Aluminum alloy sheet for can lid
The aluminum alloy plate with optimized Si, Fe, Cu, Mn, and Mg composition addresses the challenge of balancing strength and toughness for can lids, enabling efficient recycling and reduced emissions by allowing the use of scrap materials, thereby enhancing both pressure resistance and formability.
Patent Information
- Application Number
- PCT/JP2024/015114
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional aluminum alloy plates for can lids face challenges in achieving both high strength and toughness, particularly when recycling scrap materials from can bodies, leading to increased CO2 emissions and reduced recyclability due to the need for more new metal to adjust composition, which affects pressure resistance and formability.
An aluminum alloy plate with specific composition ranges of Si, Fe, Cu, Mn, and Mg, allowing for the blending of scrap materials from 3104 aluminum alloy can bodies, enhancing strength and toughness while reducing new metal usage and emissions, with a yield strength and tensile strength ratio that balances pressure resistance and formability.
The alloy plate achieves high strength and toughness, enabling efficient recycling of scrap materials, reducing CO2 emissions, and providing adequate pressure resistance for positive pressure can lids without increasing plate thickness, thus improving environmental impact and manufacturing efficiency.
Smart Images

Figure JP2024015114_24102024_PF_FP_ABST
Abstract
Description
Aluminum alloy plate for can lids CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This international application claims the benefit of Japanese Patent Application No. 2023-067372, filed with the Japan Patent Office on April 17, 2023, the entire disclosure of which is incorporated herein by reference.
[0002] The present disclosure relates to an aluminum alloy sheet for can ends.
[0003] In recent years, with the rise of environmental awareness, CO 2 There is a demand for aluminum alloy sheets with low CO emissions. 2 The compounding of new aluminum ingots in the casting process indirectly contributes significantly to these emissions.
[0004] The production of primary aluminum ingots uses a large amount of electricity during the refining process and produces a large amount of CO 2 Therefore, reducing the amount of virgin aluminum used and increasing the horizontal recycling rate will reduce CO emissions in the manufacture of aluminum alloy sheets. 2 This will lead to reduced emissions.
[0005] Generally, CO generated when aluminum scrap is remelted and cast 2 It is said that waste emissions can be reduced to about one-thirtieth of that when producing virgin aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used worldwide is extremely large, and further improving the horizontal recycling rate for these cans will have a significant impact on reducing the environmental impact.
[0006] Among these, can ends made of 5182 aluminum alloy (AA5182 alloy) have lower upper limits for the compositional specifications of Si, Fe, Cu, Mn, etc. than can bodies made of 3104 aluminum alloy (AA3104 alloy), making it difficult to incorporate scrap derived from can stock containing 3104 aluminum alloy.
[0007] For example, if can scrap (UBC: Used Beverage Can) generated in the market is blended as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will likely exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.
[0008] Therefore, compared with the aluminum alloy sheet for can bodies, the aluminum alloy sheet for can ends uses a larger amount of virgin metal to adjust the composition to that of 5182 aluminum alloy, resulting in a low recyclability. Therefore, by changing the can ends to an alloy whose composition is easily blended with 3104 aluminum alloy, the virgin metal usage rate for can ends can be significantly reduced.
[0009] Patent Documents 1 to 5 disclose aluminum alloy sheets for can lids that have compositions relatively close to those of 3104 aluminum alloy, which has excellent recyclability.
[0010] Japanese Patent Application Laid-Open No. 2001-73106 Japanese Patent Application Laid-Open No. 9-070925 Japanese Patent Application Laid-Open No. 11-269594 Japanese Patent Application Laid-Open No. 2000-160273 Japanese Patent Application Laid-Open No. 2016-160511
[0011] The problem of using an alloy for can lids with a composition similar to that of 3104 aluminum alloy is that it reduces the pressure resistance of the can lid and the toughness of the material. The pressure resistance of a can lid is the internal pressure value when the can lid is inverted against the pressure inside the can, and is the resistance value when the internal pressure of the can increases unexpectedly due to a change in the external environment.
[0012] In particular, positively pressurized cans for beer and carbonated beverages require high pressure resistance. Generally, the stronger the material and the thicker the plate, the greater the pressure resistance. For this reason, the lids of positively pressurized cans are made of high-strength 5182 aluminum alloy, which contains a large amount of magnesium, a component that contributes to increased strength.
[0013] In contrast, if conventional 3104 aluminum alloy is used for can lids, the pressure resistance is significantly reduced, and there is a high risk that the lid will invert and leak contents if the internal pressure of the can suddenly increases. Furthermore, if the plate thickness is increased to increase the pressure resistance, this will result in an increase in the weight and cost of the lid.
[0014] Furthermore, the toughness of the material affects the formability and openability of the lid. If the material has low toughness, cracks may occur during molding, especially at the rivet and countersink areas of the lid. Also, if the internal pressure of the can suddenly increases, cracks may occur at the score area, increasing the risk of the can contents leaking. These cracks occur particularly along the rolling direction. Therefore, the material must have toughness against tensile stress and bending stress in directions perpendicular to the rolling direction.
[0015] However, aluminum alloy sheets for can lids, which have chemical compositions relatively close to those of the conventional 3104 aluminum alloy, do not satisfy either or both of the above-mentioned two problems, i.e., material strength (i.e., pressure resistance of the lid) and toughness (i.e., formability and openability).
[0016] One aspect of the present disclosure is to provide an aluminum alloy sheet for can ends that can achieve both high strength and high toughness while incorporating scrap raw materials derived from can stock.
[0017] In one embodiment of the present disclosure, the silicon (Si) content is 0.27% by mass or more and 0.39% by mass or less, the iron (Fe) content is 0.35% by mass or more and 0.55% by mass or less, the copper (Cu) content is 0.17% by mass or more and 0.25% by mass or less, the manganese (Mn) content is 0.75% by mass or more and 0.95% by mass or less, the magnesium (Mg) content is 2.2% by mass or more and 2.8% by mass or less, and the balance is aluminum (Al) and unavoidable impurities or contains aluminum (Al) and unavoidable impurities, and the 0.2% proof stress σ 0.2 , tensile strength σ B , and the average value σ of 0.2% proof stress and tensile strength fm Among the evaluation values S calculated by the following formula (1) using min The aluminum alloy sheet for can ends has a compressive strength of 330 MPa or more and 390 MPa or less.
[0018] S = σ fm / (σ 0.2 / σ B) ... (1) According to this configuration, it is possible to achieve both high strength and high toughness in the aluminum alloy sheet while blending scrap raw materials derived from can stock. That is, it is possible to blend a certain amount of scrap 3104 aluminum alloy for can bodies, reduce the usage rate of virgin metal, and reduce CO 2 Furthermore, it is possible to obtain an aluminum alloy sheet for can ends with high formability that can be used for positive pressure can ends, which require high pressure resistance.
[0019] Fig. 1 is an explanatory diagram of an L-ST cross section, and Fig. 2 is a graph showing an example of the relationship between the cold rolling rate and the strength anisotropy.
[0020] Hereinafter, embodiments to which the present disclosure is applied will be described with reference to the drawings.
[0021] [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for can lids of the present disclosure (hereinafter also simply referred to as "alloy sheet") contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn), and magnesium (Mg).
[0022] The lower limit of the Si content is 0.27% by mass, preferably 0.30% by mass. If the Si content is less than 0.27% by mass, the amount of Si precipitated during the processing heat of the hot rolling and cold rolling after the solution treatment may decrease, and the strength of the alloy sheet may be insufficient.
[0023] The average Si content of 3104 aluminum alloy specified in JIS-H-4000: 2014 is 0.30% by mass. Therefore, by setting the Si content to 0.27% by mass or more, preferably 0.30% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0024] The upper limit of the Si content is 0.39 mass%, preferably 0.35 mass%. If the Si content exceeds 0.39 mass%, Mg 2 The amount of Si particles increases, and the toughness of the alloy plate decreases.
[0025] The lower limit of the Fe content is 0.35% by mass, preferably 0.40% by mass. The average Fe content of the 3104 aluminum alloy is 0.40% by mass. Therefore, by setting the Fe content to 0.40% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0026] The upper limit of the Fe content is 0.55% by mass. If the Fe content exceeds 0.55% by mass, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, crack propagation paths are created, and the toughness of the alloy plate decreases.
[0027] The lower limit of the Cu content is 0.17% by mass, preferably 0.20% by mass. If the Cu content is less than 0.17% by mass, the strength of the alloy sheet is reduced due to a lack of Cu, which increases strength by solid solution or precipitation. Note that the strength of the alloy sheet is significantly increased by precipitating Cu during hot rolling and cold rolling after solution treatment.
[0028] The average Cu content of the 3104 aluminum alloy is 0.15% by mass, so by making the Cu content 0.17% by mass or more, it is possible to blend a large amount of 3104 aluminum alloy scrap.
[0029] The upper limit of the Cu content is 0.25 mass %. If the Cu content exceeds 0.25 mass %, the toughness of the alloy plate decreases.
[0030] The lower limit of the Mn content is 0.75 mass%, preferably 0.80 mass%. If the Mn content is less than 0.75 mass%, the amount of Mn that increases strength by solid solution or precipitation will be insufficient, resulting in a decrease in the average strength of the alloy plate.
[0031] The average Mn content of the 3104 aluminum alloy is 1.1 mass% and the average Mn content of the 5182 aluminum alloy is 0.35 mass%. Therefore, by setting the Mn content to 0.75 mass% or more, it is possible to blend more 3104 aluminum alloy scrap than in the conventional 5182 aluminum alloy.
[0032] The upper limit of the Mn content is 0.95% by mass, preferably 0.90% by mass. If the Mn content exceeds 0.95% by mass, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, crack propagation paths are formed, and the toughness of the alloy plate decreases.
[0033] The lower limit of the Mg content is 2.2% by mass. If the Mg content is less than 2.2% by mass, there will be insufficient Mg, which increases strength through solid solution, and the average strength of the alloy sheet will decrease. Note that the strength of the alloy sheet will be significantly increased by precipitating Mg during hot rolling and cold rolling after solution treatment.
[0034] The upper limit of the Mg content is 2.8% by mass. The average Mg content standard for 3104 aluminum alloy is 1.05% by mass, and the average Mg content standard for 5182 aluminum alloy is 4.5% by mass. Therefore, by setting the Mg content to 2.8% by mass or less, it is possible to incorporate a large amount of 3104 aluminum alloy scrap while reducing the amount of additional Mg-containing raw material.
[0035] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10 mass%. By including Ti, the ingot structure of the alloy plate is refined. The alloy plate may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass%. Furthermore, the alloy plate may also contain chromium (Cr). The upper limit of the Cr content is preferably 0.10 mass%.
[0036] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, Mg, Ti, Zn, and Cr in the respective ranges described above, with the balance consisting of aluminum and unavoidable impurities or including aluminum and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%. The balance may contain substances other than aluminum and unavoidable impurities.
[0037] <Material strength and pressure resistance> Rolled aluminum alloy sheets have material anisotropy, and their strength varies in the 0°, 45°, and 90° directions relative to the rolling direction. When the pressure inside the can increases, deformation begins in the direction with the lowest strength.
[0038] Therefore, the alloy sheet of the present disclosure has a 0.2% yield strength σ in each of the 0° direction, 45° direction, and 90° direction relative to the rolling direction. 0.2 , tensile strength σ B , and the average value σ of 0.2% proof stress and tensile strength fm The minimum evaluation value S is the minimum value of the evaluation values S (S0°, S45°, and S90°) calculated by the following formula (1) using min (=min(S0°, S45°, S90°)) is 330 MPa or more and 390 MPa or less.
[0039] S = σ fm / (σ 0.2 / σ B ) ... (1) The pressure resistance value of the lid formed of an aluminum alloy plate is empirically the minimum evaluation value S min and the plate thickness t, there is a strong positive correlation with the value V of the following formula (2).
[0040] V = t2.27 × S min ... (2) Therefore, the minimum evaluation value S of the alloy plate min By setting the minimum evaluation value S to 330 MPa or more, it is possible to form a lid having sufficient pressure resistance without increasing the plate thickness. min The minimum evaluation value S is preferably 360 MPa or more. min By setting the pressure to 360 MPa or more, the pressure resistance of the lid can be further improved.
[0041] In addition, the minimum evaluation value S min If the minimum evaluation value S exceeds 390 MPa, the material strength becomes excessively high, and the toughness of the material decreases. In other words, shear bands are more likely to occur due to the tensile stress and bending stress that occur in the material during forming, and forming cracks are more likely to occur. min By setting the compressive strength to 390 MPa or less, it is possible to achieve both strength of the material (i.e., pressure resistance of the lid) and toughness (i.e., formability and openability).
[0042] 0.2% proof stress σ in formula (1) 0.2 and tensile strength σ B is measured by the method specified in JIS-Z-2241: 2011. The plate thickness t is measured, for example, with a microgauge.
[0043] <Toughness> It is known that the toughness of the aluminum alloy plate affects the formability of the lid and the force required to open the score (i.e., opening force).
[0044] (Number of repeated bending) A repeated bending test is one of the evaluation indices for the toughness of an aluminum alloy sheet. For a given sheet thickness, the more repeated bending times an aluminum alloy sheet can be subjected to, the more excellent its toughness.
[0045] The repeated bending test is carried out as follows. For example, a test piece cut into a strip having a width of 12.5 mm and a length of 200 mm is placed so that the bending ridge is parallel to the rolling direction of the alloy plate. Both ends of this test piece are fixed with chucks, and a tension of 200 N is applied.
[0046] In this state, the test piece is repeatedly bent by rotating the other chuck 90° left and right, using a jig with a bending radius of 2.0 mm as a fulcrum, which is positioned 150 mm in the longitudinal direction of the test piece from the end of the test piece fixed to one of the immovable chucks, and the number of bends until the test piece breaks is measured.
[0047] The number of bending times is counted as one bending operation to either the left or right by 90° and one operation returning to the original position. If the wire breaks during bending, the angle Θ (0°-90°) is read and the number of repeated bending times N is calculated using the following formula (3). In formula (3), N 0 is the total number of times that the test piece was bent 90° to either the left or right and returned to the original 0° position from the 90° bent position until it broke.
[0048] N=N 0 +Θ / 90 ... (3) Repeated bending evaluation is more disadvantageous as the plate thickness increases, so it is necessary to consider it by correcting it with a standard plate thickness. Therefore, the normalized number of repeated bending times N is normalized by the following formula (4) using a plate thickness of 0.235 mm as the standard. swhere t (mm) is the thickness of the test piece.
[0049] N s = N × t / 0.235 (4) Normalized number of repeated bending N of the aluminum alloy sheet of the present disclosure s Preferably, the number is 17 or more.
[0050] (Second-phase particles) Toughness is affected by strength and the distribution of second-phase particles. That is, the higher the strength and the higher the density of second-phase particles, the lower the toughness. In particular, when the contents of Mg and Si are high, the distribution of Mg 2 As a result, Mg 2 The Si particles act as crack initiation points and propagation paths, which reduces toughness.
[0051] The aluminum alloy sheet of the present disclosure has an area of 0.3 μm in the L-ST cross section of the width direction central portion shown by the diagonal line in FIG. 2 More than Mg 2 The ratio of the total area of the Si particles in the L-ST cross section is preferably 0.2% or less. In Fig. 1, L indicates the longitudinal direction, ST indicates the plate thickness direction, and LT indicates the width direction.
[0052] Mg 2 The area ratio of Si particles can be measured, for example, by the following method. First, a measurement sample is cut, and the surface to be measured (i.e., the L-ST cross section) is mechanically polished to a mirror finish. Next, the polished surface (i.e., the L-ST cross section) is observed using an SEM (scanning electron microscope), and 10 fields of view are obtained in the central region of the plate thickness. The acceleration voltage of the SEM is 15 kV, the magnification is 1000 times, and the range of one field of view is 0.012 mm. 2 The image is taken as is, and a COMPO (backscattered electron composition) image is obtained.
[0053] The captured COMPO image is analyzed using the image analysis software "ImageJ." Specifically, the most frequent value of the image brightness in 256 gradations is defined as the background brightness, and particles with brightness lower than the value obtained by subtracting 30 from the most frequent brightness are defined as Mg particles. 2 It is determined to be a Si particle.
[0054] Determined Mg 2 Among the Si particles, 0.3 μm 2The total area of particles with an area of 0.3 μm or more was calculated and divided by the photographed area of 10 fields of view (i.e., the total photographed area), resulting in an area of 0.3 μm 2 More than Mg 2 The percentage of the total area of the Si particles in the L-ST cross section is calculated.
[0055] <Strength Anisotropy> It is known that materials with a low cold rolling reduction (hereinafter abbreviated as cold rolling reduction) have high toughness. In addition, the higher the cold rolling reduction, the higher the 0.2% proof stress σ 0.2_90° , 0.2% proof stress σ in the 0° direction 0.2_0° Therefore, the difference in 0.2% yield strength between the 0° direction and the 90° direction with respect to the rolling direction, that is, the strength anisotropy, can be associated with the cold rolling rate of the material.
[0056] The alloy sheet of the present disclosure has a 0.2% yield strength σ in the direction of 0° relative to the rolling direction, which is calculated by formula (5). 0.2_0° From this, 0.2% proof stress σ in the direction 90° to the rolling direction 0.2_90° It is preferable that the value D obtained by subtracting the above is −12 MPa or more and 12 MPa or less.
[0057] D = σ 0.2_0° -σ 0.2_90° ... (5) 0.2% proof stress σ in the 0° direction relative to the rolling direction 0.2_0° From this, 0.2% proof stress σ in the direction 90° to the rolling direction 0.2_90° The material structure meaning of the strength anisotropy minus can be explained as follows.
[0058] After hot rolling or annealing, the material is in a recrystallized state, with a high concentration of isotropic Cube orientation. From this point, plastic deformation by cold rolling transforms the Cube orientation into a rolling texture with anisotropy in the rolling direction. Furthermore, the larger the cold rolling rate, the more the crystal grains are elongated in the rolling direction, so the diameter of the crystal grains along the 0° direction relative to the rolling direction increases, while the change in the diameter of the crystal grains along the 90° direction relative to the rolling direction becomes smaller than in the 0° direction.
[0059] The structural changes caused by these rolling processes and the 0.2% yield strength σ 0.2The relationship between these two is expressed by the Hall-Petch equation as shown in Equation (6): In Equation (6), κ is the resistance to sliding of the grain boundary, and d is the grain size.
[0060] σ 0.2 ∝κ×d−½ (6) The resistance κ has different values when tension is applied in the 0° direction or 90° direction relative to the rolling direction. This is because the degree of integration of the rolling texture, which is anisotropic in the rolling direction, increases with an increase in the cold reduction ratio, and the resistance to sliding of the grain boundaries changes depending on the tension direction.
[0061] In addition, in the direction of 0° from the rolling direction, the grains elongate and their diameters increase with increasing cold rolling, whereas in the direction of 90° from the rolling direction, the change in grain size with increasing cold rolling is relatively small. The cumulative effect of these effects results in strength anisotropy with increasing cold rolling.
[0062] <Method for producing aluminum alloy sheet> The aluminum alloy sheet of the present disclosure can be produced, for example, as follows: First, an aluminum alloy having the composition of the aluminum alloy sheet of the present disclosure is subjected to a semi-continuous casting method (i.e., DC casting) according to a conventional method to produce an ingot.
[0063] Next, the four sides of the ingot, excluding the front and rear ends, are chamfered. The ingot is then placed in a soaking furnace for homogenization. The temperature in the homogenization is preferably, for example, 470°C or higher and 620°C or lower. The time for the homogenization is preferably, for example, 1 hour or higher and 20 hours or lower.
[0064] When the homogenization temperature is 400°C or higher, segregation of the ingot structure is easily eliminated. Furthermore, when the homogenization temperature is 450°C or higher, Mg 2 The homogenization temperature is 470°C or higher, preferably 550°C or higher, and the Mg 2 The re-dissolution of Si particles is promoted, and the strength and toughness of the alloy plate can be further improved. On the other hand, if the temperature in the homogenization treatment is 620°C or less, local melting of the aluminum alloy is unlikely to occur.
[0065] When the homogenization treatment time is 1 hour or more, the temperature of the entire slab becomes uniform, segregation of the ingot structure is easily eliminated, and Mg 2 The longer the homogenization time, the easier it is to redissolve the Si particles. 2 The Si particles can be redissolved. However, if the homogenization treatment time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.
[0066] After the homogenization treatment, the ingot is subjected to hot rolling. The hot rolling process includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of mm by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several mm by, for example, tandem rolling, and the plate material is wound into a coil to form a hot-rolled coil.
[0067] If the total reduction rate of the finish rolling is high, a recrystallized structure is formed after coiling, and the concentration of the isotropic Cube orientation can be increased. If the coiling temperature of the finish rolling is high, a recrystallized structure is formed after coiling, and the concentration of the Cube orientation can be increased.
[0068] Following the hot rolling, the plate material is cold rolled. In the cold rolling, the hot rolled coil is rolled until the product plate thickness is reached. The cold rolling may be either single rolling or tandem rolling. In the cold rolling by single rolling, it is preferable to perform the rolling in two or more passes.
[0069] Furthermore, by subjecting the coil to solution treatment during cold rolling to redissolve Mg and other elements, it is possible to obtain an alloy sheet with high strength and reduced final cold rolling rate, suppressing the anisotropy of the material. For example, by performing heat treatment (i.e., annealing) at a target solid temperature of 440°C or higher using a continuous annealing furnace (CAL), followed by forced cooling by air cooling or the like, it is possible to effectively increase the strength of the alloy sheet.
[0070] Furthermore, by setting the finishing temperature of cold rolling in intermediate passes other than the final pass to 120°C or higher, Si, Cu, and Mg are finely precipitated and age-hardened, thereby increasing the strength of the alloy sheet. Furthermore, by setting the finishing temperature to 130°C or higher, the strength of the alloy sheet can be further increased.
[0071] When no solution treatment is performed during cold rolling, the cold rolling rate is preferably 80% or more. When the cold rolling rate is 80% or more, the strength of the alloy sheet can be increased. Furthermore, the lower the cold rolling rate, the more isotropic Cube orientation remains, so the cold rolling rate is preferably 92% or less.
[0072] When solution treatment is performed during cold rolling, the cold rolling rate after solution treatment (i.e., annealing) is preferably 50% or more. By resolving Mg and other elements through solution treatment, the strength of the alloy sheet can be increased even if the cold rolling rate is low. Furthermore, the lower the cold rolling rate, the more isotropic Cube orientation remains, so the cold rolling rate is preferably 80% or less.
[0073] The cold rolling rate R (%) is the thickness t after hot rolling or solution treatment. 0 (mm), product thickness after cold rolling t 1 (mm) is calculated using the following formula (7).
[0074] R = (t 0 -t 1 ) / t 0 × 100 (7) The product plate thickness can be appropriately selected so as to obtain a desired pressure resistance. As shown in the above formula (2), the pressure resistance improves as the plate thickness increases. The product plate thickness can be selected according to the value V of formula (2), and is preferably such that the value V is 13.0 or more, preferably 14.0 or more. As described above, the aluminum alloy plate of the present disclosure can suppress an increase in plate thickness in order to maintain a high pressure resistance.
[0075] Coils that have been cold-rolled to the product thickness are pre-coated on a painting line, etc. The surface of the cold-rolled coil is degreased, cleaned, and chemically treated, and then painted, followed by a paint baking process.
[0076] Chemical solutions such as chromate-based and zirconium-based solutions are used in chemical conversion treatments. Epoxy-based and polyester-based paints are used. These can be selected according to the application. In the paint baking process, the coil is heated to a peak metal temperature (PMT) of 220°C to 270°C for approximately 30 seconds or less. The lower the PMT, the more the recovery of the material is suppressed, and the higher the strength of the alloy plate can be maintained.
[0077] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained.
[0078] (1a) High strength and high toughness of the aluminum alloy sheet can be achieved while incorporating scrap raw materials derived from can stock. That is, a certain amount of scrap 3104 aluminum alloy for can bodies can be incorporated, reducing the rate of virgin metal usage and reducing CO 2 Furthermore, it is possible to obtain an aluminum alloy sheet for can ends with high formability that can be used for positive pressure can ends, which require high pressure resistance.
[0079] [2. Other Embodiments] Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take on various forms.
[0080] (2a) In addition to the aluminum alloy sheet of the above embodiment, the present disclosure also includes various embodiments such as a member made of this aluminum alloy sheet and a method for manufacturing this aluminum alloy sheet.
[0081] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. Also, part of the configuration of the above embodiments may be omitted. Furthermore, at least part of the configuration of the above embodiments may be added to, replaced with, or the like, the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified by the wording of the claims are embodiments of the present disclosure.
[0082] 3. Examples The following describes the details of tests conducted to confirm the effects of the present disclosure and the evaluation results thereof.
[0083] <Production of Aluminum Alloy Sheets> As examples and comparative examples, aluminum alloy sheets S1 to S11 shown in Tables 1 and 2 were produced. Specific production procedures are described below.
[0084] First, an ingot containing the components (% by mass) of Alloy Nos. 1 to 5 shown in Table 3, with the balance being aluminum and unavoidable impurities, was produced by semi-continuous casting. The ingot contained 0.10% by mass or less of Ti, 0.25% by mass or less of Zn, 0.10% by mass or less of Cr, and 0.15% by mass or less of unavoidable impurities.
[0085] Next, the four sides of the ingot, excluding the front and rear ends, were chamfered. The ingot was then placed in a furnace and subjected to homogenization treatment. The homogenization treatment temperature is shown in Table 1. After the homogenization treatment, the ingot was removed from the furnace, and immediately hot rolling was started to produce a rolled sheet.
[0086] Furthermore, for S1, S2, S6-S9, and S11, the rolled sheets after hot rolling were cold rolled until they reached the CAL thickness shown in Table 1. Thereafter, the rolled sheets having the CAL thickness were annealed in a continuous annealing furnace (CAL). The CAL temperature during annealing is as shown in Table 1. After annealing, the rolled sheets were cooled to room temperature by air cooling. After cooling, the rolled sheets were cold rolled again. The target cold reduction ratios in cold rolling after annealing are as shown in Table 1.
[0087] For S3-S5 and S10, the hot-rolled sheets were subjected to cold rolling without annealing. The target cold rolling reduction ratios are shown in Table 1.
[0088] The product thickness after cold rolling in S1-S11 (i.e., t in Equation (7)) 1 ) was in the range of approximately 0.235±0.03 mm.
[0089] In S1-S11, after cold rolling, paint was applied to the sheet surface, and a paint baking treatment was carried out for about 30 seconds. The practical temperature (PMT) during paint baking is shown in Table 1. Aluminum alloy sheets S1-S11 were obtained by baking the paint. Furthermore, the sheet thicknesses (i.e., product sheet thicknesses) of the aluminum alloy sheets S1-S11 measured with a microgauge are shown in Table 1.
[0090]
[0091]
[0092]
[0093] <Evaluation of Aluminum Alloy Sheets> (Tensile Properties) Three No. 5 test pieces defined in JIS-Z-2241: 2011 were prepared from each of the aluminum alloy sheets S1-S11 by milling. The longitudinal directions of the three test pieces extended in directions forming angles of 0°, 45°, and 90° with respect to the rolling direction, respectively.
[0094] These test pieces were subjected to a tensile test in accordance with JIS-Z-2241:2011 to measure the 0.2% yield strength and tensile strength. 0.2 and tensile strength σ B The measurement results and the average value σ of 0.2% yield strength and tensile strength fm The results are shown in Tables 1 and 2.
[0095] Furthermore, three evaluation values S were calculated from the measurement results of the tensile tests in the 0° direction, the 45° direction, and the 90° direction relative to the rolling direction and from the formula (1). The minimum evaluation value S was the minimum of these evaluation values S. min is shown in Table 2.
[0096] (Toughness) In the aluminum alloy plates of S1-S11, the area of 0.3 μm was measured by the measurement method described in the embodiment. 2 More than Mg 2 The ratio of the total area (area ratio) of the Si particles in the L-ST cross section was calculated. The measurement results are shown in Table 2.
[0097] For the aluminum alloy plates S1-S11, the number of repeated bendings and the normalized number of repeated bendings were calculated using the measurement method described in the embodiment and equations (3) and (4). The results are shown in Table 2.
[0098] (Strength Anisotropy) For the aluminum alloy plates S1 to S11, the strength anisotropy (i.e., value D) was calculated from the formula (5) explained in the embodiment. The results are shown in Table 2.
[0099] (Scrap Blending Ratio) With respect to the compositions of the aluminum alloy plates S1 to S11, it was determined whether the possible blending ratio of 3104 aluminum alloy scrap was 50 mass % or more. The results are shown in Table 2.
[0100] In Table 2, aluminum alloy plates designated as "≧50" can contain 50 mass% or more of 3104 aluminum alloy. The possible blending ratio of 3104 aluminum alloy scrap is determined based on Table 4.
[0101] Table 4 shows the relationship between the blending ratios of 3104 aluminum alloy and 5182 aluminum alloy and the average values of the component specifications. The first row of Table 4 shows the average values of the component specifications of 3104 aluminum alloy, and the second row shows the average values of the component specifications of 5182 aluminum alloy.
[0102] For example, when the compounding ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.
[0103] Therefore, when the proportions of each component of the aluminum alloy sheet are equal to or greater than the above-mentioned values of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of 3104 aluminum alloy sheet is 50% by mass or more. As the blending ratio of 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase and the content of Mg decreases. The aluminum alloy sheets S1-S10 can be blended with 50% by mass or more of 3104 aluminum alloy scrap.
[0104]
[0105] (Evaluation) The aluminum alloy plates S1-S9 have a lower Mg content than the aluminum alloy plate S11, but have high strength (i.e., S min ) In addition, the aluminum alloy sheets S1-S7, which had been subjected to a higher homogenization treatment temperature, exhibited high strength and a high number of repeated bending times. For example, when comparing S6-S7 and S8-S9, S6-S7 has a higher strength than S8-S9, even though the process and paint baking temperature are the same, because the homogenization treatment temperature is higher.
[0106] Furthermore, the lower the paint baking temperature (PMT), the higher the strength of the alloy sheet. For example, when comparing S3-S5, S6-S7, and S8-S9, the examples with lower paint baking temperatures showed higher strength values.
[0107] Aluminum alloys S1-S7 are Mg 2 The area ratio of Si particles was small, 0.2% or less. Comparing S1-S7 with S8-S9, it was found that increasing the homogenization temperature increased the area ratio of Mg 2 It can be seen that the area ratio of Si particles can be significantly reduced. Furthermore, when comparing S6-S7 with S8-S9, for example, 2 S6-S7, which has a small area ratio of Si particles, has the same strength as S8-S9, but can be repeatedly bent many times, resulting in high strength and high toughness.
[0108] The number of repeated bending times varies depending on the strength. 2 Comparing S3-S5 and S6-S7, which have a relatively small area ratio of Si particles and the same cold rolling rate, S3-S5, which has lower strength than S6-S7, has a much higher number of repeated bending times than S6-S7.
[0109] Furthermore, the number of repeated bending cycles also varies depending on the anisotropy of the material structure. For example, when S1-S2, which has a strength anisotropy of -12 MPa or more and 10 or less, is compared with S6-S8, which has a strength anisotropy of less than -12 MPa, the strengths are relatively similar, but the number of repeated bending cycles for S1-S2 is much higher than for S6-S8. Furthermore, when S1-S2 and S3-S5 are compared, the number of repeated bending cycles is similar, but S1-S2 has a higher strength than S3-S5. S1-S2 is a material with a lower cold rolling rate and smaller anisotropy of the material structure than S3-S8, and has high strength and high toughness.
[0110] As shown in Figure 2, when comparing S1, S2, and S3, there is a negative correlation between strength anisotropy and cold rolling. In highly tough materials in which the cold rolling is suppressed to 50% or more and 80% or less by intermediate annealing or the like, the absolute value of strength anisotropy is thought to be maximum in the negative direction at a cold rolling of 80%. Here, based on the trend in Figure 2, it is estimated that the strength anisotropy at a cold rolling of 80% will be -12 MPa, so -12 MPa can be said to be the lower limit of strength anisotropy.
[0111] Similarly, the absolute value of strength anisotropy is considered to be maximum in the positive direction at a cold rolling rate of 50%, and from the trend in Figure 2, the strength anisotropy at a cold rolling rate of 50% is estimated to be 15 MPa. On the other hand, the lower the cold rolling rate, the closer the material is to a recrystallized state, which is an isotropic material structure with small anisotropy, so it is unlikely that the absolute value of strength anisotropy will monotonically increase in the positive direction. Therefore, with reference to S1, S2, and S11, it is considered appropriate that the strength anisotropy at a cold rolling rate of 50% is about 12 MPa.
Claims
1. The silicon (Si) content is 0.27% by mass or more and 0.39% by mass or less, the iron (Fe) content is 0.35% by mass or more and 0.55% by mass or less, the copper (Cu) content is 0.17% by mass or more and 0.25% by mass or less, the manganese (Mn) content is 0.75% by mass or more and 0.95% by mass or less, the magnesium (Mg) content is 2.2% by mass or more and 2.8% by mass or less, and the balance is aluminum (Al) and unavoidable impurities or contains the aluminum (Al) and the unavoidable impurities, and the 0.2% proof stress σ 0.2 , tensile strength σ B , and the average value of 0.2% yield strength and tensile strength σ fm Among the evaluation values S calculated by the following formula (1) using min The aluminum alloy sheet for can ends has a compressive strength of 330 MPa or more and 390 MPa or less. fm / (σ 0.2 / σ B ) ... (1) 2. The aluminum alloy sheet for can lids according to claim 1, wherein the area of the L-ST cross section in the widthwise center portion is 0.3 μm 2 More than Mg 2 The aluminum alloy sheet for can ends, wherein the ratio of the total area of Si particles in the L-ST cross section is 0.2% or less.
3. The aluminum alloy sheet for can lids according to claim 1 or 2, wherein the minimum evaluation value S min is 360 MPa or more and 390 MPa or less, and the 0.2% proof stress σ in the 0° direction with respect to the rolling direction is 0.2_0° From the above, the 0.2% yield strength σ 0.2_90° The aluminum alloy sheet for can ends, wherein the value obtained by subtracting 4. The aluminum alloy sheet for can lids according to claim 2, wherein a test piece cut into a rectangular shape having a width of 12.5 mm and a length of 200 mm is repeatedly bent 90° in a direction in which the bending ridgeline is parallel to the rolling direction and then returned to the 0° position. The number of repeated bending operations N, which is the number of bending operations until the test piece breaks, is normalized by the plate thickness t of the test piece and the following formula (2) to obtain a normalized number of repeated bending operations N: s The aluminum alloy sheet for can ends has a strength of 17 times or more. s = N × t / 0.235 ... (2) 5. The aluminum alloy sheet for can lids according to claim 3, wherein a test piece cut into a rectangular shape having a width of 12.5 mm and a length of 200 mm is repeatedly bent by bending the test piece 90° in a direction in which the bending ridge line is parallel to the rolling direction and then returning it to the 0° position. The number of repeated bending operations N until the test piece breaks is normalized by the plate thickness t of the test piece and the following formula (2) to obtain a normalized number of repeated bending operations N: s The aluminum alloy sheet for can ends has a strength of 17 times or more. s = N × t / 0.235 ... (2)
Citation Information
Patent Citations
Plate surface protective agent for planographic plate
JP1989269594A
Aluminum alloy laminate for can cover adapted to recycling and manufacture thereof
JP1997070925A
Aluminum alloy sheet for can end
JP2000160273A
Manufacture of aluminum alloy hard sheet for can-top
JP2001073106A
Aluminum alloy sheet for negative pressure can-top
JP2016160511A