METHOD FOR PRODUCING L10-TYPE FeNi ORDERED ALLOY

The proposed method for manufacturing FeNi ordered alloys, involving a molding process and subsequent nitriding and denitrification steps, addresses the issue of reverse reactions and lattice structure irregularity, resulting in improved magnetic properties by reducing hydrogen contact and promoting a regular lattice.

WO2024219327A1PCT designated stage expired Publication Date: 2024-10-24NICHIA CORP +1
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014806
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-04-12
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing nitriding and denitrifying method for manufacturing FeNi ordered alloys often results in insufficient nitridation, leading to a reverse reaction with hydrogen, which hinders the formation of a regular lattice structure and deteriorates magnetic properties.

Method used

A method involving a molding process to reduce the specific surface area of the FeNi alloy, followed by nitriding and denitrification steps, including a re-nitriding and pulverization process to suppress the reverse reaction and enhance magnetic properties.

Benefits of technology

This method effectively produces FeNi ordered alloys with improved magnetic properties by reducing the contact area with hydrogen and promoting a regular lattice structure, resulting in enhanced magnetic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014806_24102024_PF_FP_ABST
    Figure JP2024014806_24102024_PF_FP_ABST
Patent Text Reader

Abstract

To provide a more efficient production method for obtaining an L10-type FeNi ordered alloy having excellent magnetic characteristics. The present invention relates to a method for producing an L10-type FeNi ordered alloy, the method including: a molding step for obtaining a molded article by molding a FeNi alloy; a nitriding step for nitriding the molded article to obtain a nitride; and a denitrification step for subjecting the nitride to a denitrification treatment to obtain an L10-type FeNi ordered alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing L10 type FeNi ordered alloy

[0001] The present invention is 0 L1 having a regular structure of type 0 The present invention relates to a method for producing an FeNi (iron-nickel) ordered alloy (hereinafter also referred to as an FeNi superlattice).

[0002] FeNi superlattices are expected to be used as magnetic materials with high heat resistance and as magnetic device materials for magnetic recording, etc. For example, Patent Document 1 discloses an FeNi superlattice with a high L1 order of 0.5 or more. 0 A method for producing an FeNi ordered alloy of this type is disclosed. In the disclosed method, an FeNi alloy is nitrided by a nitriding treatment to obtain a nitride, and then nitrogen is removed from the nitride by a denitriding treatment to produce an FeNi superlattice by a nitriding-denitriding method.

[0003] Patent No. 6332359

[0004] In the nitriding and denitriding method disclosed in Patent Document 1, a reverse reaction occurs between the generated nitride FeNiN and the hydrogen generated at the same time, and a part of the FeNiN is converted into Fe. 2 Ni 2 It has been newly discovered that such insufficiently nitrided nitrides are converted to N. When such nitrides are denitrified, it becomes difficult to form an ordered lattice, resulting in a problem of reduced magnetic properties.

[0005] The present invention provides an L1 magnetic material with excellent magnetic properties. 0 The present invention aims to provide a more efficient manufacturing method for obtaining an ordered FeNi alloy of this type.

[0006] A method for producing an FeNi ordered alloy according to one embodiment of the present disclosure includes a forming step of forming an FeNi alloy to obtain a formed product, a nitriding step of nitriding the formed product to obtain a nitride, and a denitriding step of denitriding the nitride to obtain an L1 0 L1 including a denitrification step to obtain an FeNi ordered alloy of the type 0 This invention relates to a method for producing an ordered FeNi alloy of this type.

[0007] According to the present disclosure, L1 0 It is possible to provide a more efficient manufacturing method for obtaining an ordered FeNi alloy of this type.

[0008] 1 is a flowchart of a method for producing an FeNi ordered alloy according to one embodiment of the present disclosure; 2 is a flowchart of a method for producing an FeNi ordered alloy including a pulverization step according to one embodiment of the present disclosure; 3 is a flowchart of a method for producing an FeNi ordered alloy including a pulverization step and a re-nitriding step according to one embodiment of the present disclosure. 0 FIG. 1 is a schematic diagram showing the lattice structure of an FeNi ordered structure of the type.

[0009] Hereinafter, embodiments of the present invention will be described in detail. However, the embodiments described below are examples for embodying the technical concept of the present invention, and the present invention is not limited to the following. Furthermore, numerical ranges indicated using "to" indicate ranges that include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. Furthermore, in the following embodiments, parts that are identical or equivalent to each other will be described using the same reference numerals.

[0010] L1 in this embodiment 0 The method for producing the FeNi ordered alloy of the type includes a forming step of forming the FeNi alloy to obtain a formed product, a nitriding step of nitriding the formed product to obtain a nitride, and a denitriding step of denitriding the nitride to obtain an L1 0 1A shows the L1 process of this embodiment, which includes a forming step S1, a nitriding step S2, and a denitriding step S5. 0 1B is a flowchart of a method for manufacturing an FeNi ordered alloy of the present embodiment, including a forming step S1, a nitriding step S2, a crushing step S3, and a denitriding step S5. 0 1C is a flowchart of a method for manufacturing an FeNi ordered alloy of the present embodiment, including a forming step S1, a nitriding step S2, a crushing step S3, a re-nitriding step S4, and a denitriding step S5. 0 1 is a flowchart of a method for producing an FeNi ordered alloy of the type.

[0011] The nitriding / denitriding method used in this embodiment includes a nitriding step S2 in which the FeNi alloy is nitrided by nitriding treatment, and a denitriding step S5 in which nitrogen is desorbed from the nitride by denitriding treatment, thereby obtaining L1 0In the nitriding step S2, FeNi is converted into Fe as shown in the following reaction formula: 2 Ni 2 The nitride FeNiN is produced in two steps via N: FeNi + 1 / 2NH 3 → Fe 2 Ni 2 N + 3 / 4H 2 Fe 2 Ni 2 N + 1 / 2NH 3 → FeNiN + 3 / 4H 2

[0012] In the second nitriding reaction, a reverse reaction occurs between the produced FeNiN and hydrogen, and part of the FeNiN is converted to Fe 2 Ni 2 N. An ideal ordered alloy is one with an order degree of 1, L1 0 The ordered FeNi alloy of this type can be produced by denitrifying FeNiN, which has an ordered structure in which Fe layers and Ni layers are alternately arranged, as shown in Figure 2. On the other hand, FeNiN, which is insufficiently nitrided, 2 Ni 2 In the case of NiN, the FeNi alloy does not have a regular structure in which Fe and Ni layers are alternately arranged, and even after denitrification, it does not become an FeNi ordered alloy with regular alignment. In this embodiment, the specific surface area of ​​the FeNi alloy is reduced by molding the FeNi alloy before the nitriding step S2. As a result, the contact area with hydrogen is reduced in the nitriding step S2, suppressing the reverse reaction between the generated FeNiN and hydrogen, and achieving high magnetic properties.

[0013] <Forming Step S1> In the forming step S1, the FeNi alloy is formed into a formed product. The forming method is not particularly limited, and examples thereof include hand pressing and rolling with a roller compactor.

[0014] The average particle size of the FeNi alloy used in the forming step S1 can be, for example, 10 nm or more, preferably 50 nm or more, and more preferably 100 nm or more. The upper limit of the average particle size can be, for example, 5000 nm or less, preferably 1000 nm or less, and more preferably 500 nm or less. The average particle size can be measured from a scanning electron microscope (SEM) image.

[0015] On the other hand, the molded product of the FeNi alloy may have a smaller specific surface area than the FeNi alloy before molding. For example, the molded product of the FeNi alloy may be formed into a bulk body by molding and have a larger volume than the FeNi alloy powder before molding. The molded product of the FeNi alloy may have a general shape such as a sphere, a disk, a cone, a cylinder, a rectangular parallelepiped, or a polyhedron. For example, the molded product of the FeNi alloy may be spherical, or may have a slight unevenness on the surface, and in the case of a disk, at least a part of the surface forming the disk may be elliptical. From the viewpoint of being able to reduce the specific surface area and promoting nitriding, a shape that reduces the specific surface area is preferred, and a general shape such as a sphere, disk, rectangular parallelepiped, or polyhedron is preferable to a cylindrical shape.

[0016] As described above, the FeNi alloy molded product only needs to have a smaller specific surface area than the FeNi alloy before molding. However, if the shape of the FeNi alloy molded product is, for example, a rectangular parallelepiped, it can be considered to have a major axis, a minor axis shorter than the major axis, and a height axis shorter than the minor axis. In this case, the major axis length may be 1 μm or more and 1 m or less, preferably 10 μm or more and 100 cm or less, more preferably 50 μm or more and 50 cm or less, even more preferably 100 μm or more and 10 cm or less, and particularly preferably 500 μm or more and 5 cm or less. The minor axis length may be 0.5 μm or more and 1 m or less, preferably 5 μm or more and 50 cm or less, more preferably 20 μm or more and 50 cm or less, even more preferably 50 μm or more and 20 cm or less, and particularly preferably 200 μm or more and 5 cm or less. The height axis is shorter than the minor axis, preferably 5 μm or more and 5 cm or less, and even more preferably 50 μm or more and 1 cm or less. When the major axis length, minor axis length, and height axis are within the above ranges, the product has a constant specific surface area, which reduces the reverse reaction caused by molding, and has a constant volume, which promotes nitriding. If the shape of the molded product is cylindrical, a circle with the same major axis length and minor axis length can be considered to have the height axis. If the shape is spherical or polyhedral, it is difficult to uniquely determine the major axis length, minor axis length, and height axis, but it is preferable that the shape has a surface area and volume close to the above-mentioned shape.

[0017] The FeNi alloy used in the forming step S1 may have a disordered structure. The disordered structure here may be one in which the atomic arrangement is random and does not have regularity, or one in which the L1 0 It is also possible that no peaks of the ordered structure of the type are observed.

[0018] The ratio of the number of moles of Fe to the total number of moles of Fe and Ni in the FeNi used in the molding step S1 may be 0.4 or more and 0.6 or less, preferably 0.45 or more and 0.55 or less, and more preferably 0.48 or more and 0.52 or less.

[0019] The FeNi alloy used in the forming step S1 can be produced, for example, by reducing FeNi oxide.

[0020] [Reduction Step] The reduction method in the reduction step is not particularly limited, and examples include a method in which FeNi oxide is heat-treated in a reducing gas atmosphere. The flow rate of the reducing gas can be 0.1 L / min to 15.0 L / min, preferably 0.5 to 10.0 L / min, per 8.5 g of FeNi oxide. The heat treatment temperature can be, for example, 300°C to 700°C, preferably 450°C to 700°C. The heat treatment time can be, for example, 0.5 hours to 10 hours, preferably 1.0 hours to 5 hours. Examples of reducing gases include hydrogen and carbon monoxide, with hydrogen being preferred in terms of reducibility.

[0021] The ratio of the number of moles of Fe to the total number of moles of Fe and Ni in the FeNi oxide may be 0.4 or more and 0.6 or less, preferably 0.45 or more and 0.55 or less, and more preferably 0.48 or more and 0.52 or less.

[0022] The FeNi oxide used in the reduction step may contain Fe oxide or Ni oxide, or may contain an oxide containing Fe and Ni, where an oxide containing Fe and Ni means that a single oxide particle contains Fe element and Ni element.

[0023] The Fe oxide is not particularly limited, but may be FeO, Fe 2 O 3 , Fe 3 O 4 Other examples include oxides obtained by oxidizing raw materials such as iron metal, iron hydroxide, iron carbonate, iron chloride, iron iodide, iron bromide, iron sulfate, iron nitrate, iron phosphate, and iron oxalate.

[0024] The Ni oxide is not particularly limited, but examples thereof include NiO, and also include oxides obtained by oxidizing raw materials such as nickel metal, nickel hydroxide, nickel carbonate, nickel chloride, nickel iodide, nickel bromide, nickel sulfate, nickel nitrate, nickel phosphate, and nickel oxalate.

[0025] The oxide containing Fe and Ni used in the reduction step can be produced by a step of mixing a solution containing Fe and Ni with a precipitant to obtain a precipitate containing Fe and Ni (precipitation step), and a step of heat-treating the precipitate to obtain an oxide containing Fe and Ni (oxidation step). This method makes it easy to control the average particle size and particle size distribution of the obtained oxide containing Fe and Ni, and also makes it easy to achieve a uniform distribution of Fe and Ni elements in the oxide containing Fe and Ni.

[0026] [Precipitation Step] In the precipitation step, an Fe raw material and an Ni raw material are dissolved in a strongly acidic solution to prepare a solution containing Fe and Ni.

[0027] The Fe raw material and the Ni raw material are not limited as long as they can be dissolved in an acidic solution. Examples of the Fe raw material include iron metal, iron oxide, iron hydroxide, iron carbonate, iron chloride, iron iodide, iron sulfate, iron nitrate, iron phosphate, and iron oxalate, among which iron metal, iron carbonate, iron sulfate, and iron chloride are preferred. Examples of the Ni raw material include nickel metal, nickel oxide, nickel hydroxide, nickel carbonate, nickel chloride, nickel iodide, nickel sulfate, nickel nitrate, nickel phosphate, and nickel oxalate, among which nickel metal, nickel carbonate, nickel sulfate, and nickel chloride are preferred. Examples of the acidic solution include sulfuric acid, nitric acid, hydrochloric acid, and phosphoric acid. The concentration of the solution containing Fe and Ni can be appropriately adjusted within a range in which the Fe raw material and the Ni raw material are substantially soluble in the acidic solution.

[0028] The ratio of the number of moles of Fe to the total number of moles of Fe and Ni in the solution containing Fe and Ni may be 0.4 or more and 0.6 or less, preferably 0.45 to 0.55, and more preferably 0.48 to 0.52.

[0029] A precipitate containing Fe and Ni is obtained by reacting a solution containing Fe and Ni with a precipitant. The reaction between the solution containing Fe and Ni and the precipitant may be carried out by adding the precipitant to the solution containing Fe and Ni, or by adding the solution containing Fe and Ni to the precipitant. The solution containing Fe and Ni referred to here may be any solution containing Fe and Ni upon reaction with the precipitant. Alternatively, the raw materials containing Fe and Ni may be prepared as separate solutions, and each solution may be added to react with the precipitant. Even when prepared as separate solutions, the concentrations of the raw materials are appropriately adjusted so that each raw material is substantially soluble in the acidic solution. The precipitant is not limited as long as it reacts with the solution containing Fe and Ni to produce a precipitate, and examples of the precipitant include oxalic acid and alkaline solutions such as sodium hydroxide aqueous solution, sodium bicarbonate aqueous solution, potassium hydroxide aqueous solution, and lithium hydroxide aqueous solution. A precipitate can also be obtained by blowing carbon dioxide gas into the solution containing Fe and Ni. Examples of precipitates that can be produced include oxalates, carbonates, and hydroxides.

[0030] The precipitation step may include a step of separating and washing the precipitate. For example, methods for separating the precipitate include adding a solvent (preferably water) to the obtained precipitate and mixing it, followed by filtration, decantation, or the like. Furthermore, the separated precipitate can be washed by repeating the same process.

[0031] After separating the precipitate, it is preferable to remove the solvent from the separated material in order to prevent the precipitate from redissolving in the remaining solvent during the heat treatment in the subsequent oxidation step and from aggregating when the solvent evaporates. Specific examples of the method for removing the solvent include, for example, drying in an oven at 70°C or higher and 200°C or lower for 5 hours to 12 hours. After drying, particle size adjustment may be performed by crushing or pulverization, if necessary.

[0032] [Oxidation Step] The oxidation step is a step of obtaining an oxide containing Fe and Ni by heat-treating the precipitate containing Fe and Ni obtained in the precipitation step. In the oxidation step, the precipitate can be converted into an oxide by, for example, heat treatment. When the precipitate is heat-treated, it must be performed in the presence of oxygen, and can be performed in an air atmosphere, for example. Furthermore, since it must be performed in the presence of oxygen, it is preferable that the non-metallic part of the precipitate contains oxygen atoms. Furthermore, when a precipitate containing Fe and Ni is used in the oxidation step, FeNi oxide is obtained. Furthermore, the particle size of the obtained FeNi oxide may be adjusted by crushing or pulverization, as necessary.

[0033] The heat treatment temperature in the oxidation step (hereinafter referred to as the oxidation temperature) is not particularly limited, but can be, for example, 200° C. or higher and 800° C. or lower, and preferably 350 to 450° C. The heat treatment time can be, for example, 4 hours or higher and 24 hours or lower, and preferably 4 hours or higher and 12 hours or lower.

[0034] The oxide particles obtained are oxide particles in which Fe and Ni are thoroughly mixed microscopically within the oxide particles, and which reflect the shape, particle size distribution, etc. of the precipitates.

[0035] <Nitriding Step S2> In the nitriding step S2, the FeNi molded product obtained in the molding step S1 is nitrided to obtain a nitride containing Fe and Ni (hereinafter referred to as the nitride). The nitriding method is not particularly limited as long as it can produce a nitride from the FeNi alloy. Examples of the nitriding method include gas nitriding using ammonia gas or nitrogen, plasma nitriding, and nitriding using a metal amide, which involves contacting the FeNi alloy with a nitrogen-containing compound. Specifically, the nitriding is performed by heat-treating pre-prepared FeNi under a flow of a nitrogen-containing compound such as ammonia gas. The flow rate of the nitrogen-containing compound can be 0.1 L / min to 10 L / min per gram of FeNi, preferably 0.5 to 5 L / min. The heat treatment temperature can be, for example, 300°C to 500°C, preferably 310 to 475°C, and more preferably 330 to 450°C. The heat treatment time can be, for example, 5 to 50 hours, preferably 10 to 20 hours.

[0036] The nitrides obtained in the nitriding step S2 include FeNiN, Fe 2 Ni 2 N, etc., and L1 0 In order to obtain an ordered FeNi alloy of this type, it is preferable that the proportion of FeNiN is large. FeNiN has a crystal structure as shown in FIG. 2 and can be identified from the XRD diffraction pattern. 2 Ni 2 The proportion of FeNi nitrides such as N can be 90 mass% or more of the total. The proportion of FeNiN in the nitrides can be 50 mass% or more, preferably 80 mass% or more. The proportion of nitrides and the proportion of FeNiN after the nitriding step S2 can be calculated by analyzing the XRD diffraction pattern using the reference intensity ratio (RIR) method.

[0037] The nitrogen content of the nitride obtained by nitriding may be 9.5% by mass or more and 11.5% by mass or less, preferably 9.6% by mass or more and 11.3% by mass or less, and more preferably 9.8% by mass or more and 11.2% by mass or less. When nitriding is accelerated and the nitride contains only FeNiN, the nitrogen content of the nitride is approximately 10.9%, and it is considered that the closer to this value the more nitriding has progressed. Furthermore, the nitrogen content of the nitride can be measured by an inert gas fusion-thermal conductivity method. This inert gas fusion-thermal conductivity method includes an error of less than 0.3% by mass.

[0038] <Denitriding step S5> In the denitriding step S5, the FeNi nitride obtained in the above-mentioned nitriding step S2 is denitrified to obtain L1 0A FeNi ordered alloy of this type is obtained. Specifically, the FeNi nitride obtained in the nitriding step S2 can be denitrified by heat treating it in a hydrogen atmosphere. The flow rate of hydrogen in the denitrification treatment can be set to 0.01 L / min or more and 10 L / min or less, and preferably 0.1 L / min or more and 5 L / min or less, per gram of FeNi nitride. The heat treatment temperature can be set to, for example, 100°C or more and 450°C or less. The lower limit of the heat treatment temperature is preferably 200°C or more, and more preferably 220°C or more. The upper limit of the heat treatment temperature is preferably 400°C or less, and more preferably 350°C or less. The heat treatment time can be set to, for example, 1 hour or more and 24 hours or less, and preferably 4 to 18 hours.

[0039] L1 0 When the FeNi ordered alloy contains sulfur, the sulfur content is preferably 2.0 mass% or less, more preferably 1.5 mass% or less. The lower limit of the sulfur content may be 0.01 mass%, and preferably 0.03 mass% or more.

[0040] <<Pulverization Step S3>> After the nitriding step S2, it is preferable to include a pulverization step S3 in which the nitride is pulverized to obtain pulverized nitride. A flowchart of this embodiment is shown in FIG. 1B. The pulverization step S3 is a step in which the nitride polycrystalline body is pulverized to approximate single-domain particles. The pulverization method is not particularly limited, and examples thereof include a planetary mill, a jet mill, a ball mill, a roller mill, and a pin mill.

[0041] When a planetary mill is used as the pulverization method, the diameter of the beads used can be 0.1 mm to 3 mm, preferably 0.3 mm to 1 mm. The rotation speed can be, for example, 10 rpm to 30,000 rpm, 30 rpm to 10,000 rpm, or 100 rpm to 5,000 rpm. The pulverization time can be 5 minutes to 180 minutes, preferably 15 minutes to 60 minutes.

[0042] <<Re-nitriding Step S4>> After the pulverizing step S3, it is preferable to include a re-nitriding step S4 in which the pulverized nitride is re-nitrided to obtain a re-nitrided nitride. A flowchart of this embodiment is shown in FIG. 1C. Pulverizing may reduce the proportion of the ordered structure, resulting in a decrease in magnetic properties, but the re-nitriding step S4 increases the proportion of the ordered structure again, thereby suppressing the decrease in magnetic properties. The re-nitriding step S4 can be performed in the same manner as the nitriding step S2.

[0043] The nitrogen content in the re-nitrided nitride is not particularly limited, but may be 10.2 mass % or more and 11.5 mass % or less, and preferably 10.8 mass % or more and 11.2 mass % or less.

[0044] L1 obtained by the manufacturing method of this embodiment 0 The ordered FeNi alloy of the L1 type 0 It has a regular structure of the type L1 0 The ordered alloy of this type means that the degree of order is 0.1 or more, preferably 0.5 or more. The upper limit of the degree of order may be 1 or less. The degree of order S here indicates the degree of ordering in the FeNi superlattice. 0 The ordered structure of the type is based on a face-centered cubic lattice and has a lattice structure as shown in Figure 2. In this figure, the uppermost layer in the stacked structure of the (001) plane of the face-centered cubic lattice is the I site, and the intermediate layer located between the uppermost layer and the lowermost layer is the II site. In this case, if the proportion of metal A present in the I site is x and the proportion of metal B present is 1-x, the proportion of metal A and metal B present in the I site is expressed as AxB1-x. Similarly, if the proportion of metal B present in the II site is x and the proportion of metal A present is 1-x, the proportion of metal A and metal B present in the II site is expressed as A1-xBx. Note that x satisfies 0.5≦x≦1. In this case, the degree of order S is defined as S=2x-1.

[0045] L1 0 The ordered FeNi alloy of L1 0When the particles have a regular structure, the lower limit of the average particle size can be, for example, 10 nm or more, preferably 50 nm or more, and more preferably 100 nm or more. The upper limit of the average particle size can be, for example, 5,000 nm or less, preferably 1,000 nm or less, and more preferably 500 nm or less. The average particle size can be measured from a scanning electron microscope (SEM) image.

[0046] L1 0 The FeNi ordered alloy of this type may be composed of secondary particles formed by aggregation of primary particles, and in this case, the lower limit of the average particle size of the primary particles may be, for example, 10 nm or more, preferably 30 nm or more, and more preferably 50 nm or more. The upper limit of the average particle size of the primary particles may be, for example, 1000 nm or less, and preferably 500 nm or less. The average particle size of the primary particles can be calculated by analyzing the XRD pattern using the Williamson-Hall method.

[0047] L1 0 The ratio of the number of moles of Fe to the total number of moles of Fe and Ni in the FeNi ordered alloy of this type may be 0.4 to 0.6, preferably 0.45 to 0.55, and more preferably 0.48 to 0.52. The number of moles of Fe and Ni can be measured by inductively coupled plasma (ICP) emission spectroscopy or energy dispersive X-ray spectroscopy (EDS) using an electron microscope.

[0048] The present disclosure will be explained in more detail with reference to the following examples, but the present disclosure is not limited to these examples in any way.

[0049] Preparation Example 1 An oxalate containing Fe, Ni and S, with a molar ratio of iron to nickel of 1:1, was obtained by a coprecipitation process using a sulfate.

[0050] [Oxidation Step] 50 g of the obtained oxalate containing Fe, Ni, and S was heat-treated in air at 400° C. for 8 hours. After cooling, an oxide containing Fe, Ni, and S was obtained.

[0051] [Reduction step] 8.5 g of an oxide containing Fe, Ni, and S was heat-treated at 450°C for 1.5 hours in a hydrogen gas atmosphere (hydrogen flow rate 1 L / min). After cooling, an FeNi alloy containing S was obtained. The sulfur content in the alloy was 0.03 mass%. The sulfur content was measured by dissolving the alloy in hydrochloric acid using an ICP-AES method (apparatus name: Optima 8300), and was defined as the weight ratio of S to the total weight of Fe, Ni, and S.

[0052] Example 1 <Forming step S1> A forming die having a cavity of 2 cm in diameter and 4 cm in height and fitted with a lower punch was filled with 2 g of the FeNi alloy obtained in Production Example 1. Thereafter, an upper punch was fitted, and the die was pressed with a hydraulic press at 1 ton / cm. 2 The mixture was compressed at a pressure of 0.15 for 1 minute to obtain a disk-shaped molded product weighing 2 g, having a diameter of 2 cm and a thickness of 2 mm.

[0053] <Nitriding step S2> 2 g of the molded product obtained in the molding step S1 was heat-treated in an ammonia gas atmosphere (ammonia flow rate 1 L / min) at 415°C for 60 hours to obtain a nitride. The nitrogen content in the nitride was 10.9 mass%.

[0054] <<Pulverization step S3>> 1 g of the nitride obtained in the nitriding step S2 and 60 g of stainless steel balls with a diameter of 1 mm were filled into a high-hardness stainless steel container, and pulverization treatment was carried out using a planetary ball mill at 600 rpm for 30 minutes to obtain a pulverized nitride.

[0055] <<Re-nitriding Step S4>> The pulverized nitride obtained in the pulverization step S3 was subjected to a heat treatment at 400° C. for 10 hours in an ammonia gas atmosphere (ammonia flow rate 1 liter / min), to obtain a re-nitrided nitride.

[0056] <Denitriding step S5> The nitride obtained in the re-nitriding step S4 is heat-treated at 250°C for 15 hours in a hydrogen gas atmosphere (hydrogen flow rate 1 liter / min) to form L1 0 An ordered FeNi alloy of the L1 type was obtained. 0The sulfur content in the ordered alloy of this type was 0.03 mass%. It was confirmed that the sulfur content was approximately the same as that of the S-containing FeNi alloy obtained in the reduction step. The sulfur content was measured by dissolving the obtained FeNi alloy in hydrochloric acid and using ICP-AES, and was expressed as the weight ratio of S to the total weight of Fe, Ni, and S.

[0057] Example 2 The same procedure as in Example 1 was carried out except that the pulverization step S3 and the re-nitriding step S4 were not carried out. 0 An ordered FeNi alloy of this type was obtained.

[0058] Example 3 The same procedure as in Example 1 was carried out except that the re-nitriding step S4 was not carried out and the denitriding step S5 was carried out at 200°C for 5 hours. 0 An ordered FeNi alloy of this type was obtained.

[0059] Example 4 The same procedure as in Example 1 was carried out except that the pulverization step S3 was carried out at 600 rpm for 60 minutes and the denitrification step S5 was carried out at 250°C for 5 hours. 0 An ordered FeNi alloy of this type was obtained.

[0060] Example 5 The same procedure as in Example 1 was carried out except that the pulverization step S3 was carried out at 600 rpm for 5 minutes. 0 An ordered FeNi alloy of this type was obtained.

[0061] Example 6 The same procedure as in Example 1 was carried out except that the pulverization step S3 was carried out at 600 rpm for 15 minutes, the re-nitriding step S4 was carried out at 400 ° C for 3 hours, and the denitriding step S5 was carried out at 250 ° C for 5 hours. 0 An ordered FeNi alloy of this type was obtained.

[0062] Comparative Example 1 The same procedure as in Example 1 was carried out except that the molding step S1, the crushing step S3, and the re-nitriding step S4 were not carried out. 0 An ordered FeNi alloy of this type was obtained.

[0063] The magnetic properties of the FeNi ordered alloys produced in each example and comparative example were evaluated by the method described below. The results, along with the manufacturing conditions, are shown in Table 1. The N content of the FeNi ordered alloys produced in Examples 1 and 5 and Comparative Example 1 was also measured by the method described below. The results are shown in Table 2.

[0064] <Coercive force, saturation magnetization> The magnetic particles obtained in each example were packed into a sample container together with paraffin wax, and after the paraffin wax was melted using a dryer, the easy axis of magnetization was aligned in an orienting magnetic field of 16 kA / m. This magnetically oriented sample was pulse-magnetized in a magnetizing magnetic field of 32 kA / m, and the coercive force (kA / m) and saturation magnetization (Am) were measured using a VSM (vibrating sample magnetometer) with a maximum magnetic field of 16 kA / m. 2 The coercive force and saturation magnetization of the ordered alloy of Comparative Example 1 were both set at 1.0, and relative values ​​were calculated.

[0065] <Nitrogen Content> Using the magnetic particles obtained in Examples 1 and 5 and Comparative Example 1, the nitrogen content was measured by the inert gas fusion-thermal conductivity method (EMGA-820 manufactured by Horiba, Ltd.).

[0066]

[0067]

[0068] In Comparative Example 1, in which the compacting step S1 was not performed, both the coercive force and saturation magnetization of the FeNi ordered alloy were low. On the other hand, in Example 2, in which the compacting step S1 was performed, both the magnetic properties were improved. Furthermore, in Example 3, in which the pulverizing step S3 was performed, and in Examples 1, 4 to 6, in which the pulverizing step S3 and the re-nitriding step S4 were performed, the magnetic properties were further improved.

[0069] <Technical Ideas> This specification includes the following various technical ideas.

[0070] (Item 1) A forming step of forming an FeNi alloy to obtain a formed product, a nitriding step of nitriding the formed product to obtain a nitride, and a denitriding step of denitriding the nitride to obtain an L1 0 L1 includes a denitrification step to obtain an FeNi ordered alloy of the type 0 Method for producing ordered FeNi alloys of this type.

[0071] (Item 2) The method according to item L1 of item 1, further comprising a pulverization step of pulverizing the nitride to obtain pulverized nitride after the nitriding step, and a denitrification step of denitrifying the pulverized nitride after the pulverization step. 0 Method for producing ordered FeNi alloys of this type.

[0072] (Item 3) The method according to item L1 of item 2, further comprising a re-nitriding step of re-nitriding the pulverized nitride to obtain a re-nitrided nitride after the pulverization step, and after the re-nitriding step, denitriding the re-nitrided nitride in the denitriding step. 0 Method for producing ordered FeNi alloys of this type.

[0073] (Item 4) The method according to any one of Items 1 to 3, wherein the molded product is nitrided at 300°C or higher and 500°C or lower in the nitriding step. 0 Method for producing ordered FeNi alloys of this type.

[0074] (Item 5) The method according to item L1 of item 4, wherein the nitriding step is performed by nitriding the molded product at a temperature of 330°C or higher and 450°C or lower. 0 Method for producing ordered FeNi alloys of this type.

[0075] (Item 6) The method according to any one of Items 1 to 5, wherein the molded product is contacted with a nitrogen-containing compound in the nitriding step. 0 Method for producing ordered FeNi alloys of this type.

[0076] (Item 7) The method according to any one of Items 1 to 6, wherein the nitride is denitrified at 100°C or higher and 450°C or lower in the denitrification step. 0 Method for producing ordered FeNi alloys of this type.

[0077] S1 Molding process S2 Nitriding process S3 Grinding process S4 Re-nitriding process S5 Denitrification process

Claims

1. A forming step of forming an FeNi alloy to obtain a formed product, a nitriding step of nitriding the formed product to obtain a nitride, and a denitriding step of denitrifying the nitride to obtain an L1 0 L1 includes a denitrification step to obtain an FeNi ordered alloy of the type 0 A method for producing an FeNi ordered alloy of this type.

2. The method according to claim 1, further comprising a crushing step of crushing the nitride to obtain crushed nitride after the nitriding step, and after the crushing step, in the denitriding step, the crushed nitride is denitrified. 0 A method for producing an FeNi ordered alloy of this type.

3. The method according to claim 2, further comprising a re-nitriding step of re-nitriding the pulverized nitride to obtain a re-nitrided nitride after the pulverization step, and after the re-nitriding step, the re-nitrided nitride is denitrided in the denitriding step. 0 A method for producing an FeNi ordered alloy of this type.

4. The L1 according to any one of claims 1 to 3, wherein in the nitriding step, the molded product is nitrided at 300°C or higher and 500°C or lower. 0 A method for producing an FeNi ordered alloy of this type.

5. The L1 method according to claim 4, wherein the molded product is nitrided at 330° C. or higher and 450° C. or lower in the nitriding step. 0 A method for producing an FeNi ordered alloy of this type.

6. The method according to any one of claims 1 to 5, wherein in the nitriding step, the molded product is contacted with a nitrogen-containing compound. 0 A method for producing an FeNi ordered alloy of this type.

7. The L1 according to any one of claims 1 to 6, wherein in the denitrification step, the nitride is denitrified at 100°C or higher and 450°C or lower. 0 A method for producing an FeNi ordered alloy of this type.