-shaped sealing material. As a result, the yield of products to which this sealing method and sealing structure 1 are applied tends to be high.
[0018] As shown in FIG. 4 , a sealing method using a strip-shaped sealant 10 may involve compressing the sealant 10 while the first end 11 and the second end 12 are aligned parallel to the main surface F1. This method requires a space approximately twice the width of the sealant 10 where the first end 11 and the second end 12 are aligned parallel to the main surface F1. In addition, a gap may form along the side of the sealant 10 between the first end 11 and the second end 12, making it difficult to achieve high watertightness. In particular, when using a robot arm to place the sealant in a location requiring sealing, for example, to reduce labor, the actual placement of the sealant may deviate by several millimeters from the intended placement. High-precision placement of the sealant, as with manual placement, is unlikely. Thus, the sealing method shown in FIG. 4 is not particularly advantageous in terms of space saving and high watertightness.
[0019] 1, the one end 11 and the other end 12 are overlapped so as to be aligned in a direction perpendicular to the main surface F1, which makes it easy to reduce the space occupied by the sealing material 10 even in the area where the one end 11 and the other end 12 are aligned. Furthermore, after extensive research, the inventors have found that high water-stopping properties are easily achieved by satisfying the condition of the above formula (1). For example, waterproofness conforming to IPX7 can be achieved.
[0020] As shown in Figure 3, before the sealing material 10 is compressed to obtain the seal structure 1, a gap G is generated near the portion where one end 11 and the other end 12 are overlapped. The volume of this gap G is thought to be proportional to t * w0, which is the product of the thickness t and width w0 of the sealing material 10 before compression. In order to achieve high water stoppage, it is thought to be important that the sealing material 10 is compressed and deformed so as to eliminate the gap G. After extensive trial and error, the inventors of the present invention have newly discovered that by adjusting the sealing method and sealing structure so that the condition of the above formula (1) is satisfied, the sealing material 10 expands in the longitudinal direction as the sealing material 10 is compressed, making it easier to eliminate the gap G and achieving high water stoppage.
[0021] In the above-described sealing method and sealing structure 1, for example, the condition of the following formula (2) is further satisfied. In this case, high water-stopping properties are more likely to be achieved. The value of the left side of formula (2) is 0.06 mm -1 More than 0.07 mm -1 More than 0.08 mm -1 More than 0.09 mm -1 or more, or 0.10 mm -1 (w1-w0) / (t*w0)≧0.05 mm -1 Formula (2)
[0022] 1 , for example, a strip-shaped sealing material 10 is arranged in an annular shape on a plate-shaped first member 21 so as to surround the space 5. Then, a plate-shaped second member 22 is arranged facing the first member 21, and the sealing material 10 is pressed by the first member 21 and the second member 22, compressing the sealing material 10. In this way, a sealing structure 1 is obtained in which the space 5 is sealed in a waterproof manner.
[0023] As long as the condition of formula (1) is satisfied, the compressibility R of the sealing material 10 in the sealing method and sealing structure 1 C is not limited to a specific value. C is expressed by the following formula (3): C is, for example, 15% or more. In this case, high water-stopping properties are more likely to be achieved. In formula (3), t is the thickness of the sealing material 10 before compression, and t1 is the thickness of the sealing material 10 after compression. The compression ratio R C is the compression ratio at a portion away from the overlapping portion 15. C [%]=100×(t-t1) / t Formula (3)
[0024] Compression rate R C may be 18% or more, 20% or more, 25% or more, 30% or more, 32% or more, 35% or more, 40% or more, or 45% or more. C is, for example, 90% or less. C may be 85% or less, 80% or less, 75% or less, 70% or less, 65% or less, or 60% or less.
[0025] In the sealing method and the sealing structure 1, the length L of the overlapping portion 15 in the longitudinal direction of the sealing material 10 O is not limited to a specific value. O is, for example, 5 mm or more. In this case, high water stopping properties are more likely to be achieved.
[0026] Length L O The length L may be 8 mm or more, 10 mm or more, 15 mm or more, 20 mm or more, 25 mm or more, 30 mm or more, 35 mm or more, or 45 mm or more. O is, for example, 100 mm or less, and may be 90 mm or less, 80 mm or less, 70 mm or less, or 50 mm or less.
[0027] 3, each of the one end 11 and the other end 12 may have an end surface extending perpendicular to the main surface F1. With such a configuration, processing of the sealing material 10 for the sealing method tends to be easy.
[0028] 5, the one end 11 and the other end 12 may each have an end face that is an inclined surface extending at an angle with respect to the main surface F1 and a plane perpendicular to the main surface F1. In this case, it is possible to prevent the distance between the one end 11 and the other end 12 from suddenly changing in the length direction of the sealing material 10 before the sealing material 10 is compressed.
[0029] 6 and 7 , the other end 12 may be formed by bending a portion of the sealing material 10 around the other end 12. In addition, the one end 11 may have an end face that is a slope that extends at an angle with respect to the main surface F1 and a plane perpendicular to the main surface F1. In this case, compression of the sealing material 10 may cause the other end 12 to deform along the slope that is the end face of the one end 11. This makes it easier to achieve high water-stopping properties.
[0030] 8 , at least one selected from the group consisting of a portion including an end of one end 11 in the length direction of the sealing material 10 and a portion including an end of the other end 12 in the length direction of the sealing material 10 may protrude from the overlapping portion 15. In this case, the one end 11 and the other end 12 may intersect perpendicularly with each other to form the overlapping portion 15, or the one end 11 and the other end 12 may intersect obliquely to form the overlapping portion 15.
[0031] The sealing material 10 includes a pressure-sensitive adhesive layer 10p and a foam 10f that form the main surface F1, and is not limited to a specific sealing material as long as the sealing method satisfies the condition of formula (1) above. As shown in Figure 2, the sealing material 10 may further include, for example, a pressure-sensitive adhesive layer 10q that forms the other main surface F2. The pressure-sensitive adhesive layer 10q may be omitted from the sealing material 10, and the sealing material 10 may include only the foam 10f and the pressure-sensitive adhesive layer 10p.
[0032] The width w0 of the sealing material 10 is not limited to a specific value as long as it satisfies the condition of the above formula (1). The width w0 is, for example, 3 to 20 mm, and may be 5 to 15 mm or 5 to 10 mm. When the width of the sealing material 10 differs between the one end 11 and the other end 12, the larger width is defined as the width w0.
[0033] The thickness t of the sealing material 10 is not limited to a specific value as long as it satisfies the condition of the above formula (1). The thickness t is, for example, 1 to 40 mm, and may be 1 to 30 mm or 3 to 15 mm.
[0034] The structure of the foam 10f is not limited to a specific structure. For example, the foam 10f may have a closed-cell structure. In this case, the interior of the foam 10f has high liquid-tightness, and the seal structure 1 is more likely to have high water-stopping properties.
[0035] The foam 10f may have, for example, a semi-closed or semi-open cell structure. In this case, the foam 10f contains open cells before compressive deformation, and when the foam 10f is compressively deformed to generate a predetermined compressive strain, the open cells are closed, resulting in a change to a structure similar to a closed cell structure. The foam may have, for example, an open cell structure.
[0036] The material of the foam 10f is not limited to a specific material. The foam 10f may be, for example, a rubber foam or a resin foam. Examples of resin foam include urethane foam, silicone foam, and acrylic foam.
[0037] The foam 10f is preferably a rubber foam. In this case, the seal structure 1 is more likely to have high water-stopping properties. The rubber foam can be obtained, for example, by foaming a rubber composition containing rubber, a foaming agent, and a cross-linking agent.
[0038] The rubber may be, for example, an olefin-based elastomer, a styrene-based elastomer, a butyl-based elastomer, a vinyl chloride-based elastomer, or natural rubber. Examples of olefin-based elastomers are ethylene-propylene rubber (EPM) and ethylene-propylene-diene rubber (EPDM). Examples of styrene-based elastomers are styrene-butadiene rubber (SBR), styrene-butadiene-styrene rubber (SBS), styrene-isoprene-styrene rubber (SIS), styrene-ethylene-butadiene rubber, styrene-ethylene-butylene-styrene rubber (SEBS), styrene-isobutylene-styrene block rubber (SIBS), and styrene-isoprene-propylene-styrene rubber. Examples of butyl-based elastomers are butyl rubber, polyisobutylene rubber, polybutene, polyisoprene rubber, and nitrile butadiene rubber (NBR). Examples of vinyl chloride-based elastomers are chloroprene rubber and chlorosulfonated polyethylene rubber.
[0039] The rubber is preferably an olefin-based elastomer, more preferably EPDM, in which case the seal structure 1 is more likely to have high water-stopping properties.
[0040] EPDM is a rubber obtained by copolymerizing ethylene, propylene, and dienes. By copolymerizing dienes in addition to ethylene and propylene, unsaturated bonds are introduced, making it possible to crosslink the rubber with a crosslinking agent.
[0041] Examples of dienes include 5-ethylidene-2-norbornene, 1,4-hexadiene, and dicyclopentadiene. These dienes may be used alone or in combination of two or more. When the diene contains dicyclopentadiene, the degree of crosslinking can be improved.
[0042] The EPDM preferably has long chain branches. The method for introducing long branched chains into the EPDM is not limited to a specific method, and any known method can be used. If the EPDM has long chain branches, the rubber composition can be foamed well.
[0043] The diene content in the EPDM (diene content) is, for example, 1% by mass or more, preferably 2% by mass or more, and more preferably 3% by mass or more. The diene content is, for example, 20% by mass or less, preferably 15% by mass or less. This makes the rubber foam less susceptible to surface shrinkage and cracking.
[0044] The foaming agent may be an organic foaming agent or an inorganic foaming agent.
[0045] Examples of organic blowing agents include azo blowing agents, N-nitroso blowing agents, hydrazide blowing agents, semicarbazide blowing agents, fluorinated alkane blowing agents, triazole blowing agents, and other known organic blowing agents. Examples of azo blowing agents include azodicarboxylic acid amide (ADCA), barium azodicarboxylate, azobisisobutyronitrile (AIBN), azocyclohexylnitrile, and azodiaminobenzene. Examples of N-nitroso blowing agents include N,N'-dinitrosopentamethylenetetramine (DTP), N,N'-dimethyl-N,N'-dinitrosoterephthalamide, and trinitrosotrimethyltriamine. Examples of hydrazide-based blowing agents include 4,4'-oxybis(benzenesulfonylhydrazide) (OBSH), paratoluenesulfonylhydrazide, diphenylsulfone-3,3'-disulfonylhydrazide, 2,4-toluenedisulfonylhydrazide, p,p-bis(benzenesulfonylhydrazide) ether, and benzene-1,3-disulfonylhydrazide, allylbis(sulfonylhydrazide). Examples of semicarbazide-based blowing agents include p-toluenesulfonylsemicarbazide and 4,4'-oxybis(benzenesulfonylsemicarbazide). Examples of fluorinated alkane-based blowing agents include trichloromonofluoromethane and dichloromonofluoromethane. An example of a triazole-based blowing agent is 5-morpholyl-1,2,3,4-thiatriazole. The organic blowing agent may be thermally expandable microparticles in which a thermally expandable substance is encapsulated in microcapsules. Examples of such thermally expandable fine particles include commercially available products such as Microsphere (trade name, manufactured by Matsumoto Yushi Co., Ltd.).
[0046] Examples of inorganic foaming agents include bicarbonates, carbonates, nitrites, borohydrides, inorganic azides, and other known inorganic foaming agents. Examples of bicarbonates include sodium bicarbonate and ammonium bicarbonate. Examples of carbonates include sodium carbonate and ammonium carbonate. Examples of nitrites include sodium nitrite and ammonium nitrite. Examples of borohydrides include sodium borohydride. These foaming agents may be used alone or in combination of two or more.
[0047] The amount of the foaming agent is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, and more preferably 10 parts by mass or more, relative to 100 parts by mass of rubber. The amount of the foaming agent is, for example, 50 parts by mass or less, and preferably 30 parts by mass or less.
[0048] Examples of crosslinking agents include sulfur compounds such as sulfur (S8) and 4,4'-dithiodimorpholine, selenium, magnesium oxide, lead monoxide, quinoid compounds such as p-quinone dioxime, p,p'-dibenzoylquinone dioxime, and poly-p-dinitrosobenzene, polyamines, nitroso compounds such as p-dinitrosobenzene, organic peroxides, resins, and ammonium salts such as ammonium benzoate. Examples of organic peroxides include dicumyl peroxide, dimethyldi(t-butylperoxy)hexane, 1,1-di(t-butylperoxy)cyclohexane, and α,α'-di(t-butylperoxy)diisopropylbenzene. Examples of resins include alkylphenol-formaldehyde resins and melamine-formaldehyde condensates. These crosslinking agents may be used alone or in combination.
[0049] The crosslinking agent is preferably sulfur (S8) and a sulfur compound, a quinoid compound, or an organic peroxide. Sulfur (S8) and a sulfur compound are advantageous from the viewpoints of excellent mechanical strength and foaming properties. Quinoid compounds are advantageous from the viewpoints of reducing the sulfur atom content, reducing corrosiveness, and excellent foaming properties. Organic peroxides are advantageous from the viewpoints of improving adhesion to an object and step-following ability, etc., to realize the seal structure 1.
[0050] The mixing ratio of the crosslinking agent is, for example, 0.05 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, per 100 parts by mass of rubber. The mixing ratio of the crosslinking agent is, for example, 30 parts by mass or less, preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of rubber.
[0051] A quinoid compound and an organic peroxide may be used in combination as a crosslinking agent. In this case, sufficient crosslinking is likely to occur on the surface of the foam 10f. When a quinoid compound and an organic peroxide are used in combination, the blending ratio of the organic peroxide is, for example, 1 part by mass or more, and more preferably 10 parts by mass or more, per 100 parts by mass of the quinoid compound. The blending ratio is, for example, 100 parts by mass or less, and preferably 50 parts by mass or less, per 100 parts by mass of the quinoid compound.
[0052] The rubber composition desirably contains a foaming aid and a crosslinking aid. Examples of the foaming aid include urea-based foaming aids, salicylic acid-based foaming aids, benzoic acid-based foaming aids, and metal oxides such as zinc oxide. Preferred are urea-based foaming aids and metal oxides. These foaming aids may be used alone or in combination of two or more.
[0053] The blending ratio of the foaming aid is, for example, 0.5 parts by mass or more, and preferably 1 part by mass or more, per 100 parts by mass of rubber. The blending ratio is, for example, 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of rubber.
[0054] Examples of crosslinking coagents include thiazoles, thioureas, dithiocarbamic acids, guanidines, sulfenamides, thiurams, xanthic acids, aldehyde ammonia, and aldehyde amines. Among these, thiazoles, thioureas, dithiocarbamic acids, or thiurams are preferably used as crosslinking coagents. Examples of thiazoles include dibenzothiazyl disulfide and 2-mercaptobenzothiazole. Examples of thioureas include diethylthiourea, trimethylthiourea, and dibutylthiourea. Examples of dithiocarbamic acids include sodium dimethyldithiocarbamate, sodium diethyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, and zinc dibenzyldithiocarbamate. Examples of guanidines include diphenylguanidine and di-o-tolylguanidine. Examples of sulfenamides are benzothiazyl-2-diethylsulfenamide and N-cyclohexyl-2-benzothiazylsulfenamide. Examples of thiurams are tetramethylthiuram monosulfide, tetramethylthiuram disulfide, and tetrabenzylthiuram disulfide. Examples of xanthogenates are sodium isopropylxanthogenate and zinc isopropylxanthogenate. Examples of aldehyde ammonias are acetaldehyde ammonia and hexamethylenetetramine. Examples of aldehyde amines are n-butylaldehyde aniline and butyraldehyde monobutylamine.
[0055] The crosslinking aid may be an alcohol. Examples of alcohols include monohydric alcohols such as ethanol, dihydric alcohols such as ethylene glycol, trihydric alcohols such as glycerin, and polyols (polyoxyethylene glycols) such as polyethylene glycol and polypropylene glycol. As the alcohol, a polyol is preferably used. In this case, the number-average molecular weight of the polyol is, for example, 200 or more, preferably 300 or more. The number-average molecular weight of the polyol is, for example, 10,000 or less, preferably 5,000 or less.
[0056] These crosslinking aids may be used alone or in combination of two or more kinds.
[0057] When sulfur or a sulfur compound is used as the crosslinking agent, it is desirable to use a thiazole, a thiourea, a dithiocarbamic acid, or a thiuram as the crosslinking aid, from the viewpoint of ensuring a good foam shape and flexibility of the foam 10f.
[0058] When a quinoid compound is used as the crosslinking agent, alcohols, more preferably polyols, are preferably used as the crosslinking aid from the viewpoint of reducing corrosiveness. In particular, when a p-quinonedioxime derivative is used as the quinoid compound, the use of polyethylene glycol is advantageous. When polyethylene glycol is used as the polyol, the rubber composition can be crosslinked well and excellent foamability can be easily ensured.
[0059] The mixing ratio of the cross-linking aid is, for example, 0.01 part by mass or more, preferably 0.02 part by mass or more, and more preferably 0.06 part by mass or more, per 100 parts by mass of rubber. The mixing amount is, for example, 20 parts by mass or less, preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of rubber.
[0060] The rubber composition may contain additives such as lubricants (processing aids), pigments, fillers, flame retardants, and softeners, as needed.
[0061] Examples of lubricants include stearic acid, its esters, stearin-based compounds such as zinc stearate, and paraffin. These lubricants may be used alone, or two or more types of lubricants may be used in combination. The blending ratio of the lubricant is, for example, 0.1 parts by mass or more, and preferably 1 part by mass or more, per 100 parts by mass of rubber. The blending ratio is, for example, 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of rubber.
[0062] An example of the pigment is carbon black. A single pigment may be used, or two or more pigments may be used in combination. The blending ratio of the pigment is, for example, 1 part by mass or more, and preferably 2 parts by mass or more, per 100 parts by mass of rubber. The blending ratio is, for example, 50 parts by mass or less, and preferably 30 parts by mass or less, per 100 parts by mass of rubber.
[0063] The filler may be an inorganic filler, an organic filler, or any other known filler. Examples of inorganic fillers include calcium carbonate, magnesium carbonate, silicic acid and its salts, clay, talc, mica powder, bentonite, silica, alumina, aluminum silicate, and aluminum powder. An example of an organic filler is cork. These fillers may be used alone, or two or more fillers may be used in combination. The compounding ratio of the filler is, for example, 10 parts by mass or more, preferably 30 parts by mass or more, and more preferably 50 parts by mass or more, per 100 parts by mass of rubber. The compounding ratio is, for example, 300 parts by mass or less, preferably 200 parts by mass or less, per 100 parts by mass of rubber.
[0064] Examples of flame retardants include hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide. These flame retardants may be used alone, or two or more types of flame retardants may be used in combination. The blending ratio of the flame retardant is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and more preferably 15 parts by mass or more, per 100 parts by mass of rubber. The blending ratio is, for example, 200 parts by mass or less, preferably 150 parts by mass or less, and more preferably 100 parts by mass or less, per 100 parts by mass of rubber.
[0065] Examples of softeners include petroleum oils, asphalts, low-molecular-weight polymers, organic acid esters, and thickeners. Examples of petroleum oils include paraffinic process oils such as paraffin oil, naphthenic process oils, drying oils or animal and vegetable oils, and aromatic process oils. An example of drying oils or animal and vegetable oils is linseed oil. Examples of organic acid esters include phthalate esters such as di-2-ethylhexyl phthalate (DOP) and dibutyl phthalate (DBP), phosphate esters, higher fatty acid esters, and alkyl sulfonates. Petroleum oils or asphalts are preferably used as softeners, and paraffinic process oils are more preferably used. These softeners may be used alone, or two or more types of softeners may be used in combination. The blending ratio of the softener is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, per 100 parts by mass of rubber. The compounding ratio is, for example, 300 parts by mass or less, and more desirably 200 parts by mass or less, per 100 parts by mass of rubber.
[0066] The rubber composition may contain known additives such as plasticizers, antioxidants, antioxidants, colorants, anti-fungal agents, and non-rubber polymers depending on the purpose and application.
[0067] In the seal member 10, the adhesive layer 10p and the adhesive layer 10q are not limited to any specific layer as long as they contain an adhesive. The adhesive layer 10p and the adhesive layer 10q each contain, for example, a rubber-based polymer. The rubber-based polymer is, for example, a synthetic rubber such as a thermoplastic elastomer or a thermosetting elastomer.
[0068] Examples of thermoplastic elastomers include olefin-based elastomers, styrene-based elastomers, butyl-based elastomers, and vinyl chloride-based elastomers. Examples of olefin-based elastomers include ethylene-propylene rubber (EPM) and ethylene-propylene-diene rubber (EPDM). Examples of styrene-based elastomers include styrene-butadiene rubber (SBR), styrene-butadiene-styrene rubber (SBS), styrene-isoprene-styrene rubber (SIS), styrene-ethylene-butadiene rubber, styrene-ethylene-butylene-styrene rubber (SEBS), styrene-isobutylene-styrene block rubber (SIBS), and styrene-isoprene-propylene-styrene rubber. Examples of butyl-based elastomers include butyl rubber, polyisobutylene rubber, polybutene, polyisoprene rubber, and nitrile butadiene rubber (NBR). Examples of vinyl chloride-based elastomers include chloroprene rubber or chlorosulfonated polyethylene rubber.
[0069] Examples of thermosetting elastomers are silicone rubber, fluororubber, acrylic rubber, and polyamide rubber.
[0070] The rubber-based polymer is preferably a thermoplastic elastomer, more preferably a styrene-based elastomer or a butyl-based elastomer.
[0071] The weight-average molecular weight of the rubber-based polymer is, for example, 30,000 or more, preferably 50,000 or more, and more preferably 100,000 or more. The weight-average molecular weight of the rubber-based polymer is, for example, 5,000,000 or less, preferably 3,000,000 or less, and more preferably 1,000,000 or less. In this case, the main surfaces F1 and F2 formed by the pressure-sensitive adhesive layer 10p and the pressure-sensitive adhesive layer 10q, respectively, tend to have the desired adhesive strength. The weight-average molecular weight is measured using gel permeation chromatography in polystyrene equivalent terms.
[0072] Each of the adhesive layer 10p and the adhesive layer 10q may or may not contain a filler. When each of the adhesive layer 10p and the adhesive layer 10q contains a filler, the tackiness of the sealing material 10 can be easily adjusted to a desired range. The filler material is not limited to a specific material. The filler includes, for example, an inorganic substance. Examples of inorganic substances include calcium carbonate, magnesium carbonate, clay, talc, mica, bentonite, silica, alumina, aluminum silicate, and aluminum.
[0073] When each of the pressure-sensitive adhesive layer 10p and the pressure-sensitive adhesive layer 10q contains a filler, the content of the filler in each pressure-sensitive adhesive layer is not limited to a specific value. For example, the content of the filler in each pressure-sensitive adhesive layer is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and more preferably 20 parts by mass or more, per 100 parts by mass of the rubber-based polymer. The content of the filler is, for example, 300 parts by mass or less, preferably 250 parts by mass or less, and more preferably 200 parts by mass or less, per 100 parts by mass of the rubber-based polymer.
[0074] Each of the pressure-sensitive adhesive layer 10p and the pressure-sensitive adhesive layer 10q preferably further contains a tackifier, which makes it easier for the main surfaces F1 and F2 formed by the pressure-sensitive adhesive layer 10p and the pressure-sensitive adhesive layer 10q, respectively, to have adhesive strength.
[0075] The tackifier is not limited to a specific substance. The tackifier may be, for example, a specific resin. Examples of such resins include rosin-based tackifier resins, terpene-based tackifier resins, hydrocarbon-based tackifier resins, phenol-based tackifier resins, ketone-based tackifier resins, polyamide-based tackifier resins, epoxy-based tackifier resins, and elastomer-based tackifier resins. Examples of rosin-based tackifier resins include unmodified rosin, modified rosin, rosin phenol-based resins, and rosin ester-based resins. Examples of terpene-based tackifier resins include terpene-based resins, terpene-phenol-based resins, styrene-modified terpene-based resins, aromatic-modified terpene-based resins, and hydrogenated terpene-based resins. Examples of hydrocarbon-based tackifier resins include aliphatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic-aromatic petroleum resins, aliphatic-alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone-based resins, and coumarone-indene-based resins. Examples of aromatic hydrocarbon resins include styrene-based resins and xylene-based resins. Examples of phenolic tackifying resins are alkylphenolic resins, xylene formaldehyde resins, resols, and novolacs.The tackifier is preferably an alicyclic cyclic hydrocarbon or aromatic hydrocarbon resin.
[0076] The content of the tackifier in each of the pressure-sensitive adhesive layer 10p and the pressure-sensitive adhesive layer 10q is not limited to a specific value. For example, the content of the tackifier in each pressure-sensitive adhesive layer is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and more preferably 20 parts by mass or more, per 100 parts by mass of the rubber-based polymer. The content of the tackifier is, for example, 200 parts by mass or less, preferably 100 parts by mass or less, and more preferably 80 parts by mass or less, per 100 parts by mass of the rubber-based polymer.
[0077] The thickness of each of the pressure-sensitive adhesive layer 10p and the pressure-sensitive adhesive layer 10q is not limited to a specific value. The thickness is, for example, 50 to 400 μm. The thickness of each of the pressure-sensitive adhesive layer 10p and the pressure-sensitive adhesive layer 10q may be 70 μm or more, or 80 μm or more. The thickness of the adhesive layer 10 may be 300 μm or less, or 250 μm or less.
[0078] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0079] Example 1: Kraton SBS resin D1155 and Arakawa Chemical Industries, Ltd. tackifier Alcon M115 were kneaded at blending ratios of 100 parts by mass and 35 parts by mass, respectively, to obtain a mixture. This mixture was hot-pressed at 150°C and 4 MPa to obtain a 100 μm-thick PSA layer according to Example 1. The styrene content of the SBS resin D1155 was 35% by mass. A laminate was obtained by attaching the PSA layer according to Example 1 to both main surfaces of Nitto Denko Corporation's Foam No. 6800. Foam No. 6800 was an EPDM foam with a closed-cell structure. The laminate was placed in an oven maintained at 140°C and subjected to a pressure of 2 kPa for 5 minutes to bond the PSA layer and foam. The laminate was then cut to a width (w0) of 10 mm to obtain a strip-shaped sealing material according to Example 1. The thickness (t) of the sealing material according to Example 1 was 6 mm, and the length of the sealing material was 350 mm. The end faces at both ends in the length direction of the sealing material according to Example 1 extended perpendicular to the main surface of the sealing material.
[0080] Two acrylic plates each having a thickness of 10 mm were prepared. The sealing material according to Example 1 was arranged in a ring shape on one of the acrylic plates as shown in FIG. 1. At this time, the plates were overlapped so that one end and the other end of the sealing material in the length direction were aligned in a direction perpendicular to the main surface of the sealing material. In addition, the dimension L of the overlapping portion of the one end and the other end of the sealing material in the length direction was OThe distance between the two acrylic plates was adjusted to 50 mm. In this state, the other acrylic plate was placed so that the two acrylic plates faced each other, and a spacer of a predetermined size was placed between the two acrylic plates to adjust the distance between the two acrylic plates. As a result, the sealing material was compressed at a compression rate of 33%. In this manner, the sealing structure of Example 1 was obtained. In this sealing structure, the overlapping portions of one end and the other end of the sealing material in the longitudinal direction were visually inspected, and the width w1 (maximum width) of the sealing material after compression at the overlapping portion was determined. As a result, the width w1 was 17.91 mm. The value of (w1 - w0) / (t * w0) was calculated from the thickness t, width w0, and width w1. The results are shown in Table 1.
[0081] Example 2 The sealing material of Example 2 and the sealing structure of Example 2 using the sealing material of Example 2 were obtained in the same manner as Example 1, except for the following points. The thickness of the foam No. 6800 was adjusted so that the thickness t of the sealing material was 3 mm. In producing the sealing structure, the compression rate of the sealing material was adjusted to 35%. In the sealing structure of Example 2, the width w1 of the sealing member after compression at the overlapping portion was 13.32 mm.
[0082] Example 3 A sealing material according to Example 3 and a sealing structure according to Example 3 using the sealing material according to Example 3 were obtained in the same manner as in Example 1, except for the following points. The thickness of the foam No. 6800 was adjusted so that the thickness t of the sealing material was 3 mm. In producing the sealing structure, the dimension L of the overlapping portion was O The width w1 of the seal member after compression at the overlapping portion was adjusted to 14.40 mm. The compression rate of the seal material was adjusted to 50%. In the seal structure according to Example 3, the width w1 of the seal member after compression at the overlapping portion was adjusted to 14.40 mm.
[0083] Example 4 The sealing material of Example 4 and the sealing structure of Example 4 using the sealing material of Example 4 were obtained in the same manner as in Example 1, except for the following points. The thickness of the foam No. 6800 was adjusted so that the thickness t of the sealing material was 3 mm. In addition, the laminate was cut so that the width w0 of the sealing material was 5 mm. In producing the sealing structure, the dimension L of the overlapping portion was OThe width w1 of the seal member after compression at the overlapping portion was 7.23 mm.
[0084] Example 5 A sealing material according to Example 5 and a sealing structure according to Example 5 using the sealing material according to Example 5 were obtained in the same manner as in Example 1, except for the following points. In the sealing material according to Example 5, as shown in FIG. 5, both end faces in the longitudinal direction of the sealing material were processed to form inclined surfaces that extend inclined relative to the main surface of the sealing material and a plane perpendicular to this main surface. The length of the inclined surface in the longitudinal direction of the sealing material was 15 mm. In producing the sealing structure, the dimension L of the overlapping portion was O The width w1 of the seal member after compression at the overlapping portion was adjusted to 18.87 mm.
[0085] Example 6 A sealing material according to Example 6 and a sealing structure according to Example 6 using the sealing material according to Example 6 were obtained in the same manner as in Example 1, except for the following points. In the sealing material according to Example 6, as shown in FIG. 6 , both end faces in the longitudinal direction of the sealing material were processed to form inclined surfaces that extended at an angle relative to the main surface of the sealing material and a plane perpendicular to the main surface. The length of the inclined surfaces in the longitudinal direction of the sealing material was 15 mm. As shown in FIG. 6 , in fabricating the sealing structure, one end face in the longitudinal direction of the sealing material was treated as one end, and a portion adjacent to the other end face was bent to form the other end. The compression ratio of the sealing material was adjusted to 50%. In the sealing structure according to Example 6, the width w1 of the sealing member after compression at the overlapping portion was 16.84 mm.
[0086] Example 7 A sealing material according to Example 7 and a sealing structure according to Example 7 using the sealing material according to Example 7 were obtained in the same manner as in Example 1, except for the following points. In the sealing material according to Example 7, as shown in FIG. 7 , both end faces in the longitudinal direction of the sealing material were processed to form inclined surfaces that extended at an angle relative to the main surface of the sealing material and a plane perpendicular to the main surface. The length of the inclined surfaces in the longitudinal direction of the sealing material was 15 mm. As shown in FIG. 7 , in fabricating the sealing structure, one end face in the longitudinal direction of the sealing material was treated as one end, and a portion adjacent to the other end face was bent to form the other end. The compression ratio of the sealing material was adjusted to 50%. In the sealing structure according to Example 7, the width w1 of the sealing member after compression at the overlapping portion was 17.87 mm.
[0087] Example 8 A sealing material according to Example 8 and a sealing structure according to Example 8 using the sealing material according to Example 8 were obtained in the same manner as in Example 1, except for the following points. The thickness t of the sealing material according to Example 8 was 5 mm. As shown in FIG. 8 , one end and the other end of the sealing material in the longitudinal direction were perpendicularly intersected, and the compression ratio of the sealing material was adjusted to 60%, forming an overlapping portion. A portion of the sealing material including one end in the longitudinal direction and a portion of the sealing material including the other end in the longitudinal direction protruded from the overlapping portion. The width w1 of the sealing member after compression at the overlapping portion was 13.35 mm.
[0088] Example 9 A seal structure according to Example 9 was obtained in the same manner as in Example 8, except that the compression rate of the seal material was changed to 40%. In the seal structure according to Example 9, the width w1 of the seal material after compression at the overlapping portion was 12.86 mm.
[0089] Example 10 A seal structure according to Example 10 was obtained in the same manner as in Example 8, except that the compression rate of the seal material was changed to 20%. In the seal structure according to Example 10, the width w1 of the seal material after compression at the overlapping portion was 12.68 mm.
[0090] Comparative Example 1 A seal structure according to Comparative Example 1 was obtained in the same manner as in Example 1, except for the following points: O The width w1 of the seal member after compression at the overlapping portion was 19.62 mm.
[0091] Comparative Example 2 A sealing material according to Comparative Example 2 and a sealing structure according to Comparative Example 2 using the sealing material according to Comparative Example 2 were obtained in the same manner as in Example 1, except for the following points. The thickness of the foam No. 6800 was adjusted so that the thickness t of the sealing material was 3 mm. In producing the sealing structure, the dimension L of the overlapping portion was O The width w1 of the sealing member after compression at the overlapping portion was adjusted to 15.65 mm.
[0092] Comparative Example 3 A sealing material according to Comparative Example 3 and a sealing structure according to Comparative Example 3 using the sealing material according to Comparative Example 3 were obtained in the same manner as in Example 1, except for the following points. The thickness of the foam No. 6800 was adjusted so that the thickness t of the sealing material was 3 mm. In producing the sealing structure, the dimension L of the overlapping portion was O The width w1 of the seal member after compression at the overlapping portion was 14.81 mm.
[0093] Comparative Example 4 A sealing material according to Comparative Example 4 and a sealing structure according to Comparative Example 4 using the sealing material according to Comparative Example 4 were obtained in the same manner as in Example 1, except for the following points. The laminate was cut so that the width w0 of the sealing material was 5 mm. In producing the sealing structure, the dimension L of the overlapping portion was O The width w1 of the sealing member after compression at the overlapping portion was adjusted to 17.11 mm.
[0094] Comparative Example 5 A seal structure according to Comparative Example 5 was obtained in the same manner as in Example 1, except for the following points: O The width w1 of the sealing member after compression at the overlapping portion was adjusted to 19.89 mm.
[0095] Comparative Example 6 A sealing material according to Comparative Example 6 and a sealing structure according to Comparative Example 6 using the sealing material according to Comparative Example 6 were obtained in the same manner as in Example 1, except for the following points. The laminate was cut so that the thickness t of the sealing material was 3 mm and the width w0 of the sealing material was 5 mm. In producing the sealing structure, the dimension L of the overlapping portion was O The width w1 of the sealing member after compression at the overlapping portion was adjusted to 9.66 mm.
[0096] (Evaluation of Watertightness) The sealing structures according to each Example and Comparative Example were submerged in a water tank filled with water up to a height of 1 meter, and after 30 minutes had passed, the sealing structures were removed from the water tank and checked for water leakage into the space surrounded by the sealing material to determine whether they conformed to the IPX7 standard. If there was no water leakage, it could be evaluated as conforming to the IPX7 standard. As a result, the sealing structures according to each Example were evaluated as conforming to the IPX7 standard. On the other hand, water leakage was confirmed in the sealing structures according to each Comparative Example, and they were evaluated as not conforming to the IPX7 standard.
[0097] When comparing the evaluation results of the watertightness of the sealing structures of each example with the evaluation results of the watertightness of the sealing structures of each comparative example, it can be understood that high watertightness can be achieved when the conditions of the above formula (1) are satisfied.
[0098]
[0099] A first aspect of the present invention includes a method of sealing a space surrounded by a strip-shaped sealing material, the strip-shaped sealing material having a pressure-sensitive adhesive layer and a foam that form one main surface, with one end and the other end overlapping each other so that the one end and the other end are aligned in a direction perpendicular to the main surface, and compressing the sealing material in a direction perpendicular to the main surface, thereby sealing a space surrounded by the sealing material in a waterproof manner, wherein (w1-w0) / (t*w0)≦0.15 mm -1 The following condition is satisfied: w1 is the width of the sealing material after compression at the overlapping portion of the one end and the other end; w0 is the width of the sealing material before compression; and t is the thickness of the sealing material before compression.
[0100] A second aspect of the present invention provides the sealing method according to the first aspect, wherein the compressibility of the sealing material is 15% or more.
[0101] A third aspect of the present invention provides the sealing method according to the first or second aspect, wherein a dimension of the overlapping portion in the length direction of the sealing material is 5 mm or more.
[0102] A fourth aspect of the present invention provides a strip-shaped sealing material having a foam and an adhesive layer forming one main surface, wherein one end and the other end in the length direction of the sealing material are overlapped so that the one end and the other end are aligned in a direction perpendicular to the main surface, the sealing material is compressed in the direction perpendicular to the main surface, and a space surrounded by the sealing material is sealed in a waterproof manner, and (w1-w0) / (t*w0)≦0.15 mm -1 The following condition is satisfied: w1 is the width of the sealing material after compression at the overlapping portion of the one end and the other end; w0 is the width of the sealing material before compression; and t is the thickness of the sealing material before compression.
[0103] A fifth aspect of the present invention is a strip-shaped sealing material comprising: an adhesive layer forming one main surface; and a foam, wherein when one end and the other end in the length direction of the sealing material are overlapped so that the one end and the other end are aligned in a direction perpendicular to the main surface, and the sealing material is compressed in a direction perpendicular to the main surface to seal a space surrounded by the sealing material in a waterproof manner, (w1-w0) / (t*w0)≦0.15 mm. -1 The present invention provides a sealing material that can satisfy the following condition, wherein: w1 is the width of the sealing material after compression at the overlapping portion of the one end and the other end; w0 is the width of the sealing material before compression; and t is the thickness of the sealing material before compression.
Claims
1. A method for sealing a space surrounded by a band-shaped sealing material having a pressure-sensitive adhesive layer and a foam body on one of its main surfaces, the method comprising: compressing the sealing material in a direction perpendicular to the main surface while overlapping one end and the other end in the length direction of the band-shaped sealing material so that the one end and the other end are aligned in a direction perpendicular to the main surface; and sealing the space surrounded by the sealing material in a waterproof manner; (w 1 -w 0 ) / (t*w 0 )≦0.15mm -1 The condition is satisfied, and in the above condition, w 1 is the width of the compressed sealing material at the overlapping portion of the one end and the other end, and w 0 is the width of the seal before compression; and t is the thickness of the seal before compression.
2. The sealing method according to claim 1, wherein the compressibility of the sealing material is 15% or more.
3. The sealing method according to claim 1, wherein the dimension of the overlapping portion in the longitudinal direction of the sealing material is 5 mm or more.
4. A band-shaped sealing material having an adhesive layer and a foam that forms one of the main surfaces, one end and the other end in the length direction of the sealing material are overlapped so that the one end and the other end are aligned in a direction perpendicular to the main surface, the sealing material is compressed in the direction perpendicular to the main surface, and a space surrounded by the sealing material is sealed in a waterproof manner, (w 1 -w 0 ) / (t*w 0 )≦0.15mm -1 The condition is satisfied, and in the above condition, w 1 is the width of the compressed sealing material at the overlapping portion of the one end and the other end, and w 0 is the width of the seal before compression; and t is the thickness of the seal before compression.
5. A band-shaped sealing material comprising an adhesive layer forming one of the main surfaces and a foam, wherein the sealing material is compressed in a direction perpendicular to the main surface in a state where one end and the other end in the length direction of the sealing material are overlapped so that the one end and the other end are aligned in a direction perpendicular to the main surface, and a space surrounded by the sealing material is sealed in a waterproof manner, (w 1 -w 0 ) / (t*w 0 )≦0.15mm -1 In the above condition, w 1 is the width of the compressed sealing material at the overlapping portion of the one end and the other end, and w 0 is the width of the seal before compression; and t is the thickness of the seal before compression.
Citation Information
Patent Citations
JP1982075262U
Sealing material and sealing technique for automobile parts
JP1996198033A
Annular seal and seal member
JP2004245271A
Multi-part housing seal, method for the automated application of a multi-part housing seal, and housing comprising a multi-part housing seal
US20230041058A1