Viscosity reducer and preparation method therefor and use thereof, and method for improving crude-oil pollution resistance of drilling fluid
By using a viscosity reducer composed of matrix and particles in the drilling fluid, the problem of increased viscosity of the drilling fluid after the invasion of crude oil is solved, the rheological properties of the drilling fluid are maintained and the electrical stability is improved, and the production cost is reduced.
Patent Information
- Application Number
- PCT/CN2024/083071
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-31
AI Technical Summary
After the intrusion of crude oil, the viscosity of existing drilling fluids increases and the fluidity is poor, which affects the normal circulation of drilling fluids. Moreover, existing viscosity reducing agents cannot effectively prevent the formation of wax crystal network structures, causing the drilling fluids to lose fluidity.
A viscosity reducer is used that includes a matrix and particles attached or wrapped on the matrix. The matrix has lipophilic and hydrophilic parts. The particles do not melt below 100°C, and micro-nano-scale composite particles are formed in the drilling fluid through physical adsorption. , prevent wax crystals from crystallizing and preventing the formation of wax crystal network structure.
It effectively reduces the structural viscosity of the drilling fluid, maintains good rheological properties, prevents the viscosity of the drilling fluid from increasing due to the intrusion of crude oil, improves the electrical stability of the drilling fluid, and reduces production costs.
Smart Images

Figure CN2024083071_31102024_PF_FP_ABST
Abstract
Description
Viscosity reducer, preparation method and application thereof, and method for improving drilling fluid anti-oil pollution capability
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Chinese patent application No. 202310474265.4 filed on April 27, 2023, the contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to the technical field of drilling fluids, and in particular to a viscosity reducer, a preparation method and application thereof, and a method for improving the oil-resistant pollution resistance of drilling fluids. Background Art
[0004] The widespread use of synthetic drilling fluids has garnered increasing attention on the research and application of drilling fluid treatment agents. This has, to a certain extent, driven advancements in drilling fluid technology and application, resulting in increasingly sophisticated drilling fluid systems that meet the needs of safe, smooth, and efficient drilling under a variety of operating conditions. Despite extensive research on drilling fluid viscosity reducers in recent years, few products have achieved significant performance breakthroughs, entered production, or been applied. Research remains limited and limited in scope. In particular, significant gaps remain in the research on viscosity reduction for drilling fluids invaded by high-viscosity crude oil.
[0005] When crude oil invades oil-based drilling fluid / synthetic-based drilling fluid, the drilling fluid thickens and even loses fluidity, affecting the normal circulation of the drilling fluid. In the prior art, the treatment method for crude oil invading drilling fluid usually adopts dilution method or replacement method, but this method has high treatment cost and high environmental pressure. To solve the problem of deterioration of drilling fluid rheology caused by crude oil invading drilling fluid, it is necessary to have good adaptability to drilling fluid while having a good viscosity reduction effect on crude oil. CN106318348A discloses a drilling fluid that is resistant to heavy oil pollution. Through the reasonable compounding of water, sodium bentonite, sodium carbonate, sodium carboxymethyl cellulose, low-viscosity polyanionic cellulose, fluid loss reducer A, sulfonated phenolic resin, sulfonated lignite, industrial salt, emulsifier B, emulsifier C and barite, it can maintain good rheology and improve the capacity limit of heavy oil. After the drilling fluid is contaminated by 25% heavy oil, it still has good rheology and fluid loss. However, this drilling fluid has great limitations, and there is still a lack of effective viscosity reduction methods for oil-based drilling fluids / synthetic-based drilling fluids when crude oil invades.
[0006] Summary of the Invention
[0007] The present invention aims to overcome the problem in the prior art that crude oil intrudes into oil-based drilling fluid / synthetic-based drilling fluid, resulting in thickening of the drilling fluid and poor fluidity. The present invention provides a viscosity reducer, a preparation method and application thereof, and a method for improving the oil-resistance of the drilling fluid. The viscosity reducer can improve the oil-resistance of the drilling fluid and enable the drilling fluid invaded by crude oil to maintain good rheological properties.
[0008] To achieve the above objectives, the present invention provides, in a first aspect, a viscosity reducer, comprising a matrix and particles attached to a surface of and / or encapsulated in the matrix, wherein the matrix comprises a lipophilic portion and a hydrophilic portion; the particles do not melt below 100° C., and scanning electron microscopy analysis shows that the number of particles in a 10 μm×10 μm area of the viscosity reducer is 1-1500.
[0009] Preferably, the infrared absorption spectrum of the viscosity reducer is at 700±50cm -1 The maximum absorption peak intensity (P1) in the region of 2920±70cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is not less than 0.25, preferably 0.25-0.4.
[0010] The second aspect of the present invention provides a method for preparing a viscosity reducer, comprising: mixing a matrix with particles in a molten state and then drying; the matrix comprises a lipophilic portion and a hydrophilic portion; the particles do not melt below 100°C and have a diameter of 300nm-5μm, and the mass ratio of the matrix to the particles is 1:(0.01-0.09).
[0011] A third aspect of the present invention provides use of the above-mentioned viscosity reducer in reducing the viscosity of crude oil-invaded drilling fluid.
[0012] A fourth aspect of the present invention provides a method for improving the oil-resistance of drilling fluid, the method comprising adding the above-mentioned viscosity reducer to the drilling fluid.
[0013] Preferably, the amount of the viscosity reducer is 0.05-1 part by weight, preferably 0.1-0.5 part by weight, relative to 100 parts by weight of the drilling fluid.
[0014] When crude oil invades oil-based / synthetic drilling fluids, wax crystals in the oil phase precipitate and crystallize as the fluid temperature drops, causing the drilling fluid to thicken and even lose fluidity, impacting its normal circulation. Existing viscosity reducers used in oil-based / synthetic drilling fluids generally target clay particle agglomeration to reduce viscosity, lacking wax resistance and failing to reduce the viscosity of oil-invaded drilling fluids. Conventional crude oil viscosity reducers commonly used in oilfield production and pipeline transportation, while not specifically designed to reduce crude oil viscosity, have poor compatibility with oil-based / synthetic drilling fluids and can easily affect the fluid's electrical stability.
[0015] The viscosity reducer provided by the present invention includes a matrix, and particles attached to the surface of the matrix and / or wrapped in the matrix. With the help of the lipophilic part and the hydrophilic part in the matrix, the viscosity reducer can penetrate into the oil sample in the drilling fluid, and helps the particles and the matrix to be composited through a strong physical adsorption effect. The particles can maintain the particle morphology below 100 ° C, and can provide heterogeneous nucleation sites for wax crystals before the wax crystals precipitate and crystallize. Through the synergistic effect of the matrix and the particles, they are distributed in the oil phase in the form of micro-nanoscale composite particles, without affecting the emulsification stability of the drilling fluid, resulting in changes in the wax precipitation characteristics of the oil sample in the drilling fluid, so that the wax crystals in the oil phase can form wax crystal flocs with larger size and more compact structure, greatly reducing the interface area between the wax crystals and the oil phase, and making it difficult to overlap each other to construct a three-dimensional wax crystal network structure wax crystal flocs, thereby effectively preventing the drilling fluid viscosity from increasing. Preferably, the viscosity reducer provided by the present invention can both prevent the oil-invaded drilling fluid viscosity from increasing and help improve the electrical stability of the drilling fluid.
[0016] The viscosity reducer can be applied to oil-based drilling fluids and synthetic-based drilling fluids to improve the drilling fluid's resistance to oil contamination. It can also be applied to drilling fluids invaded by crude oil to reduce the thickening problem caused by crude oil intrusion into the drilling fluid, thereby reducing the structural viscosity of the drilling fluid and maintaining good rheological properties. The oil-soluble viscosity reducer of the present invention has a simple production process, is inexpensive, and is free of secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a diagram of polymer C1 obtained in Example 1 of the present invention. 1 H NMR spectrum;
[0018] FIG2 is an infrared absorption spectrum of polymer C1 obtained in Example 1 of the present invention;
[0019] FIG3 is a gel permeation chromatogram of polymer C1 obtained in Example 1 of the present invention;
[0020] FIG4 is a SEM image of the particles used in Example 1 of the present invention;
[0021] FIG5 is a surface SEM image of the viscosity reducer prepared in Example 1 of the present invention;
[0022] FIG6 is a cross-sectional SEM image of the viscosity reducer prepared in Example 1 of the present invention;
[0023] FIG7 is an infrared absorption spectrum of the viscosity reducer prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The endpoints of the ranges and any values disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.
[0025] A first aspect of the present invention provides a viscosity reducer, comprising a matrix and particles attached to the surface of the matrix and / or encapsulated in the matrix, wherein the matrix comprises a lipophilic portion and a hydrophilic portion; the particles do not melt below 100°C, and scanning electron microscopy analysis shows that the number of particles in a 10 μm×10 μm area of the viscosity reducer is 1-1500.
[0026] According to the present invention, the viscosity reducer comprises a matrix and particles. The surface SEM image of the viscosity reducer, shown in Figure 5, shows the presence of particles attached to the matrix surface. A cross-sectional SEM image of the viscosity reducer, shown in Figure 6, also reveals the presence of particles encapsulated within the matrix. The lipophilic and hydrophilic portions of the matrix allow the viscosity reducer to penetrate the oil sample in the drilling fluid and facilitate strong physical adsorption between the particles and the matrix. The particles maintain their morphology below 100°C, providing heterogeneous nucleation sites for wax crystals before the drilling fluid temperature drops. The synergistic effect of the matrix and particles alters the wax precipitation characteristics of the oil sample in the drilling fluid, allowing the wax crystals in the oil phase to form larger, more compact flocs. These large, dense wax crystal flocs significantly reduce the interfacial area between the wax crystals and the oil phase, making it difficult for them to overlap and form a three-dimensional wax crystal network, effectively preventing an increase in drilling fluid viscosity.
[0027] In the present invention, the particles in the viscosity reducer do not melt below 100°C. It is understood that the particles can maintain their shape after heat treatment at any temperature below 100°C. By preventing the particles from melting below 100°C, the high-temperature drilling fluid intruded by crude oil can be affected by the crystallization behavior of wax crystals after it reaches the surface and before wax crystals precipitate, thereby effectively preventing an increase in drilling fluid viscosity.
[0028] In the present invention, the particle size is preferably between 300 nm and 5 μm, more preferably between 500 nm and 3 μm. By controlling the particle size within the range of 300 nm to 5 μm, the particles can provide heterogeneous nucleation sites for wax crystals. Controlling the particle size within this preferred range facilitates the interaction between the particles and the polymer with an appropriate strength, and helps the wax crystals in the oil phase form larger, more compact wax crystal flocs, further enhancing viscosity reduction.
[0029] In the present invention, the particle size of the viscosity reducer refers to the maximum straight-line distance through the interior of the particle. This is measured using the following method: a sample of the viscosity reducer is prepared and observed using a scanning electron microscope (SEM). The size of 10 particles is counted and the average value is calculated, which is recorded as the particle size. The SEM testing conditions include: a TESCAN MIRA LMS, a test voltage of 200 eV-30 keV, and a magnification of 20k-100k.
[0030] The present invention has no particular limitation on the morphology of the particles, which may be spherical or non-spherical particles. Preferably, the particles are spherical particles.
[0031] In the present invention, the particles in the viscosity reducer have good dispersibility. According to scanning electron microscopy analysis, the number of particles in the viscosity reducer in an area of 10 μm × 10 μm is 1-1500, preferably 2-1000, and more preferably 5-500. In a particularly preferred embodiment, the number of particles in the viscosity reducer in an area of 10 μm × 10 μm is 5-200. In the present invention, the number of particles in any 5 areas is counted, and the average value is calculated and recorded as the number of particles in the viscosity reducer. Controlling the dispersion of the particles within the above-mentioned preferred range is conducive to exerting the synergistic effect of the particles and the matrix, and improving the dispersibility and viscosity reduction effect of the viscosity reducer in the drilling fluid without affecting the emulsification stability of the drilling fluid.
[0032] In the present invention, an SEM image of the untreated particles is shown in Figure 4, and surface SEM images and cross-sectional SEM images of the viscosity reducer are shown in Figures 5 and 6, respectively. Figures 5 and 6 show that the viscosity reducer contains particles attached to the surface of the matrix and encapsulated within the matrix. Compared with the untreated particles, the particles in the viscosity reducer essentially maintain their original morphology and size.
[0033] In the present invention, preferably, the particles are adsorbed on the surface of the matrix and / or encapsulated in the matrix through hydrogen bonding to form micro-nanoscale composite particles. In the infrared absorption spectrum of the viscosity reducer, at 700±50cm -1 The maximum absorption peak intensity (P1) in the region of 2920±70cm-1 The ratio of the maximum absorption peak intensity (P2) in the region of the viscosity reducing agent to the maximum absorption peak intensity (P1 / P2) is not less than 0.25, preferably 0.25-0.4, and more preferably 0.3-0.35. The "maximum absorption peak" refers to the absorption peak with the highest intensity in this region. The ratio of P1 / P2 within the preferred range is conducive to the penetration of the viscosity reducing agent into the crude oil wax crystal matrix and plays a role in heterogeneous nucleation, affecting the morphology and network structure of the wax, interfering with the growth of wax crystals, and achieving a viscosity reducing effect. The reason for this may be due to the generation of hydrogen bonds between the matrix and the particles, the interaction between the particles and the matrix has an appropriate strength, and the heterogeneous nucleation effect is enhanced.
[0034] The synthesized viscosity reducer was analyzed using an FT-IR spectrometer (Nicolet iz10, Thermol Scientific Co., USA). Using the potassium bromide (KBr) pelleting method, the test product was ground with KBr (1:100 weight ratio) to prepare pellets. The samples were then placed in a Fourier transform infrared spectrometer for analysis.
[0035] According to some preferred embodiments of the present invention, the mass ratio of the matrix to the particles is 1:(0.01-0.5), preferably 1:(0.02-0.07), and more preferably 1:(0.03-0.05).
[0036] In the present invention, the mass ratio of the matrix and the particles can be measured by a density comparison method. The specific operation is as follows: the density values of the matrix and the particles are measured respectively, and then a linear curve of density versus mass composition is fitted; then the density value of the viscosity reducer is measured, and the density of the viscosity reducer is substituted into the density versus mass composition curve to obtain the mass ratio of the matrix and the particles.
[0037] According to some preferred embodiments of the present invention, the melting point of the particles is 100-160° C., preferably 130-160° C. The melting point referred to in the present invention refers to the melting point at 0.1 MPa.
[0038] Preferably, the density of the particles is 1-2 g / cm 3 , preferably 1-1.5g / cm 3 .
[0039] According to some preferred embodiments of the present invention, the lipophilicity of the particles is not less than 50%, preferably 50-70%, at 20° C. In the above preferred embodiment, the dispersibility of the viscosity reducer in the drilling fluid is improved.
[0040] In the present invention, the lipophilicity test method includes: placing 1 g of particles in 50 mL of water at 20° C., and then adding methanol dropwise until the particles are completely wetted (the particles are considered completely wetted if they are completely immersed in methanol and do not float on the surface). The amount of methanol added V (mL) is recorded, and the lipophilicity is calculated as V / (50+V)×100%.
[0041] The present invention provides a wide range of composition options for the particles, preferably those that meet the aforementioned physical properties. These particles may be organic particles, inorganic oxide particles, or organic-inorganic composite particles. For example, the organic particles may be organic polymer particles; the organic-inorganic composite particles may be organically modified inorganic particles.
[0042] In the present invention, the hydrophilic and lipophilic portions of the matrix have an appropriate ratio. Preferably, the matrix has a hydrophilic-lipophilic balance (HLB) value of 3-5. Controlling the HLB value of the matrix within this preferred range helps improve the dispersibility and penetration of the viscosity reducer in the drilling fluid. In the present invention, the hydrophilic-lipophilic balance value of the matrix is measured using the partition coefficient method.
[0043] According to some preferred embodiments of the present invention, the oleophilic portion includes at least one oleophilic functional group, the hydrophilic portion includes at least one hydrophilic functional group, and the molar ratio of the oleophilic functional groups to the hydrophilic functional groups in the matrix is 8-90:1. In this preferred embodiment, the viscosity of the oil-invaded drilling fluid is reduced while the electrical stability of the drilling fluid is improved.
[0044] Preferably, based on the total amount of the matrix, the content of the lipophilic functional groups is 80-95 wt %, more preferably 90-94 wt %.
[0045] In the present invention, the relative contents of the hydrophilic and lipophilic functional groups are determined by infrared spectroscopy to determine the characteristic functional groups, and by liquid chromatography to determine the molecular weight, thereby determining the molecular structure, and then calculated based on the number of hydrophilic and lipophilic functional groups in the molecular structure.
[0046] The present invention has no particular requirements for the structure of the matrix, as long as the matrix includes a lipophilic portion and a hydrophilic portion. Preferably, the matrix is a polymer having a weight-average molecular weight of 5,000-50,000 g / mol, preferably 6,000-30,000 g / mol, and more preferably 8,000-20,000 g / mol. In the present invention, the weight-average molecular weight of the polymer is determined using an HLC-8321GPC gel permeation chromatograph with tetrahydrofuran as the mobile phase and polystyrene as the standard.
[0047] Furthermore, the matrix may be a homopolymer or a copolymer. It is understood that when the polymer is a homopolymer, the lipophilic portion and the hydrophilic portion are present in the same structural unit; when the polymer is a copolymer, the lipophilic portion and the hydrophilic portion may be present in the same structural unit or in different structural units. Preferably, when the polymer is a copolymer, the lipophilic portion and the hydrophilic portion are present in different structural units.
[0048] The present invention has no special requirements for the arrangement of different structural units in the copolymer. The copolymer can be a random copolymer, an alternating copolymer or a block copolymer.
[0049] According to the present invention, at least one oleophilic functional group is included in the oleophilic part, and the viscosity reducer is easily penetrated into the crude oil wax crystal matrix by the oleophilic functional group, thereby affecting the wax precipitation characteristics of the oil sample in the drilling fluid and improving the viscosity reduction effect. The oleophilic functional group has the definition conventional in this area, and for example, it can be substituted or unsubstituted alkyl, alkenyl, alkynyl or aryl, etc., preferably C16-C22 alkyl, alkenyl, alkynyl or aryl. For example, hexadecyl, octadecyl, eicosyl, docosyl, hexadecenyl, octadecenyl, eicosyl, docosyl, hexadecynyl, octadecynyl, eicosyl, docosyl, decanylphenyl, undecylphenyl, dodecylphenyl, tridecylphenyl, tetradecylphenyl or hexadecylphenyl, or isomers of the above substituents.
[0050] According to a particularly preferred embodiment of the present invention, the lipophilic functional group is a C16-C22 straight-chain alkyl group, such as hexadecyl, octadecyl, eicosyl, or docosyl. In this preferred embodiment, the lipophilic moiety better matches the alkyl chain length of the wax crystals, further enhancing the drilling fluid's ability to resist oil intrusion and improving viscosity reduction.
[0051] According to the present invention, the hydrophilic portion contains at least one hydrophilic functional group. On the one hand, the hydrophilic functional group is conducive to the formation of hydrogen bond adsorption between the matrix and the particles. On the other hand, the presence of the hydrophilic functional group can avoid further aggregation of wax crystal flocs precipitated using the particles attached to the surface of the polymer as a crystallization template, thereby maintaining good rheological properties of the drilling fluid.
[0052] In the present invention, the hydrophilic functional group has a conventional definition in the art, and can be, for example, a hydroxyl group, an aldehyde group, a carboxyl group, an acid anhydride group, an amino group, a sulfonyl group, a sulfonamide group, or a carbamoyl group, preferably at least one of a hydroxyl group, a carboxyl group, an acid anhydride group, and an amino group. In the present invention, the presence of the lipophilic functional group and the hydrophilic functional group in the matrix can be determined by infrared absorption spectroscopy.
[0053] According to some preferred embodiments of the present invention, the matrix and the particles contain the same structural unit, preferably, the same structural unit is an acrylic structural unit; preferably, in the viscosity reducer, the ratio of the molar amount of the same structural unit contained in the matrix to the molar amount of the same structural unit contained in the particles is 1-30:1, preferably 5-15:1.
[0054] According to some particularly preferred embodiments of the present invention, the polymer comprises a structural unit A as shown in formula (1) and a structural unit B as shown in formula (2);
[0055] wherein R1, R2, R3, and R4 are each independently selected from a hydrogen atom, a C16-C22 alkyl group, a C16-C22 alkenyl group, a C16-C22 alkynyl group, or a C16-C22 aryl group, and at least one of R1, R2, R3, and R4 is not a hydrogen atom;
[0056] R5, R6, R7, and R8 contain at least one hydroxyl group, carboxyl group, or amino group, or R5 and R6 are connected to form an acid anhydride, or R7 and R8 are connected to form an acid anhydride.
[0057] When the polymer in the viscosity reducer has the above preferred structural composition, it is beneficial to further improve the ability of the drilling fluid to resist oil invasion and maintain good rheological properties of the drilling fluid.
[0058] Preferably, in formula (1), R1 is selected from C16-C22 alkyl, C16-C22 alkenyl, C16-C22 alkynyl or C16-C22 aryl, more preferably a C16-C22 straight-chain alkyl, such as hexadecyl, octadecyl, eicosyl, docosyl, hexadecenyl, octadecenyl, eicosyl, docosenyl, hexaynyl, octaynyl, eicosyl, docosyl, decanylphenyl, undecylphenyl, dodecylphenyl, tridecylphenyl, tetradecylphenyl or hexadecylphenyl, or isomers of the above substituents; R2, R3 and R4 are hydrogen.
[0059] Preferably, in formula (2), R5 and R6 are linked to form an anhydride, and R7 and R8 are hydrogen atoms; or, R7 and R8 are linked to form an anhydride, and R5 and R6 are hydrogen atoms.
[0060] According to the present invention, as long as the polymer comprises the aforementioned structural unit A and structural unit B, the relative amounts of structural unit A and structural unit B can be selected over a wide range, subject to ensuring that the matrix has suitable hydrophilicity and lipophilicity. To ensure suitable adhesion between the polymer and the particles and to allow the viscosity reducer to better exert its viscosity reducing effect, preferably, the molar ratio of structural unit A to structural unit B in the polymer is (1-10):1, preferably (2-5):1, and more preferably (3-4):1.
[0061] The present invention has no particular limitation on the structure of the polymer. When the polymer contains the above-mentioned structural unit A and structural unit B, there is no particular requirement for the arrangement of structural unit A and structural unit B. It can be a regular block copolymer, a partially regular block copolymer or a random copolymer. In order to avoid cumbersome production processes, the polymer in the present invention is preferably a random copolymer.
[0062] In a further preferred embodiment, the particles are at least one of polymethyl methacrylate particles, polyethyl methacrylate particles, glycidyl methacrylate particles and polyethylene terephthalate particles, preferably polymethyl methacrylate particles.
[0063] Preferably, the weight average molecular weight of the polymethyl methacrylate is 15,000-750,000 g / mol, preferably 20,000-300,000 g / mol.
[0064] According to some preferred embodiments of the present invention, the polymer can be prepared by the following method: mixing monomer a having a structure represented by formula (i), monomer b having a structure represented by formula (ii) and a solvent, and then performing a copolymerization reaction under the action of an initiator;
[0065] R1 to R8 in formula (i) and formula (ii) have the same definitions as in formula (1) and formula (2).
[0066] Preferably, the molar ratio of monomer a to monomer b is (1-10):1, preferably (2-5):1, and more preferably (3-4):1.
[0067] The present invention has a wide range of choices for the initiator, and any initiator known in the art that can be used to initiate the copolymerization reaction of monomer a and monomer b can be used in the present invention. Preferably, the initiator is benzamide peroxide.
[0068] The present invention does not particularly limit the amount of the initiator, and those skilled in the art can adjust it according to actual needs. Preferably, based on the total mass of the monomer a and the monomer b, the amount of the initiator is 0.3-1 wt%, preferably 0.3-0.5 wt%.
[0069] According to the present invention, the copolymerization reaction is carried out in the presence of a solvent. The present invention has no special requirements for the selection and amount of the solvent, as long as the reaction raw materials are fully dissolved and dispersed. The solvent can be, for example, an alkane, a halogenated alkane, an aromatic hydrocarbon, a halogenated aromatic hydrocarbon, etc., for example, benzene, toluene, xylene, pentane, hexane, octane, cyclohexane, chlorobenzene, dichlorobenzene and dichloromethane, etc. Preferably, the solvent is toluene. Preferably, the ratio of the mass of the solvent to the total mass of the monomer a and the monomer b is (2-7):1.
[0070] The present invention has no particular requirements for the mixing method and conditions. Preferably, the mixing is performed under stirring conditions. The present invention also has no particular restrictions on the stirring parameters, as long as the monomer is completely dissolved in the solvent. Preferably, the stirring rate is 400-600 rpm.
[0071] Preferably, the mixing temperature is 30-60° C., preferably 40-50° C., and the mixing time is 5-20 min, preferably 10-15 min. Under the above preferred mixing conditions, it is beneficial to ensure that the monomers are completely dissolved.
[0072] According to some preferred embodiments of the present invention, the copolymerization reaction conditions include: reaction temperature of 50-100° C., preferably 60-80° C., and reaction time of 2-12 h, preferably 5-10 h.
[0073] According to some preferred embodiments of the present invention, the preparation method comprises: mixing monomer a having a structure represented by formula (i), monomer b having a structure represented by formula (ii) and a solvent, then heating the mixture to a copolymerization temperature, and then adding an initiator to carry out a copolymerization reaction.
[0074] Preferably, the copolymerization reaction is carried out under stirring conditions, and the stirring conditions may be the same as those in the mixing.
[0075] According to the present invention, preferably, the preparation method further comprises: purifying the copolymerization product. The purification can be carried out using conventional methods in the art, for example, by washing with an organic solvent. Preferably, the organic solvent washing purification process comprises: mixing the copolymerization product with a solvent, stirring until a precipitate is generated, and then performing solid-liquid separation.
[0076] In the present invention, the organic solvent may be an alcohol, such as methanol and / or ethanol. The present invention has no particular requirements for the amount of the organic solvent used, and it is preferably in excess of the reaction product, for example, the amount of the organic solvent used may be 5-10 times the mass of the reaction product.
[0077] The present invention has no particular limitation on the solid-liquid separation method, which may be a conventional operation method in the art, such as filtration.
[0078] The present invention provides a viscosity reducer, wherein the oil-soluble viscosity reducer comprises a copolymer represented by formula I and PMMA microspheres;
[0079] Wherein, R1 is a C12-C30 straight chain or branched alkyl group; m is 10-50, and n is 5-30; the PMMA microspheres have a diameter of 300-500 nm and a cross-linking degree of 10-20%.
[0080] Preferably, in Formula I, R1 is a C16-C22 linear or branched alkyl group; and / or m / n is (1-10): 1. For example, m / n is, but not limited to, 1:1, 2:1, 3:1, 5:1, 7:1, 8:1, 9:1, 10:1.
[0081] Preferably, the structure of the copolymer is as shown in Formula II,
[0082] Preferably, the weight average molecular weight of the copolymer is 5000-50000 g / mol, preferably 8000-30000 g / mol, more preferably 8000-20000 g / mol.
[0083] Preferably, the copolymer is a random copolymer.
[0084] Preferably, the mass ratio of the copolymer to the PMMA microspheres is 1:(0.01-0.1). For example, the mass ratio of the copolymer to the PMMA microspheres is, but not limited to, 1:0.01, 1:0.03, 1:0.05, 1:0.07, 1:0.09, or 1:0.1.
[0085] The second aspect of the present invention provides a method for preparing a viscosity reducer, comprising: mixing a matrix with particles in a molten state and then drying; the matrix comprises a lipophilic portion and a hydrophilic portion; the particles do not melt below 100°C, and the mass ratio of the matrix to the particles is 1:(0.01-0.5).
[0086] The matrix and particles have the same definitions as described in the first aspect and will not be repeated here.
[0087] In the present invention, it is ensured that the matrix is mixed in a molten state and at least some of the particles do not melt. Adopting the above-mentioned preferred mixing method is conducive to improving the dispersion of the particles, forming a suitable interaction force between the matrix and the particles, and further improving the viscosity reducing effect of the viscosity reducer. In the present invention, the matrix can be melted first and then mixed with the particles, or the matrix and particles can be preliminarily mixed and then heated to melt the matrix. Preferably, the matrix and particles can be added together in a mixing device for melt blending.
[0088] In the present invention, the mixing can be performed using conventional equipment in the art, for example, in a melt blender.
[0089] According to some preferred embodiments of the present invention, the mixing conditions include: a mixing temperature of 100-180° C., preferably 120-160° C., and a mixing time of 5-30 min, preferably 10-20 min.
[0090] Preferably, the mass ratio of the matrix to the particles is 1:(0.02-0.07), more preferably 1:(0.03-0.05).
[0091] Preferably, the drying is carried out under vacuum conditions, the drying temperature is 50-100° C., preferably 60-80° C., and the drying time is 5-15 h, preferably 10-12 h.
[0092] A third aspect of the present invention provides use of the above-mentioned viscosity reducer in reducing the viscosity of crude oil-invaded drilling fluid.
[0093] A fourth aspect of the present invention provides a method for improving the oil-resistance of drilling fluid, the method comprising adding the viscosity reducer described in the first aspect to the drilling fluid.
[0094] In the present invention, the viscosity reducer can be added to the drilling fluid that is not invaded by crude oil. It can also be added to the drilling fluid during use of the drilling fluid, after being invaded by crude oil, to improve the drilling fluid's ability to resist oil pollution to suppress the viscosity of the drilling fluid after being invaded by crude oil. Since crude oil invades the drilling fluid and is typically in an underground high-temperature environment, after the drilling fluid is circulated to the ground, as the temperature decreases, crude oil wax separates out crystals, so that the drilling fluid viscosity is increased, and fluidity deteriorates or even loses fluidity, thereby affecting the normal circulation and reuse of the drilling fluid. The viscosity reducer provided by the present invention can preferably be added to the drilling fluid between crude oil wax separation crystals after the drilling fluid invades the drilling fluid, that is, after the drilling fluid is lifted to the ground and before it is cooled, it is added to the drilling fluid so that the wax crystals in the oil phase can be separated out as crystallization templates with the particles attached to the polymer surface, thereby forming a wax crystal flocculent body with a larger size and a more compact structure, thereby avoiding the problem of the overall rheological properties of the drilling fluid being deteriorated by crude oil invasion.
[0095] According to some preferred embodiments of the present invention, the amount of the viscosity reducer is 0.05-1 part by weight, preferably 0.1-0.5 part by weight, relative to 100 parts by weight of the drilling fluid.
[0096] The present invention has no particular limitation on the composition of the drilling fluid, which may be conventional oil-based drilling fluid or synthetic-based drilling fluid in the art.
[0097] In the present invention, the base oil in the oil-based drilling fluid or synthetic-based drilling fluid can be selected from a wide range of types and can be provided by any oil phase commonly used in the art. Those skilled in the art can select the base oil based on actual needs. Preferably, the base oil is selected from at least one of a mineral oil and a synthetic base oil, which are well known to those skilled in the art.
[0098] According to the present invention, the drilling fluid may also contain conventional drilling fluid treatment agents in this area, such as one or more of organoclay, emulsifier, inhibitor, plugging agent, weighting agent, wetting agent, alkaline conditioner and fluid loss reducer. Those skilled in the art can select according to actual needs, and the present invention has no particular limitation to this. According to some preferred embodiments of the present invention, the organoclay may for example be quaternary ammonium salt modified bentonite.
[0099] The present invention does not particularly limit the source of the fluid loss additive; commercially available products known to those skilled in the art may be used. For example, humic acid-based fluid loss additives, asphalt-based fluid loss additives, etc. For example, natural asphalt powder purchased from Shengli Oilfield Zhongsheng Petrochemical Co., Ltd. may be used.
[0100] According to some preferred embodiments of the present invention, the emulsifier can be at least one of a divalent metal soap of a higher fatty acid, calcium alkyl sulfonate, a fatty acid emulsifier, and an amide emulsifier. Preferably, the emulsifier comprises a primary emulsifier and a secondary emulsifier, which can be combined using conventional methods in the art. Preferably, the mass ratio of the primary emulsifier to the secondary emulsifier is 1:0.3-1.
[0101] The present invention has no particular requirements for the selection of the primary emulsifier and the secondary emulsifier, and those skilled in the art can select them according to actual needs. For example, the primary emulsifier can be a commercial product with the brand name HIEMUL purchased from Jingzhou Jiahua Technology Co., Ltd., and the secondary emulsifier can be a commercial product with the brand name HICOAT purchased from Jingzhou Jiahua Technology Co., Ltd.
[0102] According to some preferred embodiments of the present invention, the weighting agent may be barite and / or iron ore powder, preferably barite. The present invention has no particular requirements for the amount of the weighting agent, which can be adjusted according to the drilling fluid density requirement.
[0103] According to some preferred embodiments of the present invention, the alkaline regulator may be calcium oxide.
[0104] According to some preferred embodiments of the present invention, the wetting agent can be a long-chain alkane quaternary ammonium salt organic compound. For example, the wetting agent can be a commercial product with the brand name HIWET purchased from Jingzhou Jiahua Technology Co., Ltd.
[0105] In the present invention, the amounts of the emulsifier, wetting agent, fluid loss control agent, alkalinity regulator, and organic soil can be selected according to actual needs, and the present invention has no particular limitation thereto. According to some preferred embodiments of the present invention, based on 100 parts by weight of the base oil, the amount of the primary emulsifier is 1-4 parts by weight, the amount of the secondary emulsifier is 1-2 parts by weight, the amount of the wetting agent is 0.5-2 parts by weight, the amount of the fluid loss control agent is 1-5 parts by weight, the amount of the alkalinity regulator is 1-5 parts by weight, and the amount of the organic soil is 1-6 parts by weight.
[0106] The present invention will be described in detail below through examples.
[0107] The main raw materials involved in the following examples and comparative examples are as follows. Unless otherwise specified, the remaining raw materials are purchased from commercial sources.
[0108] Polymethyl methacrylate (PMMA) microspheres P1: commercially available, with a diameter of 400 nm and a density of 1-1.3 g / cm 3 , the weight-average molecular weight is 40,000 g / mol, and at 20 °C, the lipophilicity of PMMA microspheres P1 is 65%;
[0109] Polymethyl methacrylate (PMMA) microspheres P2: commercially available, with a diameter of 3 μm and a density of 1.1-1.3 g / cm 3 , the weight average molecular weight is 250000 g / mol, and at 20 °C, the lipophilicity of PMMA microspheres P2 is 50%;
[0110] Main emulsifier: brand HIEMUL, purchased from Jingzhou Jiahua Technology Co., Ltd.
[0111] Auxiliary emulsifier: brand HICOAT, purchased from Jingzhou Jiahua Technology Co., Ltd.
[0112] Organic clay: brand FBJS-147, purchased from Zhejiang Fenghong New Materials Co., Ltd.
[0113] Wetting agent: brand HIWET, purchased from Jingzhou Jiahua Technology Co., Ltd.
[0114] Fluid loss additive: natural asphalt powder, purchased from Zhongsheng Petrochemical Co., Ltd. of Shengli Oilfield;
[0115] Alkaline regulator: brand LIM, purchased from Jingzhou Jiahua Technology Co., Ltd.
[0116] Barite: purchased from Shengli Oilfield Wantai Industry and Trade Co., Ltd.
[0117] The specific conditions of the main tests involved in the following examples and comparative examples are as follows:
[0118] The polymer was measured by using a Bruker-500 AVANCE III HD nuclear magnetic resonance spectrometer from Bruker, Switzerland, at 500 MHz. 1 H NMR), the solvent was deuterated chloroform.
[0119] The synthesized oil-soluble viscosity reducer was analyzed using an FT-IR spectrometer (Nicolet iz10, Thermol Scientific Co., USA). Using the potassium bromide (KBr) pelleting method, the test product was ground with KBr (1:100) to prepare pellets. The sample was then placed in a Fourier transform infrared spectrometer for analysis.
[0120] The weight-average molecular weight of the polymer was determined using an HLC-8321GPC gel permeation chromatograph with tetrahydrofuran as the mobile phase and polystyrene as the standard sample.
[0121] Example 1
[0122] (1) Octadecanyl acrylate and maleic anhydride monomers were weighed in a molar ratio of 3:1 and added to a flask, and toluene solvent was added at a total weight ratio of toluene to monomers of 3:1. The temperature of the oil bath was controlled at 40°C and mechanical stirring was applied at a constant rate, and the stirring rate was maintained at 500 rpm. After stirring for 10 minutes to ensure that the monomers were completely dissolved in toluene, the oil bath temperature was adjusted to a reaction temperature of 80°C, and a benzamide peroxide solution (1 wt% of the monomer weight) was added dropwise. The reaction time was controlled at 8 hours to obtain a reaction product.
[0123] (2) The reaction product obtained in step (1) was poured into a 500 mL beaker, and 5 times the mass of methanol was added and stirred continuously until flocculent sediment appeared at the bottom of the beaker. After filtering and drying, the purified polymer C1 was obtained. The composition structure of polymer C1 was analyzed by nuclear magnetic hydrogen spectrum, as shown in Figure 1. As can be seen from Figure 1, the chemical shifts at δ0.9, δ1.3 and δ1.6 belong to the hydrogen proton peaks of -CH3, -CH2- and -CH-, respectively. The hydrogen proton peak at δ4.0 belongs to the hydrogen proton peak of -C=O-CH2-, and the hydrogen proton peak at δ3.5 belongs to the hydrogen proton peak of the maleic anhydride group. The infrared absorption spectrum of polymer C1 is shown in Figure 2. At 1470 and 2920 cm -1 (-CH2- stretching peak), 2960cm -1 (-CH3 stretching peak) and 1740cm -1 (Stretching peak of C=O ester group), both showed characteristic spectral bands at 1785 and 1851 cm -1 The C=O characteristic peak of the anhydride group is at 1600-1680 cm -1 The absence of characteristic peaks indicates the absence of -C=C-, indicating that the acrylate monomer and maleic anhydride undergo copolymerization, demonstrating the successful synthesis of octadecyl acrylate-maleic anhydride copolymer.
[0124] Combined NMR and IR results indicate that the polymer C1 contains structural unit A represented by formula (1) and structural unit B represented by formula (2), wherein R1 is a C18 straight-chain alkyl, R2, R3, and R4 are hydrogen atoms, R5 and R6 are connected to form anhydride, and R7 and R8 are hydrogen.
[0125] GPC characterization showed that the weight average molecular weight of polymer C1 was 11886 g / mol, as shown in Figure 3. The hydrophilic-lipophilic balance (HLB) value of the matrix was 4.5 as measured by the partition coefficient method.
[0126] (3) Polymer C1 and PMMA microspheres P2 were placed in a melt blender at a mass ratio of 1:0.03 and melt blended at 130°C for 17 min to obtain a blend;
[0127] (4) The blend obtained in step (3) was placed in a vacuum oven and vacuum dried at 80° C. for 12 h to obtain a white block product, namely, an oil-soluble viscosity reducer S1. In the viscosity reducer, both the matrix and the microspheres contain acrylic acid structural units, and the molar ratio of the acrylic acid structural units from the matrix to the acrylic acid structural units from the microspheres is 9.3:1.
[0128] An SEM image of the untreated microspheres is shown in Figure 4. Surface and cross-sectional SEM images of viscosity reducer S1 are shown in Figures 5 and 6, respectively. Figures 5 and 6 show the presence of microspheres attached to the matrix surface and encapsulated within the matrix. The microspheres in the viscosity reducer essentially retain their original morphology and size. Scanning electron microscopy analysis revealed five microspheres within a 10 μm x 10 μm area of the viscosity reducer.
[0129] The viscosity reducer S1 was tested by infrared absorption spectrum. The results are shown in Figure 7. Compared with the infrared absorption spectrum of polymer C1, it can be seen that at 705 cm -1 The maximum absorption peak intensity (P1) at the bottom of the nanostructured carbon nanotubes is significantly enhanced, indicating that the PMMA microspheres are combined with the polymer through hydrogen bonding.
[0130] In the infrared absorption spectrum of the viscosity reducer, at 705 cm -1 The maximum absorption peak intensity (P1) at 2915cm -1 The ratio of the maximum absorption peak intensity (P2) at 0.3.
[0131] Example 2
[0132] The method of Example 1 was followed, except that polymer C1 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt-blended at 130°C for 11 minutes to produce a blend. The blend was then vacuum-dried in a vacuum oven at 80°C for 12 hours to obtain a white block product, namely, oil-soluble viscosity reducer S2. In this viscosity reducer, both the matrix and the microspheres contained acrylic acid structural units, with the molar ratio of the same structural units being 5.6:1.
[0133] The viscosity reducer S2 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 28 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0134] The viscosity reducer S2 was subjected to infrared absorption spectrum test. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2920 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.35.
[0135] Example 3
[0136] (1) Hexadecyl acrylate and maleic anhydride monomers were weighed in a molar ratio of 3:1 and added to a flask, and toluene solvent was added at a total weight ratio of toluene to monomers of 3:1. The temperature of the oil bath was controlled to be 40°C and mechanical stirring was applied at a constant rate, and the stirring rate was maintained at 500 rpm. After stirring for 10 minutes to ensure that the monomers were completely dissolved in toluene, the oil bath temperature was adjusted to the reaction temperature of 80°C, and a benzamide peroxide solution (1 wt% of the monomer weight) was added dropwise. The reaction time was controlled to be 8 hours to obtain a reaction product.
[0137] (2) The reaction product obtained in step (1) was poured into a 500 mL beaker, and 5 times the mass of methanol was added and stirred continuously until flocculent matter precipitated at the bottom of the beaker. The purified polymer C2 was obtained after filtration and drying. The composition structure of the polymer C2 was analyzed by H NMR spectroscopy. The peaks in the figure were assigned as follows: 1 H NMR absorption peaks at different chemical shifts represent different types of hydrogen protons. The chemical shifts at δ0.9, δ1.3, and δ1.6 belong to the hydrogen proton peaks of -CH3, -CH2-, and -CH-, respectively. The peak at δ4.0 is for the hydrogen proton peak of -C=O-CH2-, and the hydrogen proton peak of the maleic anhydride group is at δ3.5. The hydrogen proton peak at a chemical shift of 3.5 ppm confirms the successful synthesis of polymer C2.
[0138] It is proved that the polymer C2 contains the structural unit A represented by formula (1) and the structural unit B represented by formula (2), wherein R1 is a C16 straight-chain alkyl, R2, R3, and R4 are hydrogen atoms, R5 and R6 are connected to form an acid anhydride, and R7 and R8 are hydrogen.
[0139] GPC test showed that the weight average molecular weight of polymer C2 was 10940 g / mol. The hydrophilic-lipophilic balance (HLB) value of polymer C2 was 4.6 as measured by the partition coefficient method.
[0140] (3) polymer C2 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt blended at 130°C for 17 min to obtain a blend;
[0141] (4) The blend obtained in step (3) was placed in a vacuum oven and vacuum dried at 80° C. for 12 h to obtain a white block product, which is an oil-soluble viscosity reducer S3. In the viscosity reducer, both the matrix and the microspheres contain acrylic acid structural units, and the molar ratio of the same structural units contained in the two is 6:1.
[0142] The viscosity reducer S3 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 25 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0143] The infrared absorption spectrum of viscosity reducer S3 was tested. Compared with the infrared absorption spectrum of polymer C2, the viscosity reducer S3 has a -1 The maximum absorption peak intensity (P1) at the bottom of the nanostructured carbon nanotubes is significantly enhanced, indicating that the PMMA microspheres are combined with the polymer through hydrogen bonding.
[0144] In the infrared absorption spectrum of the viscosity reducer, at 691 cm -1 The maximum absorption peak intensity (P1) in the region is the same as that at 2849 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.34.
[0145] Example 4
[0146] (1) Octadecanyl acrylate and maleic anhydride monomers were weighed in a molar ratio of 2:1 and added to a flask, and toluene solvent was added at a total weight ratio of toluene to monomers of 3:1. The temperature of the oil bath was controlled at 40°C and mechanical stirring was applied at a constant rate, and the stirring rate was maintained at 500 rpm. After stirring for 10 minutes to ensure that the monomers were completely dissolved in toluene, the oil bath temperature was adjusted to a reaction temperature of 80°C, and a benzamide peroxide solution (1 wt% of the monomer weight) was added dropwise. The reaction time was controlled at 8 hours to obtain a reaction product.
[0147] (2) The reaction product obtained in step (1) was poured into a 500 mL beaker, and 5 times the mass of methanol was added and stirred continuously until flocculent matter precipitated at the bottom of the beaker. The purified polymer C3 was obtained after filtration and drying. The composition structure of the polymer C3 was analyzed by nuclear magnetic resonance spectroscopy. The peaks in the figure were assigned as follows: 1 In the H NMR, chemical shifts at δ0.9, δ1.3, and δ1.6 belong to the hydrogen proton peaks of -CH3, -CH2-, and -CH-, respectively, but differ in intensity from the absorption peaks shown in Figure 1. The hydrogen proton peak at δ4.0 is attributed to -C=O-CH2-, while the hydrogen proton peak of the maleic anhydride group is at δ3.5. The presence of a hydrogen proton peak at a chemical shift of 3.5 ppm confirms the successful synthesis of polymer C3.
[0148] It is proved that the polymer C3 contains the structural unit A represented by formula (1) and the structural unit B represented by formula (2), wherein R1 is a C18 straight-chain alkyl, R2, R3, and R4 are hydrogen atoms, R5 and R6 are connected to form an acid anhydride, and R7 and R8 are hydrogen.
[0149] GPC test showed that the weight average molecular weight of the polymer C3 was 11192 g / mol. The hydrophilic-lipophilic balance (HLB) value of the polymer C3 was 4.6 as measured by the partition coefficient method.
[0150] (3) polymer C3 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt blended at 160°C for 12 min to obtain a blend;
[0151] (4) The blend obtained in step (3) was placed in a vacuum oven and vacuum dried at 80° C. for 12 h to obtain a white block product, which is an oil-soluble viscosity reducer S4. In the viscosity reducer, both the matrix and the microspheres contain acrylic acid structural units, and the molar ratio of the same structural units contained in the two is 8:1.
[0152] The viscosity reducer S4 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 27 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0153] The infrared absorption spectrum of viscosity reducer S4 was tested. Compared with the infrared absorption spectrum of polymer C3, the -1 The maximum absorption peak intensity (P1) at 700 cm -1 The maximum absorption peak intensity (P1) in the region of 2920 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.35.
[0154] Example 5
[0155] (1) Octadecanyl acrylate and maleic anhydride monomers were weighed in a molar ratio of 5:1 and added to a flask, and toluene solvent was added at a total weight ratio of toluene to monomers of 3:1. The temperature of the oil bath was controlled at 40°C and mechanical stirring was applied at a constant rate, and the stirring rate was maintained at 500 rpm. After stirring for 10 minutes to ensure that the monomers were completely dissolved in toluene, the oil bath temperature was adjusted to a reaction temperature of 80°C, and a benzamide peroxide solution (1 wt% of the monomer weight) was added dropwise. The reaction time was controlled at 8 hours to obtain a reaction product.
[0156] (2) The reaction product obtained in step (1) was poured into a 500 mL beaker, 5 times the mass of methanol was added and stirred continuously until flocculent matter precipitated at the bottom of the beaker, and the purified polymer C4 was obtained after filtration and drying; the composition structure of the polymer C4 was analyzed by nuclear magnetic hydrogen spectrum, and it was proved that the polymer C4 contained the structural unit A represented by formula (1) and the structural unit B represented by formula (2), wherein R1 was a C18 straight-chain alkyl, R2, R3, and R4 were hydrogen atoms, R5 and R6 were connected to form anhydride, and R7 and R8 were hydrogen.
[0157] GPC test showed that the weight average molecular weight of the polymer C4 was 12030 g / mol. The hydrophilic-lipophilic balance (HLB) value of the polymer C4 was 4.2 as measured by the partition coefficient method.
[0158] (3) polymer C4 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt blended at 160°C for 10 min to obtain a blend;
[0159] (4) The blend obtained in step (3) was placed in a vacuum oven and vacuum dried at 80° C. for 12 h to obtain a white block product, namely, the oil-soluble viscosity reducer S5. In the viscosity reducer, both the matrix and the microspheres contain acrylic acid structural units, and the molar ratio of the same structural units contained in the two is 3.4:1.
[0160] The viscosity reducer S5 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 20 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0161] The viscosity reducer S5 was subjected to infrared absorption spectrum test. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2960 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.3.
[0162] Example 6
[0163] The method of Example 2 was followed, except that polymer C1 and PMMA microspheres P1 were melt blended in a melt blender at a mass ratio of 1:0.01 at 130°C for 14 minutes to produce a blend. The resulting blend was then vacuum dried at 80°C for 12 hours to obtain a white block product, namely, oil-soluble viscosity reducer S6. In this viscosity reducer, both the matrix and the microspheres contained acrylic acid structural units, with the molar ratio of the same structural units being 28:1.
[0164] The viscosity reducer S6 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 12 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0165] The viscosity reducer S6 was subjected to infrared absorption spectrum test. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2900 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.25.
[0166] Example 7
[0167] The method of Example 2 was followed, except that polymer C1 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.07, and melt-blended at 140°C for 16 minutes to obtain a blend; the obtained blend was placed in a vacuum oven and vacuum-dried at 80°C for 12 hours to obtain a white block product, which was the oil-soluble viscosity reducer S7.
[0168] Scanning electron microscopy analysis of viscosity reducer S7, similar to Figures 5 and 6, revealed 54 microspheres within a 10 μm × 10 μm area of the viscosity reducer. Both the matrix and the microspheres contained acrylic acid structural units, with the molar ratio of these structural units being 4:1.
[0169] The viscosity reducer S7 was tested by infrared absorption spectrum. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region is the same as that at 2915 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.36.
[0170] Example 8
[0171] The method of Example 2 was followed, except that polymer C1 and PMMA microspheres P1 were melt blended in a melt blender at a mass ratio of 1:0.09 at 140°C for 15 minutes to produce a blend. The resulting blend was then vacuum dried in a vacuum oven at 80°C for 12 hours to obtain a white block product, namely, oil-soluble viscosity reducer S7. In this viscosity reducer, both the matrix and the microspheres contained acrylic acid structural units, with the molar ratio of the same structural units being 3.1:1.
[0172] The viscosity reducer S7 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that the number of the microspheres in the viscosity reducer in an area of 10 μm×10 μm was 75.
[0173] The viscosity reducer S7 was tested by infrared absorption spectrum. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2920 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.34.
[0174] Example 9
[0175] (1) Octadecanyl acrylate and maleic anhydride monomers were weighed in a molar ratio of 1:1 and added to a flask, and toluene solvent was added at a total weight ratio of toluene to monomers of 3:1. The temperature of the oil bath was controlled to be 40°C and mechanical stirring was applied at a constant rate, and the stirring rate was maintained at 500 rpm. After stirring for 10 minutes to ensure that the monomers were completely dissolved in toluene, the oil bath temperature was adjusted to a reaction temperature of 80°C, and a benzamide peroxide solution (1 wt% of the monomer weight) was added dropwise. The reaction time was controlled to be 8 hours to obtain a reaction product.
[0176] (2) The reaction product obtained in step (1) was poured into a 500 mL beaker, 5 times the mass of methanol was added and stirred continuously until flocculent matter precipitated at the bottom of the beaker, and the purified polymer C5 was obtained after filtration and drying; the composition structure of the polymer C5 was analyzed by nuclear magnetic hydrogen spectrum, and it was proved that the polymer C5 contained the structural unit A represented by formula (1) and the structural unit B represented by formula (2), wherein R1 was a C18 straight-chain alkyl, R2, R3, and R4 were hydrogen atoms, R5 and R6 were connected to form anhydride, and R7 and R8 were hydrogen.
[0177] GPC test showed that the weight average molecular weight of the polymer C5 was 10980 g / mol. The hydrophilic-lipophilic balance (HLB) value of the polymer C5 was 5 as measured by the partition coefficient method.
[0178] (3) polymer C5 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt blended at 160°C for 10 min to obtain a blend;
[0179] (4) The blend obtained in step (3) was placed in a vacuum oven and vacuum dried at 80° C. for 12 h to obtain a white block product, namely, the oil-soluble viscosity reducer S9. In the viscosity reducer, both the matrix and the microspheres contain acrylic acid structural units, and the molar ratio of the same structural units contained in the two is 1.1:1.
[0180] The viscosity reducer S9 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 21 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0181] The viscosity reducer S9 was tested by infrared absorption spectrum. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2940 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.36.
[0182] Example 10
[0183] (1) Octadecanyl acrylate and maleic anhydride monomers were weighed in a molar ratio of 7:1 and added to a flask, and toluene solvent was added at a ratio of toluene to the total mass of the monomers of 3:1. The temperature of the oil bath was controlled to be 40°C and mechanical stirring was applied at a constant rate, and the stirring rate was maintained at 500 rpm. After stirring for 10 minutes to ensure that the monomers were completely dissolved in toluene, the oil bath temperature was adjusted to the reaction temperature of 80°C, and a benzamide peroxide solution (1 wt% of the monomer mass) was added dropwise. The reaction time was controlled to be 8 hours to obtain a reaction product.
[0184] (2) The reaction product obtained in step (1) was poured into a 500 mL beaker, 5 times the mass of methanol was added and stirred continuously until flocculent matter precipitated at the bottom of the beaker, and the purified polymer C6 was obtained after filtration and drying; the composition structure of the polymer C6 was analyzed by nuclear magnetic hydrogen spectrum, which proved that the polymer C6 contained the structural unit A represented by formula (1) and the structural unit B represented by formula (2), wherein R1 was a C18 straight-chain alkyl, R2, R3, and R4 were hydrogen atoms, R5 and R6 were connected to form anhydride, and R7 and R8 were hydrogen.
[0185] GPC test showed that the weight average molecular weight of the polymer C6 was 12376 g / mol. The hydrophilic-lipophilic balance (HLB) value of the polymer C6 was 3.8 as measured by the partition coefficient method.
[0186] (3) polymer C6 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt blended at 140°C for 13 min to obtain a blend;
[0187] (4) The blend obtained in step (3) was placed in a vacuum oven and vacuum-dried at 80° C. for 12 h to obtain a white block product, namely, the oil-soluble viscosity reducer S10. In the viscosity reducer, both the matrix and the microspheres contained acrylic acid structural units, and the molar ratio of the same structural units contained in the two was 6:1.
[0188] The viscosity reducer S10 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 20 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0189] The viscosity reducer S10 was tested by infrared absorption spectrum. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2920 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.29.
[0190] Example 11
[0191] (1) Octadecanyl acrylate and maleic anhydride monomers were weighed in a molar ratio of 10:1 and added to a flask, and toluene solvent was added at a total weight ratio of toluene to monomers of 3:1. The temperature of the oil bath was controlled at 40°C and mechanical stirring was applied at a constant rate, and the stirring rate was maintained at 500 rpm. After stirring for 10 minutes to ensure that the monomers were completely dissolved in toluene, the oil bath temperature was adjusted to a reaction temperature of 80°C, and a benzamide peroxide solution (1 wt% of the monomer weight) was added dropwise. The reaction time was controlled at 8 hours to obtain a reaction product.
[0192] (2) The reaction product obtained in step (1) was poured into a 500 mL beaker, 5 times the mass of methanol was added and stirred continuously until flocculent matter precipitated at the bottom of the beaker, and the purified polymer C7 was obtained after filtration and drying; the composition structure of the polymer C7 was analyzed by nuclear magnetic hydrogen spectrum, which proved that the polymer C7 contained the structural unit A represented by formula (1) and the structural unit B represented by formula (2), wherein R1 was a C18 straight-chain alkyl, R2, R3, and R4 were hydrogen atoms, R5 and R6 were connected to form anhydride, and R7 and R8 were hydrogen.
[0193] GPC test showed that the weight average molecular weight of the polymer C7 was 16698 g / mol. The hydrophilic-lipophilic balance (HLB) value of the polymer C7 was 3.2 as measured by the partition coefficient method.
[0194] (3) polymer C7 and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt blended at 150°C for 15 min to obtain a blend;
[0195] (4) The blend obtained in step (3) was placed in a vacuum oven and vacuum dried at 80° C. for 12 h to obtain a white block product, namely, the oil-soluble viscosity reducer S11. In the viscosity reducer, both the matrix and the microspheres contain acrylic acid structural units, and the molar ratio of the same structural units contained in the two is 6:1.
[0196] The viscosity reducer S11 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that there were 18 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0197] The viscosity reducer S11 was subjected to infrared absorption spectrum test. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2920 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.21.
[0198] Example 12
[0199] The method of Example 2 was followed, except that the polymer C1 and the PMMA microspheres P1 were directly mixed at a mass ratio of 1:0.05 for 17 minutes at room temperature to obtain a mixture viscosity reducer S12.
[0200] Scanning electron microscopy characterization of the viscosity reducer S13 revealed that microspheres were attached to the surface of the polymer and had poor dispersion uniformity. Scanning electron microscopy analysis showed that there were 32 microspheres in the viscosity reducer in an area of 10 μm×10 μm.
[0201] The viscosity reducer S1 was subjected to infrared absorption spectrum test. In the infrared absorption spectrum of the viscosity reducer, at 700 cm -1 The maximum absorption peak intensity (P1) at 2920 cm -1 The ratio of the maximum absorption peak intensity (P2) at 0.12.
[0202] Example 13
[0203] The method of Example 2 was followed, except that polymer C1 and PMMA microspheres P1 were melt blended in a melt blender at a mass ratio of 1:0.5 at 140°C for 15 minutes to produce a blend. The resulting blend was then vacuum dried in a vacuum oven at 80°C for 12 hours to obtain a white block product, namely, oil-soluble viscosity reducer S13. In this viscosity reducer, both the matrix and the microspheres contained acrylic acid structural units, with the molar ratio of the same structural units being 0.6:1.
[0204] The viscosity reducer S13 was characterized by scanning electron microscopy. Similar to FIG5 and FIG6 , the scanning electron microscopy analysis showed that the number of microspheres in the viscosity reducer in an area of 10 μm×10 μm was 510.
[0205] The viscosity reducer S13 was tested by infrared absorption spectrum. In the infrared absorption spectrum of the viscosity reducer, the -1 The maximum absorption peak intensity (P1) in the region of 2920 cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is 0.5.
[0206] Comparative Example 1
[0207] Polyoctadecyl acrylate (weight average molecular weight 7000 g / mol) and PMMA microspheres P1 were placed in a melt blender at a mass ratio of 1:0.05 and melt blended at 130° C. for 17 min to obtain a blend;
[0208] The blend was then placed in a vacuum oven and dried under vacuum at 80° C. for 12 h to obtain viscosity reducer DS1.
[0209] Comparative Example 2
[0210] A silicone-fluorine viscosity reducer (purchased from Shandong Jiaozhou Petroleum Additives Co., Ltd.) was used as the viscosity reducer DS2.
[0211] Comparative Example 3
[0212] PMMA microspheres P1 were directly used as the viscosity reducer and were recorded as DS3.
[0213] Comparative Example 4
[0214] The polymer C7 prepared in Example 11 was directly used as a viscosity reducer and was recorded as DS4.
[0215] Test Case
[0216] Prepare drilling fluid:
[0217] Preparation of synthetic drilling fluid: Take 240g of continuous phase base oil, add 9g of primary emulsifier and 3g of auxiliary emulsifier, stir at high speed for 60 minutes to fully dissolve, add 60g of calcium chloride aqueous solution, stir at high speed for 60 minutes to form oil-in-water emulsion, then add 12g of organic soil, 3g of wetting agent, 10g of fluid loss reducer, and 6g of alkaline regulator, stir for 20 minutes to fully dissolve, and add barite to increase the density to 1.8g / cm 3 , and stirred for 60 minutes to obtain a synthetic-based drilling fluid.
[0218] (1) Used to illustrate that viscosity reducers improve the resistance of drilling fluids to oil invasion
[0219] The viscosity reducers prepared in the above examples and comparative examples were added to the synthetic drilling fluid. The dosage of the viscosity reducers was shown in Table 1 based on 100 parts by weight of the drilling fluid. Then, 20 wt% of crude oil from the E2S series of the Paleogene in the Cenozoic Era in the Jiyang Depression was added to the synthetic drilling fluid. 3 The crude oil in the layer was tested at 20°C using the standard test "GB / T 16783.2-2012 Field testing of drilling fluids in the petroleum and natural gas industry Part 2: Oil-based drilling fluids" to measure the apparent viscosity, dynamic shear force, and demulsification voltage of the drilling fluid. The results are shown in Table 1.
[0220] Table 1
[0221] As can be seen from the results of Table 1, adding the viscosity reducer provided by the present invention to the drilling fluid not invaded by crude oil can effectively improve the anti-oil invasion ability of the drilling fluid. Compared with the sample without the additive, the drilling fluid sample to which the viscosity reducer is pre-added has a lower growth rate of apparent viscosity and a smaller dynamic shear force after being invaded by crude oil, and can maintain suitable fluidity. While maintaining suitable fluidity, the drilling fluid invaded by crude oil can have better electrical stability. In a preferred case, it can take into account lower apparent viscosity, dynamic shear force and higher demulsification voltage, thereby being more conducive to the recycling of the drilling fluid.
[0222] (2) Used to illustrate the inhibitory effect of viscosity reducers on the viscosity increase of drilling fluids invaded by crude oil
[0223] At 65 ° C, 20 wt% crude oil was added to the synthetic drilling fluid, which was derived from E2S of the Paleogene of the Cenozoic in Jiyang Depression. 3 The crude oil in the layer was then cooled at room temperature and stirred for 5 minutes before the viscosity reducers of the above examples and comparative examples were added. The dosage of the viscosity reducers was shown in Table 2 based on 100 parts by weight of the drilling fluid. After cooling to 20° C., the apparent viscosity of the drilling fluid was tested in accordance with GB / T16783.2-2012 "Field Testing of Drilling Fluids in the Petroleum and Natural Gas Industry - Part 2: Oil-Based Drilling Fluids". The results are shown in Table 2.
[0224] Table 2
[0225] Combining the results in Table 1 and Table 2, it can be seen that the viscosity reducer provided by the present invention can be added to the drilling fluid before crude oil invasion, or can be added during the use of the drilling fluid or after crude oil invasion, and can play a role in improving the ability of the drilling fluid to resist crude oil contamination and effectively suppress the increase in viscosity of the drilling fluid invaded by crude oil.
[0226] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.
Claims
1. A viscosity reducing agent, characterized in that: The viscosity reducer comprises a matrix, and particles attached to the surface of the matrix and / or wrapped in the matrix, wherein the matrix comprises a lipophilic part and a hydrophilic part; the particles do not melt below 100° C., and according to a scanning electron microscope analysis, the number of the particles in the viscosity reducer in an area of 10 μm×10 μm is 1-1500.
2. The viscosity reducer according to claim 1, wherein In the infrared absorption spectrum of the viscosity reducer, at 700±50cm -1 The maximum absorption peak intensity (P1) in the region of 2920±70cm -1 The ratio of the maximum absorption peak intensity (P2) in the region is not less than 0.25, preferably 0.25-0.
4.
3. The viscosity reducer according to claim 1 or 2, wherein: According to the analysis by scanning electron microscope, in the viscosity reducer in the area of 10 μm×10 μm, the number of the particles is 2-1000, preferably 5-500; Preferably, the mass ratio of the matrix to the particles is 1:(0.01-0.5), preferably 1:(0.02-0.07), and more preferably 1:(0.03-0.05).
4. The viscosity reducer according to any one of claims 1 to 3, wherein: The size of the particles is 300nm-5μm, preferably 400nm-3μm; Preferably, at 20°C, the lipophilicity of the particles is not less than 50%, preferably 50-70%.
5. The viscosity reducer according to any one of claims 1 to 4, wherein: The particles are selected from at least one of organic particles, inorganic oxide particles and organic-inorganic composite particles; Preferably, the particles are at least one of polymethyl methacrylate particles, polyethyl methacrylate particles, glycidyl methacrylate particles and polyethylene terephthalate particles, preferably polymethyl methacrylate particles.
6. The viscosity reducer according to any one of claims 1 to 5, wherein: The hydrophilic-lipophilic balance value of the matrix is 3-5; Preferably, the lipophilic part contains at least one lipophilic functional group, the hydrophilic part contains at least one hydrophilic functional group, and in the matrix, the molar ratio of the lipophilic functional group to the hydrophilic functional group is 8-90:1; Preferably, based on the total amount of the matrix, the content of the lipophilic functional group is 80-95 wt %.
7. The viscosity reducer according to claim 6, wherein: The lipophilic functional group is selected from at least one of a substituted or unsubstituted ester group, an alkyl group, an alkenyl group, an alkynyl group and an aryl group, preferably a C16-C22 alkyl group, an alkenyl group, an alkynyl group or an aryl group; and / or, The hydrophilic functional group is selected from at least one of a hydroxyl group, a carboxyl group, an acid anhydride group and an amino group.
8. The viscosity reducer according to any one of claims 1 to 7, wherein: The matrix and the particles contain the same structural units; Preferably, in the viscosity reducing agent, the ratio of the molar amount of the same structural unit contained in the matrix to the molar amount of the same structural unit contained in the particles is 1-30:1, preferably 5-15:
1.
9. The viscosity reducer according to any one of claims 1 to 8, wherein: The matrix is a polymer, and the weight average molecular weight of the matrix is 5000-50000 g / mol, preferably 6000-30000 g / mol, and more preferably 8000-20000 g / mol.
10. The viscosity reducing agent according to claim 9, wherein The matrix includes a structural unit A as shown in formula (1) and a structural unit B as shown in formula (2); wherein R1, R2, R3, and R4 are each independently selected from a hydrogen atom, a C16-C22 alkyl group, a C16-C22 alkenyl group, a C16-C22 alkynyl group, or a C16-C22 aryl group, and at least one of R1, R2, R3, and R4 is not a hydrogen atom; R5, R6, R7, and R8 contain at least one hydroxyl group, carboxyl group, or amino group, or R5 and R6 are connected to form an acid anhydride, or R7 and R8 are connected to form an acid anhydride; Preferably, in the polymer, the molar ratio of the structural unit A to the structural unit B is (1-10):1, preferably (2-5):
1.
11. A method for preparing a viscosity reducing agent, comprising: The matrix is mixed with the particles in a molten state and then dried; the matrix includes a lipophilic part and a hydrophilic part; the particles do not melt below 100° C., and the mass ratio of the matrix to the particles is 1:(0.01-0.5).
12. The preparation method according to claim 11, wherein Preferably, the size of the particles is 300nm-5μm; Preferably, the mass ratio of the matrix to the particles is 1:(0.02-0.07), more preferably 1:(0.03-0.05); Preferably, the mixing conditions include: the mixing temperature is 100-180°C, preferably 120-160°C, and the mixing time is 5-30min, preferably 10-20min; Preferably, the drying is carried out under vacuum conditions, at a temperature of 60-80° C., for a time of 10-12 h.
13. Use of the viscosity reducer according to any one of claims 1 to 10 or the viscosity reducer prepared by the preparation method according to claim 11 or 12 in reducing the viscosity of crude oil invading drilling fluid.
14. A method for improving the oil pollution resistance of drilling fluid, characterized in that: The method comprises adding the viscosity reducer according to any one of claims 1 to 10 or the viscosity reducer prepared by the preparation method according to claim 11 or 12 to the drilling fluid; Preferably, the drilling fluid is an oil-based drilling fluid or a synthetic-based drilling fluid; Preferably, the amount of the viscosity reducer is 0.05-1 part by weight, preferably 0.1-0.5 part by weight, relative to 100 parts by weight of the drilling fluid.
Citation Information
Patent Citations
Pour-point-depressing and viscosity-reducing complexing agent for wax-bearing crude
CN105889756A
Method for improving rheological property of waxy crude oil
CN107011937A
Composite pour point depressant
CN108997991A
Paraffin preventing and removing agent for drilling fluid as well as preparation method and application of paraffin preventing and removing agent
CN115975611A
Compositions and Methods for Treatment of Well Bore Tar
US20090095534A1