Ash removal method for coal-based asphalt, and refined asphalt prepared thereby
Through the method of two-stage solvent extraction and flocculation reaction, the problems of high ash content and low yield in the deashing process of coal liquefied asphalt are solved, and the preparation of high-efficiency and low-ash refined asphalt is realized, which is suitable for the production of various carbon materials. Process conditions are simplified and efficiency is improved.
Patent Information
- Application Number
- PCT/CN2024/072861
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-01-17
- Publication Date
- 2024-10-31
AI Technical Summary
The existing coal liquefied asphalt deashing process has problems such as high ash content, low yield, high equipment requirements and residual impurities, making it difficult to produce high-efficiency, low-ash refined asphalt.
A two-stage solvent extraction and flocculation reaction method is adopted. The first solvent dissolves the coal-based asphalt and then mixes it with the second solvent to perform a flocculation reaction. Combined with centrifugal separation and natural sedimentation, deep deashing is achieved, and the solvent is recycled to reduce the ash content. Improve asphalt production and quality under mild conditions.
It achieves the preparation of refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1%, improving the yield and quality of asphalt. It is suitable for the preparation of mesophase pitch, carbon fiber and other materials, simplifying process conditions and improving efficiency. .
Smart Images

Figure CN2024072861_31102024_PF_FP_ABST
Abstract
Description
A deashing method for coal-based asphalt and refined asphalt obtained therefrom Technical Field
[0001] The invention belongs to the technical field of asphalt refining, and in particular relates to a deashing method for coal-based asphalt and refined asphalt obtained therefrom. Background Art
[0002] Direct coal liquefaction residues are primarily composed of inorganic and organic matter. The organic matter includes heavy liquefied oil, asphalt, and unconverted coal. The inorganic matter comprises minerals from the coal and added catalysts. Among the organic matter, heavy liquefied oil and asphalt account for approximately 50% of the residue, unconverted coal accounts for approximately 30%, and ash accounts for approximately 20%. Therefore, it is feasible to separate the approximately 50% asphalt and heavy oil from the residue for comprehensive processing and utilization, thereby extracting or preparing more valuable products.
[0003] The asphalt substances contained in the direct coal liquefaction residue need to be further deashed before they can be converted into applicable asphalt products. For example,
[0004] Patent document CN109575974A discloses a method for efficient deashing of coal liquefaction residue, which uses a two-stage static sedimentation method to remove the ash content of coal liquefaction residue to less than 100 ppm; although this method can effectively reduce the ash content in liquefied asphalt, the separation sedimentation temperature is relatively high (up to 200-280°C), and an aqueous solution of flocculants such as polyacrylamide and polyaluminum chloride needs to be added during the second-stage separation, which will cause the operating pressure of the separation device to be high, polyacrylamide and the like are easily decomposed, polyaluminum chloride is easily hydrolyzed, and flocculants are easily left in the deashed asphalt product, thereby affecting the quality of the asphalt product, and the asphalt yield is low.
[0005] Patent document CN103509576A discloses a method for separating non-affected organic matter from coal direct liquefaction residue. The method combines acid washing and alkaline washing by chemical deashing to reduce the inorganic matter content in the direct liquefaction residue from 26.1% to 6.2%. Although some surfactants or alcohols are added to the acid / alkaline solution to accelerate the sedimentation step, the number of acid / alkaline washings is large during the entire process, the amount of acid / alkaline used is large, the reaction temperature is high, and the reaction time is long.
[0006] Patent document CN105754630A discloses a method for preparing coal liquefaction asphalt. The method uses solvent extraction combined with molecular distillation to obtain light extracted asphalt liquid. After recovering the solvent, it is refined by molecular distillation to prepare refined liquefied asphalt with an ash content of 100 to 500 ppm. However, the molecular distillation process used in this method needs to be carried out under high vacuum and high temperature, so the equipment and process requirements are relatively high, and the ash content in the product is also relatively high.
[0007] Patent document CN108192650A discloses a method for preparing ultra-low ash asphalt. The patent first thermally condenses the asphalt raw material into intermediate spheres, removes the intermediate phase spheres and other insoluble matter by melting or solution filtration, and then evaporates the solvent to obtain purified asphalt with an ash content of less than 20 ppm. Although the product obtained by this process has a low ash content, this method has high requirements on the control precision of the reaction process conditions, and the product yield is low.
[0008] In view of this, how to further improve the deashing process of coal liquefaction pitch and produce refined pitch with high product yield and low ash content is a direction worthy of research.
[0009] Summary of the Invention
[0010] The purpose of the present invention is to address the problems existing in the existing coal liquefaction asphalt deashing process and provide a deashing method for reducing the ash content and quinoline insoluble matter in coal-based asphalt, so as to produce refined asphalt with ultra-low ash content for use in the subsequent preparation of carbon materials such as mesophase asphalt, needle coke, carbon fiber, foamed carbon, electrode materials, etc.; the deashing method can perform deep deashing under mild conditions, improve the deashing effect, and increase the yield of the resulting refined asphalt; and, while being able to produce refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble matter content of less than 0.1%, it can also co-produce binder asphalt with an ash content of less than 0.1% and a quinoline insoluble matter content of less than 1%.
[0011] In a first aspect, a method for deashing coal-based asphalt is provided, comprising the steps of:
[0012] i. Coal-based pitch is used as the raw material to be processed, a first solvent is added, and the mixture is fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based pitch is (0.5-4):1 (for example, 0.8:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1); the first solvent is a coal tar fraction or a coal liquefaction oil fraction, the distillation range of which is between 180 and 300° C. (for example, 180-280° C., 190-300° C., 200-250° C., 260-280° C.), and the H / C ratio is 0.6-1.0 (n / n), for example, 0.7, 0.8, or 0.9;
[0013] ii. mixing the extract obtained in step i with a second solvent in a mass ratio of 1:(1-4) (e.g., 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5) and performing a flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coke light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, having a distillation range of 70-160° C. (e.g., 80-160° C., 70-140° C., 120-160° C.) and H / C=1.1-2.3 (n / n), for example, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, 2.2;
[0014] Then, the suspension is centrifuged or subjected to natural sedimentation to separate a heavy phase and a light phase;
[0015] iii. recovering the solvent from the heavy phase obtained in step ii to obtain heavy asphalt, and optionally mixing the recovered solvent into the light phase;
[0016] The second solvent and the first solvent in the light phase are recovered separately to obtain refined asphalt with an ash content of less than 100 ppm (e.g., 1 ppm, 4 ppm, 10 ppm, 20 ppm, 50 ppm, 80 ppm) and a quinoline insoluble matter content of less than 0.1 wt% (e.g., 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.04 wt%, 0.06 wt%, 0.08 wt%).
[0017] The heavy phase obtained in step ii can be subjected to solvent recovery by vacuum distillation; the operation process of recovering the solvent by vacuum distillation is a conventional operation in the art, for example, the mixed solvent (a mixture of the first solvent and the second solvent) can be recovered by vacuum distillation at 250°C and -0.08MPa (gauge pressure) for recycling. In addition, the second solvent and the first solvent in the light phase obtained can be recovered separately. For example, it can be understood that the light phase obtained in step ii is first subjected to atmospheric distillation to recover the second solvent, and the recovered second solvent can be recycled in step ii, and then the first solvent is recovered by vacuum distillation, and the recovered first solvent can be recycled in step i; for example, the light phase obtained is first flashed at 180°C and atmospheric pressure to remove the second solvent and reuse it, and then the first solvent is recovered by vacuum distillation at 250°C and -0.08MPa (gauge pressure) and reused, and ultra-low ash refined asphalt is obtained at the bottom of the distillation kettle.
[0018] According to the deashing method provided by the present invention, by adding a step of separating the extract, it is possible to produce a refined asphalt having an ash content of less than 100 ppm and a quinoline-insoluble content of less than 0.1%, while also co-producing a binder asphalt having an ash content of less than 0.1% and a quinoline-insoluble content of less than 1%. In some embodiments, the deashing method comprises the following steps:
[0019] i. Coal-based pitch is used as the raw material to be processed, a first solvent is added, and the mixture is fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based pitch is (0.5-4):1 (for example, 0.8:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1); the first solvent is a coal tar fraction or a coal liquefaction oil fraction, the distillation range of which is between 180 and 300° C. (for example, 180-280° C., 190-300° C., 200-250° C., 260-280° C.), and the H / C ratio is 0.6-1.0 (n / n), for example, 0.7, 0.8, or 0.9;
[0020] The obtained extract is then centrifuged or subjected to natural sedimentation to obtain a first heavy phase and a first light phase; the first heavy phase is then subjected to reduced pressure distillation to recover the first solvent to obtain heavy asphalt;
[0021] ii. The first light phase separated in step i is mixed with a second solvent in a mass ratio of 1:(1-4) (for example, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5) and subjected to a flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coke light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, and its distillation range is between 70-160° C. (for example, 80-160° C., 70-140° C., 120-160° C.) and H / C=1.1-2.3 (n / n), for example, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, 2.2;
[0022] Then, the suspension is centrifuged or subjected to natural sedimentation separation to obtain a second heavy phase and a second light phase;
[0023] iii. Recovering the solvent from the second heavy phase separated in step ii to obtain a binder pitch having an ash content of less than 0.1 wt% (e.g., 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.04 wt%, 0.06 wt%, 0.08 wt%) and a quinoline-insoluble matter content of less than 1 wt% (e.g., 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.4 wt%, 0.6 wt%, 0.8 wt%), and optionally mixing the recovered solvent into the second light phase;
[0024] The second solvent and the first solvent in the second light phase are recovered separately to obtain refined asphalt with an ash content of less than 100 ppm (e.g., 1 ppm, 4 ppm, 10 ppm, 20 ppm, 50 ppm, 80 ppm) and a quinoline insoluble matter content of less than 0.1 wt% (e.g., 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.04 wt%, 0.06 wt%, 0.08 wt%).
[0025] In step i of the above method, the process of recovering the solvent from the first heavy phase by vacuum distillation is conventional in the art. For example, vacuum distillation at 250°C and -0.08 MPa (gauge pressure) can be performed to recover the first solvent for recycling. The resulting heavy asphalt can be discharged from the system and used as a product.
[0026] In step iii of the above method, the solvent in the second heavy phase can be recovered by vacuum distillation. This operation is conventional in the art, for example, by vacuum distillation at 250°C and -0.08 MPa (gauge pressure) to recover the mixture of the first solvent and the second solvent in the second heavy phase. The light liquid phase obtained after vacuum distillation (i.e., the mixture of the first solvent and the second solvent) can be directly mixed with the second light phase (supernatant) separated in step ii, and the binder asphalt is obtained at the bottom of the still.
[0027] In step iii of the above method, the second light phase (supernatant) can first be subjected to atmospheric distillation to recover the second solvent, and the recovered second solvent can be recycled in step ii, and then subjected to reduced pressure distillation to recover the first solvent, and the recovered first solvent can be recycled in step i; for example, the obtained second light phase (supernatant) is first flashed at 180°C and atmospheric pressure to remove the second solvent and reused, and then subjected to reduced pressure distillation at 250°C and -0.08MPa (gauge pressure) to recover the first solvent and reuse it, and ultra-low ash refined asphalt is obtained at the bottom of the distillation kettle.
[0028] In some embodiments, in step i, before separating the extract, a mixture of a settling aid and a wetting agent and / or activated clay is added to the extract.
[0029] In some embodiments, the sedimentation aid is an aqueous solution containing 1 to 10 wt% (e.g., 2 wt%, 4 wt%, 5 wt%, 8 wt%) of a flocculant; preferably, the flocculant is selected from one or more of polyacrylamide, polyaluminum chloride, polyaluminum sulfate, polyferric chloride, and polyferric sulfate.
[0030] In some embodiments, the wetting agent is selected from one or more of ethanol, 1-pentanol, 1-octanol, ethylene glycol, and glycerol.
[0031] In some embodiments, before separating the extract, activated clay is added to the extract, and the amount of activated clay added is 0.1-1 wt% (e.g., 0.2 wt%, 0.4 wt%, 0.5 wt%, 0.8 wt%) based on the mass of coal-based asphalt.
[0032] In some embodiments, the process conditions for adding activated clay to the extract for mixing include: a mixing temperature of 80-140°C (e.g., 90°C, 100°C, 120°C) and a mixing time of 10-60 min (e.g., 15 min, 30 min, 40 min, 50 min).
[0033] In some embodiments, before separating the extract, a mixture of a sedimentation aid and a wetting agent is added to the extract and mixed;
[0034] The process conditions for adding and mixing the mixture formed by the settling aid and the wetting agent include: a mixing temperature of 80-140° C. (e.g., 90° C., 100° C., 120° C.), stirring and mixing at a speed of 3000-8000 r / min (e.g., 3500 r / min, 4000 r / min, 5000 r / min, 6000 r / min, 7000 r / min) for 0.2-5 min (e.g., 0.4 min, 1 min, 2 min, 4 min), and then stirring and mixing at a speed of 50-500 r / min (e.g., 60 r / min, 100 r / min, 200 r / min, 300 r / min, 400 r / min) for 30-180 min (e.g., 40 min, 60 min, 100 min, 120 min, 150 min). The mixing process can be carried out in a homogenizer or a colloid mill.
[0035] In some embodiments, the amount of the sedimentation aid added is 2-10% (e.g., 3%, 4%, 5%, 8%) of the mass fraction of the extract, and the amount of the wetting agent added is 0.1-0.5% (e.g., 0.2%, 0.3%, 0.4%) of the mass fraction of the extract.
[0036] In some embodiments, in step i, the process conditions for centrifugal separation include: placing the material stream to be separated in a centrifuge, centrifuging at a constant temperature of 80 to 140° C. (e.g., 90° C., 100° C., 120° C.) for 0.5 to 10 min (e.g., 0.6 min, 1 min, 2 min, 4 min, 5 min, 8 min), and a separation factor between 500 and 3000 (e.g., 600, 800, 1000, 1500, 2000, 2500).
[0037] In some embodiments, in step i, the process conditions for natural sedimentation include: constant temperature sedimentation at 80-180°C (e.g., 90°C, 100°C, 120°C, 150°C) for 4-48 hours (e.g., 5 hours, 10 hours, 15 hours, 20 hours, 25 hours, 30 hours, 40 hours).
[0038] In some embodiments, the coal-based pitch is selected from coal tar pitch, coal tar modified pitch, or coal liquefaction pitch.
[0039] In some embodiments, based on the total weight of the coal-based asphalt, the ash content in the coal-based asphalt is 0.1 to 5 wt% (e.g., 0.2 wt%, 0.5 wt%, 1 wt%, 2 wt%, 4 wt%), and / or the quinoline insoluble matter content is 1 to 10 wt% (e.g., 2 wt%, 4 wt%, 5 wt%, 6 wt%, 8 wt%).
[0040] In some embodiments, in step i, the conditions for dissolving by the first solvent include: a dissolution temperature of 100-200°C (e.g., 120°C, 150°C, 160°C, 180°C), and a dissolution time of 15-60 min (e.g., 20 min, 30 min, 40 min, 50 min).
[0041] In some embodiments, in step ii, the conditions of the flocculation reaction include: a reaction temperature of 50-120°C (for example, 60°C, 80°C, 100°C, 110°C), a stirring speed of 80-350r / min (for example, 100r / min, 250r / min, 300r / min), and a stirring time of 10-60min (for example, 15min, 30min, 40min, 50min).
[0042] In some embodiments, in step ii, the conditions for subjecting the suspension to the centrifugal separation include: placing the suspension in a centrifuge, centrifuging at a constant temperature of 50-120°C (e.g., 60°C, 80°C, 100°C, 110°C) for 0.5-10 min (e.g., 1 min, 2 min, 4 min, 8 min), and a separation factor between 500 and 3000 (e.g., 600, 1000, 1500, 2000, 2500).
[0043] In some embodiments, the process conditions for subjecting the suspension to natural sedimentation include: constant temperature sedimentation at 50-120°C (e.g., 60°C, 80°C, 100°C, 110°C) for 6-72 hours (e.g., 8 hours, 12 hours, 20 hours, 40 hours, 60 hours, 70 hours).
[0044] The separation process conditions in step ii may be a separation operation on a suspension formed by mixing the extract and the second solvent, or a separation operation on a suspension formed by mixing the first light phase and the second solvent.
[0045] In a second aspect, a refined asphalt containing low ash and low quinoline insolubles, produced by the deashing method described above, is provided. For example, the refined asphalt has an ash content of less than 100 ppm (e.g., 1 ppm, 4 ppm, 10 ppm, 20 ppm, 50 ppm, 80 ppm) and a quinoline insoluble content of less than 0.1 wt% (e.g., 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.04 wt%, 0.06 wt%, 0.08 wt%).
[0046] To address the problems of coal-based asphalt, such as small ash particle size, high asphalt viscosity, high sulfur and nitrogen impurity content, and strong chelating ability for inorganic components, the present invention adopts a two-stage refining process. After the first stage of refining, solvent recovery is eliminated, and the resulting extract is directly mixed with a second solvent with a higher hydrogen-to-carbon ratio for flocculation, achieving efficient deashing. This not only increases asphalt yield but also improves quality. The asphalt deashing process of the present invention is simple, operates under mild conditions, and achieves high deashing efficiency, making it highly industrially feasible.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] 1) Two solvents with greatly different hydrogen-to-carbon ratios are used to perform a secondary refining treatment on coal-based asphalt. During the first-stage refining process, a first solvent (solvent with stronger solubility) with a relatively low hydrogen-to-carbon ratio is used to dissolve the coal-based asphalt to maximize the dissolution of the asphalt, thereby increasing the yield of low-ash refined asphalt. Before the second-stage refining, there is no need to recover the first solvent, but a second solvent (solvent with relatively weaker solubility) with a relatively high hydrogen-to-carbon ratio is directly added to precipitate some high-molecular-weight substances in the asphalt, thereby absorbing and agglomerating ultrafine ash particles or flocculant residues suspended in the asphalt solution, thereby achieving deep deashing, reducing impurity residues, and improving the quality of the asphalt product, thereby obtaining a coal-based refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1%;
[0049] 2) The resulting asphalt has a low ash content and can be used as a high-quality raw material for preparing carbon materials such as mesophase asphalt, lithium battery negative electrode materials, needle coke, and coated asphalt;
[0050] 3) Both the dissolution and refining processes are carried out under relatively mild conditions, which reduces the requirements for separation equipment and facilitates the use of high-efficiency separation equipment, thereby accelerating separation efficiency. Compared with existing asphalt deashing processes, the process cycle is short, the operation is simple, the reaction conditions are mild, and the yield of asphalt products is as high as 70-90%, with an ash content of only 10-100 ppm.
[0051] 4) By adding a step of separating the extract before the obtained extract is mixed with the second solvent and subjected to flocculation reaction, it is possible to produce refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1%, and at the same time, to co-produce a binder asphalt with an ash content of less than 0.1% and a quinoline insoluble content of less than 1%. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and therefore should not be regarded as limiting the scope of the present invention.
[0053] FIG1 shows a schematic diagram of a process flow of a deashing method according to an embodiment of the present invention. DETAILED DESCRIPTION
[0054] In order to understand the technical features and content of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein.
[0055] <Source of raw materials>
[0056] Coal liquefaction pitch: softening point 162°C, ash content 1.0wt%, quinoline insoluble content 4.1wt%;
[0057] Coal tar pitch: softening point 92°C, ash content 0.21wt%, quinoline insoluble content 5.2wt%;
[0058] First solvent: coal tar fraction with a content of 5-98 wt%, the distillation temperature of the coal tar fraction is 180-300° C. and H / C=0.89;
[0059] Second solvent A: naphtha with a content of 5-98 wt%, a distillation temperature of naphtha of 70-140° C. and H / C=1.98;
[0060] The second solvent B is a coal indirect liquefaction light oil with a content of 5-98 wt %, the coal indirect liquefaction light oil has a distillation temperature of 70-160° C. and H / C=2.03.
[0061] Example 1:
[0062] The deashing method of coal-based asphalt, as shown in FIG1 , comprises the following steps:
[0063] i. Add the first solvent to 1 kg of coal liquefaction pitch to be treated, mix the coal liquefaction pitch and the first solvent at a mass ratio of 1:2, and fully dissolve them at 150° C. for 30 minutes to obtain an extract;
[0064] The obtained extract was cooled to 100°C, and then 4 g of activated clay was added and mixed. After further mixing at this temperature for 30 minutes, the obtained extract mixture was placed in a high-temperature centrifuge and centrifuged at 100°C for 2 minutes with a separation factor of 1800.
[0065] Centrifugal separation obtains a first heavy phase and a first light phase, and the first heavy phase is subjected to reduced pressure distillation at 250° C. and −0.08 MPa (gauge pressure) to recover the first solvent, thereby obtaining heavy asphalt. The first light phase in the centrifuge enters step ii;
[0066] ii. mixing the first light phase separated in step i with the second solvent A in a mass ratio of 1:2 and performing a flocculation reaction under the following reaction conditions: stirring at 100° C. and 150 r / min for 30 min to obtain a suspension;
[0067] The suspension was then placed in a high-temperature centrifuge and centrifuged at 100°C for 1.5 minutes with a separation factor of 1800. After the centrifugation, a second light phase (supernatant) and a second heavy phase (heavy phase at the bottom) were obtained.
[0068] iii. After the second heavy phase (bottom heavy phase material) separated in step ii is subjected to reduced pressure distillation at 250° C. and −0.08 MPa (gauge pressure) to recover the solvent (the recovered solvent is a mixture of the first solvent and the second solvent A), the light phase (recovered solvent) obtained in the upper part of the still is mixed with the second light phase (supernatant liquid) obtained in step ii, and the binder asphalt is obtained at the bottom of the still;
[0069] The second light phase (supernatant) separated in step ii was first flashed at 160°C and atmospheric pressure to remove the second solvent A for reuse. The first solvent was then recovered and reused by reduced pressure distillation at 250°C and -0.08 MPa (gauge pressure). Ultra-low-ash refined asphalt was obtained at the bottom of the still. The test results of the resulting product are shown in Table 1.
[0070] Example 2:
[0071] The deashing method for coal-based pitch was similar to that of Example 1, except that in step i, activated clay was not added to the extract. Instead, a mixture of a settling aid and a wetting agent was added to the extract to obtain an extract mixture. Specifically, before entering the high-temperature centrifuge, the extract was cooled to 100°C, 5% of the settling aid by mass and 0.2% of ethylene glycol were added under constant temperature, and the mixture was immediately stirred at 4000 rpm for 1 minute and then at 100 rpm for 60 minutes. The settling aid was an aqueous solution containing 2% by weight of polyaluminum chloride. The remaining steps were the same as in Example 1. The test results of the resulting product are shown in Table 1.
[0072] Example 3:
[0073] The coal-based pitch deashing method was similar to that of Example 2, except that: in step i, the high-temperature centrifugal separation of the extract mixture was replaced by natural sedimentation, where the conditions for natural sedimentation separation were: constant temperature and stabilization at 140°C for 40 hours; and in step ii, the high-temperature centrifugal separation of the suspension was replaced by natural sedimentation, where the conditions for natural sedimentation separation were: constant temperature and stabilization at 100°C for 48 hours. The remaining steps were the same as in Example 2. The test results of the resulting product are shown in Table 1.
[0074] Example 4:
[0075] The coal-based pitch deashing method was similar to that of Example 1, except that in step i, the coal liquefaction pitch and the first solvent were mixed at a mass ratio of 1:0.5 and fully dissolved at 150°C for 30 minutes to obtain an extract. The remaining steps were the same as those of Example 1. The test results of the resulting product are shown in Table 1.
[0076] Example 5:
[0077] The coal-based pitch deashing method was similar to that of Example 1, except that in step i, the coal liquefaction pitch and the first solvent were mixed in a mass ratio of 1:4 and fully dissolved at 150°C for 30 minutes to obtain an extract. The remaining steps were the same as those of Example 1. The test results of the resulting product are shown in Table 1.
[0078] Example 6:
[0079] The deashing method of coal-based asphalt, as shown in FIG1 , comprises the following steps:
[0080] i. Add the first solvent to 1 kg of coal liquefaction pitch to be treated, mix the mixture at a mass ratio of 1:2.1, and fully dissolve the mixture at 180° C. for 30 minutes to obtain an extract;
[0081] The obtained extract was kept at a constant temperature of 180° C. for 42 hours for sedimentation separation to obtain a first heavy phase and a first light liquid phase; the first heavy phase was subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the first solvent to obtain heavy asphalt; the obtained first light phase was entered into step ii;
[0082] ii. flocculating the first light phase separated in step i with the second solvent B in a mass ratio of 1:4, under the following reaction conditions: stirring at 80° C. and 250 rpm for 30 min to obtain a suspension;
[0083] The suspension was then allowed to settle at a constant temperature of 80° C. for 70 hours to obtain a second light phase (supernatant) and a second heavy phase (bottom heavy phase);
[0084] iii. Recovering the solvent (the recovered solvent is a mixture of the first solvent and the second solvent B) from the second heavy phase (the bottom heavy phase) separated in step ii by reduced pressure distillation at 250° C. and −0.08 MPa (gauge pressure). The light phase (recovered solvent) obtained at the top of the still is mixed with the second light phase (supernatant) obtained in step ii, and obtaining the binder asphalt at the bottom of the still.
[0085] The second light phase (supernatant) separated in step ii was first flashed at 180°C and atmospheric pressure to remove the second solvent B for reuse. The first solvent was then recovered and reused by vacuum distillation at 250°C and -0.08 MPa (gauge pressure). Ultra-low-ash refined asphalt was obtained at the bottom of the still. The test results of the resulting product are shown in Table 1.
[0086] Example 7:
[0087] The deashing method of coal-based pitch was similar to that of Example 6, except that in step i, coal tar pitch was used as the coal-based pitch to be treated; the remaining steps were the same as those of Example 6. The test results of the obtained product are shown in Table 1.
[0088] Example 8:
[0089] The deashing method for coal-based pitch was similar to that of Example 6, except that in step i, the coal-based pitch to be treated was coal tar pitch, and in step ii, the second solvent was second solvent A. The remaining steps were the same as in Example 6. The test results of the resulting product are shown in Table 1.
[0090] Example 9:
[0091] The deashing method of coal-based asphalt comprises the following steps:
[0092] i. Add the first solvent to 1 kg of coal liquefaction pitch to be treated, mix the mixture at a mass ratio of 1:2.1, and fully dissolve the mixture at 180° C. for 30 minutes to obtain an extract;
[0093] ii. flocculating the extract obtained in step i with the second solvent B in a mass ratio of 1:4, under the following reaction conditions: stirring at 80° C. and 250 rpm for 30 min to obtain a suspension;
[0094] The suspension was then allowed to settle at a constant temperature of 80°C for 70 hours to obtain a light phase (supernatant) and a heavy phase (heavy phase at the bottom).
[0095] iii. After the heavy phase (bottom heavy phase material) separated in step ii is subjected to reduced pressure distillation at 250° C. and −0.08 MPa (gauge pressure) to recover the solvent (the recovered solvent is a mixture of the first solvent and the second solvent B), the light liquid (recovered solvent) obtained in the upper part of the still is mixed with the light phase (supernatant liquid) obtained in the separation step ii, and heavy asphalt is obtained at the bottom of the still;
[0096] The light phase (supernatant) separated in step ii was first flashed at 180°C and atmospheric pressure to remove the second solvent B for reuse. The first solvent was then recovered and reused by vacuum distillation at 250°C and -0.08 MPa (gauge pressure). Ultra-low-ash refined asphalt was obtained at the bottom of the still. The test results of the resulting product are shown in Table 1.
[0097] Comparative Example 1:
[0098] The deashing method of coal-based asphalt comprises the following steps:
[0099] i. The first solvent and the second solvent A were uniformly mixed at a mass ratio of 0.2:1 to prepare a mixed solvent; 1 kg of coal liquefaction pitch was mixed with the mixed solvent at a mass ratio of 1:2 and fully dissolved at 150° C. for 30 minutes to obtain an extract;
[0100] The extract was then kept at a constant temperature of 140°C for 60 hours to separate and extract the first light phase (supernatant) and obtain the first heavy phase; the first heavy phase was subjected to reduced pressure distillation at 250°C and -0.08 MPa (gauge pressure) to recover the mixed solvent, thereby obtaining heavy asphalt;
[0101] ii. Cooling the supernatant obtained in step i to 100° C., adding 5% by mass of a sedimentation aid and 0.2% by mass of ethylene glycol (wherein the sedimentation aid is an aqueous solution containing 2% polyaluminum chloride) to the supernatant, and stirring at a speed of 80 r / min for 60 min to obtain a suspension;
[0102] The suspension was then kept at a constant temperature of 140°C for 48 hours to separate into a second light phase (supernatant) and a second heavy phase (heavy phase at the bottom);
[0103] iii. Recovering the mixed solvent from the second heavy phase (bottom heavy phase) obtained in step ii by vacuum distillation at 250° C. and −0.08 MPa (gauge pressure). The light liquid (recovered solvent) in the upper portion of the still is introduced into the second light phase, and the binder asphalt is obtained at the bottom of the still.
[0104] The second light phase (supernatant) obtained in step ii was subjected to vacuum distillation at 250°C and -0.08 MPa (gauge pressure) to recover the mixed solvent and reuse it. Refined asphalt was obtained from the bottom of the distillation kettle. The test results of the obtained product are shown in Table 1.
[0105] Comparative Example 2:
[0106] The deashing method of coal-based asphalt comprises the following steps:
[0107] i. The first solvent and the second solvent A were uniformly mixed in a mass ratio of 1:2 to prepare a mixed solvent; 1 kg of coal tar pitch was mixed with the mixed solvent in a mass ratio of 1:2 and fully dissolved at 150° C. for 30 minutes to obtain an extract;
[0108] The obtained extract was placed in a high temperature centrifuge and centrifuged at 100°C for 2 min with a separation factor of 1800.
[0109] Separate to obtain a first heavy phase and a first light phase, and distill the first heavy phase under reduced pressure at 250°C and -0.08 MPa (gauge pressure) to recover the mixed solvent to obtain heavy asphalt; the first light phase in the centrifuge enters step ii;
[0110] ii. placing the first light phase obtained in step i in a high-temperature centrifuge and centrifuging at 100° C. for 1.5 min with a separation factor of 1800; after the centrifugation, a second light phase (supernatant) and a second heavy phase (heavy phase at the bottom) are obtained;
[0111] iii. Recovering the mixed solvent (a mixture of the first solvent and the second solvent A) by vacuum distillation from the second heavy phase (bottom heavy phase) obtained in step ii at 250° C. and −0.08 MPa (gauge pressure). The resulting light phase (mixed solvent) is mixed with the second light phase (supernatant) obtained in step ii, and the binder asphalt is obtained at the bottom of the distillation kettle.
[0112] The second light phase (supernatant) obtained in step ii was first flashed at 160°C and atmospheric pressure to remove the second solvent A for reuse. The first solvent was then recovered and reused by reduced pressure distillation at 250°C and -0.08 MPa (gauge pressure). Refined asphalt was obtained from the bottom of the still. The test results of the resulting product are shown in Table 1.
[0113] Comparative Example 3:
[0114] 1 kg of coal liquefaction pitch and 4 kg of the first solvent were added to a stirring tank and then thoroughly mixed; the stirring tank was filled with N2 to 2.0 MPa (gauge pressure), heated to 180°C, and stirred at a stirring speed of 200 r / min for 30 minutes to obtain a mixture-I; the mixture-I was then pressurized and hot filtered, and the extract obtained by filtration was subjected to reduced pressure distillation at 250°C and -0.08 MPa (gauge pressure) to recover the first solvent, thereby obtaining 0.89 kg of an extract.
[0115] The extract and 3 kg of the second solvent A were added to a stirred tank and thoroughly mixed. The stirred tank was filled with nitrogen to 0.5 MPa (gauge pressure), heated to 120° C., and stirred at 250 r / min for 20 minutes to obtain a mixture II. The mixture II was then centrifuged at 120° C. for 2 minutes with a separation factor of 1800 to obtain a bottom heavy phase and a supernatant.
[0116] The supernatant obtained by centrifugation was distilled at 160°C and atmospheric pressure to recover the second solvent A, to obtain 0.27 kg of heavy liquefied oil; the bottom heavy phase obtained by centrifugation was distilled at 160°C and atmospheric pressure to recover the second solvent A, to obtain 0.62 kg of asphalt-like substance.
[0117] Table 1 Test results of the products obtained in each embodiment and comparative example
[0118] Note: In Table 1, Ash represents the ash content in asphalt, and QI represents the quinoline insoluble content in asphalt.
[0119] As can be seen from the results in Table 1, in each embodiment, two solvents with significantly different solubility were used to perform a secondary refining treatment on the coal-based pitch. During the primary refining process, the coal-based pitch was dissolved using a first solvent with a stronger solubility to maximize the dissolution of the pitch, thereby increasing the yield of the low-ash refined pitch. Prior to the secondary refining, the first solvent did not need to be recovered, and a second solvent with a relatively weaker solubility was directly added to achieve deep deashing, reduce residual impurities, and improve the quality of the asphalt product. A coal-based refined pitch with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1% was obtained. Compared to Example 9, the methods of Examples 1-8 include the addition of a separation step for the extract. Thus, while obtaining a coal-based refined pitch with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1%, a binder pitch with low ash and quinoline insoluble contents can also be co-produced.
[0120] Although the first solvent and the second solvent are also used for extraction and purification in Comparative Examples 1-3, the process steps and process operations used are different from those of the present invention. The quality of the obtained asphalt products is poor, and the ash content of the refined asphalt is greater than 100 ppm and the quinoline insoluble matter content is greater than 0.1%.
[0121] While various embodiments of the present invention have been described above, the above description is intended to be illustrative, not exhaustive, and not limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for deashing coal-based asphalt, characterized in that: The steps include: i. Coal-based asphalt is used as the raw material to be treated, and a first solvent is added to the mixture and fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based asphalt is (0.5-4):1; the first solvent is a coal tar fraction or a coal direct liquefaction oil fraction, and its distillation range is between 180 and 300° C. and H / C=0.6-1.0; ii. The extract obtained in step i is mixed with a second solvent in a mass ratio of 1:(1-4) and then subjected to flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coking light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, and the distillation range is between 70-160° C. and H / C=1.1-2.3; Then, the suspension is centrifuged or subjected to natural sedimentation separation to obtain a heavy phase and a light phase; iii. recovering the solvent from the heavy phase obtained in step ii to obtain heavy asphalt, and optionally mixing the recovered solvent into the light phase; The second solvent and the first solvent in the light phase are recovered separately to obtain a refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1 wt%.
2. The deashing method according to claim 1, characterized in that The steps include: i. Coal-based asphalt is used as the raw material to be treated, and a first solvent is added to the mixture and fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based asphalt is (0.5-4):1; the first solvent is a coal tar fraction or a coal direct liquefaction oil fraction, and its distillation range is between 180 and 300° C. and H / C=0.6-1.0; The obtained extract is then centrifuged or subjected to natural sedimentation separation to obtain a first heavy phase and a first light phase; the first heavy phase is then subjected to reduced pressure distillation to recover the first solvent to obtain heavy asphalt; ii. The first light phase separated in step i is mixed with a second solvent in a mass ratio of 1:(1-4) and subjected to flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coking light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, and the distillation range is between 70-160° C. and H / C=1.1-2.3; Then, the suspension is centrifuged or subjected to natural sedimentation separation to obtain a second heavy phase and a second light phase; iii. After solvent recovery from the second heavy phase separated in step ii, a binder asphalt having an ash content of less than 0.1 wt% and a quinoline insoluble content of less than 1 wt% is obtained, and the recovered solvent is optionally mixed into the second light phase; The second solvent and the first solvent in the second light phase are recovered separately to obtain a refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1 wt%.
3. The deliming method according to claim 2, characterized in that In step i, before separating the extract, a mixture of a sedimentation aid and a wetting agent and / or activated clay is added to the extract; Preferably, the sedimentation aid is an aqueous solution containing 1 to 10 wt% of a flocculant; more preferably, the flocculant is selected from one or more of polyacrylamide, polyaluminium chloride, polyaluminium sulfate, polyferric chloride and polyferric sulfate; Preferably, the wetting agent is selected from one or more of ethanol, 1-pentanol, 1-octanol, ethylene glycol and glycerol.
4. The deliming method according to claim 3, characterized in that Before separating the extract, activated clay is added to the extract, and the amount of the activated clay added is 0.1-1 wt% based on the mass of the coal-based asphalt; and / or The process conditions for adding activated clay into the extract for mixing include: a mixing temperature of 80 to 140° C. and a mixing time of 10 to 60 minutes.
5. The deliming method according to claim 3, characterized in that: Before separating the extract, a mixture formed by a sedimentation aid and a wetting agent is added to the extract and mixed; The mixing process conditions include: a mixing temperature of 80 to 140° C., stirring and mixing for 0.2 to 5 minutes at a stirring speed of 3000 to 8000 r / min, and then stirring and mixing for 30 to 180 minutes at a stirring speed of 50 to 500 r / min; The added amount of the sedimentation aid accounts for 2-10% of the mass fraction of the extract, and the added amount of the wetting agent accounts for 0.1-0.5% of the mass fraction of the extract.
6. The deliming method according to any one of claims 2 to 5, characterized in that: In step i, the process conditions of the centrifugal separation include: placing the material stream to be separated in a centrifuge, centrifuging at 80-140° C. for 0.5-10 min, and the separation factor is between 500 and 3000; and / or The process conditions of natural sedimentation include: constant temperature sedimentation at 80-180° C. for 4-48 hours.
7. The deliming method according to any one of claims 1 to 6, characterized in that The coal-based asphalt is selected from coal tar asphalt, coal tar modified asphalt or coal liquefaction asphalt; Based on the total weight of the coal-based asphalt, the coal-based asphalt has an ash content of 0.1 to 5 wt%, and / or a quinoline insoluble content of 1 to 10 wt%; In step i, the conditions for dissolving by the first solvent include: a dissolving temperature of 100 to 200° C. and a dissolving time of 15 to 60 min.
8. The deliming method according to any one of claims 1 to 7, characterized in that In step ii, the conditions of the flocculation reaction include: reaction temperature of 50-120° C., stirring speed of 80-350 r / min, and stirring time of 10-60 min.
9. The deliming method according to any one of claims 1 to 8, characterized in that In step ii, the conditions for centrifuging the suspension include: placing it in a centrifuge, centrifuging it at 50-120° C. for 0.5-10 min, and the separation factor is between 500 and 3000; and / or The process conditions for subjecting the suspension to the natural sedimentation include: constant temperature sedimentation at 50-120° C. for 6-72 hours.
10. A refined asphalt containing low ash content and low quinoline insoluble matter obtained by the deashing method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for separating liquefied heavy oil and asphalt substances from direct coal liquefaction residues
CN103254933A
Asphalt substance separated from direct coal liquefaction residues and method and application thereof
CN103275744A
Method for separating liquefied heavy oil and asphalt substrate from direct coal liquefaction residues
CN103275754A
Treatment method for direct coal liquefaction residues
CN104845652A
Preparation method of coal liquefied asphalt
CN105754630A
Cited By
Method for promoting rapid oxidation of asphalt through deep eutectic solvent cyclic extraction
CN120059783A