Cu PILLAR JOINED BODY AND METHOD FOR MANUFACTURING Cu PILLAR JOINED BODY

The Cu pillar assembly with a porous Cu layer and solder layer addresses the thermal reliability issues in micro-junction technologies by enabling efficient intermetallic compound formation at low temperatures and short times, enhancing the thermal reliability of semiconductor device bonding.

WO2024219418A1PCT designated stage expired Publication Date: 2024-10-24MITSUBISHI MATERIALS CORP

Patent Information

Application Number
PCT/JP2024/015252
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing micro-junction technologies, such as the SLID method, face issues with poor thermal reliability due to the presence of low melting point solder material and require lengthy heating periods, which decreases production efficiency and increases the risk of thermal cycle failures in semiconductor devices.

Method used

A Cu pillar assembly is formed with a porous Cu layer on one pillar and a solder layer on the other, along with an intermetallic compound layer, where the porous Cu layer has a porosity of 5% to 80%, allowing for efficient diffusion and formation of intermetallic compounds at low temperatures and short times, reducing residual solder material and enhancing thermal reliability.

Benefits of technology

The method effectively promotes the formation of intermetallic compounds at low temperatures and short times, resulting in a Cu pillar assembly with excellent thermal reliability and minimal residual solder, improving the efficiency and reliability of semiconductor device bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015252_24102024_PF_FP_ABST
    Figure JP2024015252_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This Cu pillar joined body is obtained by joining a first Cu pillar and a second Cu pillar via a joining layer, wherein: the joining layer has a porous Cu layer formed on the first Cu pillar side, a solder layer formed on the second Cu pillar side, and an intermetallic compound layer formed between the porous Cu layer and the solder layer; and the porosity in the porous Cu layer is within the range of 5-80%.
Need to check novelty before this filing date? Find Prior Art

Description

Cu pillar bonded body and method for manufacturing the same

[0001] The present invention relates to a Cu pillar joining method for joining a first Cu pillar and a second Cu pillar. This application claims priority to Japanese Patent Application No. 2023-67191, filed on April 17, 2023, the contents of which are incorporated herein by reference.

[0002] In recent years, the performance of semiconductor devices has been improving, and micro-bonding technology has become increasingly important. Flip-chip mounting is a widely used mounting technology for IC chips, and as shown in Patent Document 1, for example, a method is provided in which a solder layer is formed on a protruding electrode and then the electrode is bonded by solder.

[0003] Furthermore, in order to cope with further narrowing of the pitch, bonding techniques such as the TLP method (Transient Liquid Phase Diffusion Bonding) and the SLID method (Solid-Liquid Interdiffusion) have been proposed, which bond by mutual diffusion of a solid phase and a liquid phase. In the SLID method, as shown in Patent Documents 1 and 2, a solder material is used as the material that forms the liquid phase.

[0004] JP 2018-046148 A Japanese Patent No. 6061276 A Japanese Patent No. 6369620 A

[0005] However, the SLID method uses solder as described above, but if a large amount of low-melting-point solder remains after joining, there is a risk that the heat resistance will be poor and the thermal cycle reliability and thermal reliability will be insufficient. In order to diffuse the solder and form an intermetallic compound, long heating times are required, which poses a problem of reduced production efficiency.

[0006] The present invention has been made in view of the above-mentioned circumstances, and aims to provide a Cu pillar bonded structure in which an intermetallic compound can be sufficiently formed even under low temperature and short time conditions, and in which a large amount of solder layer does not remain, resulting in excellent thermal reliability, and a method for manufacturing the Cu pillar bonded structure.

[0007] In order to solve the above problems, the inventors conducted extensive research and discovered that by forming a porous Cu layer on the bonding surface of the Cu pillar, the surface area of ​​the bonding surface of the Cu pillar is increased and the diffusion rate is increased, thereby promoting the generation of intermetallic compounds and making it possible to prevent a large amount of low-melting-point solder material from remaining after bonding.

[0008] The present invention has been made based on the above-mentioned findings, and a Cu pillar bonded body of aspect 1 of the present invention is a Cu pillar bonded body in which a first Cu pillar and a second Cu pillar are bonded via a bonding layer, wherein the bonding layer has a porous Cu layer formed on the first Cu pillar side, a solder layer formed on the second Cu pillar side, and an intermetallic compound layer formed between the porous Cu layer and the solder layer, and the porosity of the porous Cu layer is in the range of 5% or more and 80% or less.

[0009] According to the Cu pillar bonded body of aspect 1 of the present invention, the bonding layer formed between the first Cu pillar and the second Cu pillar has a porous Cu layer formed on the first Cu pillar side, a solder layer formed on the second Cu pillar side, and an intermetallic compound layer formed between the porous Cu layer and the solder layer, and the porosity of the porous Cu layer is within the range of 5% to 80%. Therefore, even under low temperature and short time conditions, the liquid phase of the molten solder layer and the solid phase of the porous Cu layer sufficiently interdiffuse to promote the generation of an intermetallic compound, thereby preventing a large amount of low-melting point solder material from remaining, and providing excellent thermal reliability.

[0010] A Cu pillar bonded body of Aspect 2 of the present invention is characterized in that, in the Cu pillar bonding method of Aspect 1, a diffusion barrier layer is formed between the second Cu pillar and the solder layer. According to the Cu pillar bonded body of Aspect 2 of the present invention, since a diffusion barrier layer is formed between the second Cu pillar and the solder layer, diffusion of metal elements constituting the solder layer into the second Cu pillar can be suppressed, and sufficient interdiffusion can occur between the liquid phase in which the solder layer is molten and the solid phase porous Cu layer, thereby enabling reliable bonding of the first Cu pillar and the second Cu pillar.

[0011] A Cu pillar bonded body of Aspect 3 of the present invention is characterized in that a second porous Cu layer is formed between the second Cu pillar and the solder layer in the Cu pillar bonded body of Aspect 1 or Aspect 2. According to the Cu pillar bonded body of Aspect 3 of the present invention, since the second porous Cu layer is formed between the second Cu pillar and the solder layer, it is possible to promote the generation of an intermetallic compound also on the second porous Cu layer side, and it is further possible to suppress the residual of a large amount of low-melting-point solder material, and it is possible to manufacture a pillar bonded body with excellent thermal reliability.

[0012] A Cu pillar bonded structure according to Aspect 4 of the present invention is characterized in that the solder layer is made of In or an In alloy in the Cu pillar bonded structure according to any one of Aspects 1 to 3. According to the Cu pillar bonded structure according to Aspect 4 of the present invention, since the solder layer is made of In or an In alloy, bonding can be performed under low-temperature conditions of 200°C or less.

[0013] A manufacturing method of a Cu pillar bonded body according to a fifth aspect of the present invention is a manufacturing method of a Cu pillar bonded body in which a first Cu pillar and a second Cu pillar are bonded, and is characterized by comprising: a porous Cu layer forming process for forming a porous Cu layer having a porosity in the range of 5% to 80% on the bonding surface of the first Cu pillar; a solder layer forming process for forming a solder layer on one surface of the second Cu pillar; a stacking process for stacking the first Cu pillar on which the porous Cu layer is formed and the second Cu pillar on which the solder layer is formed; and a joining process for heat-treating the stacked first Cu pillar and second Cu pillar at a temperature of 120°C to 200°C to generate an intermetallic compound between the porous Cu layer and the solder layer, thereby joining the first Cu pillar and the second Cu pillar.

[0014] According to the manufacturing method of a Cu pillar bonded body of aspect 5 of the present invention, a porous Cu layer having a porosity in the range of 5% to 80% is formed on the bonding surface of the first Cu pillar, the first Cu pillar and the second Cu pillar are stacked via a solder material, and heat-treated at a temperature of 120°C to 200°C. Therefore, the liquid phase of the molten solder layer and the solid phase of the porous Cu layer are sufficiently interdiffused to promote the generation of an intermetallic compound, and the remaining low-melting point solder material is suppressed, making it possible to produce a pillar bonded body with excellent thermal reliability.

[0015] A manufacturing method of a Cu pillar bonded body according to Aspect 6 of the present invention is the manufacturing method of a Cu pillar bonded body according to Aspect 5, characterized in that it further includes a diffusion barrier layer forming step of forming a diffusion barrier layer on the bonding surface of the second Cu pillar, and in the solder layer forming step, the solder layer is formed on the diffusion barrier layer. According to the manufacturing method of a Cu pillar bonded body according to Aspect 6 of the present invention, since it includes the diffusion barrier layer forming step of forming a diffusion barrier layer on the bonding surface of the second Cu pillar, it is possible to suppress diffusion of metal elements constituting the solder layer into the second Cu pillar, and it is possible to sufficiently interdiffuse the liquid phase of the molten solder layer and the solid phase porous Cu layer, thereby enabling reliable bonding of the first Cu pillar and the second Cu pillar.

[0016] A manufacturing method of a Cu pillar bonded body according to Aspect 7 of the present invention is the manufacturing method of a Cu pillar bonded body according to Aspect 5 or Aspect 6, characterized in that it includes a second porous Cu layer forming step of forming a second porous Cu layer on the bonding surface of the second Cu pillar, and in the solder layer forming step, the solder layer is formed on the second porous Cu layer. According to the manufacturing method of a Cu pillar bonded body according to Aspect 7 of the present invention, since it includes the second porous Cu layer forming step of forming a second porous Cu layer on the bonding surface of the second Cu pillar, it is possible to promote the generation of an intermetallic compound even on the second porous Cu layer side formed on the bonding surface of the second Cu pillar, and it is possible to manufacture a pillar bonded body with excellent thermal reliability.

[0017] A manufacturing method of a Cu pillar bonded body according to Aspect 8 of the present invention is characterized in that, in the manufacturing method of a Cu pillar bonded body according to any one of Aspects 5 to 7, the solder layer forming step forms a solder layer made of In or an In alloy. According to the manufacturing method of a Cu pillar bonded body according to Aspect 8 of the present invention, since the solder layer made of In or an In alloy is formed in the solder layer forming step, bonding can be performed under low-temperature conditions of 200°C or less.

[0018] According to the present invention, it is possible to provide a Cu pillar bonded structure in which an intermetallic compound can be sufficiently formed even under low temperature and short time conditions, and in which a large amount of solder layer does not remain, resulting in excellent thermal reliability, and a method for manufacturing the Cu pillar bonded structure.

[0019] 1 is an explanatory diagram of a Cu pillar bonded body according to one embodiment of the present invention; FIG. 2 is a flow chart of a method for manufacturing a Cu pillar bonded body according to one embodiment of the present invention; FIG. 3 is an explanatory diagram of a Cu pillar bonding method (method for manufacturing a Cu pillar bonded body) according to one embodiment of the present invention; FIG. 4 is an explanatory diagram of a Cu pillar bonded body according to one embodiment of the present invention;

[0020] Hereinafter, a Cu pillar bonded structure and a method for manufacturing the Cu pillar bonded structure according to an embodiment of the present invention will be described with reference to the drawings.

[0021] The Cu pillar bonded structure 1 according to this embodiment is, for example, a semiconductor device in which protruding electrodes (Cu pillars) formed on a semiconductor chip are bonded together. As shown in Fig. 1 , the Cu pillar bonded structure 1 according to this embodiment has a structure in which a first Cu pillar 11 formed on a first wafer 10 and a second Cu pillar 21 formed on a second wafer 20 are bonded via a bonding layer 30.

[0022] The bonding layer 30 includes a porous Cu layer 31 formed on the first Cu pillar 11 side, a solder layer 32 formed on the second Cu pillar 21 side, and an intermetallic compound layer 33 formed between the porous Cu layer 31 and the solder layer 32.

[0023] The porous Cu layer 31 formed on the first Cu pillar 11 side has nano-sized pores. Here, the porous Cu layer 31 has an average porosity P ave The average porosity P is in the range of 5% to 80%. ave is the average value of the porosity P calculated as follows. In this embodiment, the porosity P is calculated at three locations, and the average value of the porosity P is taken as the average porosity P ave The porosity P is calculated by determining the total area S1 of the porous Cu layer 31 and the area S2 of the pores in the porous Cu layer 31 through image analysis of the cross section of the porous Cu layer 31 using a scanning electron microscope, and then calculating the porosity P using the following formula: Porosity P (%) = (S2 / S1) × 100

[0024] On the other hand, in this embodiment, the diffusion prevention layer 22 is formed between the second Cu pillar 21 and the solder layer 32 formed on the second Cu pillar 21 side.

[0025] The diffusion prevention layer 22 prevents the metal elements constituting the solder layer 23 from diffusing toward the second Cu pillar 21. In this embodiment, the diffusion prevention layer 22 is made of Ni. The thickness of the diffusion prevention layer 22 is preferably within a range of 0.5 μm to 3 μm.

[0026] The solder layer 32 is made of a solder material made of a metal with a low melting temperature, and the melting temperature is preferably 200° C. or lower. In this embodiment, the solder layer 32 is made of In or an In alloy, and more specifically, the solder layer 32 is an In—Sn alloy (Sn concentration is 0 mass % or more and 75 mass % or less). Furthermore, it is preferable to use a low-alpha-ray material that generates a small amount of alpha rays as the solder material that makes up the solder layer 32.

[0027] The intermetallic compound layer 33 formed between the solder layer 32 and the porous Cu layer 31 is formed by mutual diffusion between the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31. The thickness of the bonding layer 30 (the total thickness of the porous Cu layer 31, the solder layer 32, and the intermetallic compound layer 33) is preferably in the range of 3 μm to 20 μm. The area ratio of the intermetallic compound layer 33 in the bonding layer 30 is preferably 50% or more, more preferably 70% or more, and even more preferably 90% or more. The upper limit of the area ratio of the intermetallic compound layer 33 in the bonding layer 30 is not particularly limited, but may be 99% or less. The area ratio of the intermetallic compound layer 33 in the bonding layer 30 is the IMC ratio, which will be described later.

[0028] Next, the manufacturing method of the Cu pillar bonded body 1 of this embodiment includes a pillar forming process S01, a porous Cu layer forming process S02, a diffusion prevention layer forming process S03, a solder material disposing process S04, a stacking process S05, and a bonding process S06, as shown in FIG. 2.

[0029] 3A and 3B, resist layers 41 and 51 are formed on one surface of the first wafer 10 and the second wafer 20. With the resist layers 41 and 51 formed, Cu plating is performed to form the first Cu pillar 11 and the second Cu pillar 21. Note that before forming the first Cu pillar 11 and the second Cu pillar 21, an adhesion layer (e.g., a Ti layer) and a seed layer (Cu layer) may be formed on one surface of the first wafer 10 and the second wafer 20.

[0030] <Porous Cu Layer Forming Step S02> Next, as shown in Fig. 3C, a porous Cu layer 31 is formed on the bonding surface of the first Cu pillar 11. In this embodiment, with the resist layer 41 formed, plating is performed as follows to form the porous Cu layer 31. Here, a method for forming the porous Cu layer 31 will be described. Examples of methods for forming the porous Cu layer 31 include a dealloying method and a direct plating method.

[0031] (Dealloying Method) In the dealloying method, copper and a metal species that is electrochemically less noble than copper are codeposited by electroplating on the bonding surface of the first Cu pillar 11 to form a copper alloy plating film, and then the less noble metal species in the copper alloy plating film are dealloyed to form the porous Cu layer 12. In this dealloying method, the deposition ratio and deposition form of copper and the metal species that are less noble than copper are respectively controlled, thereby making it possible to form a porous Cu layer 31 with a desired porosity and shape.

[0032] Copper alloy plating, which uses zinc as a metal species electrochemically less noble than copper, is formed using a copper-zinc alloy plating solution containing, for example, copper salt, zinc salt, and additives and solvents that control the deposition of copper and zinc. This copper alloy plating can be performed by electroless plating or electrolytic plating. Metal species electrochemically less noble than copper, such as Fe and Mn, can also be selected as alloy species.

[0033] In copper-zinc alloy plating, copper sulfate, zinc sulfate, zinc pyrophosphate, zinc phosphate, etc. can be used as metal salts. The copper ions and zinc ions in the copper-zinc alloy plating solution are preferably each 0.001 to 1.0 moles, and the molar ratio of copper ions to zinc ions is preferably within the range of Cu:Zn = 1:1 to 1:1000. The zinc ion concentration is made higher than the copper ion concentration because copper deposits preferentially over zinc due to the difference in standard oxidation-reduction potential.

[0034] Citric acid or pyrophosphate may also be added as a supporting salt (complexing agent). Brighteners include, for example, surfactants such as alkanolamines, glycine, serine, alanine, tyrosine, aspartic acid, glutamic acid, histidine, and salts thereof. The pH of the plating solution is preferably 2.5 or higher to adjust the balance of copper and zinc deposition. The pH of the plating solution is preferably 5 or lower. The cathode current density is preferably 0.3 A / dm 2 0.8A / dm or more 2 Set within the following range.

[0035] After the copper-zinc alloy plating film is formed, the resist layer 41 is removed using a resist stripper, followed by a dealloying process. Examples of dealloying processes for the formed copper-zinc alloy plating film include an etching reaction using a chemical solution and an electrochemical anodic reaction. In this embodiment, acid dealloying is performed by immersing and stirring the copper alloy film in a solution containing hydrochloric acid with a concentration of 0.002 mol / L to 0.5 mol / L at a temperature ranging from 20°C to 35°C for 30 minutes or more, depending on the thickness of the plating film, to remove zinc from the copper-zinc alloy plating film. This forms a porous Cu layer 31 on the bonding surface of the first Cu pillar 11.

[0036] Next, the formed porous Cu layer 31 is washed with a cleaning solvent such as ethanol, water, or acetone, and then dried in the atmosphere using dry air. In order to prevent surface oxidation, it is preferable to immerse the layer 31 in a rust inhibitor containing benzotriazole and a surfactant as its main components for a predetermined period of time.

[0037] (Direct Plating Method) In the direct plating method, a Cu plating solution containing an azole-based additive, which is a copper ion electrodeposition inhibitor, is used to perform electroplating on the bonding surface of the first Cu pillar 11, thereby forming a porous Cu layer 31 having a porous structure. After the porous Cu layer 31 is formed, the resist layer 41 is removed using a resist stripper. In this direct plating method, it is possible to form a porous Cu layer 31 having a desired porosity and shape by controlling the type and content of the additive contained in the Cu plating solution and the plating conditions.

[0038] The Cu plating solution used is an acidic electrolytic copper plating solution containing a soluble copper salt, an azole compound having two to three nitrogen atoms in a five-membered ring as a copper ion electrodeposition inhibitor, acid, and water. If necessary, a brightener, a surfactant, an antioxidant, etc. may be added. The Cu plating solution used has a copper concentration of 0.1 mol / L or more, an azole compound concentration of 10 mmol / L or more and 50 mmol / L or less, and a chloride ion concentration of 10 ppm or less.

[0039] Specific examples of soluble copper salts include copper sulfate, copper oxide, copper carbonate, copper alkanesulfonates such as copper methanesulfonate and copper propanoate, copper alkanolsulfonates such as copper isethionate and copper propanolsulfonate, and copper organic acids such as copper acetate, copper citrate, and copper tartrate. These can be used alone or in combination of two or more.

[0040] Furthermore, the acid may be an organic acid or an inorganic acid. Examples of such acids include sulfuric acid; alkanesulfonic acids such as methanesulfonic acid and propanesulfonic acid; alkanolsulfonic acids such as isethionic acid and propanolsulfonic acid; and organic acids such as citric acid and tartaric acid. These may be used alone or in combination of two or more. The water may be pure water such as ion-exchanged water or distilled water.

[0041] The plating conditions are, for example, a DC power supply with a current density of 0.1 A / dm 2 ~5 A / dm 2 Approximately, preferably 0.4 A / dm 2 ~1.0 A / dm 2 The plating time is selected so that the desired porous Cu layer 12 can be formed. When Cu plating is performed under the above conditions, the azole compound, which is a copper ion electrodeposition inhibitor, as well as the copper ions are adsorbed on the cathode surface, which is the bonding surface of the first Cu pillar 11. The presence of the azole compound strongly suppresses the electrodeposition of copper ions, giving priority to copper nucleation, and a porous Cu layer 31 is formed on the cathode surface as a copper plating film.

[0042] 3A, a diffusion prevention layer 22 is formed on the bonding surface of the second Cu pillar 21. In this embodiment, the diffusion prevention layer 22 made of Ni is formed by performing Ni plating with the resist layer 51 formed.

[0043] <Solder Layer Formation Step S04> Next, as shown in FIG. 3D , a solder material is disposed so as to be laminated on the diffusion prevention layer 22 formed on the bonding surface of the second Cu pillar 21, thereby forming a solder layer 32. In this embodiment, the solder layer 32 is formed by plating the solder material on a resist layer 51 formed thereon. After the solder layer 32 is formed, the resist layer 51 is removed using a resist remover. Here, the thickness of the solder layer 32 is preferably within a range of 1 μm to 10 μm. The solder material is composed of In or an In alloy. Specifically, the solder layer 32 is an In—Sn alloy (Sn concentration: 0 mass% to 75 mass%). Note that the solder material constituting the solder layer 32 is preferably a low-alpha-ray material that generates a low amount of alpha rays.

[0044] 3E, a first Cu pillar 11 having a porous Cu layer 31 formed on its joining surface is laminated on a second Cu pillar 21 having a diffusion barrier layer 22 and a solder layer 32 formed on its joining surface. Specifically, the first Cu pillar 11 is laminated so that the porous Cu layer 31 and the solder layer 32 are in contact with each other, thereby obtaining a laminate structure in which the first Cu pillar 11, the porous Cu layer 31, the solder layer 32, the diffusion barrier layer 22, and the second Cu pillar 21 are laminated in this order.

[0045] 3(E), the stacked first Cu pillar 11 and second Cu pillar 21 are heated while being pressed in the stacking direction to bond the first Cu pillar 11 and the second Cu pillar 21. This produces a pillar bonded body 1 in which the first Cu pillar 11 and the second Cu pillar 21 are bonded, as shown in FIG.

[0046] In this embodiment, the first Cu pillar 11 and the second Cu pillar 21 are joined by solid-liquid interdiffusion bonding (SLID) bonding, which bonds the first Cu pillar 11 and the second Cu pillar 21 by mutual diffusion between the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31. That is, the mutual diffusion between the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 forms an intermetallic compound layer 33, and the first Cu pillar 11 and the second Cu pillar 21 are joined.

[0047] In this embodiment, the pressure load in the bonding step S06 is preferably in the range of 0.1 MPa to 20 MPa. Also, in this embodiment, the bonding temperature in the bonding step S06 is preferably in the range of 120° C. to 200° C. Furthermore, in this embodiment, the holding time at the bonding temperature in the bonding step S06 is preferably in the range of 10 seconds to 3 minutes.

[0048] According to the Cu pillar bonded body 1 of this embodiment configured as described above, the bonding layer 30 formed between the first Cu pillar 11 and the second Cu pillar 21 has a porous Cu layer 31 formed on the first Cu pillar 11 side, a solder layer 32 formed on the second Cu pillar 21 side, and an intermetallic compound layer 33 formed between the porous Cu layer 31 and the solder layer 32. Since the porosity of the porous Cu layer 31 is within the range of 5% or more and 80% or less, even under low temperature and short time conditions, the liquid phase in which the solder layer 32 is molten and the solid phase of the porous Cu layer 31 sufficiently interdiffuse to promote the generation of an intermetallic compound, thereby preventing a large amount of low-melting point solder material from remaining, resulting in excellent thermal reliability.

[0049] In the Cu pillar joint body 1 of this embodiment, when a diffusion prevention layer 22 is formed on the joining surface of the second Cu pillar 21, the metal elements constituting the solder layer 13 can be prevented from diffusing toward the second Cu pillar 21, and the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 can be sufficiently interdiffused to promote the generation of intermetallic compounds, thereby ensuring reliable joining of the first Cu pillar 11 and the second Cu pillar 12.

[0050] In the Cu pillar bonding body 1 of this embodiment, when the solder layer 32 is composed of In or an In alloy, a liquid phase can be generated even at low temperatures of 200°C or less, and the first Cu pillar 11 and the second Cu pillar 12 can be reliably bonded by the SLID method.

[0051] According to the manufacturing method of the Cu pillar joint body 1 of this embodiment, a porous Cu layer 31 having a porosity in the range of 5% or more and 80% or less is formed on the joint surface of the first Cu pillar 11, the first Cu pillar 11 and the second Cu pillar 12 are stacked via the solder layer 32, and heat treatment is performed at a temperature of 120°C or more and 200°C or less.Therefore, the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 are sufficiently interdiffused with each other, promoting the generation of an intermetallic compound and preventing a large amount of low-melting point solder material from remaining, thereby making it possible to manufacture a pillar joint body 1 with excellent thermal reliability.

[0052] In the manufacturing method of the Cu pillar joint body 1 of this embodiment, if a diffusion prevention layer formation process S03 is included in which a diffusion prevention layer 22 is formed on the joint surface of the second Cu pillar 21, the metal elements constituting the solder layer 32 can be prevented from diffusing into the second Cu pillar 21, and the first Cu pillar 11 and the second Cu pillar 21 can be reliably joined.

[0053] Furthermore, in this embodiment, when a low-alpha ray material that generates a small amount of alpha rays is used as the solder material that constitutes the solder layer 32, the occurrence of soft errors can be suppressed in a semiconductor device that includes the pillar bonding structure 1 of this embodiment, and a semiconductor device that can be used stably can be constructed.

[0054] Although the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate within the scope of the technical concept of the invention. For example, in this embodiment, the diffusion prevention layer 22 made of Ni is formed, but the present invention is not limited to this and may not include a diffusion prevention layer.

[0055] In addition, in the present embodiment, the porous Cu layer is formed on the first Cu pillar side, but this is not limiting, and as in the pillar joint body 101 shown in FIG. 4 , the second porous Cu layer 34 may be formed on the second Cu pillar 21 side, and the solder layer 32 may be formed so as to contact this second porous Cu layer 34. In this case, a second intermetallic compound layer 35 is formed between the solder layer 32 and the porous Cu layer 34.

[0056] The results of confirmation experiments conducted to confirm the effectiveness of the present invention will be described below.

[0057] First, a Si wafer (thickness: 0.8 mm) with a seed layer formed on its surface was used. The seed layer was formed by sputtering a titanium layer (thickness: 100 nm) on the wafer surface and a copper layer (thickness: 500 nm) on top of the titanium layer. The Si wafer surface was patterned with photoresist to form a 75 μm diameter bump pattern (total number of bumps: 625), and a resist layer with openings was formed on the seed layer.

[0058] In Examples 1 to 12, the wafer described above was used as the first wafer, and a first Cu pillar and a porous Cu layer were formed on one surface of this first wafer. In Comparative Example 1, no porous Cu layer was formed.

[0059] Here, in Inventive Examples 1 to 6 and Comparative Example 2, a porous Cu layer was formed by a dealloying method. Copper-zinc alloy electroplating was performed using a copper-zinc alloy electroplating solution. Table 1 shows the plating conditions for the dealloying method in Inventive Examples 1 to 6. After forming the copper-zinc alloy plating layer, the resist layer was dissolved and removed using a dry film resist stripper. Next, an etching solution was used to remove the seed layer from the portion where the copper-zinc alloy plating layer was not formed. Next, the copper-zinc alloy plating layer was immersed in a solution containing hydrochloric acid at a concentration of 1.00 mol / L at 27°C, and the solution was stirred for 70 minutes to remove zinc from the copper-zinc alloy plating layer and dealloy it.

[0060]

[0061] In Inventive Examples 7 to 12 and Comparative Example 3, a porous Cu layer was formed by a direct plating method. Copper plating was performed using a copper plating bath. Table 2 shows the plating conditions for the direct plating method in Inventive Examples 7 to 12 and Comparative Example 3. In the direct plating method, after porous copper plating, the resist layer was dissolved and removed using a dry film resist stripper, and the seed layer was etched.

[0062]

[0063] The wafer described above was used as a second wafer, and a second Cu pillar, a diffusion barrier layer made of Ni, and a solder layer were formed on one surface of the second wafer by plating. The thicknesses of each were as shown in Table 3.

[0064] Then, the first Cu pillar and the second Cu pillar shown in Table 3 were stacked, and after alignment was performed using a high-precision flip-chip bonder T-300-PRO manufactured by Treky, they were pressurized at a pressure of 0.1 MPa in a nitrogen atmosphere and heat-treated at the bonding temperature shown in Table 3 for 1 minute, thereby bonding the first Cu pillar and the second Cu pillar together to obtain a pillar bonded assembly.

[0065] Here, the average porosity P in the formed porous Cu layer ave was calculated as follows. The cross section of the porous Cu layer was analyzed using a scanning electron microscope (SU-8240 manufactured by Hitachi High-Technologies Corporation) to determine the total area S1 of the porous Cu layer and the area S2 of the pores in the porous Cu layer, and the porosity P was calculated using the following formula: Porosity P (%) = (S2 / S1) × 100. The porosity P was calculated at three locations, and the average porosity P was calculated as the average value of the porosity P. ave The evaluation results are shown in Table 3.

[0066] In addition, the cross section of the joint portion of the pillar joint body was observed using a scanning electron microscope (SU-8240 manufactured by Hitachi High-Technologies Corporation), and the state of formation of metal compounds in the joint portion (IMC ratio: ratio of intermetallic compounds) was evaluated. The cross section of the joint layer of the pillar joint body was processed using a cross section polisher (CP), and an SEM image (scanning electron microscope image) and an EDS map (element map by energy dispersive X-ray spectroscopy) of Cu and the solder metals (In, Sn) were obtained. The overlapping area of ​​the solder metal (In, Sn) and the EDS map of Cu was determined to be an intermetallic compound. Then, the area ratio of metal compounds in the joint portion (IMC ratio) was calculated using the following formula. IMC ratio (%) = (EDS overlap area of ​​solder material (In, Sn) and Cu) / (EDS area of ​​solder material (In, Sn)) × 100

[0067] The IMC ratio (%) was rated as "good" when it was 90% or more, "fair" when it was 50% or more but less than 90%, and "poor" when it was less than 50%. The evaluation results are shown in Table 3.

[0068] (In Table 3, the unit of thickness is μm, Ni is the thickness of Ni observed in the EDS map and indicates the diffusion prevention layer, In is the thickness of In observed in the EDS map, and Sn is the thickness of Sn observed in the EDS map.)

[0069] In Comparative Example 1, where no porous Cu layer was formed, intermetallic compounds were not sufficiently generated under conditions of 200°C and 1 minute, and a large amount of low-melting-point solder layer remained. In Comparative Example 2, where the porosity of the porous Cu layer was 85%, intermetallic compounds were not sufficiently generated under conditions of 150°C and 1 minute, and a large amount of low-melting-point solder layer remained. In Comparative Example 3, where the porosity of the porous Cu layer was 3%, intermetallic compounds were not sufficiently generated under conditions of 200°C and 1 minute, and a large amount of low-melting-point solder layer remained.

[0070] In contrast, in Examples 1 to 12 of the present invention, in which a porous Cu layer with a porosity in the range of 5% to 80% was formed, sufficient intermetallic compounds were generated, and the remaining low-melting point solder layer was suppressed.

[0071] From the results of the above confirmatory experiments, it was confirmed that the present invention can provide a Cu pillar bonded structure that can sufficiently form an intermetallic compound even under low temperature and short time conditions, does not leave a large amount of solder layer remaining, and has excellent thermal reliability, as well as a method for manufacturing the Cu pillar bonded structure.

[0072] REFERENCE SIGNS LIST 1,101 Cu pillar bonded assembly 11 First Cu pillar 21 Second Cu pillar 30 Bonding layer 31 Porous Cu layer 32 Solder layer 33 Intermetallic compound layer

Claims

1. A Cu pillar joint body in which a first Cu pillar and a second Cu pillar are joined via a joining layer, the joining layer having a porous Cu layer formed on the first Cu pillar side, a solder layer formed on the second Cu pillar side, and an intermetallic compound layer formed between the porous Cu layer and the solder layer, the porosity of the porous Cu layer being within the range of 5% or more and 80% or less.

2. A Cu pillar bonded body according to claim 1, characterized in that a diffusion prevention layer is formed between the second Cu pillar and the solder layer.

3. A Cu pillar joint assembly as described in claim 1, characterized in that a second porous Cu layer is formed between the second Cu pillar and the solder layer.

4. The Cu pillar joint assembly according to claim 1, characterized in that the solder layer is composed of In or an In alloy.

5. A method for manufacturing a Cu pillar joint body in which a first Cu pillar and a second Cu pillar are joined, comprising: a porous Cu layer formation process for forming a porous Cu layer having a porosity in the range of 5% to 80% on a joining surface of the first Cu pillar; a solder layer formation process for forming a solder layer on one surface of the second Cu pillar; a stacking process for stacking the first Cu pillar on which the porous Cu layer is formed and the second Cu pillar on which the solder layer is formed; and a joining process for heat-treating the stacked first Cu pillar and second Cu pillar at a temperature of 120°C to 200°C to generate an intermetallic compound between the porous Cu layer and the solder layer, thereby joining the first Cu pillar and the second Cu pillar.

6. A method for manufacturing a Cu pillar joint body as described in claim 5, characterized in that it includes a diffusion prevention layer formation process for forming a diffusion prevention layer on the joint surface of the second Cu pillar, and in the solder layer formation process, the solder layer is formed on the diffusion prevention layer.

7. A method for manufacturing a Cu pillar joint body as described in claim 5, characterized in that it includes a second porous Cu layer formation process for forming a second porous Cu layer on the joint surface of the second Cu pillar, and in the solder layer formation process, the solder layer is formed on the second porous Cu layer.

8. The method for manufacturing a Cu pillar bonded body according to claim 5, characterized in that in the solder layer formation step, a solder layer made of In or an In alloy is formed.

Citation Information

Patent Citations

  • Metal pillar with cushioned tip

    US20170278815A1

  • Metallic Interconnect, a Method of Manufacturing a Metallic Interconnect, a Semiconductor Arrangement and a Method of Manufacturing a Semiconductor Arrangement

    US20190103378A1

  • Substrate joining method

    WO2015079582A1

  • Conductive pillar and method for manufacturing same, and method for manufacturing bonded structure

    WO2021145129A1

Cited By

  • Method for producing nanoporous copper structure, nanoporous copper structure, and electroless copper-plating solution