Polyamide resin, and polymerization method therefor and use thereof
By using polyamide resin polymerized from monomers such as 1,4-cyclohexanedicarboxylic acid, 1,10-decanediamine and 1,12-dodecanediamine, and controlling the trans structure ratio, the problem of traditional materials is solved. The problem of loss of transparency under high temperature has achieved high light transmittance stability of translucent LED lamp beads.
Patent Information
- Application Number
- PCT/CN2024/082157
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-31
AI Technical Summary
It is difficult for existing materials to maintain the transparency of translucent LED lamp beads under high temperature conditions. Traditional PPA materials are prone to recrystallization after SMT packaging, resulting in a loss of transparency properties and unable to meet the needs of the translucent LED field.
Using polyamide resin polymerized from monomers such as 1,4-cyclohexanedicarboxylic acid, 1,10-decanediamine and 1,12-dodecanediamine, and controlling the trans structure ratio and polymerization conditions, we developed A polyamide resin that is resistant to high temperatures, has high initial transmittance and does not recrystallize after SMT.
It achieves the polyamide resin to maintain high transparency at high temperatures, avoids recrystallization, meets the needs of the translucent LED field, and provides high initial and post-SMT light transmittance stability.
Smart Images

Figure PCTCN2024082157-FTAPPB-I100001 
Figure PCTCN2024082157-FTAPPB-I100002 
Figure PCTCN2024082157-FTAPPB-I100003
Abstract
Description
A polyamide resin and its polymerization method and application Technical Field
[0001] The present invention relates to the technical field of polymer materials, in particular to a polyamide resin and a polymerization method and application thereof. Background Art
[0002] Compared to semi-aromatic heat-resistant polyamides derived from terephthalic acid or isophthalic acid, heat-resistant polyamides derived from 1,4-cyclohexanedicarboxylic acid monomers lack benzene rings in their molecular structure and exhibit a weaker electron-withdrawing effect. Therefore, heat-resistant polyamides derived from 1,4-cyclohexanedicarboxylic acid monomers are less likely to acquire electrons during long-term UV aging, resulting in a more stable molecular structure and improved UV aging resistance.
[0003] As people's living standards improve, the demand for LED lamp beads increases, and translucent LED lamp beads have gradually emerged. They can be used in high-end fields such as outdoor transparent display screens, shopping malls, and counter display screens, and have high added value. This type of product requires not only that the material has high temperature resistance, but also that it still has good light transmittance after SMT (infrared reflow soldering) packaging. However, traditional PPA materials are difficult to achieve transparency; even through structural adjustments to achieve transparency in the initial state of the resin, recrystallization will occur during subsequent SMT packaging, the molecular chains will rearrange, the molecular chain regularity will increase, the crystallinity will increase, and the transparent properties will be lost, similar to the situation of PCT materials. There are currently no suitable materials on the market to meet the needs of the translucent LED field.
[0004] Therefore, it is necessary to develop a polyamide resin matrix with high temperature resistance and high transparency after SMT to meet the needs of the translucent LED field.
[0005] Summary of the Invention
[0006] The object of the present invention is to provide a polyamide resin which is resistant to high temperatures, has high initial light transmittance, and does not undergo recrystallization after SMT treatment, as well as a polymerization method and application thereof.
[0007] The present invention is achieved through the following technical solutions:
[0008] A polyamide resin, characterized in that, in terms of molar percentage, it comprises the following repeating units:
[0009] Diacid unit: 1,4-cyclohexanedicarboxylic acid;
[0010] The diamine units include 1,10-decanediamine and 1,12-dodecanediamine, wherein the amount of 1,10-decanediamine accounts for 76-82% of the total diamine content.
[0011] Preferably, the amount of 1,10-decanediamine in the diamine is 78-80%.
[0012] In the polyamide resin, the trans structure accounts for 81-85% of the total mass fraction. The testing method involves dissolving 5 mg of the polyamide resin in 10 mg of deuterated trifluoroacetic acid and performing a proton nuclear magnetic resonance (NMR) spectrum on the sample using a Bruker DPX400 nuclear magnetic resonance (NMR) instrument. In the proton nuclear magnetic resonance (NMR) spectrum, the cis structure peaks at 1.96 ppm, and the trans structure peaks at 1.83 ppm. The trans structure ratio of the resin is determined by NMR integration of these two peaks.
[0013] The polyamide resin has a melting point range of 321-334°C. Referring to ASTM D3418-2003, Standard Test Method for Transition Temperatures of Polymers By Differential Scanning Calorimetry, the specific testing method is as follows: the melting point of the sample is tested using a Perkin Elmer Dimond DSC analyzer in a nitrogen atmosphere at a flow rate of 50 mL / min. During the test, the temperature is first raised to 350°C at a rate of 20°C / min, held at 350°C for 2 minutes to remove the thermal history of the resin, then cooled to 50°C at a rate of 20°C / min, held at 50°C for 2 minutes, and then raised to 350°C at a rate of 20°C / min. The endothermic peak temperature at this point is defined as the melting point (T).
[0014] The relative viscosity of the polyamide resin is in the range of 1.8-2.8. The test method is to refer to GB12006.1-89 and measure the relative viscosity of the polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
[0015] The polyamide resin polymerization method of the present invention comprises the following steps: adding reaction monomers, benzoic acid, sodium hypophosphite and deionized water into a pressure autoclave, wherein the amount of benzoic acid is 1.5-3.0% of the amount of the reaction monomers, the weight of sodium hypophosphite is 0.05-0.15% of the weight of other materials except deionized water, and the weight of deionized water is 25-35% of the total weight of the materials; vacuuming and filling with inert gas (which may be high-purity nitrogen) as a protective gas, heating to 215-225° C. within 1.5-2.5 hours, and then reacting within the temperature range for 0.5-1.5 hours; then continuing the reaction at 225-235° C. and a pressure of 2.0-2.4 MPa for 1-3 hours, removing water formed during the reaction, discharging the materials after the reaction is completed, and vacuum drying the prepolymer to obtain a prepolymer product, and subjecting the prepolymer product to solid-phase viscosity-enhancing for 8-12 hours under the conditions of 240-260° C. and a pressure of 45-55 Pa to obtain the polyamide resin.
[0016] The polyamide resin of the present invention is used to prepare translucent LED-related components, such as LED lamp brackets.
[0017] The present invention has the following beneficial effects
[0018] Experiments have shown that the cis / trans structure of the polyamide resin originates from 1,4-cyclohexanedicarboxylic acid, which constitutes the diacid unit of the polyamide resin of the present invention. By controlling the molar content of each unit in the polyamide, it was unexpectedly discovered that a specific trans structure ratio can be obtained (research has found that the trans structure ratio of the polyamide resin in which 1,4-cyclohexanedicarboxylic acid constitutes the diacid unit is related to the structure and ratio of the diamine monomer. This may be because the longer the diamine monomer molecular chain, the higher the stability of the trans structure, and therefore the higher the proportion of the trans structure). This destroys the regularity of the molecular chain, resulting in not only a high initial transmittance, but also no recrystallization after SMT treatment, and still maintaining a high transmittance. DETAILED DESCRIPTION
[0019] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those skilled in the art, several variations and improvements can be made without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.
[0020] 1,4-Cyclohexanedicarboxylic acid: purity 98%, SKY CHDA, purchased from SK Chemicals;
[0021] 1,10-Decanediamine: purity 97%, D100615, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0022] 1,12-Dodecanediamine: purity 98%, D106441, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0023] 1,6-Hexanediamine: purity 99%, H103910, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0024] 1,14-Tetradecanediamine: purity 95%, SY250668, purchased from Shanghai Shaoyuan Reagent Co., Ltd.;
[0025] Benzoic acid: purity 99.5%, 242381, purchased from Sigma-Aldrich;
[0026] Sodium hypophosphite: purity 98%, S475696, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0027] The preparation method of the polyamide resin of the embodiment and comparative example is as follows: the amount of the benzoic acid substance is 1.5% of the amount of the reactive monomer substance, the weight of the sodium hypophosphite is 0.10% of the weight of the other materials except the deionized water, and the weight of the deionized water is 30% of the total weight of the materials; the autoclave is evacuated and filled with high-purity nitrogen as a protective gas, the temperature is raised to 220° C. within about 2 hours, and then the reaction is carried out within this temperature range for 1 hour; the reaction is then continued at 230° C. and a pressure of 2.2 MPa for 2 hours, and the water formed during the reaction is removed. After the reaction is completed, the material is discharged, and the prepolymer is vacuum dried to obtain a prepolymer product. The prepolymer product is solid-phase thickened at 250° C. and a pressure of 50 Pa for 8-12 hours to obtain a polyamide resin.
[0028] Various test methods:
[0029] (1) Polyamide relative viscosity test method: refer to GB12006.1-89, polyamide viscosity number determination method; the specific test method is: measure the relative viscosity of polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
[0030] (2) Polyamide resin melting point test method: refer to ASTM D3418-2003, Standard Test Method for Transition Temperatures of Polymers By Differential Scanning Calorimetry; the specific test method is: use a Perkin Elmer Dimond DSC analyzer to test the melting point of the sample; nitrogen atmosphere, flow rate is 50mL / min; during the test, first heat to 350℃ at 20℃ / min, hold at 350℃ for 2min to remove the thermal history of the resin, then cool to 50℃ at 20℃ / min, hold at 50℃ for 2min, and then heat to 350℃ at 20℃ / min, and set the endothermic peak temperature at this time as the T melting point.
[0031] (3) Polyamide cis-trans ratio test method: 5 mg of polyamide resin was dissolved in 10 mg of deuterated trifluoroacetic acid and the sample was tested by H NMR spectroscopy using a Bruker DPX400 NMR spectrometer. In the H NMR spectrum, the cis peak is at 1.96 ppm, and the trans peak is at 1.83 ppm. The trans ratio of the resin can be obtained by integrating the two peaks.
[0032] (4) SMT test: The polyamide composition was injection molded into a 60 mm x 60 mm x 0.8 mm thin plate, and the plate was placed in an SMT instrument for testing. Infrared reflow conditions: The SMT infrared reflow device was set up with the following conditions:
[0033] a Preheating stage: raise the temperature from room temperature to 150°C within 120 seconds;
[0034] b. Heating stage: raising the temperature from 150°C to 190°C within 90 seconds;
[0035] c. Reflow stage: Raise the temperature to 217°C at a heating rate of 2.5°C per second, then increase the temperature from 217°C to 260°C and then decrease it to 217°C within 80 seconds;
[0036] d Cooling stage: Lower the temperature to room temperature at a cooling rate of more than 2°C per second.
[0037] (5) Polyamide transmittance test method: Referring to ISO13468-1-2019, the polyamide resin was injection molded into a 2 mm thick smooth panel, and the initial and post-SMT transmittance tests of the material were performed using a spectrophotometer.
[0038] Table 1: Amount fraction and test results of each unit substance of polyamide resin in Examples and Comparative Examples 1-2
[0039] From Examples 1-5, it can be seen that when 1,10-decanediamine accounts for 78-80% of the molar fraction of the diamine substance, the molar fraction of the trans structure in the polyamide resin is preferably 82-84%, and both the initial transmittance and the transmittance after SMT are higher.
[0040] It can be seen from Comparative Example 1 that when the amount fraction of 1,10-decanediamine in the diamine substance is less than 78%, the amount fraction of the trans structure in the polyamide resin is less than 81%, the regularity of the resin molecular chain is relatively good, and the initial transmittance is reduced; and after SMT, the molecular chain has good regularity and is easy to recrystallize again, resulting in a significant decrease in transmittance.
[0041] As can be seen from Comparative Example 2, in Comparative Example 2, the melting point of the resin is higher than 340° C., and the injection molding temperature is close to the resin decomposition temperature, making it difficult to perform injection molding, resulting in low initial transmittance and transmittance after SMT.
[0042] Table 2: Molar fraction content and test results of each unit substance of polyamide resin in comparative examples 3-5
[0043] As can be seen from Comparative Examples 3-5, it is difficult for other types of monomers to achieve a trans-structure ratio within the scope of the present invention, achieve high light transmittance, and ensure light transmittance after SMT.
[0044] The polyamide resin of the present application has an initial light transmittance of ≥72% and a light transmittance after SMT of ≥71%.
Claims
1. A polyamide resin, characterized in that: In terms of mole percentage, it comprises the following repeating units: Diacid unit: 1,4-cyclohexanedicarboxylic acid; The diamine units include 1,10-decanediamine and 1,12-dodecanediamine, wherein the molar fraction of 1,10-decanediamine in the diamines is 76-82%.
2. The polyamide resin according to claim 1, characterized in that The amount of 1,10-decanediamine in the diamines is 78-80%.
3. The polyamide resin according to claim 1, characterized in that In the polyamide resin, the trans structure accounts for 81-85% of the polyamide resin by mass fraction.
4. The polyamide resin according to claim 1, characterized in that The melting point of the polyamide resin is in the range of 321-334°C.
5. The polyamide resin according to claim 1, characterized in that The relative viscosity of the polyamide resin is in the range of 1.8-2.
8. The test method is to refer to GB12006.1-89 and measure the relative viscosity of the polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
6. The method for polymerizing a polyamide resin according to any one of claims 1 to 5, characterized in that: The following steps are involved: Add reaction monomers, benzoic acid, sodium hypophosphite and deionized water into a pressure autoclave; the amount of benzoic acid is 1.5-3.0% of the total amount of reaction monomers, the weight of sodium hypophosphite is 0.05-0.15% of the weight of other materials except deionized water, and the weight of deionized water is 25-35% of the total weight of materials; evacuate and fill with inert gas as protective gas, raise the temperature to 215-225° C. within 1.5-2.5 hours, and then react for 0.5-1.5 hours within the temperature range; then continue to react for 1-3 hours at 225-235° C. and a pressure of 2.0-2.4 MPa, remove the water formed during the reaction, discharge the material after the reaction is completed, and obtain a prepolymer product after vacuum drying the prepolymer, and solid phase thickening the prepolymer product for 8-12 hours under the conditions of 240-260° C. and a pressure of 45-55 Pa to obtain a polyamide resin.
7. Use of the polyamide resin according to any one of claims 1 to 5, characterized in that: Used to prepare translucent LED related components.
8. Application of the polyamide resin obtained by the preparation method of claim 6, characterized in that: Used to prepare translucent LED related components.
Citation Information
Patent Citations
Polyamide resin and polyamide molded body using same
CN105814115A
Polyamide resin, polyamide composition and preparation methods
CN113929901A
Polyamide resin and polymerization method and application thereof
CN115490848A
Polyamide resin and polymerization method and application thereof
CN116589675A
Polyamide composition, polyamide composition molded article and manufacturing method of polyamide composition
JP2017155150A