Preparation method for NANO silicon carbide
Through the magnetic rotating arc plasma method and quenching technology, nanometer silicon carbide is quickly prepared at low cost and low temperature, which solves the problems of high temperature, long reaction time and high cost in the existing technology, and achieves high purity and small particle size of nanometer silicon carbide. Preparation, suitable for fields such as electronic devices and solar cells.
Patent Information
- Application Number
- PCT/CN2024/074216
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-01-26
- Publication Date
- 2024-10-31
AI Technical Summary
Existing silicon carbide preparation methods have problems such as high temperature, long reaction time, high cost, and large product particle size, which limit the wide application of nanometer silicon carbide in fields such as electronic devices and solar cells.
The magnetic rotating arc plasma method is used to crack decamethylcyclopentasiloxane in hydrogen plasma and argon plasma environments, combined with rapid cooling technology, to obtain nanometer silicon carbide. The cooling rate is ≥2000K/s to ensure the small size and size of the product. High purity.
It has achieved low-cost, low-temperature and rapid preparation of nano-silicon carbide with a particle size of 20 to 500 nm and a purity of ≥95%. It is suitable for electronic devices, solar cells and other fields.
Smart Images

Figure CN2024074216_31102024_PF_FP_ABST
Abstract
Description
A preparation method of nano silicon carbide
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on April 28, 2023, with application number CN202310493744.0 and invention name “A Method for Preparing Nano-Silicon Carbide”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention relates to the technical field of silicon carbide preparation, and in particular to a method for preparing nano silicon carbide. Background Art
[0003] Silicon carbide (SiC) has many excellent properties, such as high temperature resistance, high hardness, high mechanical strength, small thermal expansion coefficient, unique optical properties and high-temperature semiconductor properties. These properties make it widely used in functional or structural components such as electronic devices, solar cells, solar water splitting, etc. In the past few decades, scientists have proposed various methods for synthesizing SiC, including carbon thermal reduction, chemical vapor deposition (CVD), electrochemical etching, chemical etching and other methods. Among them: the carbon thermal reduction method requires high temperature and long reaction time, which causes silicon carbide to sinter into large-sized particles. The particle size of silicon carbide nanoparticles obtained by the CVD process is also generally larger. The electrochemical / chemical etching method can prepare small-sized silicon carbide nanoparticles, but its relatively high cost limits its further application.
[0004] Summary of the Invention
[0005] In view of this, the object of the present invention is to provide a method for preparing nano-silicon carbide. The preparation method provided by the present invention can obtain nano-silicon carbide at a low cost.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing nano-silicon carbide, comprising the following steps:
[0008] Using decamethylcyclopentasiloxane as a silicon-carbon precursor and argon as an arc starting atmosphere gas, the silicon-carbon precursor is cracked by a magnetic rotating arc plasma method in an environment of hydrogen plasma and argon plasma, and then rapidly cooled to obtain the nano-silicon carbide;
[0009] The cooling rate of the rapid cooling is ≥2000K / s.
[0010] Preferably, the parameters of the magnetic rotating arc plasma method include: arc current of 100-3000A, and excitation current of 100-1000A.
[0011] Preferably, the feed rate of the decamethylcyclopentasiloxane is 0.9 to 900 kg / h.
[0012] Preferably, the atmosphere for generating the hydrogen plasma environment includes hydrogen, and the volume ratio of the hydrogen to argon is (0-100):1, wherein the content of hydrogen is not zero.
[0013] Preferably, the total flow rate of hydrogen and argon is 1-4000 Nm 3 / h.
[0014] Preferably, the rapid cooling includes partition water cooling or contact air cooling.
[0015] Preferably, the quenching gas used in the contact air cooling comprises argon; the flow rate of the quenching gas is 0 to 6000 Nm 3 / h, and the flow rate of quenching gas is not 0.
[0016] Preferably, the size of the nano-silicon carbide is 20 to 500 nm.
[0017] The present invention provides a method for preparing nano-silicon carbide, comprising the following steps: using decamethylcyclopentasiloxane as a silicon-carbon precursor and argon as an arc-starting atmosphere gas, cracking the silicon-carbon precursor using a magnetic rotating arc plasma method in a hydrogen plasma and argon plasma environment, and rapidly cooling the precursor to obtain the nano-silicon carbide; the rapid cooling rate is ≥2000K / s. The decamethylcyclopentasiloxane, a silicon-carbon precursor, cracks in the hydrogen plasma and argon plasma environment to produce silicon carbide gas; the rapid cooling of the silicon carbide gas ensures that small-sized nano-silicon carbide is obtained. At the same time, the molar ratio of carbon, silicon, and oxygen in decamethylcyclopentasiloxane is 2:1:1. In a hydrogen plasma environment, the oxygen converts half of the carbon into carbon monoxide, leaving the remaining carbon and silicon in a molar ratio of exactly 1:1, resulting in only silicon carbide. Furthermore, the byproduct carbon monoxide is gaseous and does not contaminate the final silicon carbide product; the carbon monoxide can be collected and reused. Even if carbon and silicon are produced, their content is extremely low, thus ensuring the purity of the final silicon carbide. Data from the examples show that the resulting nano-silicon carbide has a purity of ≥95% and a size of 20 to 500 nm. The nano-silicon carbide obtained by the preparation method provided by the present invention is small in size. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] FIG1 is an XRD spectrum of nano-silicon carbide prepared under different quenching gas flow rates;
[0019] FIG2 is a TEM image of nano-silicon carbide prepared under different quenching gas flow rates;
[0020] FIG3 is an XRD spectrum of nano-silicon carbide prepared under different average arc powers;
[0021] FIG4 is a TEM image of nano-SiC prepared under different average arc powers. DETAILED DESCRIPTION
[0022] The present invention provides a method for preparing nano-silicon carbide, comprising the following steps:
[0023] Using decamethylcyclopentasiloxane as a silicon-carbon precursor and argon as an arc starting atmosphere gas, the silicon-carbon precursor is cracked by a magnetic rotating arc plasma method in an environment of hydrogen plasma and argon plasma, and then rapidly cooled to obtain the nano-silicon carbide;
[0024] The cooling rate of the rapid cooling is ≥2000K / s.
[0025] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0026] In the present invention, the feed rate of decamethylcyclopentasiloxane is preferably 0.9 to 900 kg / h, more preferably 0.9 to 300 kg / h, and further preferably 10 to 200 kg / h.
[0027] In the present invention, the atmosphere for generating the hydrogen plasma environment includes hydrogen. In the present invention, the argon gas serves as both an arc starting atmosphere gas and an environment for generating argon plasma. In the present invention, the volume ratio of the hydrogen and argon gases is preferably (0-100):1, wherein the content of hydrogen is not 0. In the present invention, the volume ratio of the hydrogen and argon gases is more preferably 1-50:1, and further preferably 1:1. In the present invention, the total flow rate of the hydrogen and argon gases is preferably 1-4000 Nm 3 / h, more preferably 3.6 to 2000 Nm 3 / h, more preferably 100 to 1000 Nm 3 / h.
[0028] In the present invention, the parameters of the magnetic rotating arc plasma method include: an arc current of preferably 100 to 3000 A, more preferably 120 to 1000 A, and even more preferably 150 to 300 A; and an excitation current of preferably 100 to 1000 A, more preferably 400 to 800 A. In the present invention, the arc current of preferably 100 to 3000 A corresponds to an arc operating power of 10 to 10,000 kW. In the present invention, the arc production capacity of preferably 5 to 5,000 g / min.
[0029] In the present invention, the rapid cooling preferably includes partition water cooling or contact air cooling. In the present invention, the quenching gas used in the contact air cooling preferably includes argon; the flow rate of the quenching gas is preferably 0 to 6000 Nm3 / h, and the flow rate of the quenching gas is not 0, and the flow rate of the quenching gas is more preferably 2 to 6 Nm 3 / h, more preferably 4Nm 3 / h.
[0030] In the present invention, the method for preparing nano-silicon carbide is preferably carried out in a coal-to-acetylene plasma reactor with coking inhibition and online coke cleaning functions disclosed in Chinese Patent Publication No. CN110918026A.
[0031] In the present invention, decamethylcyclopentasiloxane is used as a silicon-carbon precursor and argon is used as an arc starting atmosphere gas. In an environment of hydrogen plasma and argon plasma, the silicon-carbon precursor is cracked by a magnetic rotating arc plasma method, and then rapidly cooled to obtain the nano-silicon carbide. The specific process is preferably:
[0032] Argon gas is used to replace the air in the plasma reactor, and a power supply is started under an argon atmosphere to generate plasma. Subsequently, hydrogen gas is input to convert the atmosphere into a mixed atmosphere of argon plasma and hydrogen plasma. After stable operation, the hydraulic pump is started, and the silicon-carbon precursor is sent into the plasma reactor under the drive of the carrier gas. The silicon-carbon precursor is cracked to form silicon carbide gas, which is rapidly cooled to form nano-silicon carbide and collected. In the present invention, the device used for rapid cooling preferably includes a device for quenching gas or a water-cooling device arranged on the outer wall of the plasma reactor. In the present invention, when the rapid cooling is contact air cooling, the present invention preferably allows the quenching gas to enter the plasma reactor through a quenching nozzle. In the present invention, the quenching gas is preferably in countercurrent contact with the silicon carbide gas, which is more conducive to improving the rapid cooling efficiency.
[0033] In the present invention, the size of the nano-silicon carbide is preferably 20 to 500 nm, more preferably 100 to 300 nm.
[0034] The nano silicon carbide provided by the invention has a small size.
[0035] The preparation method of nano-silicon carbide provided by the present invention is described in detail below with reference to the examples, but they should not be understood as limiting the scope of protection of the present invention.
[0036] Example 1
[0037] The Chinese patent publication number CN110918026A discloses a coal-to-acetylene plasma reactor with coking inhibition and online coke cleaning functions for preparing nano-silicon carbide.
[0038] This embodiment illustrates that the different quenching temperature gradients brought about by the quenching gas flow rate have a significant control effect on the particle size of silicon carbide.
[0039] The specific operations are:
[0040] Argon gas was introduced to replace the air in the plasma reactor. After the air was replaced, the arc was started in the argon atmosphere. The arc current was set to 150A (corresponding to an arc operating power of 20-25kW), the excitation current was 400A, and hydrogen was introduced into the plasma reactor. After the arc ran stably under the atmosphere of hydrogen and argon, a mixed atmosphere of hydrogen plasma and argon plasma was formed (the volume ratio of H2 and Ar in the mixed atmosphere of hydrogen plasma and argon plasma was 1:1, and the total flow rate was 3.6Nm 3 / h); then the silicon-carbon precursor decamethylcyclopentasiloxane is fed through a hydraulic pump (feed rate is 0.9kg / h), decamethylcyclopentasiloxane is cracked at the arc to form silicon carbide gas, the cylinder containing quenching gas argon is opened, and the quenching gas (the flow rate of quenching gas argon is 0Nm 3 / h、2Nm 3 / h、4Nm 3 / h、6Nm 3 / h) enters the plasma reactor through a quenching nozzle, cools the generated silicon carbide gas, and collects silicon carbide powder.
[0041] Figure 1 shows the XRD spectra of nano-SiC prepared at different quenching gas flow rates. As can be seen from Figure 1, there are multiple diffraction peaks at 2θ≈35.6°, 41.4°, 60.0°, 71.4°, and 75.1°, corresponding to the diffraction crystal planes of 3C-SiC at (111), (200), (220), (311), and (222), respectively, indicating that 3C-SiC is the main crystalline phase in the product. The sample has a clear amorphous SiO2 diffraction peak at 2θ≈23°, proving that part of the product has been oxidized to SiO2; the purity of the nano-SiC is about 95%.
[0042] Figure 2 is a TEM image of nano-silicon carbide prepared under different quenching gas flow rates. It can be seen from Figure 2 that SiC particles similar to three-dimensional hexagons and spherical shapes are produced. As the quenching gas flow rate increases, large particles larger than 300 nm decrease. Overall, the particle size of the prepared products is mostly 100-300 nm, and the minimum particle size is 30 nm.
[0043] Example 2
[0044] The Chinese patent publication number CN110918026A discloses a coal-to-acetylene plasma reactor with coking inhibition and online coke cleaning functions for preparing nano-silicon carbide.
[0045] This example investigates the effect of the temperature inside the plasma torch, which is affected by the arc operating power, on the silicon carbide product.
[0046] The specific operations are:
[0047] Argon gas was introduced to replace the air in the plasma reactor. After the air was replaced, the arc was started in an argon atmosphere, and the excitation current was set to 400A. By setting the arc operating current, the arc operating power was controlled to be 13-16kW, 18-24kW, 21-29kW, and 25-28kW respectively. Hydrogen was then introduced into the plasma reactor. After the arc operated stably under the atmosphere of hydrogen and argon, a mixed atmosphere of hydrogen plasma and argon plasma was formed (the volume ratio of H2 and Ar in the mixed atmosphere of hydrogen plasma and argon plasma was 1:1, and the total flow rate was 3.6Nm 3 / h), the silicon-carbon precursor decamethylcyclopentasiloxane is fed through a hydraulic pump (feed rate is 0.9kg / h), decamethylcyclopentasiloxane is cracked at the arc to form silicon carbide gas, the cylinder containing quenching argon is opened, and the quenching gas (quenching argon gas flow rate is 4Nm 3 / h) enters the plasma reactor through a quenching nozzle, cools the generated silicon carbide gas, and collects silicon carbide powder.
[0048] FIG3 is an XRD spectrum of nano-silicon carbide prepared under different arc operating powers. As can be seen from FIG3 , five characteristic peaks of 3C-SiC are obtained under different arc operating powers, confirming that 3C-SiC is the main crystalline phase in the product, but still contains a small amount of impurity SiO2 (22°); the purity of the nano-silicon carbide is 95%.
[0049] Figure 4 shows TEM images of nano-SiC prepared at different arc operating powers. It can be seen from Figure 4 that both hexagonal and spherical SiC particles are produced, and the particle size increases with increasing arc operating power. The diffraction peak intensity of the (111) crystal plane also increases with increasing arc operating power. At low power, the minimum particle size is 20 nm, and the prepared nano-SiC particles are mostly 100-200 nm in size.
[0050] Example 3
[0051] The Chinese patent publication number CN110918026A discloses a coal-to-acetylene plasma reactor with coking inhibition and online coke cleaning functions for preparing nano-silicon carbide.
[0052] This embodiment shows the application of a larger-scale plasma reactor in the preparation of silicon carbide nanoparticles.
[0053] The specific operations are:
[0054] Argon gas was introduced to replace the air in the plasma reactor. After the air was replaced, the plasma arc was started in an argon atmosphere. The arc current was set to 3000A (corresponding to an arc operating power of 6MW) and the excitation current was set to 1000A. Hydrogen was then introduced into the plasma reactor. After the arc ran stably under the atmosphere of hydrogen and argon, a mixed atmosphere of hydrogen plasma and argon plasma was formed (the volume ratio of H2 and Ar in the mixed atmosphere of hydrogen plasma and argon plasma was 1:1, and the total flow rate was 4000Nm 3 / h); the silicon-carbon precursor decamethylcyclopentasiloxane is fed into the plasma reactor through a hydraulic pump at a feed rate of 300kg / h. The decamethylcyclopentasiloxane is cracked at the arc to form silicon carbide gas, and a large flow of quenching gas (the flow rate of the quenching gas argon is 6000Nm 3 / h) enters the plasma reactor through a quenching nozzle, cools the generated silicon carbide gas, and collects silicon carbide powder.
[0055] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing nano-silicon carbide, characterized in that: The following steps are involved: Using decamethylcyclopentasiloxane as a silicon-carbon precursor and argon as an arc-starting atmosphere gas, the silicon-carbon precursor is cracked by a magnetic rotating arc plasma method in an environment of hydrogen plasma and argon plasma, and then rapidly cooled to obtain the nano-silicon carbide; The cooling rate of the rapid cooling is ≥2000K / s.
2. The preparation method according to claim 1, characterized in that: The parameters of the magnetic rotating arc plasma method include: the arc current is 100-3000A, and the excitation current is 100-1000A.
3. The preparation method according to claim 1, characterized in that: The feed rate of the decamethylcyclopentasiloxane is 0.9-900 kg / h.
4. The preparation method according to claim 3, characterized in that: The feed rate of the decamethylcyclopentasiloxane is 0.9-300 kg / h.
5. The preparation method according to claim 1, characterized in that: The atmosphere for generating the hydrogen plasma environment includes hydrogen gas, and the volume ratio of the hydrogen gas to the argon gas is (0-100):1, wherein the content of the hydrogen gas is not zero.
6. The preparation method according to claim 5, characterized in that: The volume ratio of the hydrogen gas to the argon gas is 1:
1.
7. The preparation method according to claim 5, characterized in that: The total flow rate of hydrogen and argon is 1-4000 Nm 3 / h.
8. The preparation method according to claim 7, characterized in that: The total flow rate of hydrogen and argon is 3.6-2000 Nm 3 / h.
9. The preparation method according to claim 1, characterized in that: The rapid cooling includes partition water cooling or contact air cooling.
10. The preparation method according to claim 9, characterized in that: The quenching gas used in the contact air cooling includes argon; the flow rate of the quenching gas is 0-6000Nm 3 / h, and the flow rate of quenching gas is not 0.
11. The preparation method according to any one of claims 1 to 10, characterized in that: The size of the nano silicon carbide is 20-500nm.
Citation Information
Patent Citations
Method for preparing spherical nanometer silicon by virtue of thermal plasma method
CN106698437A
Silicon carbide and preparation method thereof
CN110921670A
Method for preparing nano silicon spheres and nano silicon wires by using magnetic rotating arc plasmas
CN112591755A
Preparation method of nano silicon carbide
CN116573646A