Method for manufacturing aluminum alloy sheet for can lid
The described method for manufacturing aluminum alloy plates for can lids addresses the challenge of achieving high strength and toughness while reducing CO2 emissions by using a specific alloy composition and process that blends scrap materials without intermediate heat treatment, resulting in a sustainable and efficient production of high-performance can lid materials.
Patent Information
- Application Number
- PCT/JP2024/015102
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
The manufacturing of aluminum alloy plates for can lids faces challenges in achieving high strength and toughness while reducing CO2 emissions, as conventional methods require significant new metal usage and intermediate heat treatment, which increases energy consumption and environmental impact.
An aluminum alloy plate composition with specific ranges of Si, Fe, Cu, Mn, and Mg is used, allowing for blending of scrap materials without intermediate heat treatment, achieved through a casting, homogenization, and rolling process that includes hot and cold rolling without heat treatment, thereby reducing new metal usage and energy consumption.
This method enables the production of aluminum alloy plates with high strength and toughness suitable for positive pressure can lids, while significantly reducing CO2 emissions by utilizing recycled materials and minimizing energy consumption.
Smart Images

Figure JP2024015102_24102024_PF_FP_ABST
Abstract
Description
Manufacturing method of aluminum alloy sheet for can lid CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This international application claims priority based on Japanese Patent Application No. 2023-067151, filed with the Japan Patent Office on April 17, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present disclosure relates to a method for manufacturing an aluminum alloy sheet for can ends.
[0003] In recent years, with the rise of environmental awareness, CO 2 There is a demand for aluminum alloy sheets with low CO emissions. 2 The compounding of new aluminum ingots in the casting process indirectly contributes significantly to these emissions.
[0004] The production of primary aluminum ingots uses a large amount of electricity during the refining process and produces a large amount of CO 2 Therefore, reducing the amount of virgin aluminum used and increasing the horizontal recycling rate will reduce CO emissions in the manufacture of aluminum alloy sheets. 2 This will lead to reduced emissions.
[0005] Generally, CO generated when aluminum scrap is remelted and cast 2 It is said that waste emissions can be reduced to about one-thirtieth of that when producing virgin aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used worldwide is extremely large, and further improving the horizontal recycling rate for these cans will have a significant impact on reducing the environmental impact.
[0006] Among these, can ends made of 5182 aluminum alloy (AA5182 alloy) have lower upper limits for the compositional specifications of Si, Fe, Cu, Mn, etc. than can bodies made of 3104 aluminum alloy (AA3104 alloy), making it difficult to incorporate scrap derived from can stock containing 3104 aluminum alloy.
[0007] For example, if can scrap (UBC: Used Beverage Can) generated in the market is blended as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will likely exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.
[0008] Therefore, compared with the aluminum alloy sheet for can bodies, the aluminum alloy sheet for can ends uses a larger amount of virgin metal to adjust the composition to that of 5182 aluminum alloy, resulting in a low recyclability. Therefore, by changing the can ends to an alloy whose composition is easily blended with 3104 aluminum alloy, the virgin metal usage rate for can ends can be significantly reduced.
[0009] Patent Documents 1 to 5 disclose aluminum alloy sheets for can lids that have compositions relatively close to those of 3104 aluminum alloy, which has excellent recyclability.
[0010] Japanese Patent Application Laid-Open No. 2001-73106 Japanese Patent Application Laid-Open No. 9-070925 Japanese Patent Application Laid-Open No. 11-269594 Japanese Patent Application Laid-Open No. 2000-160273 Japanese Patent Application Laid-Open No. 2016-160511
[0011] The problem of using an alloy for can lids with a composition similar to that of 3104 aluminum alloy is that it reduces the pressure resistance of the can lid and the toughness of the material. The pressure resistance of a can lid is the internal pressure value when the can lid is inverted against the pressure inside the can, and is the resistance value when the internal pressure of the can increases unexpectedly due to a change in the external environment.
[0012] In particular, positive pressure cans for beer and carbonated beverages require high pressure resistance. Generally, the stronger the material and the thicker the plate, the greater the pressure resistance. For this reason, the high-strength 5182 aluminum alloy, which contains a large amount of magnesium, is used for the lids of positive pressure cans.
[0013] In contrast, if conventional 3104 aluminum alloy is used for can lids, the pressure resistance is significantly reduced, and there is a high risk that the lid will invert and leak contents if the internal pressure of the can suddenly increases. Furthermore, if the plate thickness is increased to increase the pressure resistance, this will result in an increase in the weight and cost of the lid.
[0014] Furthermore, the toughness of the material affects the formability and openability of the lid. If the material has low toughness, forming cracks may occur, especially in the countersink and rivet areas of the lid. Also, if the internal pressure of the can suddenly increases, cracks may occur in the score area, increasing the risk of the can contents leaking. These cracks occur particularly along the rolling direction. Therefore, the material must have toughness against tensile stress and bending stress in the direction perpendicular to the rolling direction.
[0015] However, aluminum alloy sheets for can lids, which have chemical compositions relatively close to those of the conventional 3104 aluminum alloy, do not satisfy either or both of the above-mentioned two problems, i.e., material strength (i.e., pressure resistance of the lid) and toughness (i.e., formability and openability).
[0016] To solve these problems, it may be possible to achieve both high strength and high toughness by performing a solution heat treatment, for example, in a continuous annealing furnace, after hot rolling or during cold rolling. However, can end materials are required to be mass-produced at low cost, and in consideration of the environmental load, it is also required to reduce the energy consumption involved in production as much as possible. Therefore, it is preferable to produce them without intermediate heat treatment.
[0017] It is desirable to provide an aspect of the present disclosure that provides a method for producing an aluminum alloy sheet for can ends, which can obtain an aluminum alloy sheet for can ends that has both high strength and high toughness, while blending a scrap raw material derived from can stock, without performing intermediate heat treatment after hot rolling.
[0018] One aspect of the present disclosure is a method for producing an aluminum alloy sheet for can ends, the method comprising the steps of: casting an ingot having a silicon content of 0.20% by mass or more and 0.47% by mass or less, an iron content of 0.30% by mass or more and 0.59% by mass or less, a copper content of 0.11% by mass or more and 0.40% by mass or less, a manganese content of 0.70% by mass or more and 0.98% by mass or less, a magnesium content of 1.3% by mass or more and 3.7% by mass or less, and the balance consisting of aluminum and unavoidable impurities or containing aluminum and unavoidable impurities; homogenizing the ingot; and rolling the homogenized ingot. In the rolling step, the ingot is hot-rolled and then cold-rolled to completion without heat treatment.
[0019] According to this configuration, it is possible to achieve both high strength and high toughness in the aluminum alloy sheet while blending scrap raw material derived from can stock, without further performing a heat treatment process after hot rolling. That is, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, and to reduce the virgin metal usage rate and CO 2 Furthermore, an aluminum alloy sheet for can ends can be obtained that can be used for positive pressure can ends, which require high pressure resistance.
[0020] FIG. 1 is a schematic diagram of a repeated bending test. FIG. 2 is a flowchart of a method for manufacturing an aluminum alloy sheet according to the present embodiment. FIG. 3 is a flowchart of a repeated bending test. min 10 is a graph showing the relationship between the number of repeated bending cycles and the normalized number of bending cycles.
[0021] Hereinafter, embodiments to which the present disclosure is applied will be described with reference to the drawings.
[0022] [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for can lids of the present disclosure (hereinafter also simply referred to as "alloy sheet") contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn), and magnesium (Mg).
[0023] The lower limit of the Si content is 0.20% by mass. The average Si content standard for 3104 aluminum alloy specified in JIS-H-4000:2014 is 0.30% by mass, and the average Si content standard for 5182 aluminum alloy specified in JIS-H-4000:2014 is 0.10% by mass. Therefore, by setting the Si content to 0.20% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0024] The upper limit of the Si content is 0.47 mass%, preferably 0.30 mass%. If the Si content exceeds 0.47 mass%, Mg 2 The difference between the solid solution temperature of Si and the solidus temperature of the aluminum matrix becomes small, and the Mg present in the aluminum alloy ingot 2 It becomes difficult to dissolve a large amount of Si in the homogenization process. 2 As a result, strength and toughness decrease.
[0025] On the other hand, by setting the Si content to 0.30 mass% or less, Mg 2 In addition, coarse Mg particles can be easily removed by hot rolling. 2 Since the precipitation of Si is suppressed, better strength and toughness can be obtained without carrying out heat treatment after hot rolling.
[0026] The lower limit of the Fe content is 0.30% by mass. The average Fe content of the 3104 aluminum alloy is 0.40% by mass, and the average Fe content of the 5182 aluminum alloy is 0.18% by mass. Therefore, by setting the Fe content to 0.30% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0027] The upper limit of the Fe content is 0.59% by mass, preferably 0.55% by mass. If the Fe content exceeds 0.59% by mass, the amount of abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., giant compounds) increases. As a result, crack propagation paths are generated, and the toughness of the alloy plate decreases. On the other hand, by setting the Fe content to 0.55% by mass or less, the crystallization of the above-mentioned coarse intermetallic compounds can be suppressed when the amount of Mg added, which compensates for strength and toughness, is increased.
[0028] The lower limit of the Cu content is 0.11% by mass, preferably 0.17% by mass, and more preferably 0.20% by mass. If the Cu content is less than 0.11% by mass, the amount of Cu that increases strength through solid solution or precipitation will be insufficient, resulting in a decrease in the strength of the alloy sheet. The average Cu content standard for 3104 aluminum alloy is 0.15% by mass, and the average Cu content standard for 5182 aluminum alloy is 0.075% by mass. Therefore, by setting the Cu content to 0.11% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0029] The upper limit of the Cu content is 0.40 mass%, preferably 0.25 mass%. If the Cu content exceeds 0.40 mass%, coarse precipitates increase, and the toughness of the alloy plate decreases. Furthermore, by setting the Cu content to 0.25 mass% or less, the strength can be increased without significantly impairing the toughness.
[0030] The lower limit of the Mn content is 0.7% by mass. If the Mn content is less than 0.7% by mass, the Mn that increases strength through solid solution or precipitation is insufficient, resulting in a decrease in the average strength of the alloy sheet. The average Mn content standard for the 3104 aluminum alloy is 1.1% by mass, and the average Mn content standard for the 5182 aluminum alloy is 0.35% by mass. Therefore, by setting the Mn content to 0.7% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0031] The upper limit of the Mn content is 0.98% by mass. If the Mn content exceeds 0.98% by mass, the amount of abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds increases, which results in the formation of crack propagation paths and a decrease in the toughness of the alloy plate.
[0032] The lower limit of the Mg content is 1.3 mass%, preferably 2.6 mass%. If the Mg content is less than 1.3 mass%, the amount of Mg that increases strength through solid solution will be insufficient, resulting in a decrease in the average strength of the alloy sheet. Furthermore, by setting the Mg content to 2.6 mass% or more, better strength and toughness can be obtained without performing heat treatment after hot rolling.
[0033] The upper limit of the Mg content is 3.7% by mass. If the Mg content exceeds 3.7% by mass, the solidus temperature of the aluminum matrix decreases and the Mg content decreases. 2 The solution temperature of Si increases, so the Mg 2 It becomes difficult to dissolve Si in the homogenization process. In addition, the solidus temperature of the aluminum matrix decreases, increasing the amount of coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds. This reduces strength and toughness.
[0034] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10 mass%. By including Ti, the ingot structure of the alloy plate is refined. The alloy plate may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass%. Furthermore, the alloy plate may also contain chromium (Cr). The upper limit of the Cr content is preferably 0.10 mass%.
[0035] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, and Mg in the above-mentioned ranges, with the balance consisting of aluminum and unavoidable impurities, or including aluminum and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%. The balance may contain substances other than aluminum and unavoidable impurities.
[0036] <Material Strength and Pressure Resistance> The pressure resistance value of the lid formed of an aluminum alloy plate is 0.2% proof stress σ 0.2 , tensile strength σ B , and the average value σ of 0.2% proof stress and tensile strength fm It is empirically known that there is a strong positive correlation between the value V of the following formula (1) calculated from the sheet thickness t and the sheet thickness t (see Sumitomo Light Metal Technical Report, Vol. 54, No. 1, 2013, pp. 185-195).
[0037] V = t 2.27 ×σ fm / (σ 0.2 / σ B ) ... (1) Therefore, in a lid formed of an aluminum alloy plate, the greater the plate thickness, the more improved the pressure resistance. Since the aluminum alloy plate of the present disclosure has high material strength, an increase in plate thickness to improve pressure resistance can be suppressed.
[0038] Furthermore, the larger S calculated by the following formula (2) is, the higher the pressure resistance of the lid is. In particular, when the anisotropy of the material is taken into consideration, the smallest value of S among the three S values obtained from the measurement results of the tensile tests in the 0° direction, 45° direction, and 90° direction relative to the rolling direction is selected. min is preferably large.
[0039] S = σ fm / (σ 0.2 / σ B ) ... (2) S min is preferably 330 MPa or more, and more preferably 350 MPa or more. min By setting the thickness to such a value, it is possible to form a lid having a sufficient pressure resistance value without significantly increasing the plate thickness.
[0040] 0.2% proof stress σ in formula (1) and formula (2) 0.2 and tensile strength σ B is measured by the method specified in JIS-Z-2241: 2011. The plate thickness t is measured, for example, with a microgauge.
[0041] <Toughness> It is known that the toughness of the aluminum alloy plate affects the formability of the lid and the force required to open the score (i.e., opening force).
[0042] (Number of repeated bending tests) A repeated bending test is one of the evaluation indicators for the toughness of an aluminum alloy sheet. For a given sheet thickness, the more repeated bending tests, the better the toughness of the aluminum alloy sheet. Since cracks along the rolling direction are particularly problematic in aluminum alloy sheets, the number of repeated bending tests when the rolling direction and the bending ridge direction are parallel is important. The aluminum alloy sheet of the present disclosure can achieve a good number of repeated bending tests.
[0043] The repeated bending test is carried out according to the following procedure. For example, as shown in Fig. 1, a rectangular test piece having a width of 12.5 mm and a length of 200 mm is placed so that the bending ridgeline R is parallel to the rolling direction D of the alloy plate. Both ends of this test piece are fixed with chucks, and a tension of 200 N is applied.
[0044] In this state, the test piece is repeatedly bent by rotating the other chuck 90° left and right, using a jig with a bending radius of 2.0 mm as a fulcrum, which is positioned 150 mm in the longitudinal direction of the test piece from the end of the test piece fixed to one of the immovable chucks, and the number of bends until the test piece breaks is measured.
[0045] The number of bending times is counted as one bending operation to either the left or right by 90° and one operation returning to the original position. If the wire breaks during bending, the angle Θ (0°-90°) is read and the number of repeated bending times N is calculated using the following formula (3). In formula (3), N 0 is the total number of times that the test piece was bent 90° to either the left or right and returned to the original 0° position from the 90° bent position until it broke.
[0046] N=N 0 +Θ / 90 ... (3) Repeated bending evaluation is more disadvantageous as the plate thickness increases, so it is necessary to consider it by correcting it with a standard plate thickness. Therefore, the number of repeated bending times N is normalized by the following formula (4) using a plate thickness of 0.235 mm as the standard. s t (mm) is the thickness of the test piece.
[0047] N s= N × t / 0.235 (4) The normalized number of repeated bending of the aluminum alloy plate of the present disclosure is preferably 17 or more, and more preferably 18 or more. By setting the normalized number of repeated bending to such a number, the toughness of the aluminum alloy plate is increased, and sufficient formability of the lid can be obtained.
[0048] (Second-phase particles) Toughness is affected by strength and the distribution of second-phase particles. That is, the higher the strength and the higher the density of second-phase particles, the lower the toughness. In particular, when the contents of Mg and Si are high, the distribution of Mg 2 As a result, Mg 2 The Si particles act as crack initiation points and propagation paths, which reduces toughness.
[0049] The aluminum alloy sheet of the present disclosure has an area of 0.3 μm in the central region in the sheet thickness direction of a cross section perpendicular to the sheet surface and parallel to the rolling direction. 2 More than Mg 2 The ratio of the total area of the central region of the Si particles is preferably 0.2% or less, and more preferably 0.1% or less.
[0050] Mg 2 The area ratio of Si particles can be measured, for example, by the following method: Of the surfaces of the measurement sample, the surface to be measured (i.e., the cross section perpendicular to the rolled surface, which is the plate surface of the alloy plate, and parallel to the rolling direction) is mechanically polished to a mirror finish.
[0051] The polished surface (i.e., a cross section perpendicular to the rolled surface, which is the plate surface of the alloy plate, and parallel to the rolling direction) is observed using a scanning electron microscope (SEM) to obtain 10 fields of view. The SEM acceleration voltage is 15 kV, the magnification is 1000 times, and the range of one field of view is 0.012 mm. 2 The image is then taken and a backscattered electron composition image (COMPO) is obtained.
[0052] The photographed COMPO is analyzed using the image analysis software ImageJ. Specifically, the most frequent value of the brightness of the image in 256 gradations is taken as the brightness of the background, and particles with brightness lower than the value obtained by subtracting 30 from the brightness of the most frequent value are determined as Mg 2 It is determined to be a Si particle.
[0053] Determined Mg 2 Among the Si particles, 0.3 μm 2 The total area of particles with an area of 0.3 μm or more was calculated and divided by the photographed area of 10 fields of view. 2 More than Mg 2 The percentage of the total area of the cross section of the Si particle is calculated.
[0054] <Method for manufacturing aluminum alloy sheet> The aluminum alloy sheet of the present disclosure is obtained by the method for manufacturing an aluminum alloy sheet of the present disclosure, which includes a casting step S110, a homogenization treatment step S120, a rolling step S130, and a painting step S140, as shown in Figure 2 .
[0055] (Casting Step) In this step, an aluminum alloy having the composition of the aluminum alloy plate of the present disclosure is subjected to a conventional semi-continuous casting method (i.e., DC casting) to produce an ingot. At this time, an Al-Ti-B based grain refiner may be added to the base material. This suppresses coarsening of the crystal grains and second phase particles in the ingot.
[0056] (Homogenization Treatment Step) In this step, the surface of the ingot is chamfered, and then the ingot is placed in a soaking furnace to undergo homogenization treatment. 2 The temperature is preferably equal to or higher than the solid solution temperature of Si and equal to or lower than the solidus temperature of the aluminum matrix.
[0057] Homogenization temperature is Mg 2 If the temperature is higher than the solid solution temperature of Si, Mg, which is a second phase particle that crystallizes and precipitates in the ingot, 2 The amount of Si present can be reduced. As a result, both the strength and toughness of the aluminum alloy sheet are improved. Furthermore, the homogenization temperature can be reduced by reducing the amount of Mg 2 It is preferable that the temperature is 40°C or more higher than the solid solution temperature of Si. 2 The amount of Si present can be made extremely small.
[0058] Furthermore, by setting the homogenization temperature at or below the solidus temperature of the aluminum matrix, it is possible to produce an aluminum alloy plate without causing local melting. Furthermore, it is preferable to set the homogenization temperature at or above 10°C lower than the solidus temperature of the aluminum matrix. This allows for stable production of an aluminum alloy plate without causing local melting.
[0059] Mg 2 The solution temperature of Si and the solidus temperature of the aluminum matrix are uniquely determined by the composition of the aluminum alloy. 2 The solution temperature of Si and the solidus temperature of the aluminum matrix can be determined by inputting the composition of the aluminum alloy into, for example, "JMatPro," a thermodynamic calculation software developed by Sente Software, Inc. The CALPHAD method is used as a thermodynamic model for calculating the equilibrium diagram.
[0060] The homogenization treatment time is preferably, for example, 1 hour or more and 20 hours or less. When the homogenization treatment time is 1 hour or more, the temperature of the entire slab becomes uniform, segregation of the ingot structure is easily eliminated, and Mg 2 The longer the homogenization time, the easier it is to redissolve the Si particles. 2 The Si particles can be redissolved. However, if the homogenization treatment time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.
[0061] (Rolling Step) In this step, the homogenized ingot is rolled. This step includes a hot rolling step S131 and a cold rolling step S132.
[0062] The hot rolling process S131 includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of millimeters by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several millimeters by, for example, tandem rolling, and the plate material is wound into a coil to form a hot-rolled coil.
[0063] When the total reduction rate of the finish rolling is high, the aluminum alloy sheet becomes a recrystallized structure after coiling, and the degree of accumulation of the Cube orientation can be increased. When the coiling temperature of the finish rolling is high, the aluminum alloy sheet becomes a recrystallized structure after coiling, and the degree of accumulation of the Cube orientation can be increased. By increasing the degree of accumulation of the Cube orientation of the aluminum alloy sheet, the number of repeated bending cycles can be improved.
[0064] The cold rolling step S132 is performed following the hot rolling step S131. In cold rolling, the hot rolled coil is rolled until it has the product thickness. The cold rolling may be either single rolling or tandem rolling. In single cold rolling, it is preferable to perform rolling in two or more passes.
[0065] The cold rolling reduction (i.e., the target total reduction) is preferably 70% or more, more preferably 80% or more. By setting the lower limit of the cold rolling reduction to such a value, the strength of the aluminum alloy sheet can be increased. On the other hand, the cold rolling reduction is preferably 90% or less. By setting the upper limit of the cold rolling reduction to such a value, the anisotropy of the crystal grain structure is reduced, and the toughness against tensile stress and bending stress in a direction perpendicular to the rolling direction is improved.
[0066] The cold rolling reduction ratio R (%) is the thickness t of the hot rolled sheet. 0 (mm), product thickness after cold rolling t 1 (mm) is calculated using the following formula (5).
[0067] R = (t 0 -t 1 ) / t 0 × 100 (5) In the rolling step S130, after hot rolling the ingot, cold rolling is completed without heat treatment (i.e., annealing). That is, in the manufacturing method of the aluminum alloy sheet of the present disclosure, cold rolling is performed to the final product thickness without heat treatment of the sheet material (i.e., coil) between hot rolling and cold rolling or during cold rolling. This allows the number of steps to be significantly reduced, improving production efficiency and reducing energy consumption.
[0068] (Painting process) In this process, a paint is baked onto the plate material obtained by cold rolling the ingot. Specifically, first, a coil that has been cold rolled to the product plate thickness is precoated on a painting line or the like. The surface of the cold-rolled coil is degreased, cleaned, and chemically treated, and then painted, and then the paint is baked.
[0069] Chemical solutions such as chromate and zirconium are used in chemical conversion treatments. Epoxy and polyester paints are used. These can be selected according to the application. In the paint baking process, the coil is heated to a peak metal temperature (PMT) of 220°C or higher for approximately 30 seconds.
[0070] In this case, the lower the PMT, the more the recovery of the material is suppressed, and the strength of the alloy plate can be maintained at a high level. Therefore, the baking temperature of the paint (i.e., PMT) is preferably 270°C or lower. In addition, the cold rolling ratio can be reduced to improve toughness, and the resulting decrease in strength can be compensated for by lowering the PMT.
[0071] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained.
[0072] (1a) High strength and high toughness can be achieved in the produced aluminum alloy sheet while incorporating scrap raw materials derived from can stock. That is, since a certain amount of scrap 3104 aluminum alloy for can bodies can be incorporated into the raw materials, the virgin metal usage rate and CO 2 Furthermore, an aluminum alloy sheet for can ends can be obtained that can be used for positive pressure can ends, which require high pressure resistance.
[0073] [2. Other Embodiments] Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take on various forms.
[0074] (2a) In addition to the method for manufacturing an aluminum alloy sheet according to the above embodiment, the present disclosure also includes various forms of an aluminum alloy sheet obtained by this manufacturing method, and a member made of this aluminum alloy sheet.
[0075] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. Also, part of the configuration of the above embodiments may be omitted. Furthermore, at least part of the configuration of the above embodiments may be added to, replaced with, or the like, the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified by the wording of the claims are embodiments of the present disclosure.
[0076] 3. Examples The following describes the details of tests conducted to confirm the effects of the present disclosure and their evaluation.
[0077] <Production of Aluminum Alloy Sheets> As examples and comparative examples, aluminum alloy sheets S1 to S12 shown in Tables 1 and 2 were produced. Specific production procedures are described below.
[0078] First, an ingot containing the components (% by mass) of Alloy Nos. 1 to 7 shown in Table 3, with the balance being aluminum and unavoidable impurities, was produced by semi-continuous casting. The ingot contained 0.10% by mass or less of Ti, 0.25% by mass or less of Zn, 0.10% by mass or less of Cr, and 0.15% by mass or less of unavoidable impurities.
[0079] Next, six faces of the ingot were chamfered. After that, the ingot was placed in a furnace and subjected to homogenization treatment. The homogenization treatment temperature is as shown in Table 1. For the ingots S1-S11, the homogenization treatment temperature was the same as that of the Mg 2 The homogenization temperature was set to be equal to or higher than the solidus temperature of the aluminum matrix and equal to or lower than the solidus temperature of the Si ingot. 2 The temperature was set lower than the solid solution temperature of Si. After the homogenization treatment for 4 hours or more, the ingot was taken out of the furnace, and immediately hot rolling was started to produce a rolled sheet.
[0080] Furthermore, the rolled sheet after hot rolling was subjected to cold rolling. The target total reduction ratio in cold rolling is as shown in Table 1. The product thickness after cold rolling (i.e., t in Equation (5)) 1 ) was in the range of approximately 0.235±0.01 mm.
[0081] After cold rolling, a paint baking treatment was carried out for 30 seconds. The practical temperature (PMT) during paint baking is as shown in Table 1. Aluminum alloy sheets S1-S12 were obtained by the above steps. Furthermore, the sheet thicknesses of the aluminum alloy sheets S1-S12 measured with a microgauge (i.e., product sheet thicknesses) are shown in Table 1.
[0082]
[0083]
[0084]
[0085] <Evaluation of Aluminum Alloy Sheets> (Tensile Properties) Three No. 5 test pieces defined in JIS-Z-2241: 2011 were prepared from each of the aluminum alloy sheets S1 to S12. The longitudinal directions of the three test pieces extended in directions forming angles of 0°, 45°, and 90° with respect to the rolling direction, respectively.
[0086] These test pieces were subjected to a tensile test in accordance with JIS-Z-2241:2011 to measure the 0.2% yield strength and tensile strength. 0.2 and tensile strength σ B The measurement results and the average value σ of 0.2% yield strength and tensile strength fm The results are shown in Tables 1 and 2. Three S values were calculated from the measurement results of the tensile tests in the 0° direction, 45° direction, and 90° direction and formula (2). The minimum value of these S values, S min is shown in Table 2.
[0087] (Toughness) In the aluminum alloy plates of S1-S12, the area of 0.3 μm was measured by the measurement method described in the embodiment. 2 More than Mg 2 The ratio of the total area of the cross section of the Si particles (area ratio) was calculated. The measurement results are shown in Table 2.
[0088] For the aluminum alloy plates S1-S12, the number of repeated bendings and the normalized number of repeated bendings were calculated using the measurement method described in the embodiment and equations (3) and (4). The results are shown in Table 2.
[0089] (Scrap Blending Ratio) With respect to the compositions of the aluminum alloy plates S1 to S12, it was determined whether the possible blending ratio of 3104 aluminum alloy scrap was 50 mass% or more. The possible blending ratio of 3104 aluminum alloy scrap was determined based on Table 4.
[0090] Table 4 shows the relationship between the blending ratios of 3104 aluminum alloy and 5182 aluminum alloy and the average values of the component specifications. The first row of Table 4 shows the average values of the component specifications of 3104 aluminum alloy, and the second row shows the average values of the component specifications of 5182 aluminum alloy.
[0091] For example, when the compounding ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.
[0092] Therefore, when the proportions of each component of the aluminum alloy sheet are equal to or greater than the above-mentioned values of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of 3104 aluminum alloy sheet scrap is 50% by mass or more. As the blending ratio of 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase and the content of Mg decreases. The aluminum alloy sheets S2-S12 can be blended with 50% by mass or more of 3104 aluminum alloy scrap.
[0093]
[0094] (Evaluation) Figure 3 shows the S1-S12 aluminum alloy sheets. min The graph in FIG. 3 shows the relationship between S and the normalized number of repeated bending times. min The larger both the number of normalized repeated bending cycles and the number of normalized repeated bending cycles (i.e., the closer to the top right of the graph the plot is), the better the characteristics are.
[0095] The aluminum alloy plate of S1 has a small amount of Mg, so it has sufficient strength (i.e., S min In contrast, the aluminum alloy sheets S2 to S12 obtained by the manufacturing method of the present disclosure all had S minThe normalized number of repeated bending cycles is 17 or more.
[0096] Furthermore, the aluminum alloy sheets of S8-11, which have a high Mg content, are all S min In particular, the aluminum alloy sheets of S10 and S11 have a smaller Si content than the aluminum alloy sheets of S8 and S9, and therefore have a larger Mg content than the aluminum alloy sheets of S10 and S11. 2 The area ratio of Si particles is 0.1% or less, and both strength and toughness are particularly excellent. 2 Since the temperature is lower than the solid solution temperature of Si, Mg 2 The area ratio of Si particles increases, and the amount of S is small despite the large amount of Mg. min The normalized number of repeated bending cycles was relatively small.
[0097] For all aluminum alloys, the lower the paint baking temperature (PMT), the higher the strength (i.e., S min For example, when comparing aluminum alloy sheets S2 and S3, S4 and S5, S6 and S7, S8 and S9, and S10 and S11, the lower the paint baking temperature, the higher the S min On the other hand, the higher the paint baking temperature, the greater the normalized number of repeated bending cycles.
Claims
1. A method for manufacturing an aluminum alloy sheet for can ends, comprising: a step of casting an ingot having a silicon (Si) content of 0.20% by mass or more and 0.47% by mass or less, an iron (Fe) content of 0.30% by mass or more and 0.59% by mass or less, a copper (Cu) content of 0.11% by mass or more and 0.40% by mass or less, a manganese (Mn) content of 0.70% by mass or more and 0.98% by mass or less, a magnesium (Mg) content of 1.3% by mass or more and 3.7% by mass or less, with the remainder consisting of aluminum (Al) and unavoidable impurities or containing the aluminum and the unavoidable impurities; a step of homogenizing the ingot; and a step of rolling the homogenized ingot, wherein in the rolling step, the ingot is hot-rolled and then cold-rolled without heat treatment.
2. The method for producing an aluminum alloy sheet for can lids according to claim 1, wherein the homogenization step is carried out by subjecting the ingot to Mg 2 A method for producing an aluminum alloy sheet for can ends, comprising homogenization treatment at a temperature equal to or higher than the solidus temperature of Si and equal to or lower than the solidus temperature of the aluminum matrix.
3. A method for producing an aluminum alloy sheet for can lids according to claim 2, wherein in the casting step, an ingot is cast having a silicon (Si) content of 0.20 mass% or more and 0.47 mass% or less, an iron (Fe) content of 0.30 mass% or more and 0.55 mass% or less, a copper (Cu) content of 0.17 mass% or more and 0.25 mass% or less, a manganese (Mn) content of 0.70 mass% or more and 0.98 mass% or less, a magnesium (Mg) content of 2.6 mass% or more and 3.7 mass% or less, and the remainder consisting of aluminum (Al) and unavoidable impurities or containing the aluminum and the unavoidable impurities.
4. A method for producing an aluminum alloy sheet for can lids according to claim 3, wherein in the casting step, an ingot is cast having a silicon (Si) content of 0.20 mass% or more and 0.30 mass% or less, an iron (Fe) content of 0.30 mass% or more and 0.55 mass% or less, a copper (Cu) content of 0.17 mass% or more and 0.25 mass% or less, a manganese (Mn) content of 0.70 mass% or more and 0.98 mass% or less, a magnesium (Mg) content of 2.6 mass% or more and 3.7 mass% or less, and the remainder consisting of aluminum (Al) and unavoidable impurities or containing the aluminum and the unavoidable impurities.
5. A method for producing an aluminum alloy sheet for can lids according to claim 4, further comprising a step of baking a paint at 270°C or less on the sheet material obtained by cold rolling the ingot.
6. A method for producing an aluminum alloy sheet for can lids according to claim 5, wherein in the rolling step, cold rolling is performed at a reduction rate of 90% or less.
Citation Information
Patent Citations
Aluminum alloy laminate for can cover adapted to recycling and manufacture thereof
JP1997070925A
Aluminum alloy-laminated sheet and its production
JP1999269594A
Aluminum alloy sheet for can end
JP2000160273A
Manufacture of aluminum alloy hard sheet for can-top
JP2001073106A
Aluminum alloy sheet for negative pressure can-top
JP2016160511A