V-containing cold-rolled dual-phase steel having high strength-ductility product and production method therefor
By optimizing the chemical composition and production process, V-containing high-strength plastic cold-rolled dual-phase steel is prepared, which solves the problem of insufficient plasticity of dual-phase steel, significantly improves its tensile strength and formability, and is suitable for high-strength automotive parts.
Patent Information
- Application Number
- PCT/CN2024/082117
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-31
AI Technical Summary
Existing dual-phase steel has deficiencies in improving plasticity and is difficult to meet the needs of lightweight and high-strength automotive applications, especially in terms of the formability of cold-rolled steel plates.
By optimizing the chemical composition and production process, V-containing high-strength plastic cold-rolled dual-phase steel is prepared. The specific steps include composition design, smelting, forging, hot rolling, pickling, cold rolling and annealing, and the V content is controlled at 0.15%-0.17%. , with grain refinement and precipitation strengthening, combined with the solid solution and precipitation of C, Si, Mn, Mo, and Al elements, to form the microstructure of ferrite and martensite.
The tensile strength, yield strength and elongation after fracture of dual-phase steel are significantly improved, and the strong plastic product property reaches 14.5-22.0GPa·%. It is suitable for high-strength automotive parts and achieves better combination of formability and mechanical properties. .
Smart Images

Figure CN2024082117_31102024_PF_FP_ABST
Abstract
Description
A V-containing high-strength and high-plasticity cold-rolled dual-phase steel and its production method Technical Field
[0001] The present invention relates to the technical field of alloy production, in particular to a V-containing high-strength and high-ductility cold-rolled dual-phase steel and a production method thereof. Background Art
[0002] Steel is one of the primary raw materials used in automobile production. High-strength steel is gaining increasing importance in the pursuit of lightweight vehicles. Currently, high-strength steel is the preferred material for lightweighting in developed countries, with mainstream sedans already using over 60% of it. The European "Ultra-Light Vehicle Engineering" design plan already requires over 70% of high-strength steel. As lightweighting becomes a growing trend, high-strength steel is poised for growth. Traditional high-strength steels primarily include high-strength interstitial-free steel (HSS-IF), bake-hardened steel (BH), carbon-manganese steel (C-Mn), high-strength low-alloy steel (HSLA), and ferrite-bainite steel (FB). These traditional high-strength steels are still in production and widely used in automotive body structures and other engineering applications. In contrast, high-strength steels have more complex microstructures and offer a good balance of strength and ductility. Generally speaking, AHSS steels can be divided into three categories based on their mechanical properties and alloy type. The first generation of AHSS steels is ferrite-based, with a strength-ductility product below 15 GPa%. These steels primarily include dual-phase steels (DP), multi-phase steels (CP), transformation-induced plasticity steels (TRIP), ferritic-bainite steels (FB / SF), martensitic steels (MS / PHS), and boron steels (HF). These steels exhibit very high strength and moderate ductility. The second generation of AHSS steels is austenite-based, with a strength-ductility product exceeding 50 GPa%. These steels primarily include twin-induced plasticity steels (TWIP), shear-band-strengthened steels (SIP), and lightweight steels with induced plasticity (L-IP). In addition to very high strength, these steels also exhibit excellent ductility. The first and second generations of the AHSS family are already capable of meeting the basic structural performance requirements of most engineering materials. For example, in automotive applications, DP and TRIP steels are the primary materials. Due to their high strength and very high energy absorption capacity, they are widely used in pillars, B-pillars, crossbeams, and door beams.
[0003] With the continuous development of the automotive industry, energy conservation and emission reduction are becoming increasingly challenging. Lightweighting vehicles is one of the effective measures to address these challenges. Improving vehicle body strength can achieve lightweighting by reducing the thickness of vehicle body steel sheets. As the concept of lightweighting continues to deepen, component design is becoming increasingly complex, and the forming problem of cold-rolled steel sheet needs to be effectively addressed. This places higher demands on the performance of duplex steel, primarily regarding its strength and plasticity—the product of strength and plasticity. While ensuring sufficient strength, improving the plasticity of duplex steel can effectively enhance its formability, maximizing the application of high-strength duplex steel.
[0004] In the prior art, Chinese patent CN114107818A discloses a 1000 MPa-grade hot-dip galvanized duplex steel and its production method. The chemical composition and mass fractions of the duplex steel in this patent are as follows: C: 0.08%-0.12%, Si: 0.25%-0.55%, Mn: 2.20%-2.60%, Mo: 0.10%-0.30%, Nb: 0.02%-0.06%, Al: 0.02%-0.06%, with the remainder being Fe and unavoidable impurities. By controlling the chemical composition and production process, the duplex steel produced in this patent achieves a tensile strength of 1015 MPa-1135 MPa and an elongation of 11.5%-13.5%. Despite its high strength, its plasticity does not reach the level of high-strength-ductility-product duplex steels.
[0005] For example, Chinese patent CN111218620A discloses a high-yield ratio cold-rolled duplex steel and its manufacturing method. The chemical composition and mass fractions of the duplex steel in this patent are as follows: C: 0.05%-0.08%, Si: 0.1%-0.6%, Mn: 0.9%-1.2%, Ti: 0.03%-0.06%, Nb: 0.03%-0.06%, Al: 0.015%-0.045%, with the remainder being Fe and unavoidable impurities. By controlling the chemical composition and production process, the duplex steel produced in this patent achieves a yield strength of 500-650 MPa, a tensile strength ≥660 MPa, and an elongation ≥15%. While it exhibits good plasticity, its strength is insufficient.
[0006] Summary of the Invention
[0007] The purpose of the present invention is to provide a V-containing high-strength and high-plasticity cold-rolled dual-phase steel and a production method thereof, which, on the basis of achieving high strength, improves the plasticity of the dual-phase steel, thereby effectively improving the forming performance of the dual-phase steel, and maximizing the application of high-strength dual-phase steel.
[0008] The present invention provides a V-containing, high-strength, high-ductility cold-rolled dual-phase steel, comprising C, Si, Mn, V, Mo, Al, and Fe. The mass percentages of these components are: C: 0.19%-0.21%, Si: 0.25%-0.27%, Mn: 3.1%-3.3%, V: 0.15%-0.17%, Mo: 0.18%-0.2%, Al: 0.05%-0.07%, with the remainder being Fe and impurity elements.
[0009] Among them, C is a solid solution strengthening element and is the guarantee for the material to obtain high strength; Si and Mn can provide solid solution strengthening and improve the hardenability of austenite; Al can improve the oxidation and welding problems caused by excessive Si; Mo and V can both achieve the purpose of grain refinement and precipitation strengthening, among which the strengthening purpose of V is more significant. At the same time, a low V content will lead to a weakened strengthening effect, while a high V content will lead to an increase in the size of the precipitated phase and increase the cost. Therefore, in the present invention, the V content is controlled at 0.15%-0.17%.
[0010] The present invention provides a production method for V-containing high-strength and high-ductility cold-rolled dual-phase steel, which includes step one, component design; step two, smelting; step three, forging; step four, hot rolling; step five, pickling; step six, cold rolling; and step seven, annealing.
[0011] In step 1, according to the chemical composition and proportion of the above-mentioned duplex steel, the raw materials of the alloy components, iron ore, quicklime, ferromolybdenum, vanadium stone, aluminum oxide, iron-silicon alloy, and iron-manganese alloy, are placed in an oxidizing atmosphere furnace for melting and smelting to obtain molten steel, which is then transferred to a reducing atmosphere furnace for refining to obtain refined molten steel, and the molten steel is continuously cast to obtain steel billets;
[0012] In step 2, the steel billet obtained in step 1 is placed in a walking beam furnace and heated at 1220-1280°C for 2-3 hours to dissolve all the elements C, Si, Mn, V, Mo, and Al;
[0013] In step 3, the steel billet after solid solution treatment in step 2 is forged at a forging temperature of 1150-1200° C. to obtain a forged billet;
[0014] In step 4, the forging blank obtained in step 3 is heated to 1210-1270° C. and kept at this temperature for 2-3 hours, wherein the starting rolling temperature is 1100-1200° C. and the finishing rolling temperature is 850-950° C. to obtain a hot-rolled steel strip;
[0015] In step 5, the hot-rolled steel strip obtained in step 4 is pickled at an acid solution temperature of 75-85° C. and a pickling speed of 80-100 m / min;
[0016] In step 6, the steel strip after pickling in step 5 is cold rolled with a reduction ratio of 40% to 60%, and the thickness of the cold rolled sheet after cold rolling is 1.8 to 1.9 mm;
[0017] In step seven, the cold-rolled sheet obtained in step six is annealed. The phase transition points of the steel sheet with this composition are measured by a Gleeble 3800 thermal simulator, Ac1 = 697°C and Ac3 = 819°C. The annealing temperature is set to 715-755°C, and the temperature is kept for 8-12 minutes. The sheet is then cooled by oil quenching at a temperature of 20-50°C to obtain the dual-phase steel.
[0018] The V-containing high-strength and high-ductility cold-rolled dual-phase steel obtained by the above method has a matrix structure of ferrite and martensite, wherein the ferrite grain size is 0.98-1.70μm, the ferrite volume fraction is 45%-82%, and a large number of nanoparticles are distributed on the ferrite matrix, and the size is basically below 20nm.
[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0020] (1) The high-strength and high-ductility cold-rolled dual-phase steel of the present invention adopts a reasonable composition design. Adding a sufficient amount of C (0.19%-0.21%) can ensure sufficient yield and tensile strength; adding a certain amount of Si (0.25%-0.27%) and Mn (3.1%-3.3%) can not only promote the formation of dual-phase structure but also improve the hardenability of austenite; adding a certain amount of Al (0.05%-0.07%) can improve the oxidation and welding problems caused by excessive Si; adding a certain amount of V (0.15%-0.17%) and Mo (0.18%-0.2%) can simultaneously play a role in grain refinement and precipitation strengthening, among which the strengthening purpose of V is more significant. At the same time, a low V content will lead to a weakened strengthening effect, and a high V content will lead to an increase in the size of the precipitated phase and increase the cost. Therefore, the V content in the present invention is controlled at 0.15%-0.17%.
[0021] (2) In the production process of the high-strength and high-ductility cold-rolled dual-phase steel of the present invention, appropriate hot rolling, cold rolling and annealing process parameters are used. The purpose of hot rolling and cold rolling is to obtain a finer-grained original bainite structure, while the purpose of annealing is to obtain a typical dual-phase steel structure. Among them, the cold rolling reduction rate is controlled at 40%-60% in order to further refine the grains of the original bainite structure, and the annealing time is maintained at 8-12 minutes in order to avoid grain coarsening while obtaining a dual-phase structure. The process flow and process parameters can be used to prepare ultrafine-grained dual-phase steel, whose ferrite grain size is 0.98-1.70μm, which can obtain sufficiently fine grains and maximize the mechanical properties of the cold-rolled dual-phase steel.
[0022] (3) The high-strength-ductility cold-rolled dual-phase steel obtained by the present invention has a tensile strength of 1008-1484 MPa, a yield strength of 518-778 MPa, an elongation after fracture of 9.8%-21.84%, and a strength-ductility product of 14.5-22.0 GPa·%. This material has excellent strength-shaping and shape-matching properties, and can therefore be used as an excellent automotive component. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] FIG1 is a graph showing engineering stress-strain curves of high-strength-ductility cold-rolled dual-phase steels prepared in Examples 1-3 of the present invention;
[0024] FIG2 is a thermal expansion curve of the high-strength-ductility cold-rolled dual-phase steel prepared in Examples 1-3 of the present invention;
[0025] FIG3 : Scanning electron microscope photograph (SEM) of the high strength-ductility cold-rolled dual-phase steel prepared in Examples 1-3 of the present invention. DETAILED DESCRIPTION
[0026] To make the objectives, technical solutions and advantages of the present invention more clear, the following will be described in detail with reference to various embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0027] The professional terms used below have the same meanings as those generally understood by those skilled in the art. Various raw materials, reagents, instruments and equipment used in the present invention can be purchased on the market or prepared by existing methods.
[0028] Example 1
[0029] A method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel comprises the following steps:
[0030] Step 1: According to the chemical composition and proportions in Table 1 below, iron ore, quicklime, ferromolybdenum, vanadium stone, aluminum oxide, iron-silicon alloy, and iron-manganese alloy are placed in an oxidizing atmosphere furnace for melting and smelting to obtain molten steel, which is then transferred to a reducing atmosphere furnace for refining to obtain refined molten steel, and the molten steel is continuously cast to obtain steel billets;
[0031] Step 2: The steel billet obtained in step 1 is placed in a walking beam furnace and heated at 1220-1280°C for 2-3 hours to dissolve all the elements C, Si, Mn, V, Mo, and Al;
[0032] Step 3: Forging the steel billet after solid solution treatment in step 2 at a forging temperature of 1150-1200° C. to obtain a forged billet;
[0033] Step 4: heating the forging blank obtained in step 3 to 1210-1270° C. and holding the temperature for 2-3 hours, wherein the starting rolling temperature is 1100-1200° C. and the finishing rolling temperature is 850-950° C. to obtain a hot-rolled steel strip;
[0034] Step 5: pickling the hot-rolled steel strip obtained in step 4, with the acid solution temperature being 75-85° C. and the pickling speed being 80-100 m / min;
[0035] In step 6, the steel strip after pickling in step 5 is cold rolled with a reduction rate of 60%, and the thickness of the cold rolled sheet after cold rolling is 1.8-1.9 mm;
[0036] In step seven, the cold-rolled sheet obtained in step six is annealed at 715° C. for 12 minutes and then cooled by oil quenching at a temperature of 20-50° C. to obtain the dual-phase steel.
[0037] Example 2
[0038] A method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel comprises the following steps:
[0039] Step 1: According to the chemical composition and proportions in Table 1 below, iron ore, quicklime, ferromolybdenum, vanadium stone, aluminum oxide, iron-silicon alloy, and iron-manganese alloy are placed in an oxidizing atmosphere furnace for melting and smelting to obtain molten steel, which is then transferred to a reducing atmosphere furnace for refining to obtain refined molten steel, and the molten steel is continuously cast to obtain steel billets;
[0040] Step 2: Place the steel billet obtained in step 1 in a walking beam furnace and heat it at 1220-1280°C for 2-3 hours to dissolve all the elements C, Si, Mn, V, Mo, and Al;
[0041] Step 3: Forging the steel billet after solid solution treatment in step 2 at a forging temperature of 1150-1200° C. to obtain a forged billet;
[0042] Step 4: heating the forging blank obtained in step 3 to 1210-1270° C. and holding the temperature for 2-3 hours, wherein the starting rolling temperature is 1100-1200° C. and the finishing rolling temperature is 850-950° C. to obtain a hot-rolled steel strip;
[0043] Step 5: pickling the hot-rolled steel strip obtained in step 4, with the acid solution temperature being 75-85° C. and the pickling speed being 80-100 m / min;
[0044] In step 6, the steel strip after pickling in step 5 is cold rolled with a reduction ratio of 50%, and the thickness of the cold rolled sheet after cold rolling is 1.8-1.9 mm;
[0045] In step seven, the cold-rolled sheet obtained in step six is annealed at 735° C. for 10 minutes and then cooled by oil quenching at a temperature of 20-50° C. to obtain the dual-phase steel.
[0046] Example 3
[0047] A method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel comprises the following steps:
[0048] Step 1: According to the chemical composition and proportions in Table 1 below, iron ore, quicklime, ferromolybdenum, vanadium stone, aluminum oxide, iron-silicon alloy, and iron-manganese alloy are placed in an oxidizing atmosphere furnace for melting and smelting to obtain molten steel, which is then transferred to a reducing atmosphere furnace for refining to obtain refined molten steel, and the molten steel is continuously cast to obtain steel billets;
[0049] Step 2: The steel billet obtained in step 1 is placed in a walking beam furnace and heated at 1220-1280°C for 2-3 hours to dissolve all the elements C, Si, Mn, V, Mo, and Al;
[0050] Step 3: Forging the steel billet after solid solution treatment in step 2 at a forging temperature of 1150-1200° C. to obtain a forged billet;
[0051] Step 4: heating the forging blank obtained in step 3 to 1210-1270° C. and holding the temperature for 2-3 hours, wherein the starting rolling temperature is 1100-1200° C. and the finishing rolling temperature is 850-950° C. to obtain a hot-rolled steel strip;
[0052] Step 5: pickling the hot-rolled steel strip obtained in step 4, with the acid solution temperature being 75-85° C. and the pickling speed being 80-100 m / min;
[0053] In step 6, the steel strip after pickling in step 5 is cold rolled with a reduction ratio of 40%, and the thickness of the cold rolled sheet after cold rolling is 1.8-1.9 mm;
[0054] In step seven, the cold-rolled sheet obtained in step six is annealed at 755° C. for 8 minutes and then cooled by oil quenching at a temperature of 20-50° C. to obtain the dual-phase steel.
[0055] Table 1 is a list of chemical components of the above embodiments of the present invention;
[0056] Table 2 shows the cold rolling and annealing process parameters of the above embodiments of the present invention;
[0057] Table 3 shows the microstructure and mechanical properties of the dual-phase steel prepared in the above embodiments of the present invention.
[0058] Table 1 Chemical composition of Examples 1 to 3
[0059] Table 2 Cold rolling and annealing process parameters of Examples 1 to 3
[0060] The mechanical properties of the dual-phase steels prepared in Examples 1 to 3 were tested respectively, and the test results are shown in Table 3.
[0061] Table 3 Microstructure and mechanical properties of dual-phase steel prepared in Examples 1 to 3
[0062] As can be seen from Tables 1 to 3, the present invention can be used to prepare high-strength-ductility cold-rolled dual-phase steel plates having excellent mechanical properties, including a tensile strength of 1484 MPa, a yield strength of 778 MPa, a yield strength ratio of 52% to 77%, an elongation after fracture of 9.8% to 21.84%, and a strength-ductility product of 14.5 to 22.0 GPa·%. Furthermore, the steel plates have a suitable microstructure, including a ferrite volume fraction of 45% to 82% and a ferrite grain size of 0.98 to 1.70 μm.
[0063] Figure 1 is an engineering stress-strain curve of the high-strength-ductility cold-rolled dual-phase steel prepared in Examples 1-3 of the present invention. It can be seen that as the volume fraction of ferrite decreases, the yield strength of each embodiment first decreases and then increases, the tensile strength continues to increase, the yield strength ratio also first decreases and then increases, the elongation after fracture continues to decrease, and the strength-ductility product also decreases. Among them, the tensile strength and elongation after fracture are most affected by the change in the volume fraction of ferrite. When the volume fraction of ferrite decreases from 82% to 45%, the tensile strength increases by 476MPa, with a change rate of 47.2%; the elongation after fracture decreases by 12.04, with a change rate of 55.1%. Among the three groups of embodiments, when the volume fraction of ferrite is 82%, its strength-ductility product is the highest, at 22GPa·%.
[0064] Figure 2 shows the thermal expansion curves of the high-strength-ductility cold-rolled dual-phase steels prepared in Examples 1-3 of the present invention. It can be seen that the phase transformation points for the three examples under this alloy composition are Ac1 = 697°C, Ac3 = 819°C, and Ms = 380°C. The dual-phase steel undergoes an austenitic transformation when heated above 697°C, which ends at 819°C, transforming to a fully austenitic structure. Upon rapid cooling to 380°C, the martensitic transformation begins.
[0065] Figure 3 shows SEM images of high-strength-ductility cold-rolled dual-phase steels prepared in Examples 1-3 of the present invention. (a) shows Example 1, (b) shows Example 2, and (c) shows Example 3. As the ferrite volume fraction increases, the ferrite grain size decreases, and the size and density of the second phase precipitated in the ferrite matrix also decrease. Specifically, as the ferrite volume fraction decreases from 82% to 45%, the ferrite grain size decreases by 0.72 μm, a rate of change of 42.3%.
[0066] In summary, the high-strength-ductility cold-rolled duplex steel produced by the present invention exhibits a typical duplex steel structure, with fine grains, a low yield-to-tensile ratio, and a high strength-ductility product. The duplex steel produced by the present invention enables the manufacture and engineering application of a new generation of high-strength-ductility cold-rolled duplex steel.
[0067] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A V-containing high-strength and high-ductility cold-rolled dual-phase steel, characterized in that: The dual-phase steel includes the following components in weight percentage: C: 0.19%-0.21%, Si: 0.25%-0.27%, Mn: 3.1%-3.3%, V: 0.15%-0.17%, Mo: 0.18%-0.2%, Al: 0.05%-0.07%, and the balance is Fe and impurity elements.
2. The V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 1, characterized in that: The dual-phase steel includes the following components in weight percentage: C: 0.194%, Si: 0.264%, Mn: 3.234%, V: 0.169%, Mo: 0.198%, Al: 0.06%, and the balance is Fe and impurity elements.
3. The method for preparing a V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 1, characterized in that: The steps include: Step 1, composition design: according to the chemical composition and proportion described in claim 1, the raw materials of the alloy components are placed in an oxidizing atmosphere furnace for melting and smelting to obtain molten steel, and then transferred to a reducing atmosphere furnace for refining to obtain refined molten steel, and the molten steel is continuously cast to obtain a steel billet; Step 2, smelting: placing the steel billet obtained in step 1 in a heating furnace and heating it to dissolve all the elements C, Si, Mn, V, Mo and Al; Step 3, forging: forging the steel billet after solid solution in step 2 to obtain a forged billet; Step 4, hot rolling: rolling the forged billet obtained in step 3 under a heated state to obtain a hot-rolled steel strip; Step 5, pickling: pickling the hot-rolled steel strip obtained in step 4; Step 6, cold rolling: cold rolling the steel strip after pickling in step 5 to obtain a cold-rolled sheet; Step seven, annealing: annealing the cold-rolled sheet obtained in step six, setting the annealing temperature to 715-755° C., keeping the temperature for 8-12 minutes, and then cooling, the cooling method is oil quenching, the oil quenching temperature is 20-50° C., to obtain the dual-phase steel.
4. The method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 3, characterized in that: The heating in step 2 is carried out at 1220-1280° C. for 2-3 hours.
5. The method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 3, characterized in that: The forging temperature in step 3 is 1150-1200°C.
6. The method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 3, characterized in that: In step 4, the forging billet is rolled in a heated state, specifically: the forging billet is heated to 1210-1270°C and kept warm for 2-3h, wherein the starting rolling temperature is 1100-1200°C and the finishing rolling temperature is 850-950°C.
7. The method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 3, characterized in that: In step 5, the temperature of the acid solution is 75-85° C., and the pickling speed is 80-100 m / min.
8. The method for preparing V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 3, characterized in that: The cold rolling reduction rate in step 6 is 40%-60%, and the thickness of the cold-rolled plate after cold rolling is 1.8-1.9 mm.
9. The method for producing V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 3, characterized in that: The matrix structure of the final dual-phase steel is ferrite and martensite, wherein the ferrite grain size is 0.98-1.70 μm, the ferrite volume fraction is 45%-82%, and nanoparticles with a size of ≤20 nm are distributed on the ferrite matrix.
10. The method for producing V-containing high-strength and high-ductility cold-rolled dual-phase steel according to claim 3, characterized in that: The final obtained dual-phase steel has good strength-plasticity combination energy, with a tensile strength of 1008-1484MPa, a yield strength of 518-778MPa, an elongation after fracture of 9.8%-21.84%, and a strength-plasticity product of 14.5-22.0GPa·%.
Citation Information
Patent Citations
Low carbon cold rolling ultra-high strength dual-phase steel and preparation method thereof
CN107761007A
780 MPa-grade hot-rolled dual-phase steel with excellent hole expanding performance and preparation method of 780 MPa-grade hot-rolled dual-phase steel
CN113005367A
Deep-cold-rolled steel plate with high product of strength and elongation and preparation method
CN113186461A
DP980 cold-rolled dual-phase steel with high product of strength and elongation and low yield ratio and production method thereof
CN114606449A
V-containing cold-rolled dual-phase steel with high product of strength and elongation and production method thereof
CN116574971A
Cited By
Anti-fatigue ultra-fine grain dual-phase steel based on phase interface alloy element segregation and manufacturing process of anti-fatigue ultra-fine grain dual-phase steel
CN119876777A