Aluminum alloy sheet for tabs

The aluminum alloy plate with optimized composition for tabs addresses the challenge of balancing strength and recyclability, achieving high bending strength and toughness while reducing CO2 emissions through increased recycling of scrap materials.

WO2024219386A1PCT designated stage expired Publication Date: 2024-10-24UACJ CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015105
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional aluminum alloy plates for tabs face challenges in achieving both high bending strength and toughness while recycling scrap materials from can stock, leading to increased CO2 emissions due to the need for more new metal and reduced recyclability.

Method used

An aluminum alloy plate with specific composition ranges for Si, Fe, Cu, Mn, and Mg, along with optional Ti and Zn, is developed to enhance tensile strength and formability, allowing for increased recycling of 3104 aluminum alloy scrap, thereby reducing new metal usage and emissions.

Benefits of technology

The alloy achieves high tab bending strength and toughness, enabling efficient recycling of scrap materials while minimizing CO2 emissions and maintaining cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015105_24102024_PF_FP_ABST
    Figure JP2024015105_24102024_PF_FP_ABST
Patent Text Reader

Abstract

One embodiment of the present disclosure is an aluminum alloy sheet for tabs which contains 0.10-0.60 mass% Si, 0.20-0.70 mass% Fe, 0.10-0.40 mass% Cu, 0.5-1.2 mass% Mn, and 1.1-4.0 mass% Mg, the remainder consisting of Al and unavoidable impurities or including Al and unavoidable impurities, wherein the sheet thickness t (mm) and the tensile strength σB_0° (MPa) along a 0° direction with respect to the rolling direction satisfy relationship (1). (1): (2.7×t-0.45)×σB_0°≥67
Need to check novelty before this filing date? Find Prior Art

Description

Aluminum alloy plate for tabs CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This international application claims the benefit of Japanese Patent Application No. 2023-067404, filed with the Japan Patent Office on April 17, 2023, the entire disclosure of which is incorporated herein by reference.

[0002] The present disclosure relates to an aluminum alloy sheet for a tab.

[0003] In recent years, with the rise of environmental awareness, CO 2 There is a demand for aluminum alloy sheets with low CO emissions. 2 The compounding of new aluminum ingots in the casting process indirectly contributes significantly to these emissions.

[0004] The production of primary aluminum ingots uses a large amount of electricity during the refining process and produces a large amount of CO 2 Therefore, reducing the amount of virgin aluminum used and increasing the horizontal recycling rate will reduce CO emissions in the manufacture of aluminum alloy sheets. 2 This will lead to reduced emissions.

[0005] Generally, CO generated when aluminum scrap is remelted and cast 2 It is said that waste emissions can be reduced to about one-thirtieth of that when producing virgin aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used worldwide is extremely large, and further improving the horizontal recycling rate for these cans will have a significant impact on reducing the environmental impact.

[0006] Among these, tabs, which are mainly made of 5182 aluminum alloy (AA5182 alloy), have lower upper limits for the compositional specifications of Si, Fe, Cu, Mn, etc. than can bodies, which are made of 3104 aluminum alloy (AA3104 alloy), making it difficult to incorporate scrap derived from can stock that contains 3104 aluminum alloy.

[0007] For example, if can scrap (UBC: Used Beverage Can) generated in the market is blended as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will likely exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.

[0008] Therefore, compared with the aluminum alloy sheet for can bodies, the aluminum alloy sheet for tabs uses a larger amount of virgin metal to adjust the composition to that of 5182 aluminum alloy, resulting in a low recyclability. Therefore, by changing the tab to an alloy whose composition is easily blended with 3104 aluminum alloy, the usage rate of virgin metal for tabs can be significantly reduced.

[0009] Patent Documents 1 to 4 disclose aluminum alloy sheets for tabs with improved formability or opening properties.

[0010] Japanese Patent Laid-Open No. 5-263175 Japanese Patent Laid-Open No. 2017-066458 Japanese Patent Laid-Open No. 2017-166052 Japanese Patent Laid-Open No. 2011-225977

[0011] The problem with using an alloy for the tab with a composition similar to that of 3104 aluminum alloy is that it reduces the tab break strength and toughness of the material. Tab break strength is an index that indicates how difficult it is for the tab to break when the can is opened.

[0012] Generally, the greater the thickness and strength of the material, the greater the tab bending strength. For this reason, a high-strength 5182 aluminum alloy containing a large amount of magnesium is used for the tab.

[0013] In contrast, if the conventional 3104 aluminum alloy is used for the tab, the tab breakage strength is significantly reduced, and the tab breaks during opening, increasing the risk of can opening failure. Furthermore, if the plate thickness is increased too much to increase the tab breakage strength, it will result in an increase in tab weight and tab cost.

[0014] The toughness of the material also affects the formability and openability of the tab. If the material has low toughness, cracks may occur during forming, especially at the bent portion of the tab. There is also a risk of the base of the tab tearing during opening, or the tab separating when repeatedly opened.

[0015] However, conventional recyclable aluminum alloy sheets for tabs do not satisfy either or both of the above two problems, namely, tab breaking strength and toughness (formability and openability).

[0016] It is desirable that one aspect of the present disclosure can provide an aluminum alloy sheet for tabs that can achieve both high tab breaking strength and high toughness while blending scrap raw materials derived from can stock.

[0017] In one aspect of the present disclosure, the silicon (Si) content is 0.10 mass% or more and 0.60 mass% or less, the iron (Fe) content is 0.20 mass% or more and 0.70 mass% or less, the copper (Cu) content is 0.10 mass% or more and 0.40 mass% or less, the manganese (Mn) content is 0.5 mass% or more and 1.2 mass% or less, the magnesium (Mg) content is 1.1 mass% or more and 4.0 mass% or less, and the balance is aluminum (Al) and unavoidable impurities or contains aluminum and unavoidable impurities, and the sheet thickness t (mm) and the tensile strength σ in a direction 0° to the rolling direction are B_0° (MPa) satisfies the following formula (1).

[0018] (2.7 × t − 0.45) × σ B_0° ≧67 (1) According to this configuration, it is possible to achieve both high tab breaking strength and high toughness in the aluminum alloy sheet while blending scrap raw materials derived from can stock. That is, it is possible to blend a certain amount or more of scrap 3104 aluminum alloy for can bodies, reduce the rate of new metal usage, and reduce CO 2 Furthermore, an aluminum alloy sheet for a tab that satisfies both formability and openability can be obtained.

[0019] Fig. 1 is an explanatory diagram of an L-ST cross section. Fig. 2A is a schematic perspective view of an Erichsen cup, and Fig. 2B is a schematic plan view of the Erichsen cup. Fig. 3 is a graph showing an example of the measurement results of the sidewall height of the Erichsen cup. Fig. 4 is a graph showing the relationship between the value V and the tab bending strength in the examples.

[0020] Hereinafter, embodiments to which the present disclosure is applied will be described with reference to the drawings.

[0021] [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for a tab (hereinafter also simply referred to as "alloy sheet") of the present disclosure contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn), and magnesium (Mg).

[0022] The lower limit of the Si content is 0.10 mass%, preferably 0.20 mass%. If the Si content is less than 0.10 mass%, the amount of Si precipitated during the processing heat of hot rolling and cold rolling after solution treatment may decrease, and the tensile strength of the alloy sheet may be insufficient.

[0023] Furthermore, the average Si content standard of 3104 aluminum alloy specified in JIS-H-4000:2014 is 0.30% by mass, and the average Si content standard of 5182 aluminum alloy specified in JIS-H-4000:2014 is 0.10% by mass. Therefore, by setting the Si content to 0.20% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0024] The upper limit of the Si content is 0.60 mass%, preferably 0.40 mass%. If the Si content exceeds 0.60 mass%, Mg 2 The amount of Si particles increases, and the toughness of the alloy plate decreases.

[0025] The lower limit of the Fe content is 0.20% by mass, preferably 0.30% by mass. The average Fe content of the 3104 aluminum alloy is 0.40% by mass, and the average Fe content of the 5182 aluminum alloy is 0.18% by mass. Therefore, by setting the Fe content to 0.20% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0026] The upper limit of the Fe content is 0.70% by mass. If the Fe content exceeds 0.70% by mass, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, crack propagation paths are created, and the toughness of the alloy plate decreases.

[0027] The lower limit of the Cu content is 0.10 mass%, preferably 0.11 mass%, and more preferably 0.20 mass%. If the Cu content is less than 0.10 mass%, there will be insufficient Cu, which increases tensile strength by solid solution or precipitation, and the tensile strength of the alloy sheet will decrease. Note that the tensile strength of the alloy sheet will be significantly increased by precipitating Cu during hot rolling and cold rolling after solution treatment.

[0028] The average Cu content of the 3104 aluminum alloy is 0.15% by mass, and the average Cu content of the 5182 aluminum alloy is 0.075% by mass. Therefore, by setting the Cu content to 0.11% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0029] The upper limit of the Cu content is 0.40 mass %. If the Cu content exceeds 0.40 mass %, the toughness of the alloy plate decreases.

[0030] The lower limit of the Mn content is 0.5 mass%, preferably 0.7 mass%, and more preferably 0.8 mass%. If the Mn content is less than 0.5 mass%, the amount of Mn that increases the tensile strength by solid solution or precipitation will be insufficient, and the tensile strength of the alloy sheet will decrease.

[0031] The average Mn content of the 3104 aluminum alloy is 1.1 mass %, and the average Mn content of the 5182 aluminum alloy is 0.35 mass %. Therefore, by setting the Mn content to 0.7 mass % or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0032] The upper limit of the Mn content is 1.2 mass%, preferably 1.0 mass%. If the Mn content exceeds 1.2 mass%, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, crack propagation paths are created, and the toughness of the alloy plate decreases.

[0033] The lower limit of the Mg content is 1.1% by mass. If the Mg content is less than 1.1% by mass, there will be insufficient Mg, which increases tensile strength by solid solution or precipitation, and the tensile strength of the alloy sheet will decrease. Note that the precipitation of Mg during the hot rolling and cold rolling processes after solution treatment significantly increases the tensile strength of the alloy sheet.

[0034] The upper limit of the Mg content is 4.0% by mass, preferably 3.0% by mass. The average Mg content standard for 3104 aluminum alloy is 1.05% by mass, and the average Mg content standard for 5182 aluminum alloy is 4.5% by mass. Therefore, by setting the Mg content to 4.0% by mass or less, preferably 3.0% by mass or less, it is possible to incorporate a large amount of 3104 aluminum alloy scrap while reducing the amount of additional Mg-containing raw material.

[0035] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10% by mass. By including Ti, the ingot structure of the alloy plate is refined. If the Ti content exceeds 0.10% by mass, coarse crystals are generated during casting, and the toughness of the alloy plate is significantly reduced.

[0036] The alloy sheet may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass %. If the Zn content exceeds 0.25 mass %, the corrosion resistance of the alloy sheet will deteriorate.

[0037] Furthermore, the alloy plate may contain chromium (Cr). The upper limit of the Cr content is preferably 0.10% by mass. If the Cr content exceeds 0.10% by mass, coarse crystals are generated during casting, significantly reducing the toughness of the alloy plate.

[0038] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, Mg, Ti, Zn, and Cr in the respective ranges described above, with the balance consisting of aluminum and unavoidable impurities or including aluminum and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%. The balance may contain substances other than aluminum and unavoidable impurities.

[0039] <Thickness, Material Strength, and Tab Bending Strength> In the alloy sheet of the present disclosure, the thickness t (mm) and the tensile strength σ in the direction of 0° relative to the rolling direction B_0° (MPa) satisfies the following formula (1).

[0040] V=(2.7×t-0.45)×σ B_0° ≧67 (1) The tensile strength σ in formula (1) B_0° is measured by the method specified in JIS-Z-2241: 2011. The plate thickness t is measured, for example, with a microgauge.

[0041] Empirically, the value of the tab bending strength of an aluminum alloy tab has a strong positive correlation with the value V (i.e., the left side of formula (1)). Therefore, when the value V is 67 or more, a tab having sufficient tab bending strength can be formed.

[0042] In addition, the tensile strength σ B_0° It is preferable that the bending strength is 330 MPa or more. This makes it possible to form a tab having a sufficient value of the tab bending strength without significantly increasing the plate thickness of the alloy plate.

[0043] The mechanical significance of the relationship between the V value and tab breaking strength can be explained as follows: When the tab is pulled up to open a can, if the tab has low resistance to the load applied to it, plastic deformation begins due to localized yielding of the material before the score is properly opened. Tab breaking is a phenomenon in which the tab bends as this plastic deformation progresses.

[0044] Considering the cross section of the tab parallel to the bending ridge at the position where the tab bends, the resistance to the bending moment applied to the cross section due to the tab being pulled up is calculated by multiplying the section modulus, which is a value specific to the cross section shape, and the 0.2% proof stress σ, which is the yield strength of the material. 0.2 The higher the value, the larger the value.

[0045] The section modulus in the above cross section increases with thickness if the tab has a fixed shape, such as the general DRT type stay-on tab. Therefore, the ease with which bending due to yielding and plastic deformation begins in a tab break depends on the plate thickness and the 0.2% proof stress σ of the material.0.2 This can be explained by the following.

[0046] In addition, since tab breaking is a phenomenon that includes the progression of plastic deformation and the bending of the tab, it is necessary to take into consideration the work hardening of the material during plastic deformation. 0.2 Even if the strain rate is low and plastic deformation begins early, if the amount of work hardening during plastic deformation is large, the progress of plastic deformation is suppressed and the tab is less likely to bend.

[0047] Therefore, 0.2% yield strength σ 0.2 Instead of σ, we use tensile strength σ as an index that represents the material strength including work hardening. B_0° is introduced, and the plate thickness t and tensile strength σ B_0° The tab breaking property of the aluminum alloy plate can be evaluated by using the value V expressed by the following formula:

[0048] The tab breaking strength of an aluminum alloy plate is measured, for example, by the following procedure. A shell formed from an aluminum alloy plate is subjected to conversion processing other than scoring, and a can lid is formed as an end without scores. A tab formed from the aluminum alloy plate is then attached to the can lid. The can lid is fixed to a jig, and the tab is pulled up. The maximum load applied to the pulled-up portion at this time is taken as the tab breaking strength.

[0049] Specifically, a typical DRT type stay-on-tab mold is used to form the tab. A φ204 full-form (B64) shell mold, for example, is used to form the shell. The tab breaking strength is measured using, for example, a Pop Tear Tester, an opening tester manufactured by Reed Instruments Co., Ltd.

[0050] More specifically, a can lid formed with a dedicated jig and having a tab attached and no score is fixed to the jig. A load-applying jig is then attached to the tab-pulling portion, and the load-applying jig is fixed in place while applying a load perpendicular to the panel portion of the lid, sufficient to prevent plastic deformation of the tab. In this state, the lid is rotated at a rotation speed of 30° / sec to pull up and bend the tab. The maximum load applied to the tab-pulling portion is measured within a rotation angle range of up to 90°.

[0051] <Toughness> It is known that the formability and openability of the tab are affected by the toughness of the aluminum alloy plate.

[0052] (Number of repeated bending) A repeated bending test is one of the evaluation indices for the toughness of an aluminum alloy sheet. For a given sheet thickness, the more repeated bending times an aluminum alloy sheet can be subjected to, the more excellent its toughness.

[0053] The repeated bending test is carried out as follows. For example, a test piece cut into a strip having a width of 12.5 mm and a length of 200 mm is placed so that the bending ridge is parallel to the rolling direction of the alloy plate. Both ends of this test piece are fixed with chucks, and a tension of 200 N is applied.

[0054] In this state, the test piece is repeatedly bent by rotating the other chuck 90° left and right, using a jig with a bending radius of 2.0 mm as a fulcrum, which is positioned 150 mm in the longitudinal direction of the test piece from the end of the test piece fixed to one of the immovable chucks, and the number of bends until the test piece breaks is measured.

[0055] The number of bending times is counted as one bending operation to either the left or right by 90° and one operation returning to the original position. If the wire breaks during bending, the angle Θ (0°-90°) is read and the number of repeated bending times N is calculated using the following formula (2). In formula (2), N 0 is the total number of times that the test piece was bent 90° to either the left or right and returned to the original 0° position from the 90° bent position until it broke.

[0056] N=N 0 +Θ / 90 ... (2) Repeated bending evaluation is more disadvantageous as the plate thickness increases, so it is necessary to consider it by correcting it with a standard plate thickness. Therefore, the normalized repeated bending number N is normalized by the following formula (3) using a plate thickness of 0.245 mm as the standard. s In addition, t t (mm) is the thickness of the test piece.

[0057] N s = N × t t / 0.245 (3) (Second Phase Particles) Toughness is affected by the tensile strength and the distribution of second phase particles. That is, the higher the tensile strength and the higher the density of the second phase particles, the lower the toughness. In particular, when the contents of Mg and Si are high, the Mg 2 As a result, Mg 2 The Si particles act as crack initiation points and propagation paths, which reduces toughness.

[0058] The aluminum alloy sheet of the present disclosure has an area of ​​0.3 μm in the central region of the sheet thickness of the L-ST cross section shown by the diagonal lines in FIG. 2 More than Mg 2 The ratio of the total area of ​​the Si particles is preferably 1.0% or less.In Fig. 1, L indicates the longitudinal direction, ST indicates the plate thickness direction, and LT indicates the width direction.

[0059] Mg 2 The area ratio of Si particles can be measured, for example, by the following method. First, a measurement sample is cut, and the surface to be measured (i.e., the L-ST cross section) is mechanically polished to a mirror finish. Next, the polished surface (i.e., the L-ST cross section) is observed using an SEM (scanning electron microscope), and 10 fields of view are obtained in the central region of the plate thickness. The acceleration voltage of the SEM is 15 kV, the magnification is 500 times, and the range of one field of view is 0.049 mm. 2 The image is taken as is, and a COMPO (backscattered electron composition) image is obtained.

[0060] The captured COMPO image is analyzed using the image analysis software "ImageJ." Specifically, the most frequent value of the image brightness in 256 gradations is defined as the background brightness, and particles with brightness lower than the value obtained by subtracting 30 from the most frequent brightness are defined as Mg particles. 2 It is determined to be a Si particle.

[0061] Determined Mg 2 Among the Si particles, 0.3 μm 2 The total area of ​​particles with an area of ​​0.3 μm or more was calculated and divided by the photographed area of ​​10 fields of view (i.e., the total photographed area), resulting in an area of ​​0.3 μm 2 More than Mg 2 The percentage of the total area of ​​the Si particles in the L-ST cross section is calculated.

[0062] (Earing ratio) The number of repeated bending cycles is also affected by the texture, and the higher the concentration of Cube orientation, the better. The concentration of Cube orientation is reflected in the ear shape of an Erichsen cup E formed from an aluminum alloy sheet by an Erichsen test, as shown in Figures 2A and 2B.

[0063] Specifically, it is suggested that the greater the relative sidewall height H in the 0° / 180° direction with respect to the rolling direction RD of the aluminum alloy sheet of Erichsen Cup E, with respect to the sidewall height H in the 45° direction with respect to the rolling direction RD (i.e., ear height), the higher the degree of accumulation of Cube orientation. That is, the aluminum alloy sheet of the present disclosure includes those having a relatively large degree of accumulation of Cube orientation and a high sidewall height H in the 0° / 180° direction.

[0064] The relative sidewall height in the 0° / 180° direction to the sidewall height in the 45° direction can be evaluated using an index called earing balance. The procedure for measuring the earing balance will be described below.

[0065] The ear ratio is expressed by the left side of the following equation (4).

[0066] (h 0p -h 45p ) / h v ×100≧-7.0 ... (4) In formula (4), h 0p is the average value of the maximum sidewall heights in the first region A1 around 0° and the second region A2 around 180° with respect to the rolling direction. The first region A1 is, for example, in the range of 0°±11° with respect to the rolling direction. The second region A2 is, for example, in the range of 180°±11° with respect to the rolling direction.

[0067] h 45p is the average value of the maximum sidewall heights in the third region A3 around 45°, the fourth region A4 around 135°, the fifth region A5 around 225°, and the sixth region A6 around 315° relative to the rolling direction.

[0068] The third region A3 is, for example, in the range of 45°±22° with respect to the rolling direction. The fourth region A4 is, for example, in the range of 135°±22° with respect to the rolling direction. The fifth region A5 is, for example, in the range of 225°±22° with respect to the rolling direction. The sixth region A6 is, for example, in the range of 315°±22° with respect to the rolling direction.

[0069] h v is the average value of the minimum sidewall height in each of the seventh region A7 from 0° to 45°, the eighth region A8 from 45° to 135°, the ninth region A9 from 135° to 180°, the tenth region A10 from 180° to 225°, the eleventh region A11 from 225° to 315°, and the twelfth region A12 from 315° to 360° with respect to the rolling direction.

[0070] 3 is a graph showing an example of the measurement results of the sidewall height of an Erichsen cup. The angles shown in Fig. 3 are angles relative to the rolling direction. The distance from the center of the graph indicates the sidewall height.

[0071] In the figure, a to d are the maximum values ​​in the third area A3 to the sixth area A6, e and f are the maximum values ​​in the first area A1 and the second area A2, and g to l are the minimum values ​​in the seventh area A7 to the twelfth area A12.

[0072] The Erichsen Cup E is formed, for example, under the conditions of a blank diameter of 57 mm and a punch diameter of 33 mm. The sidewall height of the Erichsen Cup is measured using, for example, a Roncorder EC1550-H manufactured by Kosaka Laboratory Co., Ltd.

[0073] Specifically, a measurement probe is placed at the opening of the Erichsen cup with the rolling direction as the reference (0° / 180°), and the table on which the Erichsen cup is placed is rotated once to measure the height of the opening in the circumferential direction of 360°.

[0074] When formula (4) is satisfied, that is, when the earing ratio is −7.0% or more, the concentration of Cube orientation increases, and as a result, the number of repeated bending cycles of the alloy sheet can be increased.

[0075] <Method for producing aluminum alloy sheet> The aluminum alloy sheet of the present disclosure can be produced, for example, as follows: First, an aluminum alloy having the composition of the aluminum alloy sheet of the present disclosure is subjected to a semi-continuous casting method (i.e., DC casting) according to a conventional method to produce an ingot.

[0076] Next, the surface of the ingot is chamfered. Thereafter, the ingot is placed in a soaking furnace and subjected to homogenization treatment. The temperature in the homogenization treatment is preferably, for example, 470°C or higher and 620°C or lower. The time for the homogenization treatment is preferably, for example, 1 hour or higher and 20 hours or lower.

[0077] When the homogenization temperature is 400°C or higher, segregation of the ingot structure is easily eliminated. Furthermore, when the homogenization temperature is 450°C or higher, Mg 2 The homogenization temperature is 490°C or higher, preferably 550°C or higher, and the tensile strength and toughness of the alloy sheet can be improved by redissolving the Si particles. 2 The re-dissolution of Si particles is promoted, and the tensile strength and toughness of the alloy sheet can be further improved. On the other hand, if the temperature in the homogenization treatment is 620°C or less, local melting of the aluminum alloy is unlikely to occur.

[0078] When the homogenization treatment time is 1 hour or more, the temperature of the entire slab becomes uniform, segregation of the ingot structure is easily eliminated, and Mg 2 The longer the homogenization time, the easier it is to redissolve the Si particles. 2 The Si particles can be redissolved. However, if the homogenization treatment time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.

[0079] After the homogenization treatment, the ingot is subjected to hot rolling. The hot rolling process includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of mm by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several mm by, for example, tandem rolling, and the plate material is wound into a coil to form a hot-rolled coil.

[0080] If the total reduction rate of the finish rolling is high, a recrystallized structure is formed after coiling, and the concentration of the Cube orientation can be increased. If the coiling temperature of the finish rolling is high, a recrystallized structure is formed after coiling, and the concentration of the Cube orientation can be increased.

[0081] Furthermore, a high-strength alloy sheet can be obtained by subjecting a hot-rolled coil to solution treatment to redissolve Mg, etc. For example, heat treatment (i.e., annealing) is performed using a continuous annealing furnace at a target solid temperature of 440°C or higher for 30 seconds or longer, followed by forced cooling by air cooling or the like, which can effectively increase the tensile strength of the alloy sheet.

[0082] Following the hot rolling, the plate material is cold rolled. In the cold rolling, the hot rolled coil is rolled until the product plate thickness is reached. The cold rolling may be either single rolling or tandem rolling. In the cold rolling by single rolling, it is preferable to perform the rolling in two or more passes.

[0083] By setting the finishing temperature of cold rolling in intermediate passes other than the final pass to 120°C or higher, Si, Cu, and Mg are finely precipitated and age-hardened, thereby increasing the tensile strength of the alloy sheet. Furthermore, by setting the finishing temperature to 130°C or higher, the tensile strength of the alloy sheet can be further increased.

[0084] The cold rolling reduction (i.e., the target total reduction) is preferably 80% or more. When the cold rolling reduction is 80% or more, the tensile strength of the alloy sheet can be increased. The lower the cold rolling reduction, the more the Cube orientation remains. The cold rolling reduction is preferably 92% or less.

[0085] The cold rolling reduction ratio R (%) is the thickness t of the hot rolled sheet. 0 (mm), product thickness after cold rolling t 1 (mm) is calculated using the following formula (5).

[0086] R = (t 0 -t 1 ) / t 0 × 100 (5) In addition, in the above-described method for producing an aluminum alloy sheet, annealing may be performed, for example, before or after cold rolling or between passes, as long as the effects of the aluminum alloy sheet of the present disclosure are exhibited.

[0087] Coils that have been cold-rolled to the product thickness may be pre-coated in a coating line, etc. When pre-coating is performed, the surface of the cold-rolled coil is degreased, washed, and chemically treated, and then painted, followed by a paint baking process.

[0088] Chemical solutions such as chromate-based and zirconium-based solutions are used in chemical conversion treatments. Epoxy-based and polyester-based paints are used. These can be selected according to the application. In the paint baking process, the coil is heated to a peak metal temperature (PMT) of 220°C to 270°C for approximately 30 seconds or less. The lower the PMT, the more the material recovery is suppressed, and the higher the tensile strength of the alloy plate can be maintained.

[0089] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained.

[0090] (1a) High tab breaking strength and high toughness can be achieved in an aluminum alloy sheet while incorporating scrap raw materials derived from can stock. That is, a certain amount or more of scrap 3104 aluminum alloy for can bodies can be incorporated, and the rate of new metal usage can be reduced, resulting in a reduction in CO 2 Furthermore, an aluminum alloy sheet for a tab that satisfies both formability and openability can be obtained.

[0091] [2. Other Embodiments] Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take on various forms.

[0092] (2a) In addition to the aluminum alloy sheet of the above embodiment, the present disclosure also includes various embodiments such as a member made of this aluminum alloy sheet and a method for manufacturing this aluminum alloy sheet.

[0093] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. Also, part of the configuration of the above embodiments may be omitted. Furthermore, at least part of the configuration of the above embodiments may be added to, replaced with, or the like, the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified by the wording of the claims are embodiments of the present disclosure.

[0094] 3. Examples The following describes the details of tests conducted to confirm the effects of the present disclosure and the evaluation results thereof.

[0095] <Production of Aluminum Alloy Sheets> As examples and comparative examples, aluminum alloy sheets S1 to S21 shown in Tables 1 and 2 were produced. Specific production procedures are described below.

[0096] First, an ingot containing the components (% by mass) of Alloy Nos. 1 to 8 shown in Table 3, with the balance being aluminum and unavoidable impurities, was produced by semi-continuous casting. The ingot contained 0.10% by mass or less of Ti, 0.25% by mass or less of Zn, 0.10% by mass or less of Cr, and 0.15% by mass or less of unavoidable impurities.

[0097] Next, the four sides of the ingot, excluding the front and rear ends, were chamfered. The ingot was then placed in a furnace and subjected to homogenization treatment. The homogenization treatment temperature is shown in Table 1. After the homogenization treatment, the ingot was removed from the furnace, and immediately hot rolling was started to produce a rolled sheet.

[0098] The obtained rolled sheet was annealed. The annealing temperature was as shown in Table 1, and the annealing time was 30 seconds. After annealing, the rolled sheet was cooled to room temperature by air cooling. After cooling, the rolled sheet was subjected to cold rolling. The target total reduction in cold rolling was as shown in Table 1.

[0099] After cold rolling, paint was applied to the sheet surface, and a paint baking treatment was carried out for 30 seconds. The practical temperature (PMT) during paint baking is shown in Table 1. Aluminum alloy sheets S1-S21 were obtained by baking the paint. The sheet thicknesses (i.e., product sheet thicknesses) of the aluminum alloy sheets S1-S21 measured with a microgauge are also shown in Table 1.

[0100]

[0101]

[0102] <Evaluation of Aluminum Alloy Sheet> (Tensile Properties) No. 5 test pieces defined in JIS-Z-2241: 2011 were prepared from the aluminum alloy sheets of S1-S21. The longitudinal direction of the test pieces extended in a direction forming an angle of 0° with respect to the rolling direction.

[0103] A tensile test was performed on this test piece in accordance with JIS-Z-2241:2011, and the tensile strength σ B_0° The tensile strength σ B_0° The measurement results are shown in Table 2. From the measurement results of the plate thickness and tensile strength, the value of formula (1) V = (2.7 × t - 0.45) × σ B_0° The calculation results are shown in Table 2.

[0104] (Toughness) In the aluminum alloy plates of S1-S21, the area of ​​0.3 μm was measured by the measurement method described in the embodiment. 2 More than Mg 2 The ratio of the total area (area ratio) of the Si particles in the L-ST cross section was calculated. The measurement results are shown in Table 2.

[0105] For the aluminum alloy sheets S1 to S21, the earing ratio was calculated from the measurement method described in the embodiment and the left side of equation (4). The results are shown in Table 2. In the table, "-" indicates that the measurement was not performed.

[0106] For the aluminum alloy sheets S1 to S21, the normalized number of repeated bending was calculated using the measurement method described in the embodiment and equations (2) and (3). The results are shown in Table 2.

[0107] (Scrap Blending Ratio) With respect to the compositions of the aluminum alloy plates S1 to S21, it was determined whether the possible blending ratio of 3104 aluminum alloy scrap was 50 mass % or more. The results are shown in Table 2.

[0108] In Table 2, aluminum alloy plates designated as "≧50" can contain 50 mass% or more of 3104 aluminum alloy. The possible blending ratio of 3104 aluminum alloy scrap is determined based on Table 4.

[0109] Table 4 shows the relationship between the blending ratios of 3104 aluminum alloy and 5182 aluminum alloy and the average values ​​of the component specifications. The first row of Table 4 shows the average values ​​of the component specifications of 3104 aluminum alloy, and the second row shows the average values ​​of the component specifications of 5182 aluminum alloy.

[0110] For example, when the compounding ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.

[0111] Therefore, when the proportions of each component of the aluminum alloy sheet are equal to or greater than the above-mentioned values ​​of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of 3104 aluminum alloy sheet is 50% by mass or more. As the blending ratio of 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase and the content of Mg decreases. The aluminum alloy sheets S1-S21 can be blended with 50% by mass or more of 3104 aluminum alloy scrap.

[0112] (Tab Bending Strength) In addition to the aluminum alloy plates S1 to S21, a plurality of aluminum alloy plates having different plate thicknesses and tensile strengths were prepared, and the tab bending strength of each was measured by the measurement method described in the embodiment.

[0113] The measurement results, the thickness t of the aluminum alloy plate, and the tensile strength σ in the 0° direction relative to the rolling direction B_0° and the value of equation (1) V = (2.7 × t - 0.45) × σ B_0° The relationship between these is shown in Table 5 and Figure 4. Table 6 shows the components of the aluminum alloy plates used to measure the tab bending strength.

[0114] Figure 4 confirms that there is a high correlation between the value V and the tab bending strength. Note that Figure 4 shows the results using a tab with a typical DRT type stay-on tab shape, but similar trends can be seen for tabs with other shapes.

[0115]

[0116] As shown in Table 2, in the aluminum alloy plates of S11-S21, the value V, which has a strong correlation with the tab bending strength, is 67 or more, and it was confirmed that the aluminum alloy plates have a plate thickness and tensile strength that can obtain high tab bending strength.

Claims

1. The silicon (Si) content is 0.10 mass% or more and 0.60 mass% or less, the iron (Fe) content is 0.20 mass% or more and 0.70 mass% or less, the copper (Cu) content is 0.10 mass% or more and 0.40 mass% or less, the manganese (Mn) content is 0.5 mass% or more and 1.2 mass% or less, the magnesium (Mg) content is 1.1 mass% or more and 4.0 mass% or less, and the balance is aluminum (Al) and unavoidable impurities or contains the aluminum and the unavoidable impurities, and the sheet thickness t (mm) and the tensile strength σ in a direction 0° to the rolling direction B_0° (MPa) satisfies the following formula (1): (2.7×t−0.45)×σ B_0° ≧67 ... (1) 2. The aluminum alloy sheet for tabs according to claim 1, wherein the area of ​​the L-ST cross section is 0.3 μm 2 More than Mg 2 An aluminum alloy sheet for tabs, in which the ratio of the total area of ​​Si particles is 1.0% or less.

3. The aluminum alloy sheet for tabs according to claim 1 or 2, wherein the average value h of the maximum sidewall heights in the circumferential direction of an Erichsen cup formed by an Erichsen test in the region around 0° and the region around 180° with respect to the rolling direction 0p and the average value h of the maximum sidewall height in each of the regions around 45°, 135°, 225°, and 315° with respect to the rolling direction. 45p and the average value h of the minimum sidewall height in each of the regions of 0° to 45°, 45° to 135°, 135° to 180°, 180° to 225°, 225° to 315°, and 315° to 360° with respect to the rolling direction. v and the aluminum alloy sheet for tabs satisfies the following formula (2). 0p -h 45p ) / h v × 100 ≧ −7.0 ... (2) 4. An aluminum alloy sheet for tabs according to claim 1 or 2, comprising: a silicon (Si) content of 0.20 mass% or more and 0.60 mass% or less; an iron (Fe) content of 0.30 mass% or more and 0.70 mass% or less; a copper (Cu) content of 0.11 mass% or more and 0.40 mass% or less; a manganese (Mn) content of 0.7 mass% or more and 1.2 mass% or less; and a magnesium (Mg) content of 1.1 mass% or more and 3.0 mass% or less.

Citation Information

Patent Citations

  • Aluminum alloy sheet for stay-on tab

    JP1993263175A

  • Aluminum alloy sheet for tab, and method for manufacturing the same

    JP2011225977A

  • Aluminum alloy sheet for tab and manufacturing method therefor

    JP2017066458A

  • Aluminum alloy sheet for packaging container tab

    JP2017166052A

  • Manufacture of aluminum alloy rigid plate for molding

    JP1985258454A