Separator for electrochemical device and electrochemical device comprising same

The use of a porous polymer substrate with optimized amorphous and crystalline resin composition and TREF processing addresses the structural integrity and breakdown voltage issues in electrochemical device separators, improving their performance and reliability by preventing deformation and defects.

WO2024219669A1PCT designated stage expired Publication Date: 2024-10-24LG ENERGY SOLUTION LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003422
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-19
Filing Date
2024-03-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing separators for electrochemical devices face challenges in maintaining their structural integrity and breakdown voltage during the lamination process, leading to issues like deformation and defects such as Hi-Pot and low voltage defects due to pressure applied during bonding.

Method used

A porous polymer substrate with a specific composition of amorphous and crystalline polymer resins, processed through temperature rise elution fractionation (TREF), is used to enhance the mechanical properties and prevent deformation, including a weight average molecular weight of 100,000 or more and a polydispersity index of 5 or more, which improves compression resistance and breakdown voltage.

Benefits of technology

The solution effectively minimizes deformation and improves the breakdown voltage of the separator, preventing Hi-Pot and low voltage defects, thereby enhancing the overall performance and reliability of electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003422_24102024_PF_FP_ABST
    Figure KR2024003422_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a separator for an electrochemical device and an electrochemical device comprising same, wherein the compression resistance and breakdown voltage of the separator can be improved by selecting a specific type of polymer resin included in a porous polymer substrate and adjusting the polydispersity index, weight average molecular weight, content of an elution fraction at a specific temperature, and indentation depth, with respect to a polymer eluted at a high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Separator for electrochemical devices and electrochemical devices containing the same

[0001] This application is based on and claims the benefit of priority from Korean Patent Application Nos. 10-2023-0051176, 10-2023-0055916, and 10-2023-0065754, filed with the Korean Intellectual Property Office on April 19, 2023, April 28, 2023, and May 22, 2023, respectively, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a separator for an electrochemical device and an electrochemical device including the same.

[0003] Among the components of electrochemical devices, the separator comprises a porous polymer substrate located between the anode and cathode. It isolates the anode and cathode, prevents electrical short-circuiting between the two electrodes, and allows the passage of electrolytes and ions. While the separator itself does not participate in electrochemical reactions, its physical properties, such as wettability with electrolyte, degree of porosity, and thermal shrinkage, influence the performance and safety of the electrochemical device.

[0004] Accordingly, various methods have been attempted to enhance the physical properties of membranes by adding a coating layer to a porous polymer substrate and by adding various substances to the coating layer to change the properties of the coating layer. For example, inorganic substances may be added to the coating layer to enhance the mechanical strength of the membrane, or inorganic substances or hydrates may be added to the coating layer to enhance the flame retardancy and heat resistance of the polymer substrate.

[0005] The technical problem to be achieved by the present invention is to provide a separator for an electrochemical device and an electrochemical device including the same, which can improve the breakdown voltage of the separator by preventing deformation of the separator and damage to pores caused by pressure applied in a lamination process for bonding the separator and electrode.

[0006] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.

[0007] One embodiment of the present invention provides a separator for an electrochemical device, comprising a porous polymer substrate, wherein the porous polymer substrate comprises an amorphous polymer resin and a crystalline polymer resin, and wherein the weight average molecular weight (Mw) of an elution product eluted from the porous polymer substrate by temperature rising elution fractionation (TREF) is about 100,000 or more.

[0008] According to one embodiment of the present invention, the porous polymer substrate may contain about 40 wt% or less of a fraction eluted at a temperature of 35°C or lower by a temperature rising elution fractionation method.

[0009] According to one embodiment of the present invention, the content of the amorphous polymer resin in the porous polymer substrate may be about 40 wt% or less.

[0010] According to one embodiment of the present invention, the content of the crystalline polymer resin in the porous polymer substrate may be about 60 wt% or more.

[0011] According to one embodiment of the present invention, the weight ratio of the amorphous polymer resin and the crystalline polymer resin in the porous polymer substrate may be about 1:1 to 10:1.

[0012] According to one embodiment of the present invention, the deviation in the indentation depth in the porous polymer substrate may be about -5 nm or more and 5 nm or less.

[0013] According to one embodiment of the present invention, the porous polymer substrate includes a polyolefin resin, and the amorphous polymer resin may be an amorphous polyolefin resin, and the crystalline polymer resin may be a crystalline polyolefin resin.

[0014] According to one embodiment of the present invention, the polyolefin resin may be one selected from the group consisting of polyethylene; polypropylene; polybutylene; polypentene; polyhexene; polyoctene; copolymers of at least one of ethylene, propylene, butene, pentene, 4-methylpentene, hexene, or octene; and combinations thereof.

[0015] According to one embodiment of the present invention, the polyolefin resin may have an average short chain branch (SCB) of about 500 or less per 1000 total carbon atoms.

[0016] According to one embodiment of the present invention, the polyolefin resin may have a melt index (ASTM D1238, 190°C, 2.16 kg) of about 0.1 g / 10 min to 0.3 g / 10 min.

[0017] According to one embodiment of the present invention, the weight average molecular weight (Mw) of the porous polymer substrate may be about 500,000 or more and 1,000,000 or less.

[0018] According to one embodiment of the present invention, the polydispersity index (PDI) of the eluate may be about 5 or more.

[0019] According to one embodiment of the present invention, when a pressure of 8 MPa is applied at 70°C, any one or more of the following (i) to (iii) may be satisfied:

[0020] (i) The thickness reduction rate of the porous polymer substrate defined by the following mathematical formula 1 is about 10% or less:

[0021] [Mathematical Formula 1]

[0022] Thickness reduction rate (%) = (thickness of porous polymer substrate before applying pressure - thickness of porous polymer substrate after applying pressure) / thickness of porous polymer substrate before applying pressure X 100

[0023] (ii) The increase in air permeability after compression of the porous polymer substrate defined by the following mathematical formula 2 is about 185% or less:

[0024] [Equation 2]

[0025] Increase in air permeability (%) = (Air permeability after compression - Air permeability before compression) / (Air permeability before compression) X 100

[0026] (iii) The breakdown voltage of the porous polymer substrate is approximately 1,000 V or more.

[0027] According to one embodiment of the present invention, the porous polymer substrate may have a thickness of about 1 ㎛ or more and 30 ㎛ or less.

[0028] One embodiment of the present invention provides an electrochemical device including: an anode; a cathode; and a separator interposed between the anode and the cathode.

[0029] A separator for an electrochemical device according to one embodiment of the present invention can improve the breakdown voltage by minimizing deformation due to pressure applied in a lamination process by improving the weight average molecular weight and polydispersity index of an effluent eluted at high temperature.

[0030] An electrochemical device according to one embodiment of the present invention can improve battery performance by preventing Hi-Pot failure and low voltage failure.

[0031] Figure 1 is a drawing schematically illustrating a method for measuring indentation depth.

[0032] In some of the accompanying drawings, corresponding components are designated by the same reference numerals. Those skilled in the art will appreciate that the drawings illustrate elements simply and clearly and are not necessarily drawn to scale. For example, to facilitate understanding of various embodiments, the dimensions of some elements depicted in the drawings may be exaggerated relative to other elements. Furthermore, elements of known technology that are useful or essential in commercially feasible embodiments may often not be depicted so as not to obscure the spirit of various embodiments of the present invention.

[0033] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.

[0034] In this specification, “A and / or B” means “A and B, or A or B.”

[0035] In this specification, when it is said that a component is “provided on”, this does not exclude other components being placed in between, unless otherwise specifically stated, but rather means that other components may be placed thereon.

[0036] As used herein, the terms "about," "approximately," and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values ​​provided to aid understanding of the present invention.

[0037] In this specification, the characteristic of “having pores” means that the object includes a plurality of pores and that the pores are interconnected with each other, thereby allowing gaseous and / or liquid fluids to pass from one side of the object to the other side.

[0038] In this specification, the separator has a porous characteristic including a large number of pores, and acts as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the cathode and the anode in an electrochemical device.

[0039] Hereinafter, the present invention will be described in more detail.

[0040] In a secondary battery electrode assembly, a separator can be bonded to the electrode through a lamination process, and a polymer binder can be added to the coating layer composition of the separator to secure adhesion between the electrode and the separator.

[0041] Meanwhile, in the lamination process, when the process speed is increased to improve yield, the time over which heat is applied is reduced, which leads to a problem of reduced adhesive strength. While this problem is being addressed by increasing the pressure during the lamination process to improve adhesive strength, the high pressure applied to the separator causes deformation, such as a reduction in the thickness of the separator, and damage to the pores reduces the breakdown voltage of the separator, leading to Hi-pot failures and low-voltage failures.

[0042] The present invention provides a separator capable of preventing a decrease in the thickness of the separator and improving the breakdown voltage by controlling the polymer resin included in the porous polymer substrate.

[0043] In the case of polyethylene applied to the porous substrate of the membrane, crystalline and amorphous phases are mixed, and the higher the crystalline content and the narrower the molecular weight distribution at this time, the better the compression resistance that affects the degree of thickness deformation of the fabric after compression. Meanwhile, when propylene is added during the polyethylene polymerization process to improve processability in the manufacture of polyethylene film, the amorphous content increases. Accordingly, in the present invention according to one embodiment, propylene is not added during the polyethylene polymerization process or is added in a small amount below the standard value, thereby increasing or controlling the crystalline content in the manufactured porous substrate, thereby improving various properties of the membrane, such as compression resistance.

[0044] One embodiment of the present invention provides a separator for an electrochemical device, comprising a porous polymer substrate manufactured by the above method, wherein the porous polymer substrate includes an amorphous polymer resin and a crystalline polymer resin, and the weight average molecular weight (Mw) of the eluted product when analyzed by temperature rising elution fractionation (TREF) of the porous polymer substrate is about 100,000 or more.

[0045] In the manufacture of a separator for an electrochemical device according to one embodiment of the present invention, as described above, by not adding propylene or adding a small amount of propylene during the polyethylene polymerization process, the content of crystals is increased or controlled, thereby improving the weight average molecular weight and polydispersity index of the elution product eluted at high temperatures, thereby minimizing deformation due to pressure applied during the lamination process, thereby improving the breakdown voltage.

[0046] One embodiment of the present invention relates to a separator for an electrochemical device, the separator itself or a separator that can be applied to a component. Accordingly, the separator according to one embodiment of the present invention may additionally have another layer disposed on at least one surface of the porous polymer substrate, in terms of material or function, as needed. For example, in one embodiment of the present invention, the separator may have a coating layer comprising inorganic particles and / or a polymer binder, for example, an organic / inorganic composite coating layer, formed on at least one or both surfaces of the porous polymer substrate.

[0047] According to one embodiment of the present invention, the separator for an electrochemical device includes a porous polymer substrate. As described above, the separator for an electrochemical device includes a porous polymer substrate, thereby blocking electrical contact between the positive and negative electrodes while allowing lithium ions to pass through, and can implement a shutdown function at an appropriate temperature. In the present specification, the "shutdown function" may mean that the pores of the porous polymer substrate are blocked under abnormal high-temperature conditions, thereby preventing lithium ions from passing through the separator.

[0048] According to one embodiment of the present invention, the porous polymer substrate includes an amorphous polymer resin and a crystalline polymer resin. For example, the polymer resin included in the porous polymer substrate may include both crystalline and amorphous polymer resins, such that the amorphous polymer resin and the crystalline polymer resin are uniformly mixed and included, or may include both an amorphous structure and a crystalline structure within a single molecule. As described above, by the porous polymer substrate including the amorphous polymer resin and the crystalline polymer resin, the uniformity of the porous polymer substrate can be improved and the compression resistance can be increased.

[0049] According to one embodiment of the present invention, the porous polymer substrate of the present invention includes both crystalline and amorphous polymer resins contained in the porous polymer substrate by controlling the presence or absence of addition of propylene during a polyethylene polymerization process, and when the porous polymer substrate is analyzed by temperature rising elution fractionation (TREF), the weight average molecular weight (Mw) of the eluted product is about 100,000 or more. For example, when the porous polymer substrate is eluted by temperature rising elution fractionation (TREF), the weight average molecular weight (Mw) of the eluted product is about 100,000 or more and 10,000,000 or less, 200,000 or more and 9,000,000 or less, 300,000 or more and 8,000,000 or less, 400,000 or more and 7,000,000 or less, 500,000 or more and 6,000,000 or less, 600,000 or more and 5,000,000 or less, 700,000 or more and 4,000,000 or less, 800,000 or more and 3,000,000 or less, 900,000 or more and 2,000,000 or less, or It may be 900,000 or more and 1,000,000 or less. When the porous polymer substrate is eluted by temperature rising elution fractionation (TREF) within the above-described range, the weight average molecular weight (Mw) of the eluted product is controlled within the above-described range, thereby improving the uniformity of the porous polymer substrate and increasing the compressibility.

[0050] According to one embodiment of the present invention, the eluate may be eluted by temperature rising elution fractionation (TREF) at a temperature of about 90°C to 110°C. For example, the eluate may be eluted by temperature rising elution fractionation (TREF) at a temperature of about 90°C to 110°C, 91°C to 109°C, 92°C to 108°C, 93°C to 107°C, 94°C to 106°C, 95°C to 105°C, 96°C to 104°C, 97°C to 103°C, 98°C to 102°C, or 99°C to 101°C. The porous polymer substrate of the present invention includes both crystalline and amorphous polymer resins contained in the porous polymer substrate by controlling the presence or absence of propylene added during the polyethylene polymerization process. As described above, by controlling the temperature at which the elution product of the porous polymer substrate is eluted by temperature rising elution fractionation (TREF) within the above range, the uniformity of the porous polymer substrate can be improved and the compression resistance can be increased. Furthermore, the mechanical properties of the porous polymer substrate can be improved.

[0051] In this specification, the "temperature rising elution fractionation (TREF)" analysis can be measured using a TREF machine of PolymerChar. That is, the temperature rising elution fractionation method can be to melt a sample and inject it into a column at a high temperature, then gradually lower the temperature to induce crystallization of the sample, and when the sample precipitates inside the column, increase the temperature and measure the molecular weight of the eluted sample. For example, a 40 mg polymer sample is dissolved in 20 mL of trichlorobenzene solvent at 150 °C for 120 minutes and then stabilized at 100 °C for 45 minutes. After introducing this into a TREF column, it is cooled to 35 °C at a cooling rate of 0.5 °C per minute and then maintained for 15 minutes. After that, it can mean that the weight average molecular weight of the eluted polymer sample is measured while heating at a rate of 20°C per minute from 35°C to 80°C and maintaining the temperature at 5°C increments for 20 minutes, and then heating at a rate of 20°C per minute from 80°C to 120°C and maintaining the temperature at 2°C increments for 20 minutes, and then a TREF analysis graph is derived from the concentration measurement results.

[0052] According to one embodiment of the present invention, the porous polymer substrate may include about 40 wt% or less of a fraction eluted at a temperature of 35°C or lower by a temperature-rising elution fractionation method. For example, the porous polymer substrate may include a first fraction eluted at a temperature of 35°C or lower and a second fraction eluted at a temperature of more than 35°C when analyzed by a temperature-rising elution fractionation method. The first fraction may include an amorphous polymer resin. The second fraction may include a crystalline polymer resin, as the porous polymer substrate is eluted at a temperature of more than 35°C by a temperature-rising elution fractionation method. For example, the second fraction may be one eluted at a temperature of more than 35°C and less than 100°C, more than 40°C and less than 90°C, more than 50°C and less than 80°C, or more than 60°C and less than 70°C. Alternatively, the second fraction may be eluted at a temperature of 98°C or higher.

[0053] According to one embodiment of the present invention, the content of the amorphous polymer resin in the porous polymer substrate may be about 40 wt% or less. For example, the content of the amorphous polymer resin in the porous polymer substrate may be about 0 wt% to 40 wt% or less, 2 wt% to 38 wt% or less, 4 wt% to 36 wt% or less, 6 wt% to 34 wt% or less, 8 wt% to 32 wt% or less, 10 wt% to 30 wt% or less, 12 wt% to 28 wt% or less, 14 wt% to 26 wt% or less, 16 wt% to 24 wt% or less, or 18 wt% to 22 wt% or less. By controlling the content of the amorphous polymer resin in the porous polymer substrate within the above-described range, the uniformity of the porous polymer substrate can be improved, and compression resistance can be increased. Furthermore, the mechanical properties of the porous polymer substrate can be improved.

[0054] According to one embodiment of the present invention, the content of the crystalline polymer resin in the porous polymer substrate may be about 60 wt% or more. For example, the content of the crystalline polymer resin in the porous polymer substrate may be about 60 wt% or more and less than 100 wt%, 62 wt% or more and 98 wt% or less, 64 wt% or more and 96 wt% or less, 66 wt% or more and 94 wt% or less, 68 wt% or more and 92 wt% or less, 70 wt% or more and 90 wt% or less, 72 wt% or more and 88 wt% or less, 74 wt% or more and 86 wt% or less, 76 wt% or more and 84 wt% or less, or 78 wt% or more and 82 wt% or less. Alternatively, the content of the crystalline polymer resin in the porous polymer substrate may be about 70 wt% or more and 85 wt% or less. By controlling the content of the crystalline polymer resin in the porous polymer substrate within the above-described range, the uniformity of the porous polymer substrate can be improved and the compression resistance can be increased. Furthermore, the mechanical properties of the porous polymer substrate can be improved.

[0055] According to one embodiment of the present invention, the weight ratio of the amorphous polymer resin and the crystalline polymer resin in the porous polymer substrate may be about 1:1 to 10:1. For example, the weight ratio of the amorphous polymer resin and the crystalline polymer resin in the porous polymer substrate may be about 1.5:1 to 9.5:1, 2.0:1 to 9.0:1, 2.5:1 to 8.5:1, 3.0:1 to 8.0:1, 3.5:1 to 7.5:1, 4.0:1 to 7.0:1, 4.5:1 to 6.5:1, 5.0:1 to 6.0:1. By controlling the weight ratio of the amorphous polymer resin and the crystalline polymer resin in the porous polymer substrate within the above-described range, the uniformity of the porous polymer substrate can be improved, and the compression resistance can be increased. Furthermore, the mechanical properties of the porous polymer substrate can be improved.

[0056] According to one embodiment of the present invention, the content of the crystalline polymer resin in the porous polymer substrate may be about 70 wt% or more and 85 wt% or less based on 100 wt% of the porous polymer substrate. By controlling the content of the crystalline polymer resin in the porous polymer substrate within the above-described range, the indentation depth of the porous polymer substrate can be implemented to be low, and the deviation in the indentation depth can be minimized, thereby improving the insulation breakdown voltage.

[0057] According to one embodiment of the present invention, the indentation depth of the porous polymer substrate may be about 20 nm or less. For example, the indentation depth of the porous polymer substrate may be about 0 nm or more and 20 nm or less, more than 0 nm and 19 nm or less, 1 nm or more and 18 nm or less, 2 nm or more and 17 nm or less, 3 nm or more and 16 nm or less, 4 nm or more and 15 nm or less, 5 nm or more and 14 nm or less, 6 nm or more and 13 nm or less, 7 nm or more and 12 nm or less, 8 nm or more and 11 nm or less, or 9 nm or more and 10 nm or less. By controlling the indentation depth of the porous polymer substrate within the above-described range, the compression resistance of the porous polymer substrate can be improved, the thickness uniformity of the porous polymer substrate after lamination can be improved, and thickness deformation can be minimized.

[0058] In this specification, “indentation” is an analysis technique for the mechanical properties of a material, and is an experimental method that compares and analyzes the indentation marks and the load during indentation after indenting a material with a diamond indenter of various shapes. This indentation test is not only a technique for measuring the fracture toughness or hardness of a material, but has also been studied in various other directions recently, and is also used as a research technique for the elastic-plastic behavior of materials, analysis of residual stress states, adhesion tests of thin films, fracture characteristics, and phase transformation analysis. For example, when performing indentation on a fine material such as a membrane as in the present invention, nanoindentation can be applied, which applies a load of units of N (Newton) or less using an indenter.

[0059] Fig. 1 is a drawing schematically illustrating a method for measuring indentation depth. In the present specification, “indentation depth” may be measured by setting Dimension Icon (Bruker) under the following conditions, moving the tip relative to the sample surface as shown in Fig. 1, measuring the peak tapping force, and measuring the depth of the tip penetrating the sample surface at the time when the peak tapping force is measured using an atomic force microscope (AFM, Atomic Force Microscope, OSTESPA-R3, Bruker, f=300 kHz, k=26 N / m).

[0060] - Mode: Tapping (Peak Force QNM)

[0061] - Scan speed (0.3 Hz)

[0062] - Peak Force setpoint: 100 nN, Amplitude: 300 nm

[0063] - Scan angle: 90 °

[0064] According to one embodiment of the present invention, the deviation in the indentation depth in the porous polymer substrate may be about -5 nm or more and 5 nm or less. For example, the deviation in the indentation depth in the porous polymer substrate may be about -4 nm or more and 4 nm or less, -3 nm or more and 3 nm or less, -2 nm or more and 2 nm or less, -1 nm or more and 1 nm or less, -0.5 nm or more and 0.5 nm or less, or -0.1 nm or more and 0.1 nm or less. In the present specification, the deviation means the difference in variation with respect to the average, and may mean the difference in the indentation depth at a specific location of the porous polymer substrate with respect to the average of the indentation depths of the porous polymer substrate. By controlling the deviation in the indentation depth in the porous polymer substrate within the above-described range, the breakdown voltage of the porous polymer substrate can be improved.

[0065] According to one embodiment of the present invention, the porous polymer substrate may include a polyolefin-based resin. As described above, the porous polymer substrate includes a polyolefin-based resin, thereby facilitating the formation of a separator for the electrochemical device, and implementing a shutdown function when high temperatures occur during battery operation.

[0066] According to one embodiment of the present invention, the amorphous polymer resin may be an amorphous polyolefin resin. In the present specification, "amorphous" may mean that molecules are arranged without any rules. As described above, by selecting the amorphous polymer resin as an amorphous polyolefin resin, a shutdown function can be implemented when a high temperature occurs during battery operation.

[0067] According to one embodiment of the present invention, the crystalline polymer resin may be a crystalline polyolefin resin. As used herein, "crystalline" may mean that molecules are arranged in a regular manner. As described above, by selecting the crystalline polymer resin as a crystalline polyolefin resin, the mechanical properties of the porous polymer resin can be improved and the compression resistance can be improved.

[0068] In this specification, “crystallization degree” may mean the content of crystals eluted at about 98°C or higher when measured by TREF.

[0069] According to one embodiment of the present invention, the polyolefin-based resin may be one selected from the group consisting of polyethylene; polypropylene; polybutylene; polypentene; polyhexene; polyoctene; copolymers of at least one of ethylene, propylene, butene, pentene, 4-methylpentene, hexene, or octene; and combinations thereof. For example, the polyolefin-based resin may be polyethylene. By selecting the polyolefin-based resin from the above, the porous polymer substrate can include a crystalline polymer resin and an amorphous polymer resin, thereby improving the mechanical properties and compression resistance of the porous polymer.

[0070] According to one embodiment of the present invention, the polyolefin-based resin may have an average short chain branch (SCB) of about 500 or less per 1000 total carbon atoms of the polyolefin included therein. The short chain branch may be the number of methyl groups per 1000 total carbon atoms (CH3 / 1000TC). The short chain branch may interfere with the formation of a crystal structure during the crystallization process of the polymer, thereby affecting the physical properties of the substrate. The number of short chain branches may be controlled by adjusting the type and content of the monomer included in the polyolefin substrate. For example, the number of short chain branches included in the polyolefin substrate may be controlled by adjusting the type and content of the polyolefin-based polymer resin used in the polymerization process of the polymer resin used in the polyolefin substrate and / or the film forming process using the polymer resin. For example, when polymerizing a polyolefin-based polymer resin, the number of short-chain branches can be increased by increasing the content of propylene, butylene, etc., or by adding polypropylene, etc. during the film forming process. The number of short-chain branches can be confirmed by comparing the resins included in the fractions eluted at each temperature when analyzed according to the temperature rising elution fractionation method. For example, the number of short-chain branches can be confirmed as the number of CH3 per about 1000 carbon atoms using an IR detector and CH, CH2, CH3 filters used when performing the temperature rising elution fractionation method. For example, the polyolefin substrate may have an average number of short-chain branches per about 1000 total carbon atoms of about 100 to 500, 150 to 450, 200 to 400, or 250 to 350. Alternatively, the polyolefin substrate may have an average number of short-chain branches of 400 or less per 1,000 total carbon atoms. If the number of average short-chain branches exceeds the above-described range, it is detrimental to the orientation of the polyolefin-based polymer resin included in the polyolefin substrate.By controlling the number of average short-chain branches within the above-described range, the orientation of the crystalline polyolefin polymer resin can be achieved, thereby providing a polyolefin substrate having compression resistance for a lamination process.

[0071] According to one embodiment of the present invention, the polyolefin-based resin may have a melt index of about 0.1 g / 10 min to 0.3 g / 10 min. The melt index can be measured by ASTM D1238, and can be obtained by placing a sample in a cylinder and heating it to about 190° C., or placing a heated sample in the cylinder and placing a piston that applies a load of about 2.16 kg, and measuring the weight of the resin discharged through an orifice (inner diameter: 2.09 mm, length: 8 mm) located opposite the piston, and converting it into the amount passed over 10 minutes. By controlling the melt index of the polyolefin within the above-described range, the rigidity of the porous polymer substrate including the polyolefin-based resin can be determined, thereby providing a porous polymer substrate having compression resistance for a lamination process.

[0072] According to one embodiment of the present invention, the weight average molecular weight (Mw) of the porous polymer substrate may be about 500,000 or more and 3,000,000 or less. For example, the weight average molecular weight (Mw) of the porous polymer substrate may be about 500,000 or more and 2,500,000 or less, or 1,000,000 or more and 2,000,000 or less. By controlling the weight average molecular weight (Mw) of the porous polymer substrate within the above-described range, the mechanical properties and compression resistance of the porous polymer substrate can be improved. Furthermore, when different types of polyolefin resins are mixed and used or a separator is formed with a multilayer structure composed of different types of polyolefin resins, the weight average molecular weight of the polyolefin resin can be calculated by adding the weight average molecular weights according to the content ratio of each polyolefin resin.

[0073] In this specification, the weight average molecular weight (Mw) and polydispersity index can be measured by gel permeation chromatography (GPC: gel permeation chromatography, PL GPC220, Agilent Technologies), and the measurement conditions can be set as follows.

[0074] - Column: PL Olexis (Polymer Laboratories)

[0075] - Solvent: TCB (Trichlorobenzene)

[0076] - Flow rate: 1.0 ml / min

[0077] - Sample concentration: 1.0 mg / ml

[0078] - Injection volume: 200 ㎕

[0079] - Column temperature: 160 ℃

[0080] - Detector: Agilent High Temperature RI detector

[0081] - Standard: Polystyrene (corrected with a cubic function)

[0082] According to one embodiment of the present invention, in addition to the polyolefin-based resin, other resin components may be further mixed as needed, and, in addition to the resin components, filler particles may be included, for example. The filler particles may be introduced for the purpose of a pressure barrier to prevent the thickness, pore size, and porosity of the membrane substrate from being excessively reduced against the high pressure applied in the lamination process described below. The filler particles may include organic or inorganic fillers having a predetermined particle size, and are not limited to a specific component as long as they have a strength higher than that of the polyolefin-based resin.

[0083] According to one embodiment of the present invention, the porous polymer substrate may be manufactured by a method (wet method) of mixing a polyolefin resin with a plasticizer (diluent) at a high temperature to form a single phase, separating the polymer material and the plasticizer during a cooling process, extracting the plasticizer to form pores, and then performing stretching and heat-setting.

[0084] According to one embodiment of the present invention, the average size of the pores of the separation membrane and the maximum size of the pores can be easily manufactured by a person skilled in the art by controlling the mixing ratio of the plasticizer, the stretching ratio, the heat-setting treatment temperature, etc. to conform to the scope of the present invention.

[0085] According to one embodiment of the present invention, the pore size can be calculated from the pore size distribution measured using the Capillary Flow Porometer method. For example, first, the membrane to be measured is wetted with a wetting agent such as a Galwick solution, and then the air pressure on one side of the substrate is gradually increased. When the applied air pressure becomes greater than the capillary attraction of the wetting agent present in the pores, the wetting agent blocking the pores is pushed out, and the pore size and distribution are measured through the pressure and flow rate at the moment of being pushed out, and from this, the average pore size and maximum size can be confirmed.

[0086] The above porous polymer substrate may include pores having an average diameter of about 0.01 μm or more and 1 μm or less. For example, the size of the pores included in the porous polymer substrate may be about 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. By controlling the pore size of the porous polymer substrate within the above-described range, the air permeability and ionic conductivity of the entire manufactured membrane can be controlled.

[0087] According to one embodiment of the present invention, the polydispersity index (PDI) of the effluent may be about 5 or more. For example, the polydispersity index (PDI) of the effluent may be about 6 or more and 19 or less, 7 or more and 18 or less, 8 or more and 17 or less, 9 or more and 16 or less, 10 or more and 15 or less, 11 or more and 14 or less, or 12 or more and 13 or less. By controlling the polydispersity index of the effluent within the above-described range, the uniformity of the crystalline polymer resin can be improved, and the compression resistance can be improved.

[0088] According to one embodiment of the present invention, when a pressure of 8 MPa is applied at about 70°C, the separation membrane may satisfy at least one of the following (i) to (iii):

[0089] (i) The thickness reduction rate of the porous polymer substrate defined by the following mathematical formula 1 may be about 10% or less.

[0090] [Mathematical Formula 1]

[0091] Thickness reduction rate (%) = (thickness of porous polymer substrate before applying pressure - thickness of porous polymer substrate after applying pressure) / thickness of porous polymer substrate before applying pressure X 100

[0092] For example, when a pressure of 8 MPa is applied at about 70°C, the thickness reduction rate of the porous polymer substrate defined by the following mathematical formula 1 may be about 0% to 10%, 1% to 9%, 2% to 8%, 3% to 7%, or 4% to 6%. By implementing the thickness reduction rate of the porous polymer substrate within the above-described range, the compression resistance of the separation membrane can be improved.

[0093] (ii) The increase rate of air permeability after compression of the porous polymer substrate defined by the following mathematical formula 2 may be about 185% or less.

[0094] [Equation 2]

[0095] Increase in air permeability (%) = (Air permeability after compression - Air permeability before compression) / (Air permeability before compression) X 100

[0096] Whether the porous polymer substrate has compression resistance can be determined by the rate of change in air permeability of the substrate before and after compression. Before compression, the porous polymer substrate may have an air permeability of about 10 s / 100cc or more and 100 s / 100cc or less. For example, the air permeability of the porous polymer substrate may be about 10 s / 100cc or more and 90 s / 100cc or less, about 20 s / 100cc or more and 80 s / 100cc or less, about 30 s / 100cc or more and 70 s / 100cc or less, or about 40 s / 100cc or more and 60 s / 100cc or less. Alternatively, the air permeability of the porous polymer substrate may be about 50 s / 100cc or more and 80 s / 100cc or less. When the air permeability of the porous polymer substrate is within the above-described range, the air permeability of the manufactured separator can be provided within a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0097] In addition, when the porous polymer substrate is compressed at 70°C and a pressure of 8 MPa for about 10 seconds, the increase in air permeability after compression may be about 0% or more and 180% or less, 20% or more and 160% or less, 40% or more and 140% or less, 60% or more and 120% or less, or 80% or more and 100% or less. Alternatively, the porous polymer substrate after compression may have an air permeability of about 200 s / 100cc or less. A porous polymer substrate satisfying an air permeability increase rate within the above-described range can reduce the occurrence of defects due to deformation of its shape even during a lamination process. When a substrate having an air permeability exceeding about 200 s / 100cc after compression under the above conditions is used, the output and cycle characteristics of the electrochemical device may be deteriorated.

[0098] The above air permeability (s / 100cc) means the time (in seconds) it takes for about 100cc of air to pass through a porous polymer substrate or membrane of a predetermined area under a constant pressure. The above air permeability can be measured using an air permeability tester (Gurley densometer) according to ASTM D 726-58, ASTM D726-94 or JIS-P8117. For example, using a 4110N device from Gurley, air at a pressure of about 0.304kPa or air at a pressure of about 1.215 kN / m 2 About 100 cc of air under the pressure of water occupies about 1 square inch (or about 6.54 cm 2 ) can be used to measure the time it takes for a sample of about 100 cc of air to pass through a sample of about 1 square inch under a constant pressure of 4.8 inches of water at room temperature. For example, using the Asahi Seico EG01-55-1MR equipment, the time it takes for about 100 cc of air to pass through a sample of about 1 square inch can be measured.

[0099] (iii) The breakdown voltage of the porous polymer substrate may be about 1,000 V or more.

[0100] For example, when a pressure of 8 MPa is applied at about 70°C, the breakdown voltage of the porous polymer substrate may be about 1,000 V or more and 2,000 V or less, 1,100 V or more and 1,900 V or less, 1,200 V or more and 1,800 V or less, 1,300 V or more and 1,700 V or less, or 1,400 V or more and 1,600 V or less. By controlling the breakdown voltage of the porous polymer substrate within the above-described range, the insulation of the porous polymer substrate can be improved.

[0101] In this specification, the breakdown voltage may mean a voltage when the voltage is increased at a rate of about 100 mV / s on a specimen having a thickness of about 12 μm and exceeds about 0.5 mA and 3 seconds.

[0102] According to one embodiment of the present invention, the porous polymer substrate may have a thickness of about 1 ㎛ to 30 ㎛. For example, the thickness of the porous polymer substrate may be about 2 ㎛ to 29 ㎛, 3 ㎛ to 28 ㎛, 4 ㎛ to 27 ㎛, 5 ㎛ to 26 ㎛, 6 ㎛ to 25 ㎛, 7 ㎛ to 24 ㎛, 8 ㎛ to 23 ㎛, 9 ㎛ to 22 ㎛, 10 ㎛ to 21 ㎛, 11 ㎛ to 20 ㎛, 12 ㎛ to 19 ㎛, 13 ㎛ to 18 ㎛, 14 ㎛ to 17 ㎛, or 15 ㎛ to 16 ㎛. By controlling the thickness of the porous polymer substrate within the above-described range, the energy density of the separator for the electrochemical device can be improved.

[0103]

[0104] A method for manufacturing a porous polymer substrate according to one embodiment of the present invention may include the steps of: kneading and extruding a composition for a porous polymer substrate including a polymer resin; cooling the extruded composition for a porous polymer substrate to form a sheet; stretching the sheet; and forming pores in the stretched sheet; and heat-setting the sheet in which the pores are formed to manufacture a porous polymer substrate. By manufacturing a porous polymer substrate using the method described above, a porous polymer substrate including uniform pores can be manufactured.

[0105] According to one embodiment of the present invention, the method for manufacturing the porous polymer substrate may include a step of mixing and extruding a composition for a porous polymer substrate including a polymer resin. By including the mixing and extruding steps as described above, a uniform porous polymer substrate composition can be manufactured, thereby manufacturing a porous polymer substrate having uniform pore sizes.

[0106] According to one embodiment of the present invention, the composition for the porous polymer substrate may further include a plasticizer. For example, the plasticizer may be liquid paraffin oil. By including the plasticizer as described above, the plasticizer can be easily removed from the sheet, and denaturation of the polymer resin can be prevented.

[0107] According to one embodiment of the present invention, the liquid paraffin oil may have a kinematic viscosity at 40°C of about 30 cSt or more and 50 cSt or less. By preparing the kinematic viscosity of the liquid paraffin oil within the above-described range, the concentration of the plasticizer in the composition for the porous polymer substrate can be uniformly controlled.

[0108] According to one embodiment of the present invention, the weight ratio of the polymer resin and the plasticizer in the composition for the porous polymer substrate may be about 2:8 to 5:5. By adjusting the weight ratio of the polymer resin and the plasticizer in the composition for the porous polymer substrate within the above-described range, the porosity of the porous polymer substrate can be adjusted.

[0109] According to one embodiment of the present invention, the extrusion may be performed through a T-die in a twin-screw extruder. By performing the extrusion as described above, the thickness of the sheet can be easily controlled and cooling efficiency can be improved.

[0110] According to one embodiment of the present invention, the method for manufacturing the porous polymer substrate may include a step of cooling the extruded composition for the porous polymer substrate to manufacture it into a sheet.

[0111] According to one embodiment of the present invention, the temperature for cooling the sheet may be about 40° C. or more and 80° C. or less. For example, the temperature for casting through the T-die onto a roll may be about 40° C. or more and 80° C. or less. By controlling the temperature for cooling the sheet within the above-described range, the polymer resin can be implemented as crystalline, and by controlling the content of the crystalline polymer resin and the amorphous polymer resin within the porous polymer resin, the indentation depth can be reduced while simultaneously minimizing the standard deviation of the indentation depth.

[0112] According to one embodiment of the present invention, the method for manufacturing the porous polymer substrate may include a step of stretching the sheet. By including the step of stretching the sheet as described above, the thickness of the porous polymer substrate can be controlled and a thin film can be achieved.

[0113] According to one embodiment of the present invention, the stretching step may be biaxial stretching using a tender-type simultaneous stretching machine. For example, stretching may be performed in the MD (machine direction) and then in the TD (transverse direction). By performing the stretching step as described above, the sheet can be manufactured into a large-area porous polymer substrate.

[0114] According to one embodiment of the present invention, the method for manufacturing the porous polymer substrate may include a step of forming pores in the stretched sheet. For example, forming pores in the stretched sheet may be performed by removing a plasticizer contained in the porous polymer substrate using a solvent. The solvent may be methylene chloride. By including the step of forming pores in the stretched sheet as described above, a porous polymer substrate can be manufactured, and the remaining plasticizer can be minimized.

[0115] According to one embodiment of the present invention, the method may include a step of heat-setting the sheet in which the pores are formed to manufacture a porous polymer substrate. For example, the temperature of the heat-setting step may be approximately 100°C or higher and 150°C or lower. By heat-setting the sheet as described above, the heat resistance of the separator can be improved.

[0116]

[0117] According to one embodiment of the present invention, the separator for the electrochemical device may further include a coating layer formed on at least one surface of the porous polymer substrate.

[0118] According to one embodiment of the present invention, the coating layer includes a polymer binder and inorganic particles and has porous characteristics.

[0119] According to one embodiment of the present invention, the coating layer may be a porous coating layer including a plurality of pores. For example, the coating layer may be a porous coating layer including a plurality of pores within it. As described above, by including a plurality of pores, the coating layer can physically block the negative and positive electrodes while allowing lithium ions to pass through and conduct current.

[0120] According to one embodiment of the present invention, the polymer binder and the inorganic particles in the coating layer may be included in a weight ratio of about 1:99 to 30:70. The ratio may be appropriately adjusted within the above-described range, and the polymer binder may be about 1 wt% or more, 5 wt% or more, or 10 wt% or more, and the inorganic particles may be about 80 wt% or more, 85 wt% or more, 90 wt% or more, or 95 wt% or more, based on 100 wt% of the total of the polymer binder and the inorganic particles.

[0121] According to one embodiment of the present invention, the coating layer may be formed by inorganic particles being bound by a polymer binder and integrated within the layer. The pores within the coating layer may originate from interstitial volume, which is an empty space between the inorganic particles.

[0122] In one embodiment of the present invention, the porosity of the coating layer may be about 30% to 70% by volume. When the porosity of the coating layer is about 70% by volume or less, mechanical properties that can withstand the pressing process for bonding with the electrode can be secured, and also, the surface opening ratio is not too high, making it suitable for securing adhesive strength. On the other hand, when the porosity is about 30% by volume or more, it is advantageous from the perspective of ion permeability.

[0123] In this specification, the porosity of the coating layer means the ratio of the volume occupied by pores to the total volume of the coating layer, and uses volume% as its unit, and can be used interchangeably with terms such as porosity and porosity.

[0124] In this specification, porosity corresponds to a value obtained by subtracting a volume converted to the weight and density of each component of the porous polymer substrate and coating layer from the volume calculated in the thickness, width, and length of the porous polymer substrate and coating layer.

[0125] For example, the porous polymer substrate may have a porosity of about 10 vol% or more and 60 vol% or less. In one embodiment, the porosity of the porous polymer substrate may be about 15 vol% or more and 55 vol% or less, 20 vol% or more and 50 vol% or less, 25 vol% or more and 45 vol% or less, or 30 vol% or more and 40 vol% or less. When the porosity of the porous polymer substrate is in the above-described range, the ionic conductivity of the manufactured separator can be provided in a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0126] In one embodiment of the present invention, the porosity and pore size of the porous polymer substrate and coating layer can be measured by the BET 6-point method using a scanning electron microscope (SEM) image, a mercury porosimeter, a capillary flow porometer, or a porosimetry analyzer (Bell Japan Inc, Belsorp-II mini) using a nitrogen gas adsorption flow method. In this case, it may be advantageous to use a capillary flow porometer.

[0127] According to one embodiment of the present invention, the thickness of the coating layer may be formed to a thickness of about 1 μm to 20 μm on either side of the porous polymer substrate, but is not particularly limited thereto. The thickness can be adjusted to an appropriate range by those skilled in the art in terms of heat resistance or electrical resistance.

[0128] According to one embodiment of the present invention, the thickness of the porous polymer substrate and / or the coating layer, etc., can be measured using a contact-type thickness measuring device. The contact-type thickness measuring device can be, for example, VL-50S-B from Mitutoyo.

[0129] According to one embodiment of the present invention, the polymer binder usable in the coating layer is polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, It may be any one polymer resin selected from the group consisting of cyanoethylsucrose, pullulan, and carboxyl methyl cellulose, or a mixture of two or more thereof, but is not particularly limited thereto.

[0130] In one embodiment of the present invention, the inorganic particles that can be used in the coating layer are not particularly limited as long as they are electrochemically stable. That is, in one embodiment of the present invention, the inorganic particles that can be used are those that can be used in the operating voltage range of the applied electrochemical device (e.g., Li / Li). + There are no special restrictions as long as no oxidation and / or reduction reaction occurs at a voltage of 0 V to 5 V (as a reference).

[0131] According to one embodiment of the present invention, non-limiting examples of the inorganic particles include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), etc., and may include one or more of these.

[0132] According to one embodiment of the present invention, the average diameter (D) of the inorganic particles 50 ) has no special limitations, but in order to form a coating layer of uniform thickness and have an appropriate porosity, it is preferably in the range of about 0.3 ㎛ to 1 ㎛. For example, if it is less than about 0.3 ㎛, the dispersibility of inorganic particles in the slurry prepared for manufacturing the coating layer may be reduced, and if it exceeds about 1 ㎛, the thickness of the formed coating layer may increase.

[0133] In this specification, "D50 particle size" means the particle size at about 50% of the cumulative distribution of particle numbers according to particle size. The particle size can be measured using a laser diffraction method. For example, after the powder to be measured is dispersed in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and when the particles pass through the laser beam, the difference in the diffraction pattern according to particle size is measured to calculate the particle size distribution. By calculating the particle diameter at the point where 50% of the cumulative distribution of particle numbers according to particle size in the measuring device is reached, the D50 particle size can be measured.

[0134] According to one embodiment of the present invention, the method for forming the coating layer is as follows, for example. First, a polymer solution is prepared by dissolving a polymer binder in an appropriate organic solvent, or a polymer emulsion is prepared by dispersing the polymer binder in an appropriate dispersion medium. At this time, the organic solvent or dispersion medium that can be used is preferably one that has a solubility index similar to that of the polymer binder to be used and a low boiling point. This is to facilitate uniform mixing and subsequent removal of the solvent or dispersion medium. Non-limiting examples of solvents that can be used include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or mixtures thereof.

[0135]

[0136] Next, inorganic particles are added and dispersed in the polymer solution and / or polymer dispersion medium thus manufactured to manufacture a slurry for a coating layer. According to one embodiment of the present invention, the content ratio of the inorganic particles and the polymer binder is as described above, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the coating layer of the present invention to be finally manufactured.

[0137] Next, the slurry for the coating layer prepared above is applied to at least one side of the prepared porous polymer substrate and dried. The method for applying the slurry to the surface of the porous polymer substrate is not particularly limited to any one method, and any conventional method known in the art can be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof can be used.

[0138] The above drying process is performed under appropriate temperature and time conditions to minimize the occurrence of surface defects in the coating layer. The drying may be performed using a drying oven or a drying auxiliary device such as hot air within an appropriate range.

[0139] When the above separator includes a coating layer, damage caused by pressing of inorganic particles on the surface of the porous polymer substrate facing the coating layer during the lamination process can be reduced.

[0140] According to one embodiment of the present invention, the separator is interposed between the negative electrode and the positive electrode and is manufactured into an electrochemical device through a lamination process that applies heat and / or pressure to bond them. In one embodiment of the present invention, the lamination process can be performed by a roll press device including a pair of pressure rollers. That is, the negative electrode, the separator, and the positive electrode can be sequentially laminated and placed between the pressure rollers to achieve interlayer bonding. At this time, the lamination process can be performed by a hot press method.

[0141]

[0142] One embodiment of the present invention provides an electrochemical device including: an anode; a cathode; and a separator interposed between the anode and the cathode.

[0143] An electrochemical device according to one embodiment of the present invention can improve battery performance by preventing Hi-Pot failure and low voltage failure.

[0144] In the present invention, the electrochemical device is a device that converts chemical energy into electrical energy through an electrochemical reaction, and is a concept encompassing a primary battery and a secondary battery. In the present specification, the secondary battery is capable of charging and discharging, and refers to a lithium secondary battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc. The lithium secondary battery uses lithium ions as an ion conductor, and examples thereof include, but are not limited to, a non-aqueous electrolyte secondary battery including a liquid electrolyte, an all-solid-state battery including a solid electrolyte, a lithium polymer battery including a gel polymer electrolyte, and a lithium metal battery using lithium metal as an anode.

[0145] According to one embodiment of the present invention, the positive electrode has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x Mx Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-x M x A lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li in the chemical formula is replaced by an alkaline earth metal ion; a disulfide compound; or a mixture of two or more of Fe2(MoO4)3.

[0146] According to one embodiment of the present invention, the negative electrode has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode includes carbon such as lithium metal oxide, non-graphitizable carbon, and graphite carbon as the negative electrode active material; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 규소계 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함할 수 있다.

[0147] According to one embodiment of the present invention, the conductive material may be, for example, one selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, activated carbon, and polyphenylene derivatives, or a mixture of two or more conductive materials thereof. Or, the conductive material may be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials thereof.

[0148] According to one embodiment of the present invention, the current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, copper, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used.

[0149] According to one embodiment of the present invention, the binder resin may be a polymer commonly used in electrodes in the art. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.

[0150] In one embodiment of the present invention, the positive electrode slurry for producing the positive electrode active material layer may include a dispersant, and the dispersant may be a pyrrolidone-based compound. For example, it may be N-methylpyrrolidone (ADC-01, LG Chemical).

[0151] According to one embodiment of the present invention, the content of the dispersant included in the positive electrode slurry may be about 0 part by weight or more and 0.5 part by weight or less with respect to 100 parts by weight of the positive electrode slurry. For example, the content of the dispersant included in the positive electrode slurry may be about 0.05 part by weight or more and 0.4 part by weight or less with respect to 100 parts by weight of the positive electrode slurry.

[0152] According to one embodiment of the present invention, the negative electrode slurry for manufacturing the negative electrode active material layer may include a dispersant, and the dispersant may be a polypyrrolidone-based compound. For example, the dispersant may be polyvinylpyrrolidone (Polyvinylpyrrolidone, Junsei, Japan).

[0153] According to one embodiment of the present invention, the content of the dispersant included in the cathode slurry may be about 0 part by weight or more and 0.5 part by weight or less with respect to 100 parts by weight of the cathode slurry. For example, the content of the dispersant included in the cathode slurry may be about 0.05 part by weight or more and 0.4 part by weight or less with respect to 100 parts by weight of the cathode slurry.

[0154] According to one embodiment of the present invention, an electrochemical device prepared as described above can be placed in an appropriate case and an electrolyte solution is injected to manufacture a battery.

[0155] According to one embodiment of the present invention, the electrolyte is A + B - As a salt with the same structure, A + is Li + , Na + , K+ B containing an ion composed of an alkali metal cation or a combination thereof; - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 - Salts containing anions such as or combinations thereof are dissolved or dissociated in organic solvents such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone) or mixtures thereof, but are not limited thereto.

[0156] One embodiment of the present invention provides a battery module including a battery including the electrochemical element as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Examples of the device include, but are not limited to, a power tool that is powered by an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.

[0157] Hereinafter, the present invention will be described in detail using examples. However, the embodiments according to the present invention may be modified in various ways, and the scope of the present invention is not construed as being limited to the embodiments described below. The embodiments herein are provided to more fully explain the present invention to those of ordinary skill in the art.

[0158] <Example 1>

[0159] 30 parts by weight of a polymer resin (polyethylene resin, Mw: 800,000) with a log Mw of 5.5 and 70 parts by weight of liquid paraffin oil (kinematic viscosity at 40°C: 40 cSt) were fed into a twin-screw extruder, mixed, and then extruded. After extrusion, the mixture was formed into a sheet through a T-die and a cooling casting roll, and then biaxially stretched using a tenter-type simultaneous stretching machine for MD stretching and TD stretching. Liquid paraffin oil, a diluent, was extracted from the stretched sheet with methylene chloride and heat-set at about 128°C to produce a porous polymer substrate. That is, in the production of a polyethylene film in Example 1, propylene is not added during the polymerization process in order to improve compression resistance by increasing the crystal content.

[0160] The weight average molecular weight of the eluate was determined using a PolymerChar TREF machine for the above porous polymer substrate. For example, a 40 mg sample of the above porous polymer substrate was prepared, dissolved in 20 mL of trichlorobenzene solvent at 150°C for 120 minutes, and then stabilized at 100°C for 45 minutes. This was then introduced into a TREF column, cooled to 35°C at a cooling rate of 0.5°C / min, and maintained for 15 minutes. After that, the temperature was increased from 35 ℃ to 80 ℃ at a rate of 20 ℃ / min while maintaining the temperature in 5 ℃ increments for 20 minutes, and then the temperature was increased from 80 ℃ to 120 ℃ at a rate of 20 ℃ / min while maintaining the temperature in 2 ℃ increments for 20 minutes. The weight average molecular weight of the polymer sample eluted at 98 ℃ was measured while flowing the solvent trichlorobenzene into the column at a flow rate of 0.5 mL / min.

[0161] Furthermore, the weight average molecular weight measured for the porous polymer substrate and the number average molecular weight derived through GPC (Gel Permeation Chromatography) analysis were used to derive the polydispersity index using the following mathematical formula 3.

[0162] [Equation 3]

[0163] Polydispersity index (PDI) = (weight average molecular weight) / (number average molecular weight)

[0164] The log value of the weight average molecular weight (log Mw) of the eluate of the porous polymer substrate was 5.5, and the polydispersity index (PDI) of the eluate of the porous polymer substrate was 6.0.

[0165] <Example 2>

[0166] A porous polymer substrate was manufactured in the same manner as in Example 1, except that the Log Mw of the polymer resin was 6.2.

[0167] <Example 3>

[0168] A porous polymer substrate was manufactured in the same manner as in Example 1, except that the Log Mw of the polymer resin was 5.1 and the polydispersity index (PDI) was 5.2.

[0169] <Example 4>

[0170] A porous polymer substrate was manufactured in the same manner as in Example 1, except that the Log Mw of the polymer resin was 5.1 and the polydispersity index (PDI) was 9.9.

[0171] <Comparative Example 1>

[0172] Compared to Example 1 above, where propylene was not added during the polymerization process of the polyethylene resin, in Comparative Example 1, 7 parts by weight of propylene was added to 100 parts by weight of ethylene during the polymerization process of the polyethylene resin to produce a polymer resin (Mw: 800,000), and a porous polymer substrate was produced in the same manner as Example 1 except that the Log Mw of the polymer resin was 2.9.

[0173] <Comparative Example 2>

[0174] In comparison with Example 1, where propylene was not added during the polymerization process of the polyethylene resin, in Comparative Example 2, 5.5 parts by weight of propylene was added to 100 parts by weight of ethylene during the polymerization process of the polyethylene resin to produce a polymer resin (Mw: 800,000), and a porous polymer substrate was produced in the same manner as Example 1, except that the Log Mw of the polymer resin was 4.4.

[0175] <Comparative Example 3>

[0176] In comparison with Example 1, where propylene was not added during the polymerization process of the polyethylene resin, in Comparative Example 3, 3 parts by weight of propylene was added to 100 parts by weight of ethylene during the polymerization process of the polyethylene resin to produce a polymer resin (Mw: 800,000), and a porous polymer substrate was produced in the same manner as Example 1, except that the Log Mw of the polymer resin was 5.1 and the polydispersity index (PDI) was 2.3.

[0177] Comparative Example 4

[0178] In comparison with Example 1 above, in which propylene was not added during the polymerization process of the polyethylene resin, in Comparative Example 4, 1.5 parts by weight of propylene was added to 100 parts by weight of ethylene during the polymerization process of the polyethylene resin to produce a polymer resin (Mw: 800,000), and a porous polymer substrate was produced in the same manner as Example 1 except that the Log Mw of the polymer resin was 5.1 and the polydispersity index (PDI) was 3.9.

[0179] <Experimental Example 1: Measurement of Thickness Reduction Rate>

[0180] Using a contact thickness gauge (Mitutoyo, VL-50S-B), the thickness before applying pressure and the thickness after applying 8 MPa of pressure at 70°C were measured for the porous polymer substrates of Examples 1 to 4 and Comparative Examples 1 to 4, and the thickness reduction rate of the porous polymer substrate was measured according to the following mathematical equation 1. The measurement was performed at 5 points in total, including 4 points located 1 cm away from the corners and 1 point in the center, after the porous substrate was punched out to 5 x 5 cm. Then, samples at the left / middle / right positions along the TD direction were measured 3 times, and the arithmetic average was taken as the thickness of the porous polymer substrate.

[0181] [Mathematical Formula 1]

[0182] Thickness reduction rate (%) = (thickness of porous polymer substrate before applying pressure - thickness of porous polymer substrate after applying pressure) / thickness of porous polymer substrate before applying pressure X 100

[0183] Log Mw Polydispersity Index (PDI) Thickness Reduction Rate (%) Example 15.5 6.0 6.7 Example 26.2 6.0 3.8 Example 35.1 5.2 5.9 Example 45.1 9.9 3.2 Comparative Example 12.9 6.0 17.9 Comparative Example 24.4 6.0 13.1 Comparative Example 35.12 3 12.8 Comparative Example 45.13 10.9

[0184]

[0185] Referring to Table 1 above, Comparative Examples 1 and 2 showed an increase in the thickness reduction rate of the porous polymer substrate due to a low weight average molecular weight, but Examples 1 and 2 showed a decrease in the thickness reduction rate of the porous polymer substrate as the weight average molecular weight increased.

[0186] Furthermore, in Comparative Examples 3 and 4, the thickness reduction rate of the porous polymer substrate increased because the polydispersity index was low when the weight average molecular weight was the same, but in Examples 3 and 4, it was confirmed that the thickness reduction rate of the porous polymer substrate decreased as the polydispersity index increased.

[0187] According to one embodiment of the present invention, by controlling the weight average molecular weight and polydispersity index of a crystalline polymer resin included in a porous polymer substrate, the compression resistance can be improved and the thickness change rate can be reduced.

[0188] <Example 5>

[0189] Polyolefin resin (copolymer containing ethylene and propylene in a weight ratio of 96:4, weight average molecular weight: 800,000) and liquid paraffin oil (kinematic viscosity at 40°C: 40 cSt) were mixed in a weight ratio of 3:7, and 5 wt% of polypropylene was further added based on the total weight of the polyolefin resin. The mixture was fed into a twin-screw extruder, kneaded, and extruded. After extrusion, it was formed into a sheet by passing through a T-die and a cooling casting roll, and biaxially stretched using a tenter-type sequential stretching machine that stretches MD and TD. Liquid paraffin oil was extracted from the stretched sheet with methylene chloride, and heat-set at about 128°C to produce a polyolefin base material (thickness 9 ㎛).

[0190] <Example 6>

[0191] A polyolefin substrate (thickness 9 ㎛) was manufactured in the same manner as in Example 5, except that polyolefin resin (a copolymer containing ethylene and propylene in a weight ratio of 93:7) and liquid paraffin oil were mixed in a weight ratio of 3:7 and 5 wt% of polypropylene was additionally added based on the total weight of the polyolefin resin.

[0192] <Example 7>

[0193] A polyolefin substrate (thickness 9 ㎛) was manufactured in the same manner as in Example 5, except that polyolefin resin (a copolymer containing ethylene and propylene in a weight ratio of 85:15) and liquid paraffin oil were mixed in a weight ratio of 3:7 and 2 wt% of polypropylene was additionally added based on the total weight of the polyolefin resin.

[0194] <Example 8>

[0195] A polyolefin substrate (thickness 9 ㎛) was manufactured in the same manner as in Example 5, except that polyolefin resin (a copolymer containing ethylene and propylene in a weight ratio of 85:15) and liquid paraffin oil were mixed in a weight ratio of 3:7 and 3.5 wt% of polypropylene was additionally added based on the total weight of the polyolefin resin.

[0196] Comparative Example 5

[0197] A polyolefin substrate (thickness 9 ㎛) was manufactured in the same manner as in Example 5, except that polyolefin resin (a copolymer containing ethylene and propylene in a weight ratio of 70:30) and liquid paraffin oil were mixed in a weight ratio of 3:7 and 5 wt% of polypropylene was additionally added based on the total weight of the polyolefin resin.

[0198] <Comparative Example 6>

[0199] A polyolefin substrate (thickness 9 ㎛) was manufactured in the same manner as in Example 5, except that polyolefin resin (a copolymer containing ethylene and propylene in a weight ratio of 85:15) and liquid paraffin oil were mixed in a weight ratio of 3:7 and 7 wt% of polypropylene was additionally added based on the total weight of the polyolefin resin.

[0200] <Experimental Example 2: Confirmation of the content of amorphous polymer resin contained in a polyolefin substrate>

[0201] In the examples and comparative examples, the content of amorphous polyolefin polymer resin contained in the polyolefin substrate was confirmed using a TREF machine of PolymerChar. For example, 40 mg of the polyolefin substrate was dissolved in 20 mL of trichlorobenzene solvent at 150°C for 120 minutes and then stabilized at 100°C for 45 minutes. After introducing this into a TREF column, it was cooled to 35°C at a cooling rate of 0.5°C / min and maintained for 15 minutes. Thereafter, it was heated from 35°C to 80°C at a cooling rate of 20°C / min while maintaining the temperature in 5°C increments for 20 minutes, and then heated from 80°C to 120°C at a cooling rate of 20°C / min while maintaining the temperature in 2°C increments for 20 minutes. Afterwards, the solvent trichlorobenzene was passed through the column at a flow rate of 0.5 mL / min, and the weight of the eluted fraction at 35°C was measured, and the results are shown in Tables 2 and 3 below.

[0202] In addition, the average number of CH3 per 1000 carbon atoms was confirmed using the IR detector included in the machine, and is shown in Tables 2 and 3 below.

[0203] <Experimental Example 3: Confirmation of Compression Resistance According to the Content of Amorphous Polymer Resin Contained in a Polyolefin Base>

[0204] The compression permeability of the polyolefin substrates of Examples 5 and 6 and Comparative Example 5 was confirmed by measuring the time it takes for 100 cc of air to pass through a 1 square inch sample under a constant pressure of 4.8 inches of water at room temperature using Asahi seico EG01-55-1MR equipment.

[0205] Each of the above polyolefin substrates was placed on a press device, pressurized at a pressure of 8 MPa at 70°C for 10 seconds, and then the air permeability after compression was confirmed by measuring in the same manner using the above equipment.

[0206] Based on the fabric air permeability before and after compression, the air permeability increase rate was calculated according to Equation 1 above and shown in Table 2 below.

[0207] Content of amorphous resin (weight%)Average CH3 / 1000TC (unit)Air permeability of substrate before compression (s / 100cc)Air permeability of substrate after compression (s / 100cc)Air permeability increase rate (%)Example 52440709130Example 6134407011868Comparative example 54144070325364

[0208]

[0209] As can be seen from Table 2 above, in the case of Comparative Example 5, the increase rate of air permeability is 364%, while in the cases of Examples 5 and 6, the increase rates of air permeability are 30% and 68%, respectively.

[0210] <Experimental Example 4: Confirmation of Compression Resistance According to Average Short Chain Branching of Polyolefin Substrate>

[0211] Using the polyolefin substrates of Examples 7 and 8 and Comparative Example 6, the air permeability before and after compression was measured in the same manner as in Experimental Example 3.

[0212] Based on the fabric air permeability before and after compression, the air permeability increase rate was calculated according to the above mathematical formula 2 and is shown in Table 3 below.

[0213] Content of amorphous resin (weight%)Average CH3 / 1000TC (unit)Air permeability of substrate before compression (s / 100cc)Air permeability of substrate after compression (s / 100cc)Air permeability increase rate (%)Example 728240708927Example 82838070173147Comparative example 62863070211201

[0214]

[0215] As can be seen in Table 3 above, in the case of Comparative Example 6, the increase rate of air permeability is 201%, while in the cases of Examples 7 and 8, the increase rates of air permeability are 27% and 147%, respectively.

[0216] <Example 9>

[0217] 30 parts by weight of polymer resin (polyethylene resin, Mw: 1.5 million) and 70 parts by weight of liquid paraffin oil (kinematic viscosity at 40°C: 40 cSt) were fed into a twin-screw extruder, mixed, and then extruded. After extrusion, the mixture was formed into a sheet through a T-die and a cooling casting roll, and then biaxially stretched using a tenter-type simultaneous stretching machine for MD stretching and TD stretching. The liquid paraffin oil, a diluent, was extracted from the stretched sheet with methylene chloride and heat-set at approximately 128°C to produce a porous polymer substrate.

[0218] For the above porous polymer substrate, the weight ratio of the eluate eluted at 98°C was determined using PolymerChar's TREF machine. For example, 40 mg of the sample was prepared for the above porous polymer substrate, dissolved in 20 mL of trichlorobenzene solvent at 150°C for 120 minutes, and then stabilized at 100°C for 45 minutes. After this, it was introduced into a TREF column, cooled to 35°C at a cooling rate of 0.5°C / min, and then maintained for 15 minutes. After that, the temperature was increased from 35°C to 80°C at a rate of 20°C / min while maintaining the temperature at 5°C increments for 20 minutes, and then the temperature was increased from 80°C to 120°C at a rate of 20°C / min while maintaining the temperature at 2°C increments for 20 minutes. While flowing trichlorobenzene, a solvent, into the column at a flow rate of 0.5 mL / min, the weight of the polymer sample eluted at 98°C was measured. The content of the crystalline polymer resin included in the porous polymer substrate was 72 wt%.

[0219] <Example 10>

[0220] A porous polymer substrate was manufactured in the same manner as in Example 9, except that the content of the crystalline polymer resin included in the porous polymer substrate was 83 wt%.

[0221] Comparative Example 7

[0222] In the above Example 9, 7 parts by weight of polypropylene (Mw: 350,000) was added to 100 parts by weight of polyethylene (Mw: 600,000) to prepare a polymer resin (Mw: 580,000), and a porous polymer substrate was prepared in the same manner as in Example 9, except that the content of the crystalline polymer resin included in the porous polymer substrate was 66% by weight.

[0223] Comparative Example 8

[0224] In the above Example 9, 0.5 parts by weight of polypropylene (Mw: 350,000) was added to 100 parts by weight of polyethylene (Mw: 600,000) to prepare a polymer resin (Mw: 600,000), and a porous polymer substrate was prepared in the same manner as in Example 9, except that the content of the crystalline polymer resin included in the porous polymer substrate was 90% by weight.

[0225] <Experimental Example 5: Measurement of Indentation Depth and Standard Deviation>

[0226] Using a nanoindenter (Fischerscope, HM2000), the porous polymer substrate was indented with a force of 100 nN using an indenter (Vickers Indenter, tip width 0.5 ㎛), and the depth of penetration of the indenter was measured using an atomic force microscope (AFM).

[0227] After setting the Dimension Icon (Bruker) on the surface of the porous polymer substrate of Examples 9 and 10 and Comparative Examples 7 and 8 under the following conditions, the peak tapping force was measured while moving the tip relative to the sample surface as shown in Fig. 1, and the depth of the tip penetrating the sample surface at the time the peak tapping force was measured was measured using an atomic force microscope (AFM, Atomic Force Microscope, OSTESPA-R3, Bruker, f=300 kHz, k=26 N / m).

[0228] - Mode: Tapping (Peak Force QNM)

[0229] - Scan speed (0.3 Hz)

[0230] - Peak Force setpoint: 100 nN, Amplitude: 300 nm

[0231] - Scan angle: 90 °

[0232] <Experimental Example 6: Measurement of Insulation Breakdown Voltage>

[0233] For the above Examples 9 and 10 and the above Comparative Examples 7 and 8 having a thickness of 12 ㎛, a pressure of 8 MPa was applied at 70°C, and the voltage was measured when the pressure was increased at a rate of 100 mV / s and exceeded 0.5 mA for 3 seconds.

[0234] Indentation Depth (nm)Standard Deviation of Indentation Depth (nm)Insulation Breakdown Voltage (V) after CompressionExample 916.23.11,690Example 1010.71.12,687Comparative Example 723.33.8934Comparative Example 812.38.6801

[0235]

[0236] Referring to Table 4 above, it was confirmed that in Examples 9 and 10, the crystalline polymer resin was included in the porous polymer substrate in an appropriate amount above the standard value, so that the indentation depth was relatively low, and the standard deviation of the indentation depth was reduced, so that the breakdown voltage after compression increased.

[0237] In this regard, in Comparative Example 7, the porous polymer substrate contained a small amount of 66 wt% of a crystalline polymer resin, so that the indentation depth increased rapidly, and the breakdown voltage after compression increased relatively less, to 1,000 V or less, and in Comparative Example 8, the porous polymer substrate contained an excessive amount of 90 wt% of a crystalline polymer resin, so that the standard deviation of the indentation depth increased, and the breakdown voltage after compression also increased relatively less, to 1,000 V or less.

[0238] Therefore, the separator for an electrochemical device according to one embodiment of the present invention can improve the breakdown voltage after lamination by controlling the intention depth and its standard deviation by controlling the content of the crystalline polymer resin included in the porous polymer substrate.

[0239] While the present invention has been described above with reference to preferred embodiments, it will be understood by those skilled in the art or those with ordinary knowledge in the art that various modifications and changes can be made to the present invention without departing from the spirit and technical scope of the present invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.

Claims

1. Contains a porous polymer substrate, The above porous polymer substrate includes an amorphous polymer resin and a crystalline polymer resin, A separator for an electrochemical device, wherein the weight average molecular weight (Mw) of the elution product extracted from the porous polymer substrate by temperature-rising elution fractionation (TREF) is 100,000 or more.

2. In claim 1, A separator for an electrochemical device, wherein the porous polymer substrate comprises 40 wt% or less of a fraction eluted at a temperature of 35°C or lower by a temperature-increasing elution fractionation method.

3. In claim 1, A separator for an electrochemical device, wherein the content of the amorphous polymer resin in the porous polymer substrate is 40 wt% or less.

4. In claim 1, A separator for an electrochemical device, wherein the content of the crystalline polymer resin in the porous polymer substrate is 60 wt% or more.

5. In claim 1, A separator for an electrochemical device, wherein the weight ratio of the amorphous polymer resin and the crystalline polymer resin in the porous polymer substrate is 1:1 to 10:

1.

6. In claim 1, A separator for an electrochemical device, wherein the deviation in the indentation depth in the above porous polymer substrate is - 5 nm or more and 5 nm or less.

7. In claim 1, The above porous polymer substrate includes a polyolefin resin, The above amorphous polymer resin is an amorphous polyolefin resin, A separator for an electrochemical device, wherein the above crystalline polymer resin is a crystalline polyolefin resin.

8. In claim 7, A separator for an electrochemical device, wherein the polyolefin resin is one selected from the group consisting of polyethylene; polypropylene; polybutylene; polypentene; polyhexene; polyoctene; copolymers of at least one of ethylene, propylene, butene, pentene, 4-methylpentene, hexene, or octene; and combinations thereof.

9. In claim 7, The above polyolefin resin is a separator for an electrochemical device having an average short chain branch (SCB) of 500 or less per 1,000 total carbon atoms.

10. In claim 7, The above polyolefin resin is a separator for an electrochemical device having a melt index (ASTM D1238, 190°C, 2.16 kg) of 0.1 g / 10 min to 0.3 g / 10 min.

11. In claim 1, A separator for an electrochemical device, wherein the weight average molecular weight (Mw) of the porous polymer substrate is 500,000 or more and 3,000,000 or less.

12. In claim 1, A separator for an electrochemical device, wherein the polydispersity index (PDI) of the above extract is 5 or more.

13. In claim 1, A separator for an electrochemical device that satisfies at least one of the following (i) to (iii) when a pressure of 8 MPa is applied at 70°C: (i) The thickness reduction rate of the porous polymer substrate defined by the following mathematical formula 1 is 10% or less: [Mathematical Formula 1] Thickness reduction rate (%) = (thickness of porous polymer substrate before applying pressure - thickness of porous polymer substrate after applying pressure) / thickness of porous polymer substrate before applying pressure X 100 (ii) The increase in air permeability after compression of the porous polymer substrate defined by the following mathematical formula 2 is 185% or less: [Equation 2] Increase in ventilation rate (%) = (Ventilation after compression - Ventilation before compression) / (Ventilation before compression) X 100 (iii) The breakdown voltage of the porous polymer substrate is 1,000 V or more.

14. In claim 1, A separator for an electrochemical device having a thickness of 1 ㎛ or more and 30 ㎛ or less.

15. An electrochemical device comprising a positive electrode; a negative electrode; and a separator interposed between the positive electrode and the negative electrode, the separator of claim 1.

Citation Information

Patent Citations

  • Separator for lead storage battery and lead storage battery including the same

    JP2023046061A

  • Polymeric microporous film comprising polypropylene resin

    KR101442969B1

  • Separator, method for manufacturing separator, and nonaqueous electrolyte battery

    KR1020090088804A

  • Microporous polyolefin film, separator for non-aqueous secondary battery, non-aqueous secondary battery, and process for production of microporous polyolefin film

    KR1020120031236A

  • Method And Apparatus for Classifying Document Based on Object Selection