Silicone rubber emulsion and preparation method therefor, and waterborne coating

Through the synergy of solid nanoparticles and emulsifiers, Pickering emulsion and phase inversion emulsification methods are used to solve the problems of high energy consumption and safety and environmental protection in the preparation of traditional silicone rubber emulsion, and realize the preparation of silicone rubber emulsion at low cost and mild conditions, improving Improve the stability and safety of the lotion.

WO2024221551A1PCT designated stage expired Publication Date: 2024-10-31AEROSPACE RES INST OF MATERIAL & PROCESSING TECH

Patent Information

Application Number
PCT/CN2023/099405
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2023-06-09
Publication Date
2024-10-31

Smart Images

  • Figure CN2023099405_31102024_PF_FP_ABST
    Figure CN2023099405_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a silicone rubber emulsion and a preparation method therefor, and a waterborne coating. The silicone rubber emulsion comprises 100 parts of silicone rubber, 20-40 parts of an amphiphilic molecule-modified SiO2 colloid, 5-10 parts of an emulsifier, and not less than 100 parts of water. By adding the amphiphilic molecule-modified SiO2 colloid in a specific ratio to the silicone rubber emulsion, and through the synergistic cooperation of solid nanoparticles and the emulsifier, the interface between the silicone rubber and water is stabilized, and the use of emulsifier can be reduced. By means of the amphiphilicity and steric hindrance of the solid nanoparticles, the stability of the resulting Pickering emulsion is superior to that of an emulsion using a conventional emulsifier. Additionally, the preparation method can achieve the preparation of an emulsion under mild conditions through the synergistic cooperation of the solid nanoparticles and the emulsifier and by using a phase inversion emulsification method. The process does not involve high pressure, high speed, or long-time stirring, the total time spent on the preparation process can be controlled within 4 h, energy consumption can be significantly reduced, and dependency on equipment is low.
Need to check novelty before this filing date? Find Prior Art

Description

Silicone rubber emulsion, preparation method and water-based coating

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 25, 2023, with application number 202310455402.X and invention name “A silicone rubber emulsion, preparation method and water-based coating”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The invention relates to a silicone rubber emulsion, a preparation method and a water-based paint, and belongs to the technical field of water-based coatings. Background Art

[0003] Silicone rubber is a preferred substrate for ablative thermal protection coatings due to its high heat resistance, excellent flexibility, and mild curing conditions. However, conventional silicone rubber ablative thermal protection coatings require the use of organic diluents such as gasoline and acetone to reduce viscosity, which poses serious safety and environmental concerns and hinders their large-scale production and use. Developing water-based silicone rubber ablative thermal protection coatings using water as a diluent is an important approach to addressing this issue. The preparation of silicone rubber emulsions is crucial for developing water-based silicone rubber ablative thermal protection coatings, as the stability of the emulsion directly determines the coating's storage stability. However, the helical structure of silicone rubber causes its hydrophobic groups to align outward, resulting in its hydrophobic properties. Traditional methods for preparing silicone rubber emulsions require large amounts of emulsifiers and high-pressure equipment such as emulsion homogenizers, which consume high energy and carry high risks, making them unsuitable for large-scale production. Developing low-cost, mild methods for preparing silicone rubber emulsions has become an urgent task.

[0004] Summary of the Invention

[0005] The object of the present invention is to overcome the above-mentioned defects of the prior art and provide a silicone rubber emulsion, a preparation method and a water-based coating. By synergizing solid nanoparticles and an emulsifier, the interface between silicone rubber and water can be stabilized, the use of emulsifier can be reduced, and the stability of the Pickering emulsion formed by the amphiphilicity of the solid nanoparticles and their steric hindrance is superior to that of emulsions using traditional emulsifiers. In addition, the preparation method synergizes the solid nanoparticles and the emulsifier and adopts a phase inversion emulsification method, so that the emulsion can be prepared under mild conditions.

[0006] The above-mentioned purpose of the present invention is mainly achieved through the following technical solutions:

[0007] A silicone rubber emulsion comprising the following components in parts by weight:

[0008] In the above silicone rubber emulsion, the structural formula of the silicone rubber is as follows:

[0009] Wherein, R1 and R2 are any one of methyl, phenyl or oxyethyl, preferably R1 and R2 are both methyl or phenyl.

[0010] In the above silicone rubber emulsion, the preparation method of the SiO2 colloid includes:

[0011] Mix 20-40 parts by mass of silicon powder and 60-80 parts by mass of deionized water and heat to 70-90° C., add 0.1-0.2 parts by mass of NaOH and keep the mixture warm for more than 8 hours.

[0012] In the above silicone rubber emulsion, the amphiphilic molecule is a silane coupling agent, and the structural formula is:

[0013] Wherein, R1 is methyl or ethyl, and R2 is amino, epoxy or methacryloxy.

[0014] In the above silicone rubber emulsion, the preparation method of the amphiphilic molecule-modified SiO2 colloid includes:

[0015] After 100 parts by mass of SiO2 colloid is stirred and heated to 55-65°C, 1.5-3 parts by mass of amphiphilic molecules are added dropwise at a rate of 0.5-1.5 g / min, stirred and kept warm for more than 2 hours to obtain SiO2 colloid modified with amphiphilic molecules.

[0016] In the silicone rubber emulsion, the emulsifier is any one of polyethylene glycol p-isooctylphenyl ether, polyoxyethylene sorbitan monostearate, sodium dodecylbenzenesulfonate or sorbitan fatty acid ester.

[0017] In the silicone rubber emulsion, the water is deionized water.

[0018] The preparation method of the silicone rubber emulsion includes pre-emulsification and phase inversion emulsification of the silicone rubber.

[0019] A method for preparing a silicone rubber emulsion, comprising:

[0020] At a rotation speed of 500 to 1000 r / min, 100 parts by mass of silicone rubber and 5 to 10 parts by mass of emulsifier are uniformly mixed, and then 20 to 40 parts by mass of amphiphilic molecule-modified SiO2 colloid are dropwise added at a rate of 0.05 to 0.15 g / s to obtain a pre-emulsified water-in-oil structure cream;

[0021] Raising the speed to not less than 2000 r / min and adding not less than 100 parts by mass of deionized water to the pre-emulsified water-in-oil structure cream, and performing phase inversion to obtain an oil-in-water structure emulsion;

[0022] The silicone rubber emulsion is obtained by stirring.

[0023] In the above-mentioned method for preparing the silicone rubber emulsion, the silicone rubber emulsion is obtained by stirring at 200 to 1000 r / min for 30 minutes or more.

[0024] In the preparation method of the above silicone rubber emulsion, the structural formula of the silicone rubber is as follows:

[0025] Wherein, R1 and R2 are any one of methyl, phenyl or oxyethyl.

[0026] In the above-mentioned method for preparing silicone rubber emulsion, the amphiphilic molecule is a silane coupling agent, and the structural formula is:

[0027] Wherein, R1 is methyl or ethyl, and R2 is amino, epoxy or methacryloxy.

[0028] In the above-mentioned method for preparing the silicone rubber emulsion, the method for preparing the amphiphilic molecule-modified SiO2 colloid comprises:

[0029] 20-40 parts by mass of silicon powder and 60-80 parts by mass of deionized water are mixed and heated to 70-90° C., 0.1-0.2 parts by mass of NaOH are added thereto and the mixture is kept warm for 8 hours or more to obtain SiO2 colloid;

[0030] After 100 parts by mass of SiO2 colloid is stirred and heated to 55-65°C, 1.5-3 parts by mass of amphiphilic molecules are added dropwise at a rate of 0.5-1.5 g / min, and the mixture is stirred and kept warm for 2 hours or more to obtain SiO2 colloid modified with amphiphilic molecules.

[0031] In the preparation method of the silicone rubber emulsion, the emulsifier is any one of polyethylene glycol p-isooctylphenyl ether, polyoxyethylene sorbitan monostearate, sodium dodecylbenzenesulfonate or sorbitan fatty acid ester.

[0032] A silicone rubber emulsion is obtained by adopting the above preparation method.

[0033] A water-based paint comprises the silicone rubber emulsion, a curing agent, a stabilizer and a functional filler, wherein the mass percentage content of the silicone rubber emulsion is 60-80%.

[0034] A water-based coating is prepared by using the water-based paint, comprising: preparing the water-based paint on the surface of a product by spraying, brushing or scraping, and curing.

[0035] Compared with the prior art, the present invention has at least the following beneficial effects:

[0036] (1) The present invention stabilizes the interface between silicone rubber and water by adding SiO2 colloid modified by amphiphilic molecules in a specific ratio, solid nanoparticles and emulsifiers to the silicone rubber emulsion, thereby reducing the use of emulsifiers.

[0037] (2) The silicone rubber emulsion of the present invention has a Pickering emulsion stability that is better than that of an emulsion using a traditional emulsifier due to the amphiphilicity of the solid nanoparticles and their steric hindrance.

[0038] (3) The preparation method of the present invention can achieve emulsion preparation under mild conditions by synergizing solid nanoparticles with emulsifiers and adopting phase inversion emulsification method.

[0039] (4) The present invention prepares the emulsion by a phase inversion method, which does not involve high pressure, high speed, or long-term stirring. The total time of the preparation process can be controlled within 4 hours, which can significantly reduce energy consumption and has low dependence on equipment.

[0040] (5) In the process of preparing the silicone rubber emulsion of the present invention, the white cream in the "water-in-oil" state can be stored stably for a long time, and when it is used, water can be added and stirred to form an emulsion, which can overcome the problem of the traditional emulsion having relatively strict storage conditions.

[0041] (6) The chemical substances used in the preparation process of the silicone rubber emulsion of the present invention are all non-toxic or low-toxic, and have good environmental protection. The silicone rubber emulsion can be used to prepare water-based ablation-resistant heat-resistant coatings and other water-based coatings. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] FIG1 is an electron microscopic image of the methyl silicone rubber emulsion prepared in Example 1 of the present invention;

[0043] FIG2 shows the morphology of the film after curing of the methyl silicone rubber emulsion prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0044] The present invention will be described in further detail below with reference to the accompanying drawings and specific embodiments:

[0045] The silicone rubber emulsion provided in the embodiment of the present invention comprises the following components in parts by weight:

[0046] Silicone rubber, 100 parts by mass;

[0047] 20-40 parts by mass of amphiphilic molecule-modified SiO2 colloid;

[0048] Emulsifier, 5 to 10 parts by mass;

[0049] Water, not less than 100 parts by mass

[0050] In an optional embodiment, the structural formula of the silicone rubber is:

[0051] R1 and R2 are any one of methyl, phenyl or oxyethyl.

[0052] Preferably, R1 and R2 are both methyl or phenyl.

[0053] Preferably, the viscosity of the silicone rubber is not higher than 8000 mPa·s.

[0054] The method for preparing the silicone rubber emulsion provided in an embodiment of the present invention comprises the following steps:

[0055] (1) Preparation of SiO2 colloid.

[0056] Mix 20-40 parts by mass of silicon powder with 60-80 parts by mass of deionized water, add them to a three-necked flask and heat to activate the mixture at a reaction temperature of 70-90°C, then add 0.1-0.2 parts by mass of an alkaline catalyst (such as NaOH) and maintain the reaction temperature. After reacting for more than 8 hours, let it stand and filter under reduced pressure to obtain SiO2 colloid.

[0057] (2) Amphiphilic molecular modification of SiO2 colloid.

[0058] After 100 parts by mass of SiO2 colloid is stirred and heated to 55-65°C, 1.5-3 parts by mass of amphiphilic molecules are added dropwise at a rate of 0.05-0.15 g / min, stirred and kept warm for more than 2 hours to obtain SiO2 colloid modified with amphiphilic molecules.

[0059] Before adding the amphiphilic molecules, the SiO2 colloid is stirred and heated to 55-65°C, and then maintained at this temperature.

[0060] In an optional embodiment, the added amphiphilic molecule is a silane coupling agent, and the added amount is 5-10% of the solid content in the SiO2 colloid.

[0061] The structural formula of silane coupling agent is:

[0062] Among them, R1 is methyl or ethyl, and R2 is amino, epoxy or methacryloxy.

[0063] (3) Pre-emulsification of silicone rubber.

[0064] At a speed of 500-1000 r / min, add 100 parts by mass of silicone rubber and 5-10 parts by mass of emulsifier into a beaker, disperse them evenly at low speed in a disperser, and then add 20-40 parts by mass of SiO2 colloid modified with amphiphilic molecules dropwise at a rate of 0.05-0.15 g / s until a white cream with an "oil-in-water" structure is formed.

[0065] In an optional embodiment, the emulsifier added in the present invention is one of polyethylene glycol 4-isooctylphenyl ether (referred to as Triton X-100), polyoxyethylene sorbitan monostearate (referred to as Tween 60), sodium dodecylbenzenesulfonate (referred to as SDBS), and sorbitan fatty acid ester (Span 80).

[0066] (4) Phase inversion emulsification.

[0067] Increase the speed to not less than 2000 r / min, and at high speed, quickly add not less than 100 parts by mass of deionized water to the white cream in step (3), and form a white emulsion with an "oil-in-water" structure after high-speed dispersion.

[0068] After the emulsion is formed, the stirring speed is changed to low speed 200-1000 r / min, and the stirring is carried out until the bubbles are discharged, and the time is not less than 30 minutes, so that the silicone rubber emulsion is obtained.

[0069] In the aforementioned silicone rubber emulsion preparation method, an emulsifier and amphiphilic SiO2 colloid are used to synergistically emulsify the silicone rubber. The amphiphilic SiO2 nanoparticles, modified with amphiphilic molecules, possess both hydrophilic and lipophilic groups on their surfaces. These particles disperse at the silicone rubber-water interface, reducing interfacial energy and stabilizing the system. The SiO2 nanoparticles form a rigid shell at the interface, preventing the aggregation of dispersed phase droplets and resulting phase separation and demulsification. This emulsion is a typical Pickering emulsion, characterized by excellent stability and minimal emulsifier usage.

[0070] The aforementioned silicone rubber emulsion preparation method utilizes a phase inversion emulsification process to reduce equipment dependence. This method first adds an emulsifier and amphiphilic SiO2 colloid to the silicone rubber. Low-speed agitation and dispersion are then performed to form a water-in-oil emulsion. A large amount of deionized water is then added and dispersed at high speed for a short period of time. The phase inversion mechanism transforms the water-in-oil emulsion into an oil-in-water emulsion.

[0071] The present invention also provides a water-based coating comprising the silicone rubber emulsion, a curing agent, a stabilizer and a functional filler, wherein the mass percentage content of the silicone rubber emulsion is 60-80%.

[0072] The present invention also provides a water-based coating, which is prepared using the above-mentioned water-based paint, including: preparing the water-based paint on the surface of the product by spraying, brushing or scraping, and curing.

[0073] Example 1

[0074] 300g of 99% pure silicon powder and 700g of deionized water were weighed and placed in a flask with magnetic stirring. The mixture was heated to 80°C and held for 10 minutes. 2g of solid NaOH was then added and the mixture was kept warm for 8 hours to obtain an alkaline SiO2 colloid with a solid content of 30%.

[0075] 1000g of SiO2 colloid was added to a 2000ml flask equipped with a reflux condenser. The mixture was heated to 60°C in an oil bath and slowly stirred with magnetic beads. 15g of the silane coupling agent, γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH560), was weighed and added dropwise at a rate of 1g / min. The mixture was then stirred at 60°C for 2 hours to obtain the silane coupling agent-modified SiO2 colloid.

[0076] 50g of methyl silicone rubber (produced by Zhonglan Chenguang Chemical Research and Design Institute Co., Ltd.) and 2.5g of Triton X-100 were added to a 500ml beaker and dispersed at room temperature for 10min using a high-speed disperser at a speed of 500r / min. 15g of SiO2 colloid modified by KH560 was weighed and added dropwise to the mixture of methyl silicone rubber and Triton X-100 at a speed of 0.1g / s at a speed of 1000r / min to mix them thoroughly until a white paste was formed. The speed was increased to 2000r / min, 50g of deionized water was weighed, and quickly added to the beaker. After high-speed dispersion for 3min, the speed was reduced to 200r / min and dispersed for 30min until a white silicone rubber emulsion was formed with a total mass of 117.5g. As shown in Figure 1, an electron microscopic image of the methyl silicone rubber emulsion prepared in Example 1 of the present invention is shown;

[0077] The prepared methyl silicone rubber emulsion was centrifuged at a speed of 3000 r / min for 30 min, and the emulsion showed no phase separation or demulsification.

[0078] The freeze-thaw stability of the emulsion was tested according to GB / T 11175. The prepared silicone rubber emulsion was frozen at -10°C and then placed in a 25°C environment until it thawed. After repeating the cycle five times, the emulsion showed no phase separation or demulsification.

[0079] The prepared methyl silicone rubber emulsion was poured into a sealed reagent bottle. After 30 days of standing, the emulsion remained in its original state without phase separation or demulsification.

[0080] 4g of tetrapropyl orthosilicate and 0.3g of dibutyltin dioctanoate were added to the above-mentioned methyl silicone rubber emulsion, stirred evenly, and poured into a demolding test plate. After 4 hours, the methyl silicone rubber gradually solidified and dried to the surface. After 72 hours, it was completely dehydrated to form a methyl silicone rubber elastomer with a smooth surface and no cracks. Figure 2 shows the morphology of the film after curing the methyl silicone rubber emulsion prepared in Example 1 of the present invention. Performance tests were conducted, and the results are shown in Table 1. Tensile strength and elongation at break were measured in accordance with GB / T 528, shear strength was measured by breaking the bonded aluminum sheets, and unbending strength was measured in accordance with GB / T 5210.

[0081] Table 1 Summary of mechanical properties of water-based silicone rubber

[0082] Example 2

[0083] The preparation of SiO2 colloid and the modification of amphiphilic molecules are the same as those in Example 1.

[0084] Add 100g of methylphenyl silicone rubber (produced by Zhonglan Chenguang Chemical Research and Design Institute Co., Ltd.) and 7g of Triton X-100 to a 1000ml beaker and disperse at 500r / min for 10 minutes at room temperature using a high-speed disperser. Weigh 30g of silane coupling agent-modified SiO2 colloid and increase the speed to 1000r / min. At this speed, add the silane coupling agent-modified SiO2 colloid dropwise to the silicone rubber and Triton X-100 mixture at a rate of 0.1g / s, mixing thoroughly until a white paste forms. Increase the speed to 2000r / min, weigh 100g of deionized water, and quickly add it to the beaker. After high-speed dispersion for 3 minutes, reduce the speed to 200r / min and disperse for 30 minutes until a white methylphenyl silicone rubber emulsion forms.

[0085] The prepared methylphenyl silicone rubber emulsion was centrifuged at a speed of 3000 r / min for 30 min, and the emulsion showed no phase separation or demulsification.

[0086] The freeze-thaw stability of the emulsion was tested according to GB / T 11175. The prepared silicone rubber emulsion was frozen at -10°C and then placed in a 25°C environment until it thawed. After repeating the cycle five times, the emulsion showed no phase separation or demulsification.

[0087] The prepared silicone rubber emulsion was poured into a sealed reagent bottle. After 30 days of standing, the emulsion remained in its original state without phase separation or demulsification.

[0088] Example 3

[0089] The preparation of SiO2 colloid and the modification of amphiphilic molecules are the same as those in Example 1.

[0090] Add 200g of methylphenyl silicone rubber (produced by Zhonglan Chenguang Chemical Research and Design Institute Co., Ltd.) and 20g of Triton X-100 to a 1000ml beaker and disperse them at 500r / min at room temperature for 10 minutes using a high-speed disperser. Weigh 80g of silane coupling agent-modified SiO2 colloid and increase the speed to 1000r / min. At this speed, add the silane coupling agent-modified SiO2 colloid dropwise to the silicone rubber and Triton X-100 mixture at a rate of 0.15g / s and mix thoroughly until a white paste forms. Increase the speed to 2000r / min, weigh 240g of deionized water, and quickly add it to the beaker. After high-speed dispersion for 3 minutes, reduce the speed to 200r / min and disperse for 30 minutes until a white methylphenyl silicone rubber emulsion forms.

[0091] The prepared methylphenyl silicone rubber emulsion was centrifuged at a speed of 3000 r / min for 30 min, and the emulsion showed no phase separation or demulsification.

[0092] The freeze-thaw stability of the emulsion was tested according to GB / T 11175. The prepared silicone rubber emulsion was frozen at -10°C and then placed in a 25°C environment until it thawed. After repeating the cycle five times, the emulsion showed no phase separation or demulsification.

[0093] The prepared silicone rubber emulsion was poured into a sealed reagent bottle. After 30 days of standing, the emulsion showed no phase separation or demulsification, and a small amount of white precipitate was present at the bottom of the bottle.

[0094] Comparative Example 1

[0095] 100g of methylphenyl silicone rubber (produced by Zhonglan Chenguang Chemical Research and Design Institute Co., Ltd.) and 8g of Triton X-100 were dispersed in a high-speed disperser at 500 r / min for 10 minutes at room temperature. 30g of deionized water was weighed and the speed was increased to 1000 r / min. At this speed, deionized water was dropwise added to the silicone rubber and Triton X-100 mixture at a rate of 0.1g / s to mix thoroughly. The speed was increased to 2000 r / min, and 100g of deionized water was weighed and quickly added to a beaker. After high-speed dispersion for 3 minutes, the speed was reduced to 200 r / min and dispersed for 30 minutes. The mixture quickly separated and failed to form an emulsion.

[0096] Comparative Example 2

[0097] The preparation method of SiO2 colloid is the same as that of Example 1. 100g of methylphenyl silicone rubber (produced by Zhonglan Chenguang Chemical Research and Design Institute Co., Ltd.) and 7g of Triton X-100 were added to a 1000ml beaker and dispersed at room temperature for 10min using a high-speed disperser at 500r / min. 30g of unmodified SiO2 colloid was weighed and the speed was increased to 1000r / min. At this speed, the SiO2 colloid was dropped into the mixture of silicone rubber and Triton X-100 at a rate of 0.1g / s and mixed thoroughly until a white paste was formed. The speed was increased to 2000r / min, 100g of deionized water was weighed and quickly added to the beaker. After high-speed dispersion for 3min, the speed was reduced to 200r / min and dispersed for 30min until a white methylphenyl silicone rubber emulsion was formed. The emulsion showed phase separation and demulsification after standing for 24h.

[0098] In Comparative Example 1, no amphiphilic molecules were used to modify the surface of SiO2 colloid, resulting in a lower stability of the prepared emulsion. This shows that amphiphilic molecule modification plays a decisive role in improving the stability of the emulsion.

[0099] Comparative Example 3

[0100] The preparation of SiO2 colloid and the modification method of amphiphilic molecules are the same as those in Example 1.

[0101] 100g of methyl silicone rubber (produced by Zhonglan Chenguang Chemical Research and Design Institute Co., Ltd.), 5g of Triton X-100, 30g of amphiphilic molecule-modified SiO2 colloid and 100g of deionized water were added to a 1000ml beaker. After high-speed dispersion at 2000r / min for 30min, the mixture quickly separated and failed to form an emulsion.

[0102] Comparative Example 2 did not adopt the phase inversion method to prepare the emulsion, and the emulsification of the methyl silicone rubber could not be achieved, which proved that the phase inversion emulsification method has an irreplaceable role in the preparation of the emulsion.

[0103] The above description is only the best specific implementation method of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or replacements that can be easily thought of by any technician familiar with this technical field within the technical scope disclosed by the present invention should be covered by the scope of protection of the present invention.

[0104] The contents not described in detail in the specification of the present invention belong to the common knowledge of professionals in this field.

Claims

1. A silicone rubber emulsion, characterized in that: Contains the following components by mass:

2. The silicone rubber emulsion according to claim 1, characterized in that The structural formula of the silicone rubber is as follows: Wherein, R1 and R2 are any one of methyl, phenyl or oxyethyl.

3. The silicone rubber emulsion according to claim 2, characterized in that The R1 and R2 are both methyl or phenyl.

4. The silicone rubber emulsion according to claim 1, characterized in that The preparation method of the SiO2 colloid comprises: 20-40 parts by mass of silicon powder and 60-80 parts by mass of deionized water are mixed and heated to 70-90° C., 0.1-0.2 parts by mass of NaOH are added thereto and the mixture is kept warm for more than 8 hours.

5. The silicone rubber emulsion according to claim 1, characterized in that The amphiphilic molecule is a silane coupling agent, and the structural formula is: Wherein, R1 is methyl or ethyl, and R2 is amino, epoxy or methacryloxy.

6. The silicone rubber emulsion according to any one of claims 1 to 5, characterized in that: The preparation method of the amphiphilic molecule-modified SiO2 colloid comprises: After 100 parts by mass of SiO2 colloid is stirred and heated to 55-65°C, 1.5-3 parts by mass of amphiphilic molecules are added dropwise at a rate of 0.5-1.5 g / min, and the mixture is stirred and kept warm for more than 2 hours to obtain SiO2 colloid modified with amphiphilic molecules.

7. The silicone rubber emulsion according to any one of claims 1 to 5, characterized in that The emulsifier is any one of polyethylene glycol p-isooctylphenyl ether, polyoxyethylene sorbitan monostearate, sodium dodecylbenzene sulfonate or sorbitan fatty acid ester.

8. The silicone rubber emulsion according to any one of claims 1 to 5, characterized in that: The water is deionized water.

9. The method for preparing the silicone rubber emulsion according to any one of claims 1 to 8, characterized in that: Including pre-emulsification and phase inversion emulsification of silicone rubber.

10. A method for preparing a silicone rubber emulsion, characterized in that: include: At a speed of 500 to 1000 r / min, 100 parts by mass of silicone rubber and 5 to 10 parts by mass of emulsifier are uniformly mixed, and then 20 to 40 parts by mass of SiO2 colloid modified by amphiphilic molecules are dropwise added at a rate of 0.05 to 0.15 g / s to obtain a pre-emulsified cream with an oil-in-water structure; The rotation speed is increased to not less than 2000 r / min and not less than 100 parts by weight of deionized water is added to the pre-emulsified water-in-oil structure cream to obtain an oil-in-water structure emulsion through phase inversion; The silicone rubber emulsion is obtained after stirring.

11. The method for preparing the silicone rubber emulsion according to claim 10, characterized in that: The silicone rubber emulsion is obtained by stirring at 200-1000 r / min for 30 minutes or more.

12. The method for preparing the silicone rubber emulsion according to claim 10, characterized in that: The structural formula of the silicone rubber is as follows: Wherein, R1 and R2 are any one of methyl, phenyl or oxyethyl.

13. The method for preparing the silicone rubber emulsion according to claim 10, characterized in that: The amphiphilic molecule is a silane coupling agent, and the structural formula is: Wherein, R1 is methyl or ethyl, and R2 is amino, epoxy or methacryloxy.

14. The method for preparing the silicone rubber emulsion according to claim 10 or 13, characterized in that: The preparation method of the amphiphilic molecule-modified SiO2 colloid comprises: 20-40 parts by mass of silicon powder and 60-80 parts by mass of deionized water are mixed and heated to 70-90° C., 0.1-0.2 parts by mass of NaOH are added thereto and the mixture is kept warm for 8 hours or more to obtain SiO2 colloid; After 100 parts by mass of SiO2 colloid is stirred and heated to 55-65°C, 1.5-3 parts by mass of amphiphilic molecules are added dropwise at a rate of 0.5-1.5 g / min, and the mixture is stirred and kept warm for 2 hours or more to obtain SiO2 colloid modified with amphiphilic molecules.

15. The method for preparing the silicone rubber emulsion according to claim 10, characterized in that: The emulsifier is any one of polyethylene glycol p-isooctylphenyl ether, polyoxyethylene sorbitan monostearate, sodium dodecylbenzene sulfonate or sorbitan fatty acid ester.

16. A silicone rubber emulsion, characterized in that: The preparation method according to any one of claims 10 to 15 is used to obtain the 17. A water-based paint, characterized in that: The silicone rubber emulsion comprises the silicone rubber emulsion according to any one of claims 1 to 8.

18. The water-based paint according to claim 17, characterized in that It also comprises a curing agent, a stabilizer and a functional filler, wherein the mass percentage content of the silicone rubber emulsion is 60-80%.

19. A water-based coating, characterized in that The water-based coating according to claim 17 or 18 is prepared, comprising: preparing the water-based coating on the product surface by spraying, brushing or scraping, and curing.

Citation Information

Patent Citations

  • Silicone rubber composition

    CN104497573A

  • Botton-surface combined type antifouling and antiseptic nanometer polysiloxanes coating and preparation method thereof

    CN106479354A

  • Stable polyacrylate emulsion based on amphiphilic Janus SiO2 nanoparticles and preparation method of stable polyacrylate emulsion

    CN112011009A

  • Silicone rubber emulsion, preparation method and water-based paint

    CN116515297A

  • Silica-coated silicone rubber particle and cosmetic

    US20190038520A1

Cited By

  • High-stability microcapsule and emulsification process thereof

    CN121571070A