Polyester composition, and preparation method therefor and use thereof

By introducing a copolyester of terephthalic acid and cyclohexyl dimethanol units into polybutylene terephthalate and a specific plasticizer, the problem of low laser welding transmittance and flash is solved, and the Welding strength and hydrolysis resistance, suitable for the manufacture of laser welded parts.

WO2024222704A1PCT designated stage expired Publication Date: 2024-10-31JIANGSU KINGFA SCI & TECH ADVANCED MATERIALS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/089429
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing polybutylene terephthalate has low transmittance during laser welding, which easily leads to overwelding and flashing at the welding position, and its performance declines in aqueous environments, limiting its application in laser welding.

Method used

A copolyester containing terephthalic acid and cyclohexyl dimethanol units is used in combination with a specific plasticizer to increase laser transmittance and welding strength through an exchange reaction, and a laser welding polyester composition is prepared through a twin-screw extruder. Reduce foaming and spillage.

Benefits of technology

It significantly improves the transmittance and welding strength of laser welding, reduces foaming and flashing phenomena, and improves the hydrolysis resistance of the polyester composition, making it suitable for manufacturing high-quality laser welded parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024089429-FTAPPB-I100001
    Figure PCTCN2024089429-FTAPPB-I100001
  • Figure PCTCN2024089429-FTAPPB-I100002
    Figure PCTCN2024089429-FTAPPB-I100002
  • Figure PCTCN2024089429-FTAPPB-I100003
    Figure PCTCN2024089429-FTAPPB-I100003
Patent Text Reader

Abstract

Disclosed in the present invention is a polyester composition. The polyester composition comprises the following components in parts by weight: 100 parts of a PBT resin, 5-30 parts of a copolyester containing terephthalic acid and cyclohexyl dimethyl carbinol units, and 0.5-16 parts of a plasticizer, wherein the plasticizer is a fatty acid ester plasticizer containing two or more ester bond functional groups. In the present invention, by selecting the specific plasticizer and the specific-content copolyester containing the terephthalic acid and cyclohexyl dimethyl carbinol units, the laser transmittance can be effectively improved, such that the laser welding strength is improved, and the selected plasticizer does not lead to the hydrolysis of the polyester composition; moreover, foaming and overflowing in a laser welding process can be reduced by means of the copolyester containing the terephthalic acid and the cyclohexyl dimethyl carbinol unit. Therefore, the polyester composition of the present invention is suitable for laser welding.
Need to check novelty before this filing date? Find Prior Art

Description

A polyester composition and its preparation method and application Technical Field

[0001] The present invention relates to the technical field of polymer materials, in particular to a polyester composition and a preparation method and application thereof. Background Art

[0002] Due to their excellent molding processability, mechanical properties, dimensional stability, and chemical resistance, thermoplastic polyester parts are widely used in automobiles, home appliances, power tools, electronic appliances, and medical devices. However, complex structural parts are difficult to mold in a single step and must be processed into smaller parts before being joined. Consequently, a variety of joining technologies have been developed for plastic parts, including adhesive bonding, mechanical fastening, fusion bonding, and welding. Welding methods are also diverse, and are categorized by heat source, including vibration welding, hot plate welding, laser welding, and ultrasonic welding. Hot plate welding, vibration welding, and ultrasonic welding, due to the large-area heat treatment and mechanical action, are prone to over-welding and flashing at the weld site. These excess heat and mechanical action can easily affect surrounding structures. Laser welding is a well-suited joining method for thermoplastic polymers. Unlike other welding methods, laser welding generates heat through laser radiation without contact with the parts. This non-contact welding operation produces high-quality welds, offering the advantages of energy transfer without contact with the weld interface, avoiding internal stresses, and generating no thermal load. The energy delivered by the laser beam is precisely controlled in terms of area and time. The width of the weld is generally in the order of 100 microns, while the welding reaction time is in the millisecond level. Therefore, laser welding has the potential for short cycles, automation, and high integration.

[0003] Prior art technology has shown that unmodified polybutylene terephthalate (PBTA) exhibits low laser transmittance, absorbing most near-infrared laser energy. This limits the use of laser penetration welding, limiting its application in laser-welded products. Due to the narrow laser welding window, increasing the power or extending the welding time has limited success and can even lead to scorching of the welded component surface. The accumulated burnt material further reduces laser transmittance.

[0004] The existing technology uses sodium aliphatic carboxylates or aromatic sodium carboxylates to improve laser transmittance. Since weak acid and strong base salts form an alkaline environment in humid air or aqueous solution, it is extremely detrimental to the performance of polyester materials. This effect is also considered to be a base-catalyzed hydrolysis reaction.

[0005] Summary of the Invention

[0006] The object of the present invention is to provide a laser welding polyester composition having the advantages of high laser welding strength and less foaming and flashing during the laser welding process.

[0007] Another object of the present invention is to provide a preparation method and application of the laser welding polyester composition.

[0008] The present invention is achieved through the following technical solutions:

[0009] A polyester composition comprising the following components in parts by weight:

[0010] 100 parts of PBT resin;

[0011] 5-30 parts of a copolyester containing terephthalic acid and cyclohexyl dimethanol units;

[0012] 0.5-16 parts of plasticizer;

[0013] Wherein, the plasticizer is a fatty acid ester plasticizer containing ≥2 ester bond functional groups;

[0014] The copolyester containing terephthalic acid and cyclohexyl dimethanol units includes diacid units and diol units, wherein the diacid units include terephthalic acid and other diacid units, and the other diacid units include at least one of aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and aromatic dicarboxylic acids; the diol units include cyclohexyl dimethanol and other diol units, and the other diol units include at least one of aliphatic alkylene glycol, polyalkoxy glycol, alicyclic diol, and aromatic diol; and the cyclohexyl dimethanol accounts for 50-80 mol% of the total molar proportion of all diol units, and the terephthalic acid units account for 50-100 mol% of the total molar proportion of the diacid units.

[0015] When the copolyester containing terephthalic acid and cyclohexyl dimethanol units is less than 5 parts, the laser transmittance cannot be effectively improved, and when it is greater than 30 parts, the laser welding strength is not ideal. When the plasticizer is less than 0.5 parts, the laser transmittance is not ideal, and when the plasticizer is greater than 16 parts, the laser welding strength is not ideal.

[0016] Preferably, the following components are included in parts by weight:

[0017] 100 parts of PBT resin;

[0018] 13-22 parts of a copolyester containing terephthalic acid and cyclohexyl dimethanol units;

[0019] Plasticizer 4.5-13 parts.

[0020] The total molar proportion of cyclohexyl dimethanol in all diol units is 60-70 mol%.

[0021] Specifically, in the copolyester containing terephthalic acid and cyclohexyl dimethanol units, the aliphatic dicarboxylic acid is selected from at least one of glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecyl dicarboxylic acid, dodecyl dicarboxylic acid, and hexadecyl dicarboxylic acid; the alicyclic dicarboxylic acid is selected from at least one of hexahydrophthalic acid, hexahydroisophthalic acid, and hexahydroterephthalic acid; and the aromatic dicarboxylic acid is selected from at least one of terephthalic acid, phthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 4,4'-diphenyl methane dicarboxylic acid, and 4,4'-diphenyl ketone dicarboxylic acid.

[0022] The aliphatic alkylene glycol is selected from at least one of ethylene glycol, propylene glycol, pentanediol, neopentyl glycol, hexanediol, heptanediol, octanediol, nonanediol, and decanediol; the polyalkoxy glycol is selected from at least one of diethylene glycol, dipropylene glycol, dibutylene glycol, triethylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol, and polybutylene glycol; the alicyclic diol is selected from at least one of 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, spirodiol, and 1,3-cyclobutanediol; and the aromatic diol is selected from at least one of hydroquinone, resorcinol, biphenol, bisphenols, and benzyl alcohol.

[0023] Copolyesters containing terephthalic acid and cyclohexyl dimethanol units can be commercially available or can be prepared by self-production. The self-production method is as follows:

[0024] The copolyester is synthesized by direct esterification melt condensation. Terephthalic acid, cyclohexyl dimethanol monomers and other comonomers are added to a polymerization kettle, and a certain amount of catalyst is added. The molar ratio of the diol monomer to the diacid is 0.8-1.7. The polymerization kettle goes through three different stages. The first stage is completed by reacting at a reaction temperature of 230-240°C for about 4 hours or when the water output reaches 94-96% of the theoretical value. The second stage is transferred to high-temperature and low-pressure polymerization. The reaction is completed by reacting at a reaction temperature of 230-240°C and a low pressure of 0.05-0.1 MPa for 0.5-1 hour. The third stage is transferred to increase the vacuum degree to 10-80 Pa and continue the reaction for 2-4 hours. Finally, the material is discharged under the protection of a nitrogen atmosphere and cooled for granulation.

[0025] The plasticizer is selected from at least one of di(2-ethyl)hexyl phthalate, dibutyl phthalate, dioctyl terephthalate, trioctyl trimellitate, tetraoctyl pyromellitate, diisononyl phthalate, diisodecyl phthalate, diheptyl phthalate, dioctyl adipate, dioctyl sebacate, tributyl citrate, trioctyl citrate, triethyl citrate, acetyl tributyl citrate, and trioctyl acetyl citrate; preferably, at least one of fatty acid ester plasticizers having ≥3 ester functional groups (tributyl citrate, trioctyl citrate, triethyl citrate, acetyl tributyl citrate, and trioctyl acetyl citrate); more preferably, a fatty acid ester plasticizer having ≥4 ester functional groups (tetraoctyl pyromellitate). The preferred plasticizer not only has higher hydrolysis resistance but also higher laser welding strength.

[0026] The intrinsic viscosity of the PBT resin is 0.58-2.5 dl / g, which is measured after dissolving in o-cresol / chloroform solvent at 25°C.

[0027] The glass transition temperature of the copolyester containing terephthalic acid and cyclohexyl dimethanol units is in the range of 80-150°C.

[0028] You can choose to add 0-1 part of antioxidant according to actual needs. The antioxidant is a hindered phenol antioxidant, a sulfur-containing antioxidant, etc.

[0029] The laser absorber may be laser absorbing carbon black, and an optional brand is Birla's Raven M.

[0030] The preparation method of the laser welding polyester composition of the present invention comprises the following steps: uniformly mixing the components according to a proportion, extruding and granulating the components through a twin-screw extruder, with the screw speed ranging from 150 rpm to 600 rpm and the temperature ranging from 210° C. to 250° C., to obtain the laser welding polyester composition.

[0031] The laser welding polyester composition of the present invention is used to manufacture laser welding parts, such as laser radar, camera housing, motor housing, tailgate support rod, etc.

[0032] The present invention has the following beneficial effects:

[0033] The present invention discovered that the cyclohexyl dimethanol structure in a copolyester containing terephthalic acid and cyclohexyl dimethanol units can effectively exchange with PBT materials to form cyclohexyl dimethanol terephthaloyl copolymer units, thereby improving laser transmittance. By selecting a specific plasticizer and combining it with the copolyester containing terephthalic acid and cyclohexyl dimethanol units, the present invention can effectively improve laser transmittance, thereby increasing laser welding strength and enhancing the hydrolysis resistance of the polyester composition. Furthermore, the copolyester containing terephthalic acid and cyclohexyl dimethanol units can reduce foaming and flashing during laser welding, thereby improving laser welding strength. This makes the polyester composition of the present invention suitable for laser welding. DETAILED DESCRIPTION

[0034] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those skilled in the art, several variations and improvements can be made without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.

[0035] The raw materials used in the present invention come from the following sources:

[0036] PBT: PBT GX112, intrinsic viscosity 0.74 dl / g;

[0037] A copolyester containing terephthalic acid and cyclohexyl dimethanol units (hereinafter referred to as copolyester) was prepared according to the method described in the summary of the invention:

[0038] Copolyester A: terephthalic acid / 1,4-cyclohexanedimethanol / hydroquinone, cyclohexane dimethanol accounts for 50 mol% of the total molar ratio of all diol units, glass transition temperature 140°C;

[0039] Copolyester B: terephthalic acid / 1,4-cyclohexanedimethanol / hydroquinone, cyclohexane dimethanol accounts for 60 mol% of the total molar ratio of all diol units, glass transition temperature 138°C;

[0040] Copolyester C: terephthalic acid / 1,4-cyclohexanedimethanol / hydroquinone, cyclohexane dimethanol accounts for 70 mol% of the total molar ratio of all diol units, glass transition temperature 135°C;

[0041] Copolyester D: terephthalic acid / 1,4-cyclohexanedimethanol / hydroquinone, cyclohexane dimethanol accounts for 80 mol% of the total molar ratio of all diol units, glass transition temperature 134°C;

[0042] Copolyester E: terephthalic acid / adipic acid / 1,4-cyclohexanedimethanol / ethylene glycol, cyclohexane dimethanol accounts for 60 mol% of the total molar ratio of all diol units, terephthalic acid units account for 80 mol% of the total molar ratio of diacid units, and glass transition temperature is 85°C;

[0043] Copolyester F: terephthalic acid / adipic acid / 1,4-cyclohexanedimethanol / ethylene glycol, cyclohexane dimethanol accounts for 60 mol% of the total molar ratio of all diol units, terephthalic acid units account for 50 mol% of the total molar ratio of diacid units, glass transition temperature 83°C;

[0044] Copolyester G: terephthalic acid / 1,4-cyclohexanedimethanol / hydroquinone, cyclohexane dimethanol accounts for 40 mol% of the total molar ratio of all diol units, glass transition temperature 145°C;

[0045] Copolyester H: terephthalic acid / 1,4-cyclohexanedimethanol / hydroquinone, cyclohexane dimethanol accounts for 90 mol% of the total molar ratio of all diol units, glass transition temperature 132°C;

[0046] Tetraoctyl pyromellitate: TOPM, Hubei Shixing Chemical Co., Ltd.

[0047] Trioctyl trimellitate: TOTM, Guangzhou Textile;

[0048] Triethyl citrate: TEC, Guangzhou Textile;

[0049] Dibutyl phthalate: BDP, Jinan Century Tongda Chemical Co., Ltd.

[0050] Dioctyl terephthalate: DOTP, Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0051] Butylparaben: Sigma-Aldrich;

[0052] Benzyl-4-hydroxybenzoate: Hubei Kewode Chemical Co., Ltd.

[0053] N-Butylbenzenesulfonic acid amide: JZ-218, Suzhou Jinzhong Chemical;

[0054] Laser absorption of carbon black: Raven M, Birla.

[0055] The preparation method of the laser welding polyester composition of the embodiment and the comparative example is as follows: the components are mixed uniformly according to the ratio, and granulated by extrusion through a twin-screw extruder. The screw speed range is 250-500 rpm, and the temperature of each section of the screw is set to 210°C ~ 250°C to obtain a laser welding polyester composition.

[0056] Various test methods:

[0057] (1) Laser Transmittance: The polyester composition (excluding laser-absorbing carbon black) was dried in an oven at 120°C for 4 hours and then molded into 80 mm × 50 mm × 2 mm specimens (2 mm thick) using an injection molding machine at a barrel temperature of 280°C and a mold temperature of 120°C. The transmittance of the specimens at a wavelength of 980 nm was measured using a near-infrared spectrometer (wavelength: 900-1700 nm, Ocean Optics NIRQuest spectrometer).

[0058] (2) Laser weldability: The laser-transparent polyester composition was placed in an oven at 120°C and dried for 4 hours. The composition was then molded into 130 mm × 14 mm × 2 mm strips using an injection molding machine. The strips were used as welding counterparts. The laser absorption portion was prepared by using the same method as the laser polyester composition and containing a laser absorbent. The barrel temperature was 280°C and the mold temperature was 120°C. The two strips were overlapped, and the laser-transparent polyester composition strip was placed toward the laser focusing window for laser welding. Laser welding operation: The overlapped strips were placed in a plastic material laser welding system (Dazzle Laser, model WFD120 W-PCTS333SP). The laser beam was subjected to a diode laser (wavelength of 915 nm), a laser radius of 200 μm, a welding power of 20 W, a welding speed of 20 mm / s, and a welding length of 130 mm × 3 (to reduce errors, three independent welds without overlap were performed, each weld was parallel and spaced 6 mm apart). The pressure of the pneumatic holding device was 0.5 MPa. After laser welding, the specimens were conditioned at 50% relative humidity and 23 ± 2°C for 4 hours. Shear strength was tested using a tensile testing machine (Zwick / Roell Z010). Tensile testing was performed along the longitudinal axis of the welded specimens, with a span of 120 mm and a tensile speed of 5 mm / min. The average shear strength of the three parallel welds was recorded as the laser weld strength (unit: N).

[0059] (3) Evaluation of laser welding blistering and flashing:

[0060] After the laser welded specimens are subjected to tensile shear failure, the overall width of the weld on both sides after the extension of the flash is observed. When the width is ≤2mm, it can be considered that there is no flash due to blistering, and it is determined to be Level 1; when the width is >2mm and ≤2.5mm, there is slight flash due to blistering, and it is determined to be Level 2; when the width is >2.5mm and ≤3mm, there is obvious flash due to blistering, and it is determined to be Level 3; when the width is >3mm and ≤3mm, there is serious flash due to blistering, and it is determined to be Level 4.

[0061] (4) Hydrolysis resistance rating method: According to ISO 527-2 / 1A, a 4 mm thick test bar with a width of 10 mm was prepared by molding at a test speed of 5 mm / min. The tensile strength in air at 23°C was used as the initial tensile strength. The tensile specimen was placed in an autoclave, and the autoclave was filled with deionized water. The autoclave was sealed and placed in an oven at a temperature of 120°C for 200 hours. The autoclave was taken out and cooled to room temperature. The tensile strength was also tested according to ISO 527-2 / 1A at a test speed of 5 mm / min at 23°C as the tensile strength after hydrolysis. The performance retention rate was calculated based on the ratio of the tensile strength after hydrolysis to the initial tensile strength.

[0062] Note: The laser absorbing composition in the examples of the present invention and the comparative examples contains laser absorbing carbon black, while the laser transmitting composition does not contain laser absorbing carbon black. The other components are the same.

[0063] Table 1: Content (parts by weight) of each component in the laser welding polyester composition of Examples 1-6 and test results

[0064] It can be seen from Examples 1-8 that as the content of the copolyester containing terephthalic acid and cyclohexyl dimethanol units and the plasticizer increases, the laser transmittance and hydrolysis resistance increase. At the preferred addition amount of the copolyester containing terephthalic acid and cyclohexyl dimethanol units and the plasticizer, the laser welding strength is higher and the blistering and overflow are minimized.

[0065] Table 2: Content (parts by weight) of each component in the laser welding polyester composition of Examples 9-13 and test results

[0066] It can be seen from Examples 2 / 9-13 that the copolyesters with the preferred cyclohexyl dimethanol content range have better laser welding strength and resistance to blistering and flashing.

[0067] Table 3: Content (parts by weight) of each component in the laser welding polyester composition of Examples 14-17 and test results

[0068] As can be seen from Examples 4 / 14-17, the plasticizer mainly affects the hydrolysis resistance and laser welding strength. Preferably, at least one fatty acid ester plasticizer containing ≥3 ester functional groups is used; more preferably, a fatty acid ester plasticizer containing ≥4 ester functional groups is used.

[0069] Table 4: Comparative Example Laser Welding Polyester Composition Component Content (Parts by Weight) and Test Results

[0070] It can be seen from Comparative Examples 1-2 that if the copolyester of the present invention is not contained or the added amount is too low, the laser transmittance is low and the laser weldability is poor.

[0071] As can be seen from Comparative Example 3, if the copolyester content of the present invention is too high, although it has extremely high laser transmittance, the laser welding strength is reduced, and the effect of suppressing blistering and flashing is not obvious.

[0072] It can be seen from Comparative Example 4 that without the plasticizer of the present invention, the laser welding strength does not reach the level of the present invention, and the hydrolysis resistance is poor.

[0073] It can be seen from Comparative Example 5 that if the plasticizer content of the present invention is too high, the laser weldability will be reduced and the hydrolysis resistance will also be poor.

[0074] Continued Table 1:

[0075] It can be seen from Comparative Examples 6 and 7 that if the content of cyclohexyl dimethanol units in the copolyester is outside the range of the present invention, the laser weldability is significantly reduced.

[0076] It can be seen from Comparative Examples 8-10 that other types of plasticizers do not significantly improve the laser welding ability.

Claims

1. A polyester composition, It is characterized in that By weight, it includes the following components: PBT resin 100 parts; 5-30 parts of copolyester containing terephthalic acid and cyclohexyl dimethanol units; Plasticizer 0.5-16 parts; Wherein, the plasticizer is a fatty acid ester plasticizer containing ≥2 ester bond functional groups; The copolyester containing terephthalic acid and cyclohexyl dimethanol units comprises diacid units and diol units, wherein the diacid units comprise terephthalic acid and other diacid units, wherein the other diacid units comprise at least one of aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and aromatic dicarboxylic acids; the diol units comprise cyclohexyl dimethanol and other diol units, wherein the other diol units comprise at least one of aliphatic alkylene glycol, polyalkoxy glycol, alicyclic diol, and aromatic diol; and the total molar proportion of cyclohexyl dimethanol to all diol units is 50-80 mol%, and the total molar proportion of terephthalic acid units to the total molar proportion of diacid units is 50-100 mol%.

2. The polyester composition according to claim 1, It is characterized in that By weight, it includes the following components: PBT resin 100 parts; 13-22 parts of copolyester containing terephthalic acid and cyclohexyl dimethanol units; Plasticizer 4.5-13 parts.

3. The polyester composition according to claim 1, It is characterized in that The total molar proportion of cyclohexyl dimethanol to all diol units is 60-70 mol%.

4. The polyester composition according to claim 1, It is characterized in that The aliphatic dicarboxylic acid is selected from at least one of glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecyl dicarboxylic acid, dodecyl dicarboxylic acid, and hexadecyl dicarboxylic acid; the alicyclic dicarboxylic acid is selected from at least one of hexahydrophthalic acid, hexahydroisophthalic acid, and hexahydroterephthalic acid; the aromatic dicarboxylic acid is selected from at least one of terephthalic acid, phthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 4,4'-diphenyl methane dicarboxylic acid, and 4,4'-diphenyl ketone dicarboxylic acid; The aliphatic alkylene glycol is selected from at least one of ethylene glycol, propylene glycol, pentylene glycol, neopentyl glycol, hexanediol, heptanediol, octanediol, nonanediol, and decanediol; the polyalkoxy glycol is selected from at least one of diethylene glycol, dipropylene glycol, dibutylene glycol, triethylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol, and polybutylene glycol; the alicyclic diol is selected from at least one of 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, At least one of diols, spirodiols, and 1,3-cyclobutanediol; the aromatic diol is selected from at least one of hydroquinone, resorcinol, biphenol, bisphenols, and benzyl alcohol.

5. The laser welding polyester composition according to claim 1, It is characterized in that The plasticizer is selected from at least one of di(2-ethyl)hexyl phthalate, dibutyl phthalate, dioctyl terephthalate, trioctyl trimellitate, tetraoctyl pyromellitate, diisononyl phthalate, diisodecyl phthalate, diheptyl phthalate, dioctyl adipate, dioctyl sebacate, tributyl citrate, trioctyl citrate, triethyl citrate, acetyl tributyl citrate, and trioctyl acetyl citrate; preferably at least one of the fatty acid ester plasticizers containing ≥3 ester bond functional groups; more preferably, the fatty acid ester plasticizers contain ≥4 ester bond functional groups.

6. The polyester composition according to claim 1, It is characterized in that The intrinsic viscosity of the PBT resin is 0.58-2.5 dl / g, which is measured after being dissolved in o-cresol / chloroform solvent at 25°C.

7. The laser welding polyester composition according to claim 1, It is characterized in that By weight, the invention also includes 0-1 part of antioxidant and 0.1-2 parts of laser absorber.

8. A method for preparing the polyester composition according to any one of claims 1 to 7, It is characterized in that The method comprises the following steps: mixing the components uniformly according to the proportion, extruding and granulating through a twin-screw extruder, wherein the screw speed range is 150 rpm-600 rpm and the temperature range is 210° C.-250° C., and obtaining a laser welding polyester composition.

9. Use of the polyester composition according to any one of claims 1 to 7, It is characterized in that Used to manufacture laser welded parts.

Citation Information

Patent Citations

  • Polybutylene terephthalate composition with cold and hot impact resistance

    CN112625406A

  • Polyester resin composition and molded article thereof

    CN114391032A

  • Polyester composition as well as preparation method and application thereof

    CN116410579A

  • Resin composition for laser welding and molded article

    CN1863870A

  • Resin composition for laser welding and molded product

    JP2004315805A