Method for co-producing artificial rutile and iron phosphate

By co-producing artificial rutile and iron phosphate, the titanium-rich material and ferrous sulfate solution are separated by the reaction of sulfuric acid solution and ilmenite, and used to synthesize iron phosphate, solving the problem of utilization of iron-containing by-products in rutile production. problem, achieving the simultaneous comprehensive utilization of titanium and iron, improving production efficiency and economic benefits.

WO2024221584A1PCT designated stage expired Publication Date: 2024-10-31GUANGDONG UBRIDGE NEW MATERIAL TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/102942
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2023-06-27
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing process flow cannot effectively utilize the iron-containing by-products generated during the production of rutile, which limits the comprehensive utilization and value improvement of ilmenite.

Method used

A method for jointly producing artificial rutile and iron phosphate is proposed. By reacting sulfuric acid solution with ilmenite, titanium-rich material and ferrous sulfate solution are separated, and residual ferrous sulfate is removed to obtain artificial rutile, and ferrous sulfate is used. The iron solution reacts with the phosphate salt to synthesize iron phosphate, achieving simultaneous high-quality comprehensive utilization of titanium and iron.

Benefits of technology

It reduces the production process, improves production efficiency, saves costs, avoids the disadvantages of the rust method, reduces the amount of acid used, solves environmental problems, increases the economic value of iron-containing by-products, and improves the overall economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023102942_31102024_PF_FP_ABST
    Figure CN2023102942_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A method for co-producing artificial rutile and iron phosphate, belonging to the technical field of mineral processing. The method comprises the following steps: reacting a sulfuric acid solution with a reduced ilmenite, controlling the reaction conditions so as to dissolve iron without dissolving titanium, and obtaining a solid-liquid mixture; performing solid-liquid separation on the solid-liquid mixture to obtain a titanium-rich material and a ferrous sulfate solution; washing and drying the titanium-rich material to obtain artificial rutile; and reacting the ferrous sulfate solution with phosphorus salt to obtain iron phosphate. The iron removal process in the artificial rutile production process and the iron dissolution and iron salt purification processes in the iron phosphate production process are combined into one, thereby achieving synchronous high-quality comprehensive utilization of the primary components of ilmenite, namely titanium and iron, reducing the production process, improving production efficiency, saving production costs, avoiding the disadvantages of corrosion-method production, reducing the amount of acid used, solving the environmental protection problems brought about by traditional acid leaching methods, increasing the economic value of an iron-containing byproduct, and thus increasing the overall economic benefits of the production process.
Need to check novelty before this filing date? Find Prior Art

Description

A method for co-producing artificial rutile and iron phosphate

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 25, 2023, with application number 202310460215.0 and titled “Method for the joint production of artificial rutile and iron phosphate”, parts of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of mineral processing technology, and in particular to a method for co-producing artificial rutile and iron phosphate. Background Art

[0003] Rutile is a high-purity titanium dioxide with excellent properties such as high weather resistance, high strength, and low specific gravity. It is widely used in military aviation, aerospace, navigation, machinery, chemical industry, seawater desalination and other fields.

[0004] The production process of rutile will generate a large number of iron-containing by-products, but the current process flow cannot effectively utilize these iron-containing by-products, thus hindering the comprehensive utilization and value enhancement of ilmenite, making it difficult to improve the efficiency of titanium ore processing companies. Technical issues

[0005] The current process cannot effectively utilize the iron-containing by-products generated during rutile production. Technical Solutions

[0006] The main purpose of this application is to propose a method for the co-production of artificial rutile and iron phosphate, aiming to solve the technical problem that the current process cannot effectively utilize the iron-containing by-products generated during the rutile production process.

[0007] To achieve the above objectives, the present application proposes a method for co-producing artificial rutile and iron phosphate, the method comprising the following steps:

[0008] reacting the ilmenite with a sulfuric acid solution to obtain a solid-liquid mixture;

[0009] performing solid-liquid separation on the solid-liquid mixture to obtain a titanium-rich material and a ferrous sulfate solution;

[0010] removing residual ferrous sulfate from the titanium-rich material to obtain artificial rutile;

[0011] Phosphorus salt is reacted with the ferrous sulfate solution to obtain ferric phosphate.

[0012] Furthermore, the step of reacting the ilmenite with the sulfuric acid solution comprises:

[0013] performing a reduction reaction on the ilmenite raw material to obtain reduced ilmenite;

[0014] The sulfuric acid solution is used to react with the reduced ilmenite.

[0015] Furthermore, the step of subjecting the ilmenite raw material to a reduction reaction to obtain reduced ilmenite comprises:

[0016] Using granular coal and the ilmenite raw material to carry out a reduction reaction at a temperature of 1030-1100° C. to obtain a first reduction product;

[0017] Cooling the first reduction product in a closed environment to obtain a second reduction product;

[0018] The second reduction product is subjected to magnetic separation and carbon removal operation to obtain the reduced ilmenite.

[0019] Furthermore, the step of reacting the reduced ilmenite with the sulfuric acid solution comprises:

[0020] Adding a preset ratio of dilute sulfuric acid and the reduced ilmenite into a reaction container;

[0021] measuring the pH value and bubble generation of the solution in the reaction container, and adding concentrated sulfuric acid dropwise into the reaction container according to the real-time pH value and the real-time bubble generation;

[0022] The solution in the reaction container is stirred to allow the solution in the reaction container to fully react.

[0023] Furthermore, the step of performing solid-liquid separation on the solid-liquid mixture to obtain a titanium-rich material and a ferrous sulfate solution comprises:

[0024] The solid-liquid mixture is put into a belt filter for filtering to separate the titanium-rich material and the ferrous sulfate solution.

[0025] Furthermore, the step of removing the residual ferrous sulfate in the titanium-rich material to obtain artificial rutile comprises:

[0026] injecting pure water into the titanium-rich material to wash the titanium-rich material;

[0027] Dehydrating the washed titanium-rich material;

[0028] The dehydrated titanium-rich material is dried or roasted to obtain the artificial rutile.

[0029] Furthermore, after the step of dehydrating the washed titanium-rich material, the following steps are included:

[0030] Repeating the washing operation on the titanium-rich material using the washing water obtained from the dehydration operation to obtain concentrated washing water;

[0031] The step of reacting the sulfuric acid solution with ilmenite to obtain a solid-liquid mixture comprises:

[0032] The concentrated wash water, the sulfuric acid solution and the ilmenite are mixed to obtain the solid-liquid mixture through reaction.

[0033] Furthermore, the step of reacting the phosphate salt with the ferrous sulfate solution to obtain ferric phosphate comprises:

[0034] injecting hydrogen peroxide, ammonia water and the phosphate salt into the ferrous sulfate solution to obtain an oxidation product through a synthesis reaction and an oxidation reaction;

[0035] performing a filter press operation on the oxidation product to obtain a filter press solid phase;

[0036] performing a rinsing operation on the filter press solid phase to obtain a rinsed solid phase;

[0037] calcining and drying the rinsed solid phase to obtain a dry product;

[0038] The dried product is subjected to an iron removal operation to obtain the ferric phosphate.

[0039] Furthermore, after the step of performing filter press operation on the oxidation product, the method further comprises:

[0040] performing a water treatment operation on the filter press water obtained by the filter press operation to obtain ammonium sulfate, phosphorus-containing concentrated solution and pure water;

[0041] The step of injecting hydrogen peroxide, ammonia water and the phosphate salt into the ferrous sulfate solution comprises:

[0042] injecting the phosphorus-containing concentrated solution, the hydrogen peroxide solution, the ammonia solution and the phosphate salt into the ferrous sulfate solution;

[0043] The filter press solid phase is rinsed using pure water obtained by water treatment of the filter press water.

[0044] Furthermore, after the step of rinsing the filter press solid phase, the method further comprises:

[0045] performing a water treatment operation on the rinsing water obtained by the rinsing operation to obtain ammonium sulfate, a phosphorus-containing concentrated solution and pure water;

[0046] The step of injecting hydrogen peroxide, ammonia water and the phosphate salt into the ferrous sulfate solution comprises:

[0047] injecting the phosphorus-containing concentrated solution, the hydrogen peroxide solution, the ammonia solution and the phosphate salt into the ferrous sulfate solution;

[0048] The step of rinsing the filter press solid phase comprises:

[0049] The filter press solid phase is rinsed using pure water obtained by treating the rinsing water. Beneficial effects

[0050] The method for co-producing artificial rutile and iron phosphate proposed in the present application combines the iron removal process in the artificial rutile production process and the iron dissolution and iron salt purification process in the iron phosphate production process into one, thereby realizing the simultaneous high-quality comprehensive utilization of titanium and iron, the main components of ilmenite, reducing the production process, improving production efficiency, saving production costs, avoiding the drawbacks of the rusting method, reducing the amount of acid used, and solving the environmental problems caused by the traditional acid leaching method, thereby increasing the economic value of the iron-containing by-products and improving the overall economic benefits of the production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] FIG1 is a schematic diagram of the operating steps of an embodiment of a method for co-producing artificial rutile and iron phosphate according to the present application;

[0052] FIG2 is a schematic diagram of a process flow of an embodiment of a method for co-producing artificial rutile and iron phosphate according to the present application.

[0053] Implementation Methods of the Application

[0054] After conducting market research, the applicant's technical personnel discovered that with the rapid development of electric vehicles and new energy storage batteries, their demand continues to rise, and lithium iron phosphate batteries have gradually become one of the mainstream lithium battery solutions. Among them, the production process of iron phosphate is a key link in the production process of lithium iron phosphate batteries. However, the current iron phosphate production process generally suffers from problems such as insufficient raw material sources, difficult quality control, and high environmental costs.

[0055] Based on the above findings, the technical personnel of the present application have proposed a method for the co-production of artificial rutile and iron phosphate, so that the iron-containing by-products generated in the rutile production process can be used for the preparation of iron phosphate, and the process flow has been optimized and adjusted accordingly, aiming to solve the problems existing in the current iron phosphate production process, realize the synchronous and high-quality comprehensive utilization of titanium and iron in ilmenite, improve the comprehensive benefits of titanium ore processing and reduce the environmental pollution caused by the production process.

[0056] Referring to Figures 1 and 2, the method for co-producing artificial rutile and iron phosphate includes the following steps:

[0057] S1, reacting ilmenite with a sulfuric acid solution to obtain a solid-liquid mixture;

[0058] S2, performing solid-liquid separation on the solid-liquid mixture to obtain a titanium-rich material and a ferrous sulfate solution;

[0059] S3, removing the residual ferrous sulfate in the titanium-rich material to obtain artificial rutile;

[0060] S4, reacting the phosphate salt with the ferrous sulfate solution to obtain ferric phosphate.

[0061] Optionally, referring to FIG1 and FIG2 , step S1 includes:

[0062] S11, performing a reduction reaction on the ilmenite raw material to obtain reduced ilmenite;

[0063] S12, reacting the reduced ilmenite with a sulfuric acid solution.

[0064] Optionally, referring to FIG. 1 and FIG. 2 , step S11 includes:

[0065] S111, using granular coal and ilmenite raw material to carry out reduction reaction at a temperature of 1030-1100°C to obtain a first reduction product; in this step, the granular coal serves as a reducing agent and fuel; when the temperature is greater than 1030°C, solid carbon generates carbon monoxide, which in the first stage converts Fe 3+ Reduction to Fe 2+ In the second stage, Fe 2+ It is reduced to Fe, accompanied by the reduction of some TiO2. The reduction process needs to be sealed to prevent air from entering and causing oxidation of metallic iron. This reduction process can reduce 93% to 95% of the iron to metallic iron.

[0066] Among them, the ilmenite raw material can be pre-oxidized and roasted before the reduction reaction to reduce the sintering of the mineral during the reduction process and activate the iron in the ilmenite, thereby increasing the reduction rate;

[0067] S112, cooling the first reduction product in a closed environment to obtain a second reduction product;

[0068] S113, performing magnetic separation and carbon removal operation on the second reduction product to obtain reduced ilmenite.

[0069] Specifically, the high-temperature ilmenite after the above-mentioned reduction reaction needs to be rapidly cooled to reduce its temperature to 70~80°C, so that subsequent screening and magnetic separation decoking operations can be carried out to separate the fly ash and residual coke to obtain reduced ilmenite.

[0070] Optionally, referring to FIG1 and FIG2 , step S12 includes:

[0071] S121, adding a preset ratio of dilute sulfuric acid and reduced ilmenite into a reaction container;

[0072] S122, measuring the pH value (normally the pH value is about 1) and bubble generation of the solution in the reaction container, and adding concentrated sulfuric acid dropwise into the reaction container based on the real-time pH value and the real-time bubble generation;

[0073] The pH value can be manually measured by an operator, and the bubble generation can be determined by the operator through observation. The pH value and bubble generation can reflect the degree of reaction of the solution in the reaction container. The operator slowly adds concentrated sulfuric acid according to the real-time reaction of the solution, which can more accurately control the reaction process and ensure that the sulfuric acid solution can fully react with the ilmenite within the preset reaction time. The reaction container can adopt a reactor, which is used to provide a good reaction environment and is more convenient for the operator to measure the pH value and observe the real-time generation of bubbles.

[0074] S123, stirring the solution in the reaction container to allow the solution in the reaction container to fully react.

[0075] Optionally, referring to FIG1 and FIG2 , step S2 includes:

[0076] S21, putting the solid-liquid mixture into a belt filter for filtering to separate the titanium-rich material and the ferrous sulfate solution.

[0077] After the above-mentioned reaction process between the reduced ilmenite and the sulfuric acid solution (acid leaching process), the metallic iron in the reduced ilmenite will be fully dissolved by the sulfuric acid solution. The specific reaction formula is as follows:

[0078] Fe+H2SO4=FeSO4+H2↑

[0079] According to the principle of mineralization, the content of nickel, cobalt, copper, zinc, chromium, etc. in ilmenite is relatively low. By precisely controlling the acidity by adding concentrated sulfuric acid, metals that are less active than iron can basically not react during the above reaction process, but remain in the ore body. That is, by controlling the reaction conditions, iron is soluble but titanium is insoluble. The ferrous sulfate solution obtained in this way has excellent purity, while the solid phase mainly composed of TiO2 (i.e. titanium-rich material) remains in the ore body.

[0080] The composition of the ferrous sulfate solution obtained by the process method of the above embodiment is shown in the following table:

[0081] Sample No. Unit Ferric ion pHAlCaCdCoCr1 (mg / L) 02.99530.591.2302.5302 (mg / L) 02.80722.3564.210.040.960.44Sample No. Unit CuKMgMnNaNi 1 (mg / L) 0.086.647.7553.1413.050.64 2 (mg / L) 0.138.086.1435.799.310.35Sample No. Unit PbTiZnFeAS Chloride ion 1 (mg / L) 2.390.021.7558526.140.0490 2 (mg / L) 1.699.291.2860941.1200

[0082] Based on the above process flow, the iron removal process in the artificial rutile production process and the iron dissolution and iron salt purification process in the ferric phosphate production process are combined into one, thereby reducing two production processes.

[0083] Optionally, referring to FIG1 and FIG2 , step S3 includes:

[0084] S31, injecting pure water into the titanium-rich material to wash the titanium-rich material;

[0085] S32, dehydrating the washed titanium-rich material;

[0086] S33, drying or roasting the dehydrated titanium-rich material to obtain artificial rutile.

[0087] Optionally, referring to FIG1 and FIG2 , after step S32, the following steps are included:

[0088] S321, repeatedly washing the titanium-rich material with the washing water obtained from the dehydration operation to obtain concentrated washing water;

[0089] Step S1 includes:

[0090] S01, mixing concentrated washing water, sulfuric acid solution and ilmenite to obtain a solid-liquid mixture through reaction.

[0091] After the titanium-rich material undergoes the above-mentioned post-treatment processes such as washing, dehydration, and drying, the residual ferrous sulfate can be removed to obtain artificial rutile with a TiO2 content of more than 89%. Among them, the washing water obtained after washing and dehydrating the titanium-rich material can be used to repeatedly wash the titanium-rich material again through countercurrent; when the titanium-rich material has undergone multiple washing operations in the above manner, the titanium-rich material is dehydrated to obtain concentrated washing water rich in substances such as ferrous sulfate. The concentrated washing water can be returned to the acid leaching process in the above-mentioned step S1 for re-liquid preparation to be used in the reaction process of reducing ilmenite and sulfuric acid solution, thereby realizing the comprehensive recycling and utilization of water and ferrous sulfate, achieving the effect of energy saving and environmental protection.

[0092] Optionally, referring to FIG1 and FIG2 , step S4 includes:

[0093] S41, injecting hydrogen peroxide, ammonia water, and phosphate salt into the ferrous sulfate solution to obtain an oxidation product through a synthesis reaction and an oxidation reaction;

[0094] S42, performing a filter press operation on the oxidation product to obtain a filter press solid phase;

[0095] S43, performing a rinsing operation on the filter press solid phase to obtain a rinsed solid phase;

[0096] S44, performing calcination and drying operations on the rinsed solid phase to obtain a dry product;

[0097] S45, performing an iron removal operation on the dried product to obtain iron phosphate.

[0098] Optionally, referring to FIG1 and FIG2 , after step S42, the following steps are included:

[0099] S421, performing a water treatment operation on the filter press water obtained by the filter press operation to obtain ammonium sulfate, a phosphorus-containing concentrated solution, and pure water;

[0100] Step S41 includes:

[0101] S411, injecting a phosphorus concentrate, hydrogen peroxide, ammonia water and a phosphate salt into the ferrous sulfate solution;

[0102] Step S43 includes:

[0103] S431, using the pure water obtained after the filter press water body is subjected to water treatment operation to rinse the filter press solid phase.

[0104] Optionally, referring to FIG1 and FIG2 , after step S43, the following steps are included:

[0105] S432, performing a water treatment operation on the rinsing water obtained from the rinsing operation to obtain ammonium sulfate, a phosphorus-containing concentrated solution, and pure water;

[0106] Step S41 includes:

[0107] S412, injecting a phosphorus concentrate, hydrogen peroxide, ammonia water and a phosphate salt into the ferrous sulfate solution;

[0108] Step S43 includes:

[0109] S433, using the pure water obtained by water treatment operation on the rinsing water body to rinse the filter press solid phase.

[0110] The ferrous sulfate obtained after the solid-liquid separation operation of the belt filter has a high purity and can meet the production requirements of ferric phosphate. After the ferrous sulfate undergoes the above-mentioned post-treatment steps of synthesis, oxidation, filter pressing, washing, dehydration, drying, etc., impurities can be removed to obtain the ferric phosphate product.

[0111] The filtration water (i.e., filtrate) obtained after the oxidation product is subjected to a filter press operation contains substances such as phosphates and ammonium sulfate separated from the solid phase. The rinse water obtained after the filter press solid phase is subjected to a rinsing operation also contains substances such as phosphates and ammonium sulfate separated from the solid phase. After water treatment, the filter press water and the rinse water are separated to produce a phosphorus-containing concentrate, pure water, and ammonium sulfate. The phosphorus-containing concentrate is returned to step S41 for re-preparation to be used in the synthesis and oxidation steps of the ferrous sulfate solution; the pure water is used to rinse the filter press solid phase; and the ammonium sulfate is collected and can be used for subsequent processing and sale. This achieves the comprehensive recycling and reuse of the phosphorus-containing concentrate, pure water, and ammonium sulfate, achieving the beneficial effects of energy conservation, environmental protection, and zero emissions.

[0112] The present application combines the iron removal process in the artificial rutile production process and the iron dissolution and iron salt purification process in the iron phosphate production process into one, thereby realizing the synchronous high-quality comprehensive utilization of titanium and iron, the main components of ilmenite, reducing the production process, improving production efficiency, saving production costs, avoiding the drawbacks of the rusting method, reducing the amount of acid used, solving the environmental problems caused by the traditional acid leaching method, and increasing the economic value of iron-containing by-products, thereby improving the overall economic benefits of the production process.

[0113] Furthermore, the method for co-producing artificial rutile and iron phosphate provided in the embodiments of the present application also has the following beneficial effects:

[0114] First, leveraging the principle of mineralization symbiosis and the low content of nickel, cobalt, copper, zinc, and chromium in ilmenite, and precisely controlling the acidity, metals less reactive than iron essentially do not react with the sulfuric acid solution, but remain within the ore body. This allows the iron to dissolve while the titanium does not, thus achieving an extremely pure ferrous sulfate solution that is conducive to the subsequent production of high-quality iron phosphate.

[0115] Second, by utilizing the characteristic that the iron in the reduced ilmenite is embedded in the ore body in molecular form, the stability of the ferrous sulfate formation process is effectively guaranteed, and a ferrous sulfate solution with good dispersion can be generated, which is conducive to the subsequent production of high-quality iron phosphate;

[0116] 3. By controlling the stirring speed and adding concentrated sulfuric acid, the friction loss of the ore body is reduced while ensuring the normal progress of the reaction, and the recovery rate of titanium-rich materials is effectively improved;

[0117] 4. No hydrochloric acid is used in any process flow, and the final artificial rutile will not have any chloride ion residue, which is conducive to the application of artificial rutile in the field of welding materials.

[0118] It should be noted that other contents of the method for co-producing artificial rutile and iron phosphate disclosed in this application can be found in the prior art and will not be described in detail here.

[0119] It should be noted that if the embodiments of the present application involve directional indications (such as up, down, left, right, front, back, etc.), such directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0120] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present application, the descriptions of "first", "second", etc. are only for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of such features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme in which A and B are satisfied at the same time. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement it. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0121] Based on the disclosure and teachings of the above description, those skilled in the art to which this application belongs may also make changes and modifications to the above embodiments. Therefore, this application is not limited to the specific embodiments disclosed and described above, and some modifications and changes to this application should also fall within the scope of protection of the claims of this application. In addition, although some specific terms are used in this description, these terms are only for convenience of description and do not constitute any limitation to this application.

Claims

1. A method for co-producing artificial rutile and iron phosphate, It is characterized in that The method for co-producing artificial rutile and iron phosphate comprises the following steps: reacting the ilmenite with a sulfuric acid solution to obtain a solid-liquid mixture; Performing solid-liquid separation on the solid-liquid mixture to obtain a titanium-rich material and a ferrous sulfate solution; removing residual ferrous sulfate in the titanium-rich material to obtain artificial rutile; The ferrous sulfate solution is reacted with a phosphate salt to obtain ferric phosphate.

2. The method for co-producing artificial rutile and iron phosphate according to claim 1, It is characterized in that The step of reacting the ilmenite with the sulfuric acid solution comprises: Performing a reduction reaction on the ilmenite raw material to obtain reduced ilmenite; The sulfuric acid solution is used to react with the reduced ilmenite.

3. The method for co-producing artificial rutile and iron phosphate according to claim 2, It is characterized in that The step of subjecting the ilmenite raw material to a reduction reaction to obtain reduced ilmenite comprises: Using the granular coal and the ilmenite raw material to carry out a reduction reaction at a temperature of 1030-1100° C. to obtain a first reduction product; Cooling the first reduction product in a closed environment to obtain a second reduction product; The second reduction product is subjected to magnetic separation and carbon removal operation to obtain the reduced ilmenite.

4. The method for co-producing artificial rutile and iron phosphate according to claim 2, It is characterized in that The step of reacting the reduced ilmenite with the sulfuric acid solution comprises: Adding a preset ratio of dilute sulfuric acid and the reduced ilmenite into a reaction container; The pH value and bubble generation of the solution in the reaction container are measured, and concentrated sulfuric acid is added dropwise into the reaction container according to the real-time pH value and the real-time bubble generation; The solution in the reaction container is stirred to allow the solution in the reaction container to react fully.

5. The method for co-producing artificial rutile and iron phosphate according to claim 1, It is characterized in that The step of subjecting the solid-liquid mixture to solid-liquid separation to obtain a titanium-rich material and a ferrous sulfate solution comprises: The solid-liquid mixture is put into a belt filter for filtering to separate the titanium-rich material and the ferrous sulfate solution.

6. The method for co-producing artificial rutile and iron phosphate according to claim 1, It is characterized in that The step of removing residual ferrous sulfate in the titanium-rich material to obtain artificial rutile comprises: injecting pure water into the titanium-rich material to wash the titanium-rich material; Dehydrating the washed titanium-rich material; The dehydrated titanium-rich material is dried or roasted to obtain the artificial rutile.

7. The method for co-producing artificial rutile and iron phosphate according to claim 6, It is characterized in that After the step of dehydrating the washed titanium-rich material, the method further comprises: Repeating the washing operation on the titanium-rich material using the washing water obtained from the dehydration operation to obtain concentrated washing water; The step of reacting sulfuric acid solution with ilmenite to obtain a solid-liquid mixture comprises: The concentrated wash water, the sulfuric acid solution and the ilmenite are mixed to obtain the solid-liquid mixture through reaction.

8. The method for co-producing artificial rutile and iron phosphate according to claim 1, It is characterized in that The step of reacting the phosphate salt with the ferrous sulfate solution to obtain ferric phosphate comprises: injecting hydrogen peroxide, ammonia and the phosphate into the ferrous sulfate solution to obtain an oxidation product through a synthesis reaction and an oxidation reaction; Performing a filter press operation on the oxidation product to obtain a filter press solid phase; Performing a rinsing operation on the filter press solid phase to obtain a rinsed solid phase; calcining and drying the rinsed solid phase to obtain a dry product; The dried product is subjected to an iron removal operation to obtain the ferric phosphate.

9. The method for co-producing artificial rutile and iron phosphate according to claim 8, It is characterized in that After the step of performing filter pressing operation on the oxidation product, the method further comprises: The filter press water obtained by the filter press operation is subjected to a water treatment operation to obtain ammonium sulfate, a phosphorus-containing concentrated solution and pure water; The step of injecting hydrogen peroxide, ammonia water and the phosphate salt into the ferrous sulfate solution comprises: injecting the phosphorus-containing concentrated solution, the hydrogen peroxide solution, the ammonia water and the phosphate salt into the ferrous sulfate solution; The step of rinsing the filter press solid phase comprises: The filter press solid phase is rinsed using pure water obtained by water treatment of the filter press water.

10. The method for co-producing artificial rutile and iron phosphate according to claim 8, It is characterized in that After the step of rinsing the filter press solid phase, the method further comprises: Performing water treatment on the rinsing water obtained by the rinsing operation to obtain ammonium sulfate, phosphorus-containing concentrated solution and pure water; The step of injecting hydrogen peroxide, ammonia water and the phosphate salt into the ferrous sulfate solution comprises: injecting the phosphorus-containing concentrated solution, the hydrogen peroxide solution, the ammonia water and the phosphate salt into the ferrous sulfate solution; The step of rinsing the filter press solid phase comprises: The filter press solid phase is rinsed using pure water obtained by water treatment of the rinsing water.

Citation Information

Patent Citations

  • Artificial rutile preparation method

    CN104045111A

  • Method for synthesizing iron phosphate from titanium dioxide byproduct ferrous sulfate

    CN110255521A

  • Method for preparing ferric phosphate hydrate from titanium dioxide byproduct ferrous sulfate

    CN111847416A

  • Method for co-producing artificial rutile and polyferric sulfate by using sulfuric acid waste acid

    CN112408472A

  • Artificial rutile production system and titanium dioxide production system

    CN218058485U