Preparation method for Anti-corrosion modified epoxy resin
Through the cross-linking reaction of epoxy resin and organosilane, a polysiloxane covalent coupling layer is formed, which solves the problems of easy degradation of epoxy resin at high temperatures and poor impact resistance, and achieves excellent heat resistance, anti-corrosion and Flame retardant performance, suitable for the temperature resistance and corrosion requirements of petroleum and chemical equipment.
Patent Information
- Application Number
- PCT/CN2023/104113
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-06-29
- Publication Date
- 2024-10-31
AI Technical Summary
Epoxy resin is easily degraded at high temperatures, has poor hydrophobic properties, and has poor impact resistance, which limits its application in advanced materials, and its anti-corrosion properties have not been effectively improved.
By mixing epoxy resin with organosilane, soluble epoxy resin solvent and organotin catalyst for cross-linking reaction, an anti-corrosion modified epoxy resin is formed. The organosilane is hydrolyzed to generate silicone groups to form a network structure and polysiloxane. Alkane covalent coupling layer enhances heat resistance, anti-corrosion and flame retardant properties, and improves dynamic mechanical properties through organotin chain segments.
Significantly improve the heat resistance, anti-corrosion performance, flame retardant performance and high-temperature dynamic mechanical properties of epoxy resin, meet the needs of petroleum and chemical equipment for high-temperature corrosion resistance, and at the same time, construction is convenient and economical.
Smart Images

Figure PCTCN2023104113-FTAPPB-I100001 
Figure PCTCN2023104113-FTAPPB-I100002 
Figure PCTCN2023104113-FTAPPB-I100003
Abstract
Description
A method for preparing anticorrosive modified epoxy resin
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on April 24, 2023, with application number CN202310449537.5 and invention name “A method for preparing anti-corrosion modified epoxy resin”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The invention belongs to the technical field of epoxy resin modification, and particularly relates to a method for preparing an anti-corrosion modified epoxy resin. Background Art
[0003] Epoxy resins are widely used in coatings, adhesives, electronic packaging materials, and composite materials due to their low curing shrinkage, good adhesion, alkali resistance, corrosion resistance, water resistance, excellent electrical insulation, and mechanical properties. However, due to the high surface energy of the hydroxyl groups in the epoxy resin network and the high crosslink density after curing, the material has high internal stress, brittleness, poor impact resistance, easy degradation at high temperatures, and poor hydrophobicity, which limit its application in advanced materials. In recent years, with the rapid development of high-tech industries, the performance requirements for epoxy resins have become increasingly higher. Therefore, the modification of epoxy resins has great research prospects, and modified epoxy resins with excellent comprehensive performance are more popular in the market.
[0004] Chinese Patent CN 113004524A reports a method for preparing an epoxy-organic silicone resin. The method uses a vinyl-containing MT resin and a siloxane ring as raw materials. Under the action of an acidic catalyst, an equilibrium reaction occurs to produce a vinyl-containing MDT resin. This resin is then oxidized with a peroxide to produce an MDT silicone resin containing epoxy groups at its terminal ends. This resin effectively improves the mechanical properties of epoxy cured products while maintaining the good heat and weather resistance of the epoxy cured product. Chinese Patent CN 113789143A reports a room-temperature curable silicone-modified epoxy resin potting compound and its preparation method. The silicone-modified epoxy resin potting compound, produced by blending an oligosiloxane with an organic amine curing agent, exhibits increased adhesive layer flexibility and elongation at break, enhanced aging resistance, and good moisture resistance. However, there are currently few reports on improvements in the anti-corrosion properties of epoxy resins.
[0005] Summary of the Invention
[0006] In view of this, the object of the present invention is to provide a method for preparing an anti-corrosion modified epoxy resin. The anti-corrosion modified epoxy resin prepared by the present invention has excellent heat resistance, anti-corrosion performance, flame retardancy and toughness as well as dynamic mechanical properties at high temperatures.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing an anti-corrosion modified epoxy resin, comprising the following steps:
[0009] The epoxy resin, organic silane, a soluble epoxy resin solvent and an organic tin catalyst are mixed and cross-linked to obtain an anti-corrosion modified epoxy resin.
[0010] Preferably, the epoxy resin includes one or more of halogen-free epoxy resin, E51 epoxy resin and E44 epoxy resin.
[0011] Preferably, the organosilane includes one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, γ-(glycidyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, 1,2-bis(triethoxysilyl)ethane, tetraethoxysilane, methyltrimethoxysilane and vinyltriethoxysilane.
[0012] Preferably, the mass of the organosilane is 12-18% of the mass of the epoxy resin.
[0013] Preferably, the organotin catalyst is butyl stannoic acid and / or dibutyl tin dilaurate.
[0014] Preferably, the mass of the organotin catalyst is 0.2-0.3% of the mass of the epoxy resin.
[0015] Preferably, the epoxy resin soluble solvent is one or more of xylene, toluene and N,N-dimethylformamide.
[0016] Preferably, the mass of the epoxy resin soluble solvent is 40-50% of the mass of the epoxy resin.
[0017] Preferably, the temperature of the cross-linking reaction is 147-152° C.; and the time of the cross-linking reaction is 2-5 hours.
[0018] Preferably, the heating rate to the cross-linking reaction temperature is 9-11° C. / min.
[0019] Preferably, the mixing is performed by first adding the epoxy resin, organosilane and epoxy resin soluble solvent into a reactor, heating to 105-115° C., and then adding the organotin catalyst.
[0020] The present invention also provides an anti-corrosion modified epoxy resin prepared by the preparation method of the above technical solution, wherein the anti-corrosion modified epoxy resin has an epoxy equivalent of 190 to 201 g / eq and a viscosity of 4980 to 5023 mPa·s at 25°C.
[0021] The present invention provides a method for preparing an anti-corrosion modified epoxy resin, comprising the following steps: mixing an epoxy resin, an organosilane, a soluble epoxy resin solvent, and an organotin catalyst, and performing a cross-linking reaction to obtain the anti-corrosion modified epoxy resin. The present invention utilizes an organosilane to modify the epoxy resin. The organosilane hydrolyzes to produce silanols, which are further hydrolyzed to produce siloxy groups. The silanol molecules can condense and polymerize with each other to form a network-structured film that is resistant to corrosion by external acids, alkalis, salts, and the like. The siloxy groups also condense and react with epoxy groups or hydroxyl groups of the epoxy resin to form a polysiloxane covalent coupling layer, which can enhance the heat resistance, corrosion resistance, and flame retardant effect of the coating formed by the organosilane-modified epoxy resin. The addition of organosilicon segments can also toughen and improve dynamic mechanical properties at high temperatures, thereby meeting the requirements for high-temperature corrosion resistance for equipment in the petroleum and chemical industries. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] FIG1 is an infrared spectrum of the organic silicon, the heat preservation stage (30 min, 150 min, 270 min) during the reaction of Example 1, and the anti-corrosion modified resin after washing with n-butane. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing an anti-corrosion modified epoxy resin, comprising the following steps:
[0024] The epoxy resin, organic silane, a soluble epoxy resin solvent and an organic tin catalyst are mixed and cross-linked to obtain an anti-corrosion modified epoxy resin.
[0025] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used, and commercially available products known to those skilled in the art can be used.
[0026] The invention mixes epoxy resin, organosilane, soluble epoxy resin solvent and organotin catalyst to obtain a mixture.
[0027] In the present invention, the epoxy resin preferably includes one or more of halogen-free epoxy resin, E51 epoxy resin and E44 epoxy resin, more preferably halogen-free epoxy resin or E51 epoxy resin; when there are multiple epoxy resins, the present invention has no special restrictions on the ratio of different types of epoxy resins, and any ratio is acceptable; the epoxy resin is preferably an epoxy resin polymer; the halogen-free epoxy resin is sourced from Jiangsu Yangnong Jinhu Chemical Co., Ltd., model number YN3573K70.
[0028] In the present invention, the organosilane preferably includes one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, γ-(glycidyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, 1,2-bis(triethoxysilyl)ethane, tetraethoxysilane, methyltrimethoxysilane and vinyltriethoxysilane, more preferably tetraethoxysilane or methyltrimethoxysilane; when there are multiple organosilanes, the present invention has no special restrictions on the ratio of different types of organosilanes, and any ratio is acceptable; the mass of the organosilane is preferably 12 to 18% of the mass of the epoxy resin, more preferably 13 to 15%.
[0029] In the present invention, the organotin catalyst is preferably butyl stannoic acid and / or dibutyl tin dilaurate, more preferably butyl stannoic acid; when there are two organotin catalysts, the present invention has no special restrictions on the ratio of different types of organotin catalysts, and any ratio is acceptable; the mass of the organotin catalyst is preferably 0.2 to 0.3% of the mass of the epoxy resin, more preferably 0.22 to 0.25%.
[0030] In the present invention, the soluble epoxy resin solvent is preferably one or more of xylene, toluene and N,N-dimethylformamide, more preferably xylene or toluene; when there are multiple types of soluble epoxy resin solvents, the present invention has no special restrictions on the ratio of different types of soluble epoxy resin solvents, and any ratio is acceptable; the mass of the soluble epoxy resin solvent is preferably 40-50% of the mass of the epoxy resin, more preferably 42-45%.
[0031] In the present invention, the mixing is preferably performed by first adding epoxy resin, organosilane and epoxy resin soluble solvent into a reactor, heating to 105-115°C, and then adding the organotin catalyst to obtain a mixture; the heating temperature is preferably 110°C.
[0032] The present invention heats the mixture obtained by epoxy resin, organic silane and soluble epoxy resin solvent in order to achieve reaction activation energy and promote the reaction.
[0033] After obtaining the mixture, the present invention performs a cross-linking reaction on the mixture to obtain an anti-corrosion modified epoxy resin.
[0034] In the present invention, the temperature of the cross-linking reaction is preferably 147-152°C, more preferably 150°C; the time of the cross-linking reaction is preferably 2-5 hours, more preferably 2.5-4.5 hours; the heating rate to the cross-linking reaction temperature is preferably 9-11°C / min, more preferably 10°C / min.
[0035] During the cross-linking reaction, after hydrolysis, the organosilane undergoes polycondensation itself, and also undergoes condensation reaction and addition reaction with the epoxy group or hydroxyl group of the epoxy resin to form a polysiloxane covalent coupling layer, which can enhance the heat resistance and corrosion resistance of the coating formed by the organosilane-modified epoxy resin.
[0036] The structural formula of the anticorrosive modified epoxy resin prepared in Example 1 of the present invention is as follows:
[0037] Thus, the present invention cross-links the alkoxy groups of the organosilane and the hydroxyl groups in the epoxy resin to generate a copolymer, introduces a stable Si-O bond into the epoxy structure, and obtains an anti-corrosion modified epoxy resin. The P and Si in the structure work together to achieve a flame retardant effect, and the addition of the organosilicon chain segment can also toughen and improve the dynamic mechanical properties at high temperatures. Therefore, the resulting coating has excellent heat resistance, flame retardancy, and corrosion resistance, which can meet the requirements of equipment in the petroleum, chemical, and other industries for temperature and corrosion resistance. In addition, the construction is convenient and cost-effective.
[0038] The technical solutions of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention, but they should not be understood as limiting the scope of protection of the present invention.
[0039] Example 1
[0040] 330 g of halogen-free epoxy resin and 46.3 g of methyltrimethoxysilane were added to a four-necked flask, followed by 145 g of xylene. The reaction system was heated to 110°C, and then 0.76 g of butyl stannoic acid was added. The temperature was continued to rise to 150°C at a rate of 10°C / min and kept warm for 4.5 hours to obtain an anti-corrosion modified epoxy resin.
[0041] Example 2
[0042] 330 g of halogen-free epoxy resin and 46.3 g of tetraethoxysilane were added to a four-necked flask, and then 165 g of toluene was added. After the reaction system was heated to 110 ° C, 0.76 g of butyl stannoic acid was added, and the temperature was continued to rise to 150 ° C at a rate of 10 ° C / min, and kept warm for 2.5 hours to obtain an anti-corrosion modified epoxy resin.
[0043] Example 3
[0044] 330 g of halogen-free epoxy resin and 59.4 g of methyltrimethoxysilane were added to a four-necked flask, followed by 145 g of xylene. The reaction system was heated to 110°C, and then 1 g of butyl stannoic acid was added. The temperature was continued to rise to 150°C at a rate of 10°C / min and kept warm for 2.5 h to obtain an anti-corrosion modified epoxy resin.
[0045] Example 4
[0046] 330 g of halogen-free epoxy resin and 39.6 g of methyltrimethoxysilane were added to a four-necked flask, followed by 145 g of xylene. The reaction system was heated to 110°C, and then 0.76 g of butyl stannoic acid was added. The temperature was continued to rise to 150°C at a rate of 10°C / min and kept warm for 2.5 hours to obtain an anti-corrosion modified epoxy resin.
[0047] Example 5
[0048] 330 g of halogen-free epoxy resin and 49.5 g of tetraethoxysilane were added to a four-necked flask, and then 162 g of toluene was added. After the reaction system was heated to 110 ° C, 0.76 g of butyl stannoic acid was added, and the temperature was continued to rise to 150 ° C at a rate of 10 ° C / min, and kept warm for 2.5 hours to obtain an anti-corrosion modified epoxy resin.
[0049] Comparative Example 1
[0050] A halogen-free epoxy resin was used as a comparative example.
[0051] Performance Testing
[0052] The anti-corrosion modified epoxy resin and the halogen-free epoxy resin obtained in Examples 1 to 5 were respectively mixed with a polyamide curing agent (KCA2300) in a mass ratio of 5:1. The resulting mixture was coated on pretreated carbon steel with a thickness of 70 to 90 μm using a coating rod. The coated carbon steel was cured at 70° C. for 2 h to obtain a coating. The properties of the anti-corrosion modified epoxy resins obtained in Examples 1 to 5 and the halogen-free epoxy resin of Comparative Example 1 and the resulting coatings were measured. The results are shown in Tables 1 and 2.
[0053] Table 1 Performance test results of the anticorrosive modified epoxy resin obtained in Examples 1 to 5 and the halogen-free epoxy resin of Comparative Example 1
[0054] Table 2 Test results of the coatings obtained from the anticorrosive modified epoxy resins obtained in Examples 1 to 5 and the halogen-free epoxy resin of Comparative Example 1
[0055] As can be seen from Table 1, the epoxy equivalent of the anti-corrosion modified epoxy resin prepared by the present invention is 190-201 g / eq, which is higher than 185 g / eq of the halogen-free epoxy resin in Comparative Example 1; the viscosity of the anti-corrosion modified epoxy resin prepared by the present invention is 4980-5023 mPa·s / 25°C, which is lower than 5320 mPa·s / 25°C of the halogen-free epoxy resin in Comparative Example 1.
[0056] As can be seen from Table 2, the heat resistance, acid resistance and salt resistance of the coating formed by the anti-corrosion modified epoxy resin prepared in the present invention are better than those of the coating obtained by the halogen-free epoxy resin in Comparative Example 1.
[0057] (2) Infrared testing was performed on the organosilicon, the heat preservation stage (30 min, 150 min, 270 min) of the reaction process of Example 1, and the anti-corrosion modified resin after washing with n-butane. The results are shown in Figure 1.
[0058] As shown in Figure 1, the 2840 cm -1 The position is the characteristic peak of methoxy, and silicone does have a moderate absorption peak here. As the reaction proceeds, the peak intensity gradually decreases, but it still exists after 270 minutes of heat preservation, which indicates that silicone participates in the reaction but the reaction is not complete. In fact, the modified resin was precipitated and washed with n-hexane, and the washing liquid was filtered and infrared testing was performed. The results showed that 2840 cm -1 There is still an obvious absorption peak at the position, which also proves that the silicone has not reacted completely.
[0059] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A method for preparing an anticorrosive modified epoxy resin, characterized in that: The following steps are involved: The epoxy resin, organic silane, a soluble epoxy resin solvent and an organic tin catalyst are mixed and cross-linked to obtain an anti-corrosion modified epoxy resin.
2. The preparation method according to claim 1, characterized in that: The epoxy resin includes one or more of halogen-free epoxy resin, E51 epoxy resin and E44 epoxy resin.
3. The preparation method according to claim 1, characterized in that: The organosilane includes one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, γ-(glycidyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, 1,2-bis(triethoxysilyl)ethane, tetraethoxysilane, methyltrimethoxysilane and vinyltriethoxysilane.
4. The preparation method according to claim 1, 2 or 3, characterized in that: The mass of the organic silane is 12-18% of the mass of the epoxy resin.
5. The preparation method according to claim 1, characterized in that: The organic tin catalyst is butyl tin acid and / or dibutyl tin dilaurate.
6. The preparation method according to claim 1, 2 or 5, characterized in that: The mass of the organic tin catalyst is 0.2-0.3% of the mass of the epoxy resin.
7. The preparation method according to claim 1, characterized in that: The soluble epoxy resin solvent is one or more of xylene, toluene and N,N-dimethylformamide.
8. The preparation method according to claim 1, 2 or 7, characterized in that: The mass of the soluble epoxy resin solvent is 40-50% of the mass of the epoxy resin.
9. The preparation method according to claim 1, characterized in that: The temperature of the cross-linking reaction is 147-152° C.; the time of the cross-linking reaction is 2-5 hours.
10. The preparation method according to claim 9, characterized in that: The heating rate to the cross-linking reaction temperature is 9-11°C / min.
11. The preparation method according to claim 1, characterized in that: The mixing step is to first add the epoxy resin, organosilane and epoxy resin soluble solvent into a reactor, heat to 105-115° C., and then add the organotin catalyst.
12. The anticorrosive modified epoxy resin prepared by the preparation method according to any one of claims 1 to 11, characterized in that: The epoxy equivalent of the anticorrosive modified epoxy resin is 190-201 g / eq, and the viscosity at 25° C. is 4980-5023 mPa·s.
Citation Information
Patent Citations
Polysiloxane modified epoxy resin and preparation method thereof
CN110305296A
Organosilicon / MDI co-modified epoxy resin and magnesium-rich composite anticorrosive paint thereof
CN115124692A
Preparation method of polysiloxane modified epoxy resin material
CN115505239A
Alkoxy group-containing silane modified epoxy resin, its manufacturing method, epoxy resin composition and its cured product
JP2002249539A