Polyester composition, preparation method therefor, and use thereof
By using a combination of PCT resin, light diffusing agent and glass filler in the SMD type LED reflective bracket material, the light reflectivity and transmittance are improved, solving the problems of opacity and strength of existing materials, and achieving a wider angle Light emission and high temperature resistance.
Patent Information
- Application Number
- PCT/CN2024/089428
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
The existing SMD LED reflective bracket material contains titanium dioxide, which makes it opaque and limits the light-emitting angle of the lamp beads. Adding a lens to improve the light-emitting angle will increase the cost and complexity. At the same time, titanium dioxide affects the strength and toughness of the material. , causing the lamp beads to easily crack during use.
A polyester composition, including PCT resin, specific types and structures of light diffusing agents, flat glass fibers, round glass fibers and glass flakes, is mixed through a high mixer and melt blended through a twin-screw extruder. Excitation absorbs invisible light and converts it into long-wavelength light, thereby improving light reflectivity, while maintaining high light transmittance and increasing the reflection angle.
It significantly improves the light reflectivity and transmittance of the polyester composition, increases the reflection angle, is suitable for SMD type LED reflective brackets, and has high temperature resistance, solving the problem of material strength and toughness.
Smart Images

Figure CN2024089428_31102024_PF_FP_ABST
Abstract
Description
A polyester composition and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to a preparation method and application of a polyester composition. Background Art
[0002] An SMD LED reflector is made by placing a punched, electroplated metal strip into an injection mold. The LED reflector material is then injected onto the metal strip using an injection molding machine. This creates a functional LED component with a reflective cavity suitable for SMT soldering. After die bonding, wire bonding, and encapsulation, the light emitted by the LED chip is reflected at a specific angle to minimize light loss. The light is then passed through an encapsulation material such as epoxy resin or silicone to form the LED lighting or display light source. The LED reflector is a core material in LED lighting, directly impacting the brightness and lifespan of the LED light source. The LED encapsulation function provides adequate protection for the chip, preventing failure from prolonged exposure to air or mechanical damage, thereby improving chip stability.
[0003] Common materials for SMD LED reflector brackets include thermoplastic materials filled with PPA or PCT reinforced fillers and titanium dioxide. Because titanium dioxide is a light-blocking pigment, currently available SMD LED reflector brackets are opaque and light-blocking. Consequently, the encapsulated LEDs cannot achieve a 180° beam angle, as shown in Figure 1 of the specification. Currently, the industry is using a PMMA lens to maximize the beam angle of the SMD lamps, as shown in Figure 2 of the specification. While this method can improve the beam angle of the SMD lamps, it requires the addition of a lens, which increases both the manufacturing process and the cost.
[0004] At the same time, the SMD LED reflective bracket material needs to add fillers such as titanium dioxide. Although it can improve the reflectivity of the material, it has a great impact on the strength and toughness of the material, causing the SMD lamp beads to crack and die during use.
[0005] Summary of the Invention
[0006] The present invention aims to provide a polyester composition having high light reflectivity and certain light transmittance, thereby increasing the reflection angle. The present invention also discloses a preparation method and application thereof.
[0007] The present invention is achieved through the following technical solutions:
[0008] A polyester composition comprising the following components in parts by weight:
[0009] 50-80 parts of PCT resin;
[0010] 8-40 parts of filler;
[0011] Light diffuser 0.01-0.1 parts;
[0012] The filler is selected from at least one of flat glass fiber, round glass fiber, and glass flakes;
[0013] The structure of the light diffuser is
[0014] wherein R2, R3, R4, and R5 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 1 to 9 carbon atoms, a halogen atom, a heterocyclic group having 1 to 6 carbon atoms, an ester group having 1 to 6 carbon atoms, or a cyano group;
[0015] R1 is One of them.
[0016] Preferably, R1 is One of them.
[0017] Preferably, the content of the light diffusing agent is 0.0005-0.001 times the weight content of the PCT resin.
[0018] In the polyester composition, the aspect ratio (retained length / major axis diameter) of the flat glass fiber is in the range of 0.3-228, preferably 1-200, more preferably 3-100;
[0019] Preferably, the flat glass fiber has an aspect ratio of 2-7, preferably 4-6.
[0020] In the polyester composition, the aspect ratio of the round glass fiber is in the range of 2-352; preferably, the aspect ratio of the round glass fiber is in the range of 5-300, more preferably 15-200.
[0021] In the polyester composition, the D50 particle size range of the glass flakes is 5-250 microns; preferably, the D50 particle size range of the glass flakes is 10-200 microns, more preferably 20-160 microns.
[0022] The PCT resin has a melting point of 260-300° C. as measured by differential scanning calorimetry at a heating / cooling rate of 20° C. / min.
[0023] It can be selected whether to add 0-2 parts of at least one of an antioxidant and a lubricant according to actual needs.
[0024] The antioxidant may be: 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; 2,5-di-tert-butyl-4-hydroxybenzyldimethylamine; diethyl-3,5-di-tert-butyl-4-hydroxybenzyl phosphate; stearyl-3,5-di-tert-butyl-4-hydroxybenzyl phosphate; 3,5-di-tert-butyl-4-hydroxyphenyl-3,5-distearyl-thiotriazolylamine; 2,6-di-tert-butyl-4-hydroxymethylphenol; 2,4-di-(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylglycerol allyl ether)-1,3,5-triazine; N,N'-hexamethylenebis( 3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid); N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine; octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]; triethylene glycol-bis[3-(3,5-dimethyl-4-hydroxyphenyl)propionate]; triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate]; 2,2'-thiodiethyl-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, etc.
[0025] The lubricant may be: at least one of a stearate lubricant, a fatty acid lubricant, and a stearate lubricant; the stearate lubricant is selected from at least one of calcium stearate, magnesium stearate, and zinc stearate; the fatty acid lubricant is selected from at least one of fatty acids, fatty acid derivatives, and fatty acid esters; and the stearate lubricant is selected from at least one of pentaerythritol stearate.
[0026] The preparation method of the high-temperature resistant polyester composition of the present invention comprises the following components: mixing a polyester resin, a filler, and a light diffusing agent in a high-speed mixer according to a proportion, and melt-blending and extruding the mixture into granules through a twin-screw extruder to obtain the high-temperature resistant polyester composition; wherein the heating temperatures of the extruder are as follows: 250-290°C for zone 1, 260-300°C for zones 2-4, 270-310°C for zones 5-7, 260-300°C for zones 8-9, and 250-290°C for the die.
[0027] Glass fiber can be long glass fiber or chopped glass fiber. If continuous glass fiber is used, it is fed into the feeder side. Chopped glass fiber is a product that the manufacturer has pre-cut continuous glass fiber into short lengths.
[0028] The 60×60×1.0 mm molded product prepared from the high temperature resistant polyester composition of the present invention at a mold temperature of 60° C. has a light transmittance range of 53%-75% and a reflectivity range of 44%-64%.
[0029] The present invention has the following beneficial effects:
[0030] The high-temperature resistant polyester composition of the present invention, by adding a light diffusing agent of a specific content and structure, can stimulate the absorption of invisible light (wavelength range of approximately 60-380nm), converting it into blue light with a longer wavelength, while also reflecting more blue light with a wavelength in the range of 400-600nm than the original incident wavelength, thereby significantly improving the light reflectivity of the polyester composition. Simultaneously, the use of glass fillers such as flat glass fibers, round glass fibers, and glass flakes of specific content and morphology can further improve reflectivity while rarely affecting transmittance. When applied to SMD-type LED reflector brackets, the reflection angle can be increased (as shown in Figure 3 of the specification). Furthermore, the polyester composition of the present invention has the advantage of high-temperature resistance. It is suitable for preparing SMD-type LED reflector brackets. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1: Schematic diagram of the structure of opaque SMD LED reflective bracket materials currently on the market.
[0032] Figure 2: Schematic diagram of the structure of adding a PMMA lens to the SMD lamp bead.
[0033] FIG3 is a schematic diagram showing light reflection when the high temperature resistant polyester composition of the present invention is applied to an SMD type LED reflective bracket. FIG. DETAILED DESCRIPTION
[0034] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those skilled in the art, several variations and improvements can be made without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.
[0035] The raw materials used in the present invention come from the following sources:
[0036] PCT Resin A: PCT 0502, SK Chemicals. Melting point: 286°C (measured at a heating / cooling rate of 20°C / min).
[0037] PCT Resin B: PCT 0502HC, SK Chemicals. Melting point: 295°C (measured at a heating / cooling rate of 20°C / min).
[0038] Light Diffuser A:
[0039] OB-1, Zhejiang Hongyi Chemical Co., Ltd.;
[0040] Light Diffuser B:
[0041] KSN, Zhejiang Hongyi Chemical Co., Ltd.;
[0042] Light Diffuser C:
[0043] Commercially available, CAS 2866-43-5.
[0044] Light Diffuser D:
[0045] DT,(CAS No:1041-00-5),Zhejiang Hongyi Chemical Co., Ltd.;
[0046] Light diffuser E: Acrylic light diffuser powder TY-660, Hunan Jinyu Fine Chemical Co., Ltd.
[0047] Titanium dioxide: BLR-886, purchased from Longman Baili.
[0048] Round glass fiber A: brand ECS10-03-568H, manufacturer JUSHI;
[0049] Flat glass fiber A: flatness ratio is 2, CPIC;
[0050] Flat glass fiber B: chopped, flatness ratio of 3, manufactured by CPIC;
[0051] Flat glass fiber C: chopped, flatness ratio of 4, manufactured by CPIC;
[0052] Flat glass fiber D: chopped, flatness ratio 6, CPIC;
[0053] Glass flakes were purchased from Glassflake Company in the UK and then screened to obtain raw materials with specific particle sizes.
[0054] Glass flake A: D50 = 11.6 μm;
[0055] Glass flake B: D50 = 23.5 μm;
[0056] Glass flake C: D50 = 158.4 μm;
[0057] Glass flake D: D50 = 199.5 μm;
[0058] Glass flake E: D50 = 5.3 μm;
[0059] Glass flake F: D50 = 239.7 μm;
[0060] The D50 particle size is measured using a Malvern wet-type laser particle size analyzer to determine the particle size corresponding to the 50% cumulative distribution percentage. Examples and Comparative Examples: Preparation of a high-temperature-resistant polyester composition: A polyester resin, filler, and light diffuser are mixed in a high-speed mixer according to the desired ratio. The mixture is melt-blended and extruded into pellets through a twin-screw extruder to obtain a high-temperature-resistant polyester composition. The extruder is heated at the following temperatures: 250-290°C for zone 1, 260-300°C for zones 2-4, 270-310°C for zones 5-7, 260-300°C for zones 8-9, and 250-290°C for the die. The retained aspect ratio of the glass fiber can be controlled by adjusting the shear strength of the screw, or the glass fiber can be pre-crushed to a particle size close to the designed range.
[0061] Various test methods:
[0062] (1) Test method for aspect ratio of glass fiber and D50 particle size of glass flakes in high temperature resistant polyester compositions:
[0063] Glass fiber aspect ratio: Weigh 100g of material sample and ablate it at 800℃ for 1h and cool it to obtain the glass fiber in the material. Disperse the obtained glass fiber evenly in 200ml of water, pour 10ml of the glass fiber suspension into a culture dish, select several areas using a microscope, and project the glass fiber areas onto a screen. Take pictures, test the length of the glass fiber in the pictures and make a normal distribution graph. The value corresponding to the median in the normal distribution graph is the glass fiber retention length. The ratio of glass fiber retention length / glass fiber diameter (or flat glass fiber major axis diameter) is taken as the glass fiber aspect ratio.
[0064] Glass flake D50 particle size: A 100g sample was ablated at 800°C for 1 hour and then cooled to obtain glass flakes. The resulting glass flakes were evenly dispersed in 200ml of water and the particle size was measured using a Malvern Panalytical laser particle size analyzer. The D50 particle size of the glass flakes was obtained from the test results.
[0065] (2) Light transmittance: The light transmittance of sample A (2856K) was measured using an SGW-820 (WGT-2S) light transmittance meter. A test piece with a length of 60 mm, a width of 60 mm, and a thickness of 1 mm was prepared by injection molding.
[0066] (3) Reflectance: Measured using a Color Eye 7000A colorimeter. Test pieces with a length of 60 mm, a width of 60 mm, and a thickness of 1 mm were prepared by injection molding at a mold temperature of 60°C. The reflectance was evaluated using the reflectance at 460 nm as a representative value.
[0067] Table 1: Content of each component (parts by weight) and test results of polyester compositions of Examples 1-7
[0068] It can be seen from Examples 2 / 4-6 that the light diffusing agents containing the structure of the present invention can significantly improve the light reflectivity, and the polyester composition also has a relatively high light transmittance.
[0069] Table 2: Content of each component (parts by weight) and test results of polyester compositions of Examples 8-15
[0070] It can be seen from Examples 2 / 7-9 that when the content of the light diffusing agent is preferably 0.0005-0.001 times the weight content of the PCT resin, both the transmittance and the reflectivity are higher.
[0071] Table 2:
[0072] It can be seen from Examples 2 / 10-15 that as the aspect ratio increases, the transmittance increases but the reflectivity decreases. In order to prepare an SMD type LED reflective bracket, the aspect ratio of the circular glass fiber is preferably 5-300, more preferably 15-200.
[0073] Table 3: Content of each component (parts by weight) and test results of polyester compositions of Examples 16-25
[0074] It can be seen from Examples 16-19 that the preferred aspect ratio of the flat glass fiber is 4-6, which results in higher transmittance and reflectivity.
[0075] Table 3:
[0076] It can be seen from Examples 16 / 20-25 that as the aspect ratio increases, the transmittance increases but the reflectivity decreases. In order to prepare an SMD type LED reflective bracket, the aspect ratio of the circular glass fiber is preferably 1-200, more preferably 3-100.
[0077] Table 4: Content of each component (parts by weight) and test results of polyester compositions of Examples 26-31
[0078] It can be seen from Examples 26-31 that as the D50 particle size of the glass flakes increases, the transmittance increases but the reflectivity decreases. The preferred D50 particle size is 10-200 microns, and more preferably 20-160 microns.
[0079] Table 5: Content of each component (parts by weight) and test results of comparative polyester composition
[0080] It can be seen from Example 2 and Comparative Example 1 that the traditional light diffusing agent cannot achieve the effects of high light transmittance and high reflection.
[0081] It can be seen from Comparative Examples 2 / 3 / 4 that if the light diffusing agent content is too low, not only the reflectivity is low, but also the transmittance is insufficient; if the light diffusing agent content is too high, the transmittance is too low.
[0082] [Corrected 09.05.2024 according to Rule 26] It can be seen from Comparative Example 5 that although titanium dioxide can significantly improve the reflectivity, it will also seriously reduce the transmittance.
Claims
1. A polyester composition, characterized in that By weight, it includes the following components: 50-80 parts of PCT resin; 8-40 parts of filler; Light diffuser 0.01-0.1 part; The filler is selected from at least one of flat glass fiber, round glass fiber and glass flakes; The structure of the light diffuser is wherein R2, R3, R4, and R5 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 1 to 9 carbon atoms, a halogen atom, a heterocyclic group having 1 to 6 carbon atoms, an ester group having 1 to 6 carbon atoms, and a cyano group; R1 is One of them.
2. The polyester composition according to claim 1, characterized in that R1 is One of them.
3. The polyester composition according to claim 1, characterized in that The weight content of the light diffusing agent is 0.0005-0.001 times the weight content of the PCT resin.
4. The polyester composition according to claim 1, characterized in that In the polyester composition, the aspect ratio of the flat glass fiber is in the range of 0.3-228, preferably 1-200, more preferably 3-100; the flatness ratio of the cross section of the flat glass fiber is 2-7, preferably 4-6.
5. The polyester composition according to claim 1, characterized in that In the polyester composition, the aspect ratio of the round glass fiber is in the range of 2-352, preferably 5-300, more preferably 15-200.
6. The polyester composition according to claim 1, characterized in that In the polyester composition, the D50 particle size range of the glass flakes is 5-250 microns, preferably 10-200 microns, and more preferably 20-160 microns.
7. The polyester composition according to claim 1, characterized in that The melting point of the PCT resin measured by differential scanning calorimetry at a heating and cooling rate of 20°C / min is 260-300°C.
8. The polyester composition according to claim 1, characterized in that By weight, the invention further comprises 0-2 parts of auxiliary agent, wherein the auxiliary agent is selected from at least one of an antioxidant and a lubricant.
9. The method for preparing the polyester composition according to any one of claims 1 to 8, characterized in that: The invention comprises the following components: polyester resin, filler and light diffuser are mixed according to a proportion, the mixture is melt-blended and extruded into granules through an extruder to obtain a high-temperature resistant polyester composition; wherein the heating temperatures of the extruder are as follows: 250-290°C for zone 1, 260-300°C for zones 2-4, 270-310°C for zones 5-7, 260-300°C for zones 8-9 and 250-290°C for the die.
10. Use of the polyester composition according to any one of claims 1 to 8, characterized in that: Used to prepare SMD type LED reflector bracket.
Citation Information
Patent Citations
Light aging resistant photodiffusion polycarbonate composite material and preparation method thereof
CN103772940A
Light-diffusion anti-dazzle PC material and preparation method thereof
CN104672840A
Light-diffusing flame-retardant polycarbonate material for LED lighting, and preparation method thereof
CN107245233A
Polyester composition as well as preparation method and application thereof
CN116987367A
Resin composition for forming light diffusion plates, light diffusion plate, display device, and electronic apparatus
JP2020071401A