Preparation method for cardanol-modified epoxy resin
Through the ring-opening addition reaction of cardanol and liquid epoxy resin, cardanol-modified epoxy resin with excellent water resistance and toughness is prepared, which solves the problem of insufficient toughness of epoxy resin and achieves low-temperature curing and cost-effectiveness. promote.
Patent Information
- Application Number
- PCT/CN2023/104416
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-06-30
- Publication Date
- 2024-10-31
AI Technical Summary
After curing, epoxy resin has problems such as insufficient toughness, poor impact resistance and easy cracking. Traditional toughening methods will reduce heat resistance and modulus, and are costly or difficult to process.
Cardanol is used to perform a ring-opening addition reaction with liquid epoxy resin and a catalyst to prepare cardanol-modified epoxy resin. The hydrophobic chain and phenolic hydroxyl group of cardanol are used to improve the water resistance and toughness of the material, and to achieve low-temperature curing.
The prepared cardanol-modified epoxy resin has excellent water resistance, strength and toughness, can be cured at low temperature, shortens the coating cycle, has low cost, and the process is simple and easy to operate.
Smart Images

Figure PCTCN2023104416-FTAPPB-I100001
Abstract
Description
Preparation method of cardanol-modified epoxy resin
[0001] This application claims priority to a Chinese patent application filed with the Patent Office of China on April 25, 2023, with application number CN202310444938.1 and invention name “A method for preparing a cardanol-modified epoxy resin”, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The invention belongs to the technical field of epoxy resin modification, and particularly relates to a method for preparing a cardanol-modified epoxy resin. Background Art
[0003] Epoxy resins generally refer to polymers containing two or more epoxy groups within their molecules. They possess excellent adhesion, mechanical properties, electrical insulation, chemical stability, high and low temperature resistance, low shrinkage, ease of processing, good stress transfer, and low cost. They are widely used in adhesives, electronic instruments, light industry, construction, machinery, aerospace, coatings, bonding, as well as electronic and electrical insulation materials and advanced composite matrix materials.
[0004] Epoxy resin is a highly cross-linked thermosetting material with a three-dimensional network structure. This makes it difficult for molecular chains to slide and results in high internal stress. This leads to insufficient toughness, poor impact resistance, and cracking after curing. Therefore, achieving both softness and toughness in epoxy resins has been a topic of great interest. Traditional epoxy resin toughening methods, such as those using rubber elastomers, achieve significant toughness gains but also reduce the system's heat resistance and modulus. While toughening epoxy resins with thermoplastic resins does not reduce the material's modulus or heat resistance, they require high dosages, have poor solubility and fluidity, and are difficult to cure into films. TLCP-toughened epoxy resins significantly improve toughness with lower dosages, but are costly and difficult to process. Therefore, the coatings industry urgently needs a modified epoxy resin that is cost-effective, can be cured at low temperatures, and exhibits excellent water resistance and toughness in the cured paint film.
[0005] Summary of the Invention
[0006] In view of this, the object of the present invention is to provide a method for preparing a cardanol-modified epoxy resin. The cardanol-modified epoxy resin prepared by the present invention has excellent water resistance, strength and toughness, and the coating prepared therefrom can achieve low-temperature curing.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a cardanol-modified epoxy resin, comprising the following steps:
[0009] Liquid epoxy resin, cardanol and a catalyst are mixed and subjected to a ring-opening addition reaction to obtain a cardanol-modified epoxy resin.
[0010] Preferably, the liquid epoxy resin is E51 liquid epoxy resin and / or E54 liquid epoxy resin.
[0011] Preferably, the epoxy equivalent of the liquid epoxy resin is 180 to 190 g / eq.
[0012] Preferably, the catalyst is triphenylphosphine and / or a triphenylphosphine derivative.
[0013] Preferably, the triphenylphosphine derivative includes one or more of butyltriphenylphosphine bromide, ethyltriphenylphosphine chloride, ethyltriphenylphosphine bromide and ethyltriphenylphosphine iodide.
[0014] Preferably, the mass of the catalyst is 0.5-1% of the mass of the liquid epoxy resin.
[0015] Preferably, the mass ratio of the cardanol to the liquid epoxy resin is (20-30):(90-100).
[0016] Preferably, the temperature of the ring-opening addition reaction is 100-120° C.; and the time of the ring-opening addition reaction is 2-3 h.
[0017] Preferably, the heating rate to the ring-opening addition reaction temperature is 0.5-1°C / min.
[0018] Preferably, after the ring-opening addition reaction, the method further comprises: cooling the product obtained from the ring-opening addition reaction to room temperature by passing through a cold water bath.
[0019] Preferably, the ring-opening addition reaction is carried out under stirring conditions; the stirring rate is 130-150 r / min.
[0020] The present invention also provides a cardanol-modified epoxy resin prepared by the preparation method described in the above technical solution, wherein the cardanol-modified epoxy resin has a viscosity of 24630 to 26800 cp.s and a forward impact strength of 45 to 65 J / cm 2 , reverse impact strength is 30~53J / cm 2 .
[0021] The present invention provides a method for preparing a cardanol-modified epoxy resin, comprising the following steps: mixing a liquid epoxy resin, cardanol and a catalyst, and performing a ring-opening addition reaction to obtain the cardanol-modified epoxy resin. The present invention utilizes cardanol to react with the epoxy groups of an epoxy resin under the action of a catalyst to prepare a cardanol-modified epoxy resin. Cardanol is a mixture of phenolic compounds with unsaturated long side-chain hydrocarbon groups. The benzene ring of cardanol is rigid and can improve the strength of the cardanol-modified epoxy resin. Hydrophobic forces exist between the longer hydrophobic chains in the molecular structure, and the hydrophobic chains can hinder the penetration of water molecules, thereby providing the cardanol-modified epoxy resin with excellent water resistance. The hydrophobic chains can also limit molecular diffusion, thereby extending the pot life of the coating based on the cardanol-modified epoxy resin. The flexible long-chain alkane structure in cardanol can enhance the flexibility of the cardanol-modified epoxy resin, thereby improving its toughness. In addition, the phenolic hydroxyl group in cardanol is a polar group, which can provide better bonding properties, reduce reaction activity, and accelerate resin reaction. The coating prepared from the cardanol-modified epoxy resin can be cured at room temperature or low temperature, shortening the coating cycle of the cardanol-modified epoxy resin coating. DETAILED DESCRIPTION
[0022] The present invention provides a method for preparing a cardanol-modified epoxy resin, comprising the following steps:
[0023] Liquid epoxy resin, cardanol and a catalyst are mixed and subjected to a ring-opening addition reaction to obtain a cardanol-modified epoxy resin.
[0024] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used, and commercially available products known to those skilled in the art can be used.
[0025] The invention mixes liquid epoxy resin, cardanol and a catalyst to obtain a mixture.
[0026] In the present invention, the liquid epoxy resin is preferably E51 liquid epoxy resin and / or E54 liquid epoxy resin, more preferably E51 liquid epoxy resin; when the liquid epoxy resin is E51 liquid epoxy resin and E54 liquid epoxy resin, the present invention has no special limitation on the ratio of the two liquid epoxy resins, and any ratio is acceptable; the epoxy equivalent of the liquid epoxy resin is preferably 180 to 190 g / eq, more preferably 182 to 188 g / eq.
[0027] In the present invention, the catalyst is preferably triphenylphosphine and / or a triphenylphosphine derivative, more preferably a triphenylphosphine derivative; the triphenylphosphine derivative preferably includes one or more of butyltriphenylphosphine bromide, ethyltriphenylphosphine chloride, ethyltriphenylphosphine bromide and ethyltriphenylphosphine iodide, more preferably butyltriphenylphosphine bromide, ethyltriphenylphosphine chloride or ethyltriphenylphosphine bromide; when there are multiple catalysts, the present invention has no special restrictions on the ratio of different types of catalysts, and any ratio is acceptable; the mass of the catalyst is preferably 0.5-1% of the mass of the liquid epoxy resin, more preferably 0.5-0.8%.
[0028] In the present invention, the mass ratio of the cardanol to the liquid epoxy resin is preferably (20-30):(90-100), more preferably (20-27):(90-100).
[0029] Cardanol is the main component of cashew nutshell liquid (CNSL). Its chemical structure is a phenol structure containing long-chain unsaturated alkanes. It is biorenewable and inexpensive.
[0030] The present invention utilizes cardanol to react with the epoxy groups of an epoxy resin under the action of a catalyst to prepare a cardanol-modified epoxy resin. The phenolic hydroxyl groups in the cardanol structure can provide good bonding properties, reduce reaction activity, accelerate resin reaction, achieve low-temperature curing of the coating, and shorten the coating cycle. The hydrophobic interaction between the longer hydrophobic chains in the molecular structure can, on the one hand, limit molecular diffusion, thereby extending the pot life of the coating based on the cardanol-modified epoxy resin. On the other hand, the hydrophobicity of the paint film can be improved. The hydrophobic chains can hinder the penetration of water molecules, thereby improving the water resistance of the paint film. The flexible long-chain alkane structure in the cardanol can enhance the flexibility of the cardanol-modified epoxy resin, thereby improving its toughness.
[0031] After obtaining the mixture, the present invention performs a ring-opening addition reaction on the mixture to obtain a cardanol-modified epoxy resin.
[0032] In the present invention, the temperature of the ring-opening addition reaction is preferably 100-120°C, more preferably 110-120°C; the time of the ring-opening addition reaction is preferably 2-3 hours, more preferably 2 hours; the heating rate to the ring-opening addition reaction temperature is preferably 0.5-1°C / min, more preferably 0.6-0.8°C / min; the ring-opening addition reaction is preferably carried out under stirring; the stirring rate is preferably 130-150r / min, more preferably 140-150r / min.
[0033] After the ring-opening addition reaction, the present invention preferably further comprises: cooling the product obtained from the ring-opening addition reaction to room temperature in a cold water bath; the room temperature is preferably 24-30°C, more preferably 24-29°C.
[0034] The present invention utilizes the phenolic hydroxyl groups of cardanol to react easily with epoxy groups under the action of a catalyst to prepare a CNSL-modified epoxy resin, which can improve the water resistance and toughness of the paint film and make the cured coating have stronger toughness, strength and water resistance.
[0035] The cardanol-modified epoxy resin prepared by the present invention can be used to prepare coatings, achieving low-temperature curing, shortening the coating cycle, reducing coating defects, using biorenewable raw materials, and being inexpensive. Furthermore, the preparation process does not generate the three wastes. The preparation method of the present invention has a simple process, is easy to operate, and is convenient for industrial implementation.
[0036] The present invention also provides a cardanol-modified epoxy resin prepared by the preparation method described in the above technical solution, wherein the cardanol-modified epoxy resin has a viscosity of 24630 to 26800 cp.s and a forward impact strength of 45 to 65 J / cm 2 , reverse impact strength is 30~53J / cm 2 .
[0037] The technical solutions of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention, but they should not be understood as limiting the scope of protection of the present invention.
[0038] Example 1
[0039] 95 g of E51 liquid epoxy resin (epoxy equivalent 186.6 g / eq, viscosity 12680 cp.s), 23 g of cardanol and 0.76 g of butyltriphenylphosphine bromide were added to a 500 mL four-necked flask. The resulting mixture was stirred at 130 rpm and heated to 100 ° C at 0.5 ° C / min for 2 h. Then, the temperature was cooled to 26 ° C and taken out to obtain a cardanol-modified epoxy resin. The viscosity of the modified epoxy resin was 25630 cp.s after testing.
[0040] Example 2
[0041] 90 g of E51 liquid epoxy resin (epoxy equivalent weight 182.8 g / eq, viscosity 14200 cp.s), 25 g of cardanol, and 0.9 g of ethyltriphenylphosphine chloride were added to a 500 mL four-necked flask. The resulting mixture was stirred at 140 rpm and heated to 105°C at 0.6°C / min for 2 h. The mixture was then cooled to 24°C and removed to obtain a cardanol-modified epoxy resin. The viscosity of the modified epoxy resin was 26800 cp.s after testing.
[0042] Example 3
[0043] 100 g of E51 liquid epoxy resin (epoxy equivalent 184.6 g / eq, viscosity 14000 cp.s), 20 g of cardanol and 0.6 g of ethyltriphenylphosphonium bromide were added to a 500 mL four-necked flask. The resulting mixture was stirred at 145 rpm and heated to 115 ° C at 1 ° C / min for 2 h. Then the temperature was cooled to 29 ° C and taken out to obtain a cardanol-modified epoxy resin. The viscosity after modification was tested to be 24630 cp.s.
[0044] Example 4
[0045] 98 g of E51 liquid epoxy resin (epoxy equivalent 187.5 g / eq, viscosity 13500 cp.s), 24 g of cardanol and 0.784 g of butyltriphenylphosphine bromide were added to a 500 mL four-necked flask. The resulting mixture was stirred at 150 rpm and heated to 120 ° C at 0.8 ° C / min for 2 h. Then, the temperature was cooled to 27 ° C and taken out to obtain a cardanol-modified epoxy resin. After testing, the viscosity of the modified epoxy resin was 25200 cp.s.
[0046] Example 5
[0047] 93 g of E51 liquid epoxy resin (epoxy equivalent 183.7 g / eq, viscosity 13050 cp.s), 27 g of cardanol and 0.651 g of ethyltriphenylphosphine iodide were added to a 500 mL four-necked flask. The resulting mixture was stirred at 140 rpm and heated to 117 ° C. at 0.7 ° C. / min for 2 h. The mixture was then cooled to 24 ° C. and taken out to obtain a cardanol-modified epoxy resin. The viscosity of the modified epoxy resin was 26730 cp.s after testing.
[0048] Performance Testing
[0049] 20 g of the cardanol-modified epoxy resin obtained in Examples 1 to 5 was added with 12 g of N,N-dimethylbenzylamine (BDMA) and 8 g of methylhexahydrophthalic anhydride (MeHHPA) for a curing experiment. The test standard was GB / T 2423.5-2019. The results are shown in Table 1.
[0050] Table 1 Performance test results of cardanol modified epoxy resin cured products obtained in Examples 1 to 5
[0051] As shown in Table 1, the forward impact strength of the cardanol-modified epoxy resin cured product prepared by the present invention is 45-65 J / cm 2 , much higher than the blank sample's forward impact strength of 9 to 11 J / cm 2 The reverse impact strength of the cardanol modified epoxy resin prepared by the present invention is 30 to 53 J / cm 2 , much higher than the reverse impact strength of the blank sample 5~6J / cm 2, indicating that the cured product formed by the cardanol-modified epoxy resin prepared by the present invention has excellent toughness.
[0052] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a cardanol-modified epoxy resin, characterized in that: The following steps are involved: Liquid epoxy resin, cardanol and a catalyst are mixed and subjected to a ring-opening addition reaction to obtain a cardanol-modified epoxy resin.
2. The preparation method according to claim 1, characterized in that: The liquid epoxy resin is E51 liquid epoxy resin and / or E54 liquid epoxy resin.
3. The preparation method according to claim 1 or 2, characterized in that: The epoxy equivalent of the liquid epoxy resin is 180 to 190 g / eq.
4. The preparation method according to claim 1, characterized in that: The catalyst is triphenylphosphine and / or a triphenylphosphine derivative.
5. The preparation method according to claim 4, characterized in that: The triphenylphosphine derivatives include one or more of butyltriphenylphosphine bromide, ethyltriphenylphosphine chloride, ethyltriphenylphosphine bromide and ethyltriphenylphosphine iodide.
6. The preparation method according to claim 1, 2, 4 or 5, characterized in that: The mass of the catalyst is 0.5-1% of the mass of the liquid epoxy resin.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the cardanol to the liquid epoxy resin is (20-30):(90-100).
8. The preparation method according to claim 1 or 7, characterized in that: The temperature of the ring-opening addition reaction is 100-120° C.; the time of the ring-opening addition reaction is 2-3 hours.
9. The preparation method according to claim 8, characterized in that: The heating rate to the ring-opening addition reaction temperature is 0.5-1°C / min.
10. The preparation method according to claim 1, characterized in that: After the ring-opening addition reaction, the method further comprises: cooling the product obtained from the ring-opening addition reaction to room temperature by using a cold water bath.
11. The preparation method according to claim 1 or 9, characterized in that: The ring-opening addition reaction is carried out under stirring conditions; the stirring rate is 130-150 r / min.
12. The cardanol-modified epoxy resin prepared by the preparation method according to any one of claims 1 to 11, characterized in that: The cardanol modified epoxy resin has a viscosity of 24630-26800 cp.s and a forward impact strength of 45-65 J / cm 2 , reverse impact strength is 30~53J / cm 2 .
Citation Information
Patent Citations
Cardanol modified epoxy polyol
CN105960424A
Cardanol modified epoxy polyol
CN105992784A
Preparation method of high-toughness epoxy resin
CN113683752A
Cardanol-modified epoxy resin composition
KR100559055B1
Cited By
Phosphorus-bromine synergistic cardanol polyol as well as preparation method and application thereof
CN122145509A