Graphite negative electrode material, preparation method therefor and use thereof
By using a hydrophilic functional group polymer material coating layer on the graphite anode material, the problem of insufficient hydrophilicity and electrolyte wettability of the graphite anode material is solved, and its performance and processing performance in lithium-ion batteries are improved.
Patent Information
- Application Number
- PCT/CN2023/090924
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Existing graphite anode materials in lithium-ion batteries have problems such as poor hydrophilicity, poor electrolyte wettability and limited binder binding ability, resulting in high energy consumption and poor peeling force of thick electrode plates.
Polymer materials with hydrophilic functional groups are used as the coating layer of the graphite negative electrode material. By tightly coating with the graphite surface, the electrical and mechanical properties are improved, and the dispersion and peeling strength are improved in the aqueous slurry.
It improves the hydrophilicity and electrolyte wettability of the graphite anode material, enhances the peeling strength with the pole piece, simplifies the pulping process, reduces energy consumption, and improves the processing performance of lithium-ion batteries.
Smart Images

Figure PCTCN2023090924-FTAPPB-I100001
Abstract
Description
A graphite negative electrode material and its preparation method and application Technical Field
[0001] The present application belongs to the field of lithium-ion battery technology, for example, a graphite negative electrode material and its preparation method and application. Background Art
[0002] In today's society, the concept of "carbon neutrality" has gained widespread acceptance, and lithium-ion batteries have achieved breakthrough developments over the past few years. Graphite holds a pivotal position in the field of lithium-ion battery anode materials, currently the mainstream anode material. Graphite boasts high crystallinity and excellent conductivity, and its layered structure is ideal for lithium ion insertion and extraction. Furthermore, graphite offers advantages such as low cost and widespread availability. Consequently, since the commercialization of lithium-ion batteries at the end of the last century, no material has been able to challenge graphite's dominance.
[0003] Since its advent, graphite materials have been extensively studied by researchers. To date, both natural and artificial graphite have been developed to a very complete level. An important technical route to improve the performance of graphite is to coat the surface of the graphite material. The current mainstream coating scheme is to coat the graphite surface with a layer of amorphous carbon to improve its cycling performance. On the one hand, amorphous carbon can improve the density and stability of the SEI film generated on the graphite surface. On the other hand, it can constrain the graphite surface, reduce the shedding of the carbon layer, and inhibit abnormal lithium removal and lithium insertion behavior. The precursors of amorphous carbon selected by researchers are mainly materials such as asphalt, phenolic resin, and polyimide.
[0004] CN115881901A discloses a negative electrode material, a preparation method thereof, and a lithium-ion battery. The negative electrode material includes a graphite material, at least part of the surface of the graphite material is provided with a coating layer, the material of the coating layer includes hard carbon, the median particle size of the graphite material is D1, the median particle size of the negative electrode material is D2, and the median particle size D2 of the negative electrode material and the median particle size D1 of the graphite material satisfy the following relationship D2 D1≤1μm. The preparation method of the negative electrode material includes the following steps: adding a graphite material to a polymer solution, atomizing to obtain a precursor of a polymer solution-coated graphite material, adding the precursor to a polar solvent, removing the solvent to obtain a graphite material coated with a polymer, wherein the polymer is insoluble in the polar solvent, and the polymer solution includes at least one of a polyimide acid solution, a polyethersulfone solution, and a polyvinylidene fluoride solution. This technical solution uses polyimide as a hard carbon precursor. Through the polyimide material coating and sintering process, the graphite surface is evenly coated with a layer of hard carbon, which can improve the cycle stability of the negative electrode material and the fast charging performance under low temperature conditions.
[0005] Although the "coating-sintering" process can improve the cycle stability of negative electrode materials to a certain extent, graphite materials currently have some problems, such as poor hydrophilicity, difficulty dispersing in aqueous slurries, poor electrolyte wettability, and limited binding ability with binders. These issues lead to challenges in the production of negative electrode plates, such as high energy consumption and poor peel strength when thickly coating the plates.
[0006] Therefore, how to provide a negative electrode material that has good cycle stability and electrical properties, good dispersibility, good electrolyte wettability, high binding strength with the binder, and good processing performance has become a technical problem that needs to be solved urgently.
[0007] Summary of the Invention
[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0009] The present application provides a graphite negative electrode material, its preparation method, and application. By selecting a polymer material with hydrophilic functional groups as the coating layer of the graphite negative electrode material, the graphite negative electrode material prepared in this application not only has good electrical properties, but also good hydrophilicity and high mechanical properties. It has high dispersibility in aqueous slurry, improves the peel strength between the graphite negative electrode material and the electrode sheet, and simplifies the negative electrode slurrying process, reduces energy consumption, and improves processing performance, making it suitable for the preparation of lithium-ion batteries.
[0010] This application adopts the following technical solutions:
[0011] In a first aspect, an embodiment of the present application provides a graphite negative electrode material, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0012] The material of the coating layer includes a polymer material having a hydrophilic functional group.
[0013] The embodiment of the present application selects a polymer material with hydrophilic functional groups as the coating layer of the graphite negative electrode material. On the one hand, the coating layer tightly coats the graphite surface and acts like an artificial SEI film, so that the graphite negative electrode material has good electrical properties. On the other hand, the material of the coating layer includes a polymer material with hydrophilic functional groups, so that the prepared graphite negative electrode material has good hydrophilicity and high dispersibility in aqueous slurry, and has high mechanical properties. There is a high peel strength between the graphite negative electrode material and the electrode sheet. At the same time, the negative electrode slurrying process is simplified, energy consumption is reduced, and processing performance is improved, which is suitable for the preparation of lithium-ion batteries.
[0014] It should be noted that the coating layer at least covers a portion of the graphite surface.
[0015] The following are optional technical solutions for the embodiments of the present application, but are not intended to limit the technical solutions provided in the present application. Through the following optional technical solutions, the objectives and beneficial effects of the present application can be better achieved and realized.
[0016] As an optional technical solution of an embodiment of the present application, the hydrophilic functional group includes any one of a hydroxyl group, a carboxyl group, a sulfonic acid group, a cyano group or an amino group, or a combination of at least two of them.
[0017] In one embodiment, the polymer material is selected from any one or a combination of at least two of lithium acrylate homopolymer, lithium acrylate copolymer, nanocellulose, sodium carboxymethyl cellulose, sodium alginate, polyvinyl alcohol, polyethylene glycol or locust bean gum.
[0018] As an optional technical solution of the embodiment of the present application, the lithium acrylate homopolymer includes the following raw materials in parts by weight: 100 parts of acrylic acid, 40-100 parts of lithium hydroxide monohydrate, and 0.1-4 parts of initiator;
[0019] In the embodiment of the present application, the raw materials for preparing lithium acrylate homopolymer are as follows, based on 100 parts by weight of acrylic acid:
[0020] The weight parts of the lithium hydroxide monohydrate can be 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts or 100 parts, etc.
[0021] The weight proportion of the initiator can be 0.1 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts or 4 parts, etc.
[0022] It should be noted that the present embodiment does not have any special selection of initiators for preparing lithium acrylate homopolymers. All initiators commonly used in the art for preparing polyacrylic acid are applicable, including but not limited to ammonium persulfate.
[0023] In one embodiment, the lithium acrylate homopolymer is prepared by the following method, which comprises the following steps:
[0024] (1) in a protective atmosphere, acrylic acid and a solvent are mixed, an initiator is added thereto, and polymerization is carried out to obtain polyacrylic acid;
[0025] (2) adding lithium hydroxide monohydrate to the reaction system obtained in step (1) to carry out a neutralization reaction to obtain the lithium acrylate homopolymer.
[0026] In one embodiment, the solvent in step (1) is water.
[0027] In one embodiment, the protective gas in step (1) includes nitrogen.
[0028] In one embodiment, the mixing temperature in step (1) is room temperature.
[0029] In one embodiment, the mixing method in step (1) includes stirring, and the stirring speed is 200-400 rpm, for example, it can be 200 rpm, 220 rpm, 240 rpm, 260 rpm, 280 rpm, 300 rpm, 320 rpm, 340 rpm, 360 rpm, 380 rpm or 400 rpm.
[0030] In one embodiment, the mixing time in step (1) is 20 to 60 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes.
[0031] In one embodiment, the temperature of the reaction system when the initiator is added in step (1) is 60-80°C, for example, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C or 80°C.
[0032] In one embodiment, the polymerization process of step (1) includes: polymerizing at 60-80°C (for example, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C or 80°C, etc.) for 3-9h (for example, 3h, 4h, 5h, 6h, 7h, 8h or 9h, etc.), heating to 80-90°C (for example, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C, etc.) and continuing polymerization for 1-3h (for example, 1h, 1.5h, 2h, 2.5h or 3h, etc.), then evacuating the reaction system for 20-40min (for example, 20min, 25min, 30min, 35min or 40min, etc.), and cooling to room temperature to obtain the polyacrylic acid.
[0033] In one embodiment, the neutralization reaction time in step (2) is 40 to 80 min, for example, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min or 80 min.
[0034] In one embodiment, the temperature of the neutralization reaction in step (2) is room temperature.
[0035] In one embodiment, the method for preparing the lithium acrylate homopolymer comprises the following steps:
[0036] (1) In a protective atmosphere, at room temperature and a rotation speed of 200 to 400 rpm, acrylic acid and a solvent are mixed for 20 to 60 minutes, the temperature is raised to 60 to 80° C., an initiator is added thereto, polymerization is carried out at 60 to 80° C. for 3 to 9 hours, the temperature is raised to 80 to 90° C., and polymerization is continued for 1 to 3 hours. The reaction system is then evacuated for 20 to 40 minutes and cooled to room temperature to obtain polyacrylic acid;
[0037] (2) adding lithium hydroxide monohydrate to the reaction system obtained in step (1) at room temperature to carry out a neutralization reaction for 40 to 80 minutes to obtain the lithium acrylate homopolymer.
[0038] As an optional technical solution of the embodiment of the present application, the lithium acrylate copolymer includes the following raw materials in parts by weight: 100 parts of at least two propylene compounds, 40-100 parts of lithium hydroxide monohydrate, and 0.1-4 parts of an initiator;
[0039] The acrylic compound includes acrylic acid, methyl methacrylate, acrylamide, acrylonitrile or 2-hydroxyethyl acrylate.
[0040] In the embodiment of the present application, the raw materials for preparing the lithium acrylate copolymer are as follows, based on 100 parts by weight of the propylene compound:
[0041] The weight parts of the lithium hydroxide monohydrate can be 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts or 100 parts, etc.
[0042] The weight proportion of the initiator can be 0.1 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts or 4 parts, etc.
[0043] It should be noted that the present embodiment does not have any special selection of initiators for preparing lithium acrylate copolymers. All initiators commonly used in the art for preparing acrylic copolymers are applicable, including but not limited to ammonium persulfate.
[0044] In one embodiment, the lithium acrylate copolymer is prepared by the following method, which comprises the following steps:
[0045] (A) mixing at least two propylene compounds and a solvent in a protective atmosphere, adding an initiator thereto, and polymerizing to obtain an acrylic copolymer;
[0046] (B) adding lithium hydroxide monohydrate to the reaction system obtained in step (A) for neutralization reaction to obtain the lithium acrylate copolymer.
[0047] In one embodiment, the solvent in step (A) is water.
[0048] In one embodiment, the protective gas in step (A) comprises nitrogen.
[0049] In one embodiment, the mixing temperature in step (A) is room temperature.
[0050] In one embodiment, the mixing method in step (A) includes stirring, and the stirring speed is 200-400 rpm, for example, it can be 200 rpm, 220 rpm, 240 rpm, 260 rpm, 280 rpm, 300 rpm, 320 rpm, 340 rpm, 360 rpm, 380 rpm or 400 rpm.
[0051] In one embodiment, the mixing time in step (A) is 20 to 60 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes.
[0052] In one embodiment, the temperature of the reaction system when the initiator is added in step (A) is 60-85°C, for example, 60°C, 62°C, 65°C, 67°C, 70°C, 72°C, 75°C, 77°C, 80°C, 81°C, 83°C or 85°C, etc.
[0053] In one embodiment, the polymerization process of step (A) comprises: at 60-85°C (for example, 60°C, 62°C, 65°C, 67°C, 70°C, 72°C, 75°C, 77°C, 80°C, 81°C, 83°C or 85°C, etc.), polymerizing for 3-9h (for example, 3h, 4h, 5h, 6h, 7h, 8h or 9h, etc.), heating to 80-95°C (for example, 80°C, 81°C, 82°C, 83°C, 85°C, etc.), The polymerization is continued for 1 to 3 h (for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h), and then the reaction system is evacuated for 20 to 40 min (for example, 20 min, 25 min, 30 min, 35 min or 40 min), and cooled to room temperature to obtain the acrylic copolymer.
[0054] In one embodiment, the neutralization reaction time in step (B) is 40 to 80 min, for example, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min or 80 min.
[0055] In one embodiment, the neutralization reaction temperature in step (B) is room temperature.
[0056] In one embodiment, the preparation method of the lithium acrylate copolymer comprises the following steps:
[0057] (A) in a protective atmosphere, at room temperature and a rotation speed of 200-400 rpm, mixing an propylene compound and a solvent B for 20-60 minutes, raising the temperature to 60-85° C., adding an initiator thereto, polymerizing at 60-85° C. for 3-9 hours, raising the temperature to 80-95° C., and continuing polymerization for 1-3 hours, then evacuating the reaction system for 20-40 minutes and cooling to room temperature to obtain the acrylic copolymer;
[0058] (B) adding lithium hydroxide monohydrate to the reaction system obtained in step (A) at room temperature for a neutralization reaction of 40 to 80 minutes to obtain the lithium acrylate copolymer.
[0059] Compared with lithium acrylate homopolymer, lithium acrylate copolymer has better flexibility and higher mechanical properties while ensuring better ion conductivity, which enables the coating to adhere more tightly to the graphite surface and not fall off.
[0060] As an optional technical solution of an embodiment of the present application, based on the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.1% to 3%, for example, it can be 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.3%, 2.5%, 2.7% or 3%, etc.
[0061] By controlling the mass content of the coating layer in the graphite negative electrode material within a specific range, the embodiments of the present application can produce a graphite negative electrode material having both high cycle stability and good hydrophilicity and peel strength. If the mass percentage of the coating layer in the graphite negative electrode material is too high, the coating layer is too thick, and the cycle stability of the prepared graphite negative electrode material is poor; if the mass percentage of the coating layer in the graphite negative electrode material is too low, the coating layer is too thin, and the hydrophilicity and peel strength of the prepared graphite negative electrode material are poor.
[0062] In one embodiment, the average particle size of the graphite is 5 to 30 μm, for example, 5 μm, 7 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 23 μm, 25 μm, 27 μm or 30 μm.
[0063] In a second aspect, an embodiment of the present application provides a method for preparing the graphite negative electrode material as described in the first aspect, the preparation method comprising the following steps:
[0064] (S1) mixing a polymer material having a hydrophilic functional group with a solvent to obtain a polymer material slurry;
[0065] (S2) adding graphite to the polymer material slurry obtained in step (S1), mixing uniformly, and then drying to obtain the graphite negative electrode material.
[0066] In an embodiment of the present application, the solid content of the slurry obtained by mixing the polymer material slurry and graphite is 30% to 50%, for example, it can be 30%, 32%, 35%, 38%, 40%, 42%, 46% or 50%.
[0067] As an optional technical solution of the embodiment of the present application, the solvent in step (S1) is selected from any one or a combination of at least two of water, methanol, ethanol, N-methylpyrrolidone or N,N-dimethylformamide, preferably water.
[0068] As an optional technical solution of an embodiment of the present application, the mixing method in step (S1) includes mechanical stirring.
[0069] In one embodiment, the rotation speed of the mechanical stirring is 100 to 5000 rpm (for example, 100 rpm, 500 rpm, 1000 rpm, 1200 rpm, 1500 rpm, 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm, 4000 rpm or 5000 rpm, etc.), more preferably 1200 to 2000 rpm;
[0070] In one embodiment, the mixing time in step (S1) is 10 to 200 min (for example, it can be 10 min, 20 min, 40 min, 60 min, 80 min, 100 min, 120 min, 140 min, 160 min, 180 min or 200 min, etc.), and can further be 40 to 80 min.
[0071] If the mixing time is too short, it will result in uneven dispersion; if the mixing time is too long, it will cause energy waste.
[0072] As an optional technical solution of an embodiment of the present application, the drying temperature is 80-250°C, for example, it can be 80°C, 90°C, 100°C, 120°C, 150°C, 180°C, 200°C, 230°C or 250°C.
[0073] It should be noted that the present invention does not impose any particular restrictions on the drying method, as long as it can fully remove moisture. Exemplary drying methods include, but are not limited to, stirring drying, vacuum drying, oven drying, spray drying, etc.
[0074] In one embodiment, the drying step further includes a post-processing step.
[0075] In one embodiment, the post-processing method includes breaking up the dried product and screening it.
[0076] In one embodiment, the method for preparing the graphite negative electrode specifically comprises the following steps:
[0077] (S1) mixing a polymer material having a hydrophilic functional group with a solvent for 10 to 200 minutes at a rotation speed of 100 to 5000 rpm to obtain a polymer material slurry;
[0078] (S2) adding graphite to the polymer material slurry obtained in step (S1), mixing the mixture evenly, drying the mixture at 80-250° C., breaking the mixture up and sieving the mixture to obtain the graphite negative electrode material.
[0079] In a third aspect, an embodiment of the present application provides a use of the graphite negative electrode material as described in the first aspect in the preparation of a lithium-ion battery.
[0080] This application has the following beneficial effects:
[0081] (1) The present application selects a polymer material with hydrophilic functional groups as the coating layer of the graphite negative electrode material and controls the content of the coating layer in the graphite negative electrode material within a specific range. The prepared graphite negative electrode material improves the hydrophilicity of the graphite negative electrode material while maintaining good electrical properties, so that it has good electrolyte wettability, and at the same time improves the peel strength between the graphite negative electrode material and the electrode sheet. It also simplifies the negative electrode pulping process, reduces energy consumption, and improves processing performance, making it suitable for preparing lithium-ion batteries;
[0082] (2) The graphite negative electrode material provided in the present application has good hydrophilicity and is easy to disperse evenly in an aqueous solution, shortening the time required for uniform dispersion, and its dispersion time is 30 to 60 minutes; it also has a high peel strength, and the peel strength between it and the electrode is 15.3 to 23.3 N / m; at the same time, it also has good electrical properties, with an initial efficiency of 94.1 to 95.0%, a gram capacity of 360.9 to 362.3 mA / h, and a 50-week cycle capacity retention rate of 96.2% to 97.9%.
[0083] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0084] To facilitate understanding of the present application, the present application lists the following examples. Those skilled in the art should understand that the examples are only provided to help understand the present application and should not be considered as specific limitations of the present application.
[0085] The sources of some components in the following examples and comparative examples are as follows:
[0086] Graphite: Qingdao Luowei New Materials Co., Ltd., average particle size between 10-20μm;
[0087] Nanocellulose: Guilin Qihong Technology Co., Ltd.;
[0088] Sodium alginate: Anaiji Chemical;
[0089] Polyvinyl alcohol: Anaiji Chemical, molecular weight about 15,000;
[0090] Polyethylene glycol: Anaiji Chemical, molecular weight about 6000;
[0091] Asphalt: Qingdao Luowei New Materials Co., Ltd.
[0092] Preparation Example 1
[0093] This preparation example provides a lithium acrylate homopolymer 1 and a preparation method thereof, and the preparation method is as follows:
[0094] (1) Acrylic acid (10 g) was dissolved in deionized water (200 g), nitrogen was introduced, and the mixture was stirred at room temperature and a rotation speed of 300 rpm for 40 minutes. The mixture was then heated to 75°C and ammonium persulfate (0.07 g) was added. The mixture was polymerized at 75°C for 4 hours, and then the temperature was raised to 85°C for a further 2 hours. The reaction system was then evacuated for 30 minutes and cooled to room temperature to obtain polyacrylic acid.
[0095] (2) At room temperature, 6 g of a monohydrated lithium hydroxide aqueous solution was added to the reaction system obtained in step (1) for neutralization reaction for 60 min to obtain a solution containing the lithium acrylate homopolymer (solid content: 6.82%), which was recorded as lithium acrylate homopolymer 1.
[0096] Preparation Example 2
[0097] This preparation example provides a lithium acrylate homopolymer 2 and a preparation method thereof, and the preparation method is as follows:
[0098] (1) Acrylic acid (10 g) was dissolved in deionized water (200 g), nitrogen was introduced, and the mixture was stirred at room temperature and a rotation speed of 200 rpm for 60 min. The mixture was then heated to 75°C and ammonium persulfate (0.07 g) was added. The mixture was polymerized at 75°C for 3 h, and then the temperature was raised to 85°C for a further 2 h. The reaction system was then evacuated for 30 min and cooled to room temperature to obtain polyacrylic acid.
[0099] (2) At room temperature, 6 g of a monohydrated lithium hydroxide aqueous solution was added to the reaction system obtained in step (1) for neutralization reaction for 50 min to obtain a solution containing the lithium acrylate homopolymer (solid content: 6.65%), which was recorded as lithium acrylate homopolymer 2.
[0100] Preparation Example 3
[0101] This preparation example provides a lithium acrylate homopolymer 3 and a preparation method thereof, and the preparation method is as follows:
[0102] (1) Acrylic acid (10 g) was dissolved in deionized water (200 g), nitrogen was introduced, and the mixture was stirred at room temperature and a rotation speed of 400 rpm for 20 minutes. The mixture was then heated to 75°C and ammonium persulfate (0.07 g) was added. The mixture was polymerized at 75°C for 5 hours, and then the temperature was raised to 90°C and the polymerization was continued for 1 hour. The reaction system was then evacuated for 20 minutes and cooled to room temperature to obtain polyacrylic acid.
[0103] (2) At room temperature, 4 g of lithium hydroxide monohydrate aqueous solution was added to the reaction system obtained in step (1) for neutralization reaction for 80 min to obtain a solution containing the lithium acrylate homopolymer (solid content of 5.80%), which was recorded as lithium acrylate homopolymer 3.
[0104] Preparation Example 4
[0105] This preparation example provides a lithium acrylate copolymer 1 and a preparation method thereof, and the preparation method is as follows:
[0106] (A) Acrylic acid (8 g), acrylonitrile (2 g), and acrylamide (1 g) were dissolved in deionized water (200 g), and nitrogen was introduced. The mixture was stirred at room temperature and 300 rpm for 30 min, and then the temperature was raised to 80°C. Ammonium persulfate (0.05 g) was added, and polymerization was carried out at 80°C for 6 h. The temperature was then raised to 88°C and polymerization was continued for 2 h. The reaction system was then evacuated for 30 min and cooled to room temperature.
[0107] (B) To the reaction system obtained in step (A), 4 g of lithium hydroxide monohydrate aqueous solution was added at room temperature for neutralization reaction for 60 min to obtain a solution containing the acrylic acid copolymer (solid content of 6.85%), which was recorded as acrylic acid lithium copolymer 1.
[0108] Preparation Example 5
[0109] This preparation example provides a lithium acrylate copolymer 2 and a preparation method thereof, and the preparation method is as follows:
[0110] (A) Acrylic acid (8 g), methyl methacrylate (1 g), and 2-hydroxyethyl acrylate (1 g) were dissolved in deionized water (200 g), and nitrogen was introduced. The mixture was stirred at room temperature and a rotation speed of 400 rpm for 20 min, and then the temperature was raised to 75°C. Ammonium persulfate (0.05 g) was added thereto, and polymerization was carried out at 75°C for 5 h. The temperature was then raised to 85°C and polymerization was continued for 2 h. The reaction system was then evacuated for 30 min and cooled to room temperature.
[0111] (B) To the reaction system obtained in step (A), 4 g of lithium hydroxide monohydrate aqueous solution was added at room temperature for neutralization reaction for 70 min to obtain a solution containing the acrylic acid copolymer (solid content of 5.73%), which was recorded as acrylic acid lithium copolymer 2.
[0112] Preparation Example 6
[0113] This preparation example provides a lithium acrylate copolymer 3 and a preparation method thereof, and the preparation method is as follows:
[0114] (A) Acrylic acid (8 g), 2-hydroxyethyl acrylate (1 g), and acrylamide (1 g) were dissolved in deionized water (200 g), and nitrogen was introduced. The mixture was stirred at room temperature and 200 rpm for 60 min, and then the temperature was raised to 75°C. Ammonium persulfate (0.07 g) was added, and polymerization was carried out at 80°C for 5 h. The temperature was then raised to 85°C and polymerization was continued for 2 h. The reaction system was then evacuated for 30 min and cooled to room temperature.
[0115] (B) An aqueous solution containing 4 g of lithium hydroxide monohydrate was added to the reaction system obtained in step (A) at room temperature for neutralization reaction for 40 minutes to obtain a solution containing the acrylic acid copolymer (solid content of 6.78%), which was recorded as acrylic acid lithium copolymer 3.
[0116] Example 1
[0117] This embodiment provides a graphite negative electrode material (GRA-1) and a preparation method thereof, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0118] The material of the coating layer is the acrylic acid homopolymer provided in Preparation Example 1;
[0119] Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.99%.
[0120] The preparation method of the graphite negative electrode material is as follows:
[0121] (S1) mixing 14.66 g of the solution of lithium acrylate homopolymer provided in Preparation Example 1 (containing 1 g of lithium acrylate homopolymer) with 150 g of water at a rotation speed of 1500 rpm for 60 min to obtain a polymer material slurry;
[0122] (S2) Adding 100 g of graphite to the polymer material slurry obtained in step (S1) and mixing for 30 minutes, removing moisture by spray drying, collecting the powder, and then drying it at 100°C for 1 hour to fully evaporate the moisture, breaking it up and sieving it to obtain the graphite negative electrode material, which is recorded as GRA-1.
[0123] Example 2
[0124] This embodiment provides a graphite negative electrode material (GRA-2) and a preparation method thereof, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0125] The materials of the coating layer are acrylic acid homopolymer and nanocellulose provided in Preparation Example 2;
[0126] Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.99%.
[0127] The preparation method of the graphite negative electrode material is as follows:
[0128] (S1) mixing 12.03 g of the lithium acrylate homopolymer solution provided in Preparation Example 2 (containing 0.8 g of lithium acrylate homopolymer), 0.2 g of nanocellulose, and 150 g of water at a rotation speed of 2000 rpm for 40 minutes to obtain a polymer material slurry;
[0129] (S2) Adding 100 g of graphite to the polymer material slurry obtained in step (S1) and mixing for 30 minutes, removing moisture by spray drying, collecting the powder, and then drying it at 100°C for 1 hour to fully evaporate the moisture, breaking it up and sieving it to obtain the graphite negative electrode material, which is recorded as GRA-2.
[0130] Example 3
[0131] This embodiment provides a graphite negative electrode material (GRA-3) and a preparation method thereof, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0132] The materials of the coating layer are acrylic acid homopolymer and sodium alginate provided in Preparation Example 3;
[0133] Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.99%.
[0134] The preparation method of the graphite negative electrode material is as follows:
[0135] (S1) Mixing 13.79 g of the lithium acrylate homopolymer solution provided in Preparation Example 3 (including 0.8 g of lithium acrylate homopolymer), 0.2 g of sodium alginate, and 150 g of water at a rotation speed of 1200 rpm for 80 minutes to obtain a polymer material slurry;
[0136] (S2) Adding 100 g of graphite to the polymer material slurry obtained in step (S1) and mixing for 30 minutes, removing moisture by spray drying, collecting the powder, and then drying it at 100°C for 1 hour to fully evaporate the moisture, breaking it up and sieving it to obtain the graphite negative electrode material, which is recorded as GRA-3.
[0137] Example 4
[0138] This embodiment provides a graphite negative electrode material (GRA-4) and a preparation method thereof, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0139] The material of the coating layer is the acrylic acid copolymer provided in Preparation Example 4;
[0140] Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.99%.
[0141] The preparation method of the graphite negative electrode material is as follows:
[0142] (S1) Mixing 14.60 g of the lithium acrylate copolymer solution provided in Preparation Example 4 (containing 1 g of the lithium acrylate copolymer) with 150 g of water at a rotation speed of 1500 rpm for 30 minutes to obtain a polymer material slurry;
[0143] (S2) Adding 100 g of graphite to the polymer material slurry obtained in step (S1) and mixing for 30 minutes, removing moisture by spray drying, collecting the powder, and then drying it at 100°C for 1 hour to fully evaporate the moisture, breaking it up and sieving it to obtain the graphite negative electrode material, which is recorded as GRA-4.
[0144] Example 5
[0145] This embodiment provides a graphite negative electrode material (GRA-5) and a preparation method thereof, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0146] The material of the coating layer is the acrylic acid copolymer and polyvinyl alcohol provided in Preparation Example 5;
[0147] Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.99%.
[0148] The preparation method of the graphite negative electrode material is as follows:
[0149] (S1) Mixing 13.96 g of the lithium acrylate copolymer solution provided in Preparation Example 5 (containing 0.8 g of the lithium acrylate copolymer), 0.2 g of polyvinyl alcohol, and 150 g of water at a rotation speed of 1500 rpm for 30 minutes to obtain a polymer material slurry;
[0150] (S2) Adding 100 g of graphite to the polymer material slurry obtained in step (S1) and mixing for 30 minutes, removing moisture by spray drying, collecting the powder, and then drying it at 100°C for 1 hour to fully evaporate the moisture, breaking it up and sieving it to obtain the graphite negative electrode material, which is recorded as GRA-5.
[0151] Example 6
[0152] This embodiment provides a graphite negative electrode material (GRA-6) and a preparation method thereof, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0153] The material of the coating layer is the acrylic acid copolymer and polyethylene glycol provided in Preparation Example 6;
[0154] Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.99%.
[0155] The preparation method of the graphite negative electrode material is as follows:
[0156] (S1) Mixing 11.80 g of the lithium acrylate copolymer solution provided in Preparation Example 6 (including 0.8 g of the lithium acrylate copolymer), 0.2 g of polyethylene glycol, and 150 g of water at a rotation speed of 1500 rpm for 30 minutes to obtain a polymer material slurry;
[0157] (S2) Adding 100 g of graphite to the polymer material slurry obtained in step (S1) and mixing for 30 minutes, removing moisture by spray drying, collecting the powder, and then drying it at 100°C for 1 hour to fully evaporate the moisture, breaking it up and sieving it to obtain the graphite negative electrode material, which is recorded as GRA-6.
[0158] Example 7
[0159] This embodiment provides a graphite negative electrode material (GRA-7) and a preparation method thereof. The only difference from Example 1 is that the material of the coating layer is nanocellulose, and other conditions are the same as those in Example 1.
[0160] Example 8
[0161] This embodiment provides a graphite negative electrode material (GRA-8) and a preparation method thereof. The only difference from Example 1 is that the material of the coating layer is sodium alginate, and other conditions are the same as those in Example 1.
[0162] Example 9
[0163] This embodiment provides a graphite negative electrode material (GRA-9) and a preparation method thereof. The difference from Example 1 is that, based on the mass percentage of the graphite negative electrode material being 100%, the mass percentage of the coating layer is 0.12%;
[0164] In step (S1), 1.76 g of the solution of lithium acrylate homopolymer provided in Preparation Example 1 (containing 0.12 g of lithium acrylate homopolymer) was used;
[0165] Other conditions are the same as in Example 1.
[0166] Example 10
[0167] This embodiment provides a graphite negative electrode material (GRA-10) and a preparation method thereof. The difference from Example 1 is that, based on the mass percentage of the graphite negative electrode material being 100%, the mass percentage of the coating layer is 3%;
[0168] In step (S1), 48.99 g of the solution of lithium acrylate homopolymer provided in Preparation Example 1 (containing 3 g of lithium acrylate homopolymer) was used;
[0169] Other conditions are the same as in Example 1.
[0170] Example 11
[0171] This embodiment provides a graphite negative electrode material (GRA-11) and a preparation method thereof. The difference from Example 1 is that, based on the mass percentage of the graphite negative electrode material being 100%, the mass percentage of the coating layer is 0.07%;
[0172] In step (S1), 1.03 g of the solution of lithium acrylate homopolymer provided in Preparation Example 1 (containing 0.07 g of lithium acrylate homopolymer) was used;
[0173] Other conditions are the same as in Example 1.
[0174] Example 12
[0175] This embodiment provides a graphite negative electrode material (GRA-12) and a preparation method thereof. The difference from Example 1 is that, based on the mass percentage of the graphite negative electrode material being 100%, the mass percentage of the coating layer is 3.5%;
[0176] In step (S1), 51.32 g of the solution of lithium acrylate homopolymer provided in Preparation Example 1 (containing 3.5 g of lithium acrylate homopolymer) was used;
[0177] Other conditions are the same as in Example 1.
[0178] Comparative Example 1
[0179] This comparative example provides a graphite negative electrode material (GRA-REF), which is graphite without any treatment and is denoted as GRA-REF.
[0180] Comparative Example 2
[0181] This comparative example provides a graphite negative electrode material (GRA-asphalt) and a preparation method thereof, wherein the graphite negative electrode material comprises graphite and a coating layer coated on the surface of the graphite;
[0182] The material of the coating layer is high-temperature asphalt (residual carbon content 56%);
[0183] Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the sintered carbon coating layer is 0.99%.
[0184] The preparation method of the graphite negative electrode material is as follows:
[0185] Take 300g of graphite negative electrode material and 5.36g of high-temperature asphalt in a mixer, mix them thoroughly for 1h, put the mixed materials into a graphite crucible, and send them into a high-sand kiln; heat them to 1200℃ under nitrogen protection and keep them warm for 2h; take out the sample after the surface is completely carbonized, cool it to room temperature, and mechanically break up the material and sieve it to obtain the asphalt-coated carbonized product.
[0186] The performance of the graphite negative electrode materials provided in the above embodiments and comparative examples was tested using the following test methods:
[0187] (1) Dispersion test
[0188] The graphite negative electrode material, conductive agent and binder provided in the above embodiments and comparative examples were dissolved in deionized water in a mass percentage of 95:1:4 and mixed to obtain a slurry (solid content of 40%). The slurries were dispersed for 30 min, 60 min, 90 min and 120 min, respectively, and sieved (mesh size of 400 mesh). If the sieve was smooth without obvious residue, the slurry was considered to be uniformly dispersed.
[0189] (2) Peel strength test
[0190] The uniformly dispersed slurry tested by the dispersion test was evenly coated on the copper foil current collector, vacuum dried to obtain the negative electrode sheet, and the peeling force test was carried out according to the GB / T 2790-1995 standard.
[0191] (3) Button battery cycle performance test
[0192] The negative electrode materials provided in the above embodiments and comparative examples were respectively mixed with conductive carbon black, sodium carboxymethyl cellulose, and polyacrylic acid binder in a ratio of 95:0.5:1:3.5 to prepare a slurry, evenly coated on a copper foil, and dried to form a negative electrode plate; the negative electrode plate was placed in an argon atmosphere glove box to make a button battery, a polypropylene microporous membrane was used as a diaphragm, the electrolyte used was 1 mol / L lithium hexafluorophosphate (the solvent was a mixture of ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, and fluoroethylene carbonate in a volume ratio of 30:30:30:10), and the counter electrode used was a metal lithium sheet; the main evaluation indicators were the first efficiency, gram capacity, and 50-week cycle capacity retention rate of the button battery.
[0193] At 25°C and normal pressure, the button cell was discharged at a constant current rate of 0.1C to a voltage of 0.005V, then discharged at a constant current rate of 0.05C to a voltage of 0.005V. The discharge specific capacity at this point was recorded, which was the initial lithium insertion capacity. The button cell was then charged at a constant current rate of 0.1C to a voltage of 1.5V. The charge specific capacity at this point was recorded, which was the initial lithium removal capacity, denoted as gram capacity in this patent. The button cell was subjected to 50 cycle charge and discharge tests according to the above method, and the lithium removal capacity was recorded each time.
[0194] First coulombic efficiency of negative electrode active material (first efficiency, %) = first lithium removal capacity / first lithium insertion capacity × 100%;
[0195] Cycle capacity retention rate of negative electrode active material (%) = 50th delithiation capacity / first delithiation capacity × 100%.
[0196] The performance test results of the graphite negative electrode materials provided in the above examples and comparative examples are shown in Table 1 below:
[0197] Table 1
[0198] As can be seen from the above table, this application selects a polymer material with hydrophilic functional groups as the coating layer of the graphite negative electrode material, and controls the content of the coating layer in the graphite negative electrode material within a specific range. The prepared graphite negative electrode material improves the hydrophilicity of the graphite negative electrode material while maintaining good electrical properties, so that it has better electrolyte wettability, and at the same time improves the peeling strength between the graphite negative electrode material and the electrode sheet. The dispersion time is 30 to 60 minutes, the peeling strength is 15.3 to 23.3 N / m, the first efficiency is 94.1 to 95.0%, the gram capacity is 360.9 to 362.2 mA / h, and the 50-week cycle capacity retention rate is 96.2% to 97.9%.
[0199] Furthermore, the present application can further improve the hydrophilicity, peel strength and cycle stability of the graphite negative electrode material by using a polymer material including lithium acrylate homopolymer or lithium acrylate copolymer as the coating layer material. The dispersion time is 30 minutes to obtain a uniformly dispersed slurry with a peel strength of 17.8 to 23.3 N / m and a 50-week cycle capacity retention rate of 97.0% to 97.9%.
[0200] Compared with Example 1, if the content of the coating layer in the graphite negative electrode material is too little (Example 11), the hydrophilicity and peel strength of the prepared graphite negative electrode material are poor; if the mass percentage of the coating layer in the graphite negative electrode material is too high (Example 12), although the peel strength is further improved, the first efficiency, gram capacity, and cycle capacity retention rate of the graphite material all decrease to a certain extent.
[0201] Compared with Example 1, if graphite without a coating layer is directly used as the negative electrode material (Comparative Example 1), its hydrophilicity and peel strength are relatively poor; the graphite material prepared by the asphalt coating-carbonization process (Comparative Example 2) has achieved certain improvements in electrical properties, but there is no obvious difference in dispersibility and peel strength compared with the original sample (Comparative Example 1).
[0202] In summary, the present application selects a polymer material with hydrophilic functional groups as the coating layer of the graphite negative electrode material, and controls the content of the coating layer in the graphite negative electrode material within a specific range. The prepared graphite negative electrode material improves the hydrophilicity of the graphite negative electrode material while maintaining good electrical properties, so that it has good electrolyte wettability, and at the same time improves the peeling strength between the graphite negative electrode material and the electrode sheet. It also simplifies the negative electrode slurrying process, reduces energy consumption, and improves processing performance, making it suitable for the preparation of lithium-ion batteries.
[0203] The applicant declares that while the above-mentioned embodiments are used to illustrate the detailed process flow of the present application, the present application is not limited to the above-mentioned detailed process flow, which does not mean that the present application must rely on the above-mentioned detailed process flow in order to be implemented. Those skilled in the art should understand that any improvements to the present application, equivalent replacements for the raw materials of the present application's products, addition of auxiliary ingredients, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present application.
Claims
1. A graphite negative electrode material, comprising graphite and a coating layer coated on the surface of the graphite; The material of the coating layer includes a polymer material having a hydrophilic functional group.
2. The graphite negative electrode material according to claim 1, wherein The hydrophilic functional group includes any one of a hydroxyl group, a carboxyl group, a sulfonic acid group, a cyano group or an amino group, or a combination of at least two of them.
3. The graphite negative electrode material according to claim 1 or 2, wherein The polymer material is selected from any one or a combination of at least two of lithium acrylate homopolymer, lithium acrylate copolymer, nanocellulose, sodium carboxymethyl cellulose, sodium alginate, polyvinyl alcohol, polyethylene glycol or locust bean gum.
4. The graphite negative electrode material according to claim 3, wherein The lithium acrylate homopolymer comprises the following raw materials in parts by weight: 100 parts of acrylic acid, 40-100 parts of lithium hydroxide monohydrate, and 0.1-4 parts of initiator; Optionally, the lithium acrylate homopolymer is prepared by the following method, which comprises the following steps: (1) in a protective atmosphere, acrylic acid and a solvent are mixed, an initiator is added thereto, and polymerization is performed to obtain polyacrylic acid; (2) adding lithium hydroxide monohydrate to the reaction system obtained in step (1) to carry out a neutralization reaction to obtain the lithium acrylate homopolymer; Optionally, the polymerization process of step (1) comprises: polymerizing at 60-80° C. for 3-9 hours, heating to 80-90° C. and continuing polymerization for 1-3 hours, then evacuating the reaction system for 20-40 minutes, and cooling to room temperature to obtain polyacrylic acid; Optionally, the neutralization reaction time in step (2) is 40 to 80 minutes.
5. The graphite negative electrode material according to claim 3 or 4, wherein The lithium acrylate copolymer comprises the following raw materials in parts by weight: 100 parts of at least two propylene compounds, 40-100 parts of lithium hydroxide monohydrate, and 0.1-4 parts of an initiator; The acrylic compound includes acrylic acid, methyl methacrylate, acrylamide, acrylonitrile or 2-hydroxyethyl acrylate; Optionally, the lithium acrylate copolymer is prepared by the following method, which comprises the following steps: (A) in a protective atmosphere, uniformly mixing at least two propylene compounds and a solvent, adding an initiator thereto, and polymerizing to obtain an acrylic copolymer; (B) adding lithium hydroxide monohydrate to the reaction system obtained in step (A) for neutralization reaction to obtain the lithium acrylate copolymer; Optionally, the polymerization process of step (A) comprises: polymerizing at 60-85° C. for 3-9 hours, heating to 80-95° C. and continuing the reaction for 1-3 hours, evacuating the reaction system for 20-40 minutes, and cooling to room temperature to obtain an acrylic copolymer; Optionally, the neutralization reaction time in step (B) is 40 to 80 minutes.
6. The graphite negative electrode material according to any one of claims 1 to 5, wherein: Taking the mass percentage of the graphite negative electrode material as 100%, the mass percentage of the coating layer is 0.1% to 3%; Optionally, the average particle size of the graphite is 5 to 30 μm.
7. A method for preparing the graphite negative electrode material according to any one of claims 1 to 6, the preparation method comprising the following steps: (S1) mixing a polymer material having a hydrophilic functional group with a solvent to obtain a polymer material slurry; (S2) adding graphite to the polymer material slurry obtained in step (S1), mixing evenly, and then drying to obtain the graphite negative electrode material.
8. The preparation method according to claim 7, wherein: The solvent in step (S1) is selected from any one of water, methanol, ethanol, N-methylpyrrolidone or N,N-dimethylformamide or a combination of at least two thereof, and may further be water.
9. The preparation method according to claim 7 or 8, wherein: The mixing method in step (S1) includes mechanical stirring; Optionally, the rotation speed of the mechanical stirring is 100 to 5000 rpm, more preferably 1200 to 2000 rpm; Optionally, the mixing time in step (S1) is 10 to 200 min, more preferably 40 to 80 min.
10. The preparation method according to any one of claims 7 to 9, wherein: The drying temperature is 80-250°C; Optionally, the drying further includes a post-processing step; Optionally, the post-processing method includes breaking up and sieving the dried product.
11. A use of the graphite negative electrode material according to any one of claims 1 to 6, wherein the graphite negative electrode material is used to prepare a lithium ion battery.
Citation Information
Patent Citations
Negative-electrode active material for non-aqueous secondary battery, and negative electrode and non-aqueous secondary battery using said active material
CN104106162A
Artificial graphite negative electrode material connected with binder on surface and preparation method and application thereof
CN115799506A
Negative electrode material for use in non-aqueous secondary battery and method of producing the same
JP2001167755A
Active material and non-aqueous electrolyte battery using the same, and battery producing method
JP2002246020A