Semi-aromatic polyamide composition, and preparation method therefor and use thereof
By using a mixture of PA6T/6I and PAMXD6 and specific carbon fiber in semi-aromatic polyamide, combined with the amide exchange effect of PA66 and aniline black dye, the problem of traditional materials being difficult to balance mechanical properties and surface appearance is solved, achieving high rigidity and Good looking composite material with improved 'floating fiber' problem and flowability.
Patent Information
- Application Number
- PCT/CN2024/089733
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
It is difficult for traditional semi-aromatic polyamides to take into account the surface appearance of the material while improving its mechanical properties. Especially when filled with high proportions of glass fiber and carbon fiber, surface problems such as ‘floating fibers’ are prone to occur, which affects the dimensional stability and electrical properties of the material.
By selecting a mixture of PA6T/6I and PAMXD6 in semi-aromatic polyamide as the matrix, and combining it with carbon fiber with a specific fiber diameter and elastic modulus, the rigidity and surface appearance of the material are optimized, and PA66 is added for amide exchange to slow down the crystallization rate. , using aniline black as a dye to cover the 'floating fiber' problem, and performing melt granulation in a twin-screw extruder.
It achieves a balance between high rigidity and good appearance of the material, significantly improves the problem of 'floating fibers', improves the surface effect and fluidity of the composite material, and ensures efficient injection molding and surface quality of the material.
Smart Images

Figure PCTCN2024089733-FTAPPB-I100001 
Figure PCTCN2024089733-FTAPPB-I100002 
Figure PCTCN2024089733-FTAPPB-I100003
Abstract
Description
Semi-aromatic polyamide composition and preparation method and application thereof
[0001] Related applications
[0002] This application claims priority to Chinese patent application No. 2023104748523, filed on April 27, 2023, entitled “Semi-aromatic polyamide composition, preparation method and application thereof”, the entire text of which is hereby incorporated by reference. Technical Field
[0003] The present application relates to the technical field of polymer materials, and in particular to a semi-aromatic polyamide composition and a preparation method and application thereof. Background Art
[0004] Polyamide is a general term for thermoplastic resins containing repeating amide groups in their molecular backbone. They possess excellent mechanical properties, friction and wear resistance, self-lubrication, shock absorption, and sound absorption, and are resistant to oils, alkalis, weak acids, and common organic solvents. However, their disadvantage is their high water absorption, which affects their dimensional stability and electrical properties. Polyamides are categorized into aliphatic polyamides, aromatic polyamides, semi-aromatic polyamides, polyimides, and copolyamides. Semi-aromatic polyamides are a general term for polyamides whose molecular backbone contains both aromatic rings and aliphatic chains.
[0005] With the steady progress of the transformation and upgrading of "plastic replacing steel", the requirements for the mechanical properties of plastic materials are gradually increasing. Although in the product design process, the lack of mechanical strength of plastic materials can be compensated by structural design or increasing wall thickness, there is still an urgent need for a composite material that takes into account both the rigidity and surface appearance of the material to further promote the application of plastic replacing steel. In order to further improve the strength of semi-aromatic polyamides, traditional methods usually add high levels of reinforcing materials such as glass fiber and carbon fiber to the system, but even so, the elastic modulus of the composite material is difficult to reach above 30GPa. At the same time, with a high proportion of glass fiber and carbon fiber filling, the fluidity of the material will be significantly deteriorated, which makes it easy to have surface problems such as "floating fibers". In summary, the traditional modification of semi-aromatic polyamides is difficult to take into account both the mechanical properties and surface appearance of the material.
[0006] Summary of the Invention
[0007] Based on this, according to various embodiments of the present application, a semi-aromatic polyamide composition, a preparation method and an application thereof are provided.
[0008] The technical solution is as follows:
[0009] Based on this, the present application provides a semi-aromatic polyamide composition, which has both high rigidity and good appearance.
[0010] This application is implemented through the following technical solutions.
[0011] A semi-aromatic polyamide composition, comprising the following components in percentage by mass:
[0012] The semi-aromatic polyamide is a mixture of PA6T / 6I and PAMXD6 or PA6T / 6I; in the PA6T / 6I, the molar ratio of 6T to 6I is (68-72):(28-32);
[0013] In the mixture of PA6T / 6I and PAMXD6, the mass ratio of PA6T / 6I to PAMXD6 is (70-92):(8-30);
[0014] The diameter of the single fiber of the carbon fiber is 5 μm to 7 μm, and the elastic modulus e of the carbon fiber satisfies 240 GPa≤e≤380 GPa.
[0015] In one embodiment, the PA6T / 6I is prepared by polymerizing raw materials including hexamethylenediamine, terephthalic acid, isophthalic acid, a catalyst and a nucleating agent at 210° C. to 240° C.
[0016] In one embodiment, the dye is nigrosine.
[0017] In one embodiment, the relative viscosity of the PA6T / 6I is measured according to ASTM D 789-2006 and is 2.2-2.7.
[0018] In one embodiment, the relative viscosity of PAMXD6 is measured according to ASTM D 789-2006 and is 2.4-2.9.
[0019] In one embodiment, in the mixture of PA6T / 6I and PAMXD6, the mass ratio of PA6T / 6I to PAMXD6 is (65-85.5):(14.5-35).
[0020] In one embodiment, the aliphatic polyamide is PA66.
[0021] In one embodiment, the relative viscosity of the PA66 is measured according to ASTM D 789-2006 and is 2.7 to 3.2.
[0022] The present application also provides a method for preparing the semi-aromatic polyamide composition as described above, comprising the following steps:
[0023] Mix the components, melt, granulate and extrude.
[0024] In one embodiment, the extrusion is carried out in a twin-screw extruder, and the conditions of the twin-screw extruder include: a screw aspect ratio of 48:1, a barrel temperature of 260° C. to 340° C., and a screw speed of 200 rpm to 400 rpm.
[0025] The present application also provides applications of the semi-aromatic polyamide composition described above in the fields of automobiles, sports equipment, medical devices or aviation.
[0026] The details of one or more embodiments of the present application are set forth in the description below, and other features, objects, and advantages of the application will become apparent from the description and from the claims thereof. DETAILED DESCRIPTION
[0027] To facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant examples. The preferred embodiments of the present application are provided in the examples. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0028] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of this application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0029] The terms "preferably," "more preferably," and the like in this application refer to embodiments of the present application that may provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of this application.
[0030] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein are understood to include any and all subranges subsumed therein.
[0031] Unless otherwise indicated, all percentages, fractions, and ratios are calculated based on the total weight of the compositions herein. Unless otherwise indicated, all masses relating to listed ingredients refer to the active ingredient content and therefore do not include solvents or byproducts that may be present in commercially available materials. The term "mass percentage content" herein may be expressed using the symbol "%." Unless otherwise indicated, all molecular weights herein are weight-average molecular weights expressed in Daltons. Unless otherwise indicated, all formulations and testing herein took place at 25°C. The terms "comprise," "include," "contain," "have," "have," and other variations herein are intended to encompass non-exclusive inclusions, and do not distinguish between these terms. The term "comprising" means that additional steps and ingredients that do not affect the end result may be added. The compositions and methods / processes herein comprise, consist of, and consist essentially of the essential elements and limitations described herein, as well as any additional or optional ingredients, components, steps, or limitations described herein. The terms "efficacy," "performance," "effect," and "efficacy" are not used herein to distinguish between.
[0032] The weights of the relevant components mentioned in the examples of this application may not only refer to the specific content of each component, but also represent the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the examples of this application, it is within the scope disclosed in the examples of this application. Specifically, the weights described in the examples of this application may be mass units known in the chemical industry such as ug, mg, g, and kg.
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are intended only to describe specific embodiments and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0034] The present application provides a semi-aromatic polyamide composition, which comprises the following components in percentage by mass:
[0035] The semi-aromatic polyamide is a mixture of PA6T / 6I and PAMXD6 or PA6T / 6I; in PA6T / 6I, the molar ratio of 6T to 6I is (68-72):(28-32);
[0036] In the mixture of PA6T / 6I and PAMXD6, the mass ratio of PA6T / 6I to PAMXD6 is (70-92):(8-30);
[0037] The single fiber diameter of the carbon fiber is 5μm~7μm, and the elastic modulus e of the carbon fiber satisfies 240GPa≤e≤380GPa, e includes but is not limited to 240GPa, 250GPa, 260GPa, 270GPa, 280GPa, 290GPa, 310GPa, 320GPa, 330GPa, 340GPa, 350GPa and 380GPa, preferably, e is 240GPa~290GPa.
[0038] This application selects PA6T / 6I as the matrix in a semi-aromatic polyamide composition, while limiting the molar ratio of 6T to 6I units to improve the rigidity of the composition. This is then compounded with carbon fibers having a specific fiber diameter and elastic modulus, resulting in a better interfacial bonding effect between the carbon fibers and the semi-aromatic polyamide, improving the rigidity of the material while further optimizing the surface appearance. Furthermore, the applicant unexpectedly discovered that the addition of a semi-aromatic polyamide, PAMXD6, to the composition, and limiting the mass ratio of PAMXD6 to PA6T / 6I, not only further improves the rigidity of the composition, but also, due to the amide exchange reaction between MXD6 and PA6T / 6I, can slow the crystallization rate of both materials to a certain extent. When combined with high mold temperatures, the composite material achieves a better appearance and significantly improves the "floating fiber" problem.
[0039] In a specific example, the precursor type of the carbon fiber is polyacrylonitrile-based. It can be understood that in this application, the carbon fiber uses PAN-based carbon fiber prepared from polyacrylonitrile.
[0040] It is understood that in the present application, PA6T / 6I refers to poly (hexamethylene terephthalamide / isophthalamide), wherein the diacids in the monomers are terephthalic acid and isophthalic acid, and the diamine in the monomers is hexamethylenediamine.
[0041] It is understood that in the present application, PAMXD6 is poly(m-xylylenediamine adipamide), wherein the diacid in the monomer is adipic acid and the diamine in the monomer is m-xylylenediamine.
[0042] In a specific example, PA6T / 6I is prepared by polymerizing raw materials including hexamethylenediamine, terephthalic acid, isophthalic acid, a catalyst and a nucleating agent at 210° C. to 240° C.
[0043] More specifically, the preparation of PA6T / 6I includes the following steps:
[0044] Hexamethylenediamine, terephthalic acid, isophthalic acid, a catalyst, a nucleating agent and water are mixed in a pressure autoclave, vacuumed, filled with inert gas, heated to 210°C to 220°C, kept warm for 0.5h to 1.5h, then heated to 230°C to 240°C, kept at a constant temperature of 230°C to 240°C and a constant pressure of 2.1MPa to 2.3MPa for 1.5h to 2.5h, discharged, dried to prepare a prepolymer product; and solid-phase thickening of the prepolymer product for 8h to 12h to prepare PA6T / 6I.
[0045] In one specific example, the dye is nigrosine.
[0046] This application selects aniline black as a dye, which can effectively cover the white spots caused by floating fibers through its own "coloring" effect. Moreover, aniline black does not have the "nucleating effect" like traditional black pigments, and will not accelerate the crystallization rate of the system, further improving the surface effect of the composite material.
[0047] In one specific example, the nucleating agent is benzoic acid.
[0048] In one specific example, the catalyst is sodium hypophosphite.
[0049] In one specific example, the inert gas is nitrogen.
[0050] In one specific example, the molar ratio of terephthalic acid to isophthalic acid is 70:30.
[0051] In one specific example, the molar ratio of hexamethylenediamine to terephthalic acid is 102:70.
[0052] In a specific example, the molar ratio of hexamethylenediamine to isophthalic acid is 102:30.
[0053] In a specific example, the amount of the nucleating agent is 2% to 3% of the total amount of hexamethylenediamine, terephthalic acid, and isophthalic acid. More specifically, the amount of the nucleating agent is 2.5% of the total amount of hexamethylenediamine, terephthalic acid, and isophthalic acid.
[0054] In a specific example, the weight of the catalyst is 0.05% to 0.15% of the total weight of hexamethylenediamine, terephthalic acid, isophthalic acid, the catalyst, and the nucleating agent. More specifically, the weight of the catalyst is 0.1% of the total weight of hexamethylenediamine, terephthalic acid, isophthalic acid, the catalyst, and the nucleating agent.
[0055] In a specific example, the weight of water is 25% to 35% of the total weight of the feed, more specifically, the weight of water is 30% of the total weight of the feed.
[0056] In a specific example, the conditions for solid phase adhesion include: a temperature of 220° C. to 280° C. and a vacuum degree of 45 Pa to 55 Pa. More specifically, the conditions for solid phase adhesion include: a temperature of 250° C. and a vacuum degree of 50 Pa.
[0057] In a specific example, the relative viscosity of PA6T / 6I measured according to ASTM D 789-2006 is 2.2-2.7.
[0058] In a specific example, the preparation of PAMXD6 includes the following steps:
[0059] m-Xylylenediamine, adipic acid, a catalyst, a nucleating agent and water are mixed in a pressure autoclave, vacuumed, filled with inert gas, heated to 210°C to 220°C, kept warm for 0.5h to 1.5h, then heated to 230°C to 240°C, kept at a constant temperature of 230°C to 240°C and a constant pressure of 2.1MPa to 2.3MPa for 1.5h to 2.5h, discharged, dried to prepare a prepolymer product; and solid-phase thickening of the prepolymer product for 8h to 12h to prepare PAMXD6.
[0060] In one specific example, the nucleating agent is benzoic acid.
[0061] In one specific example, the catalyst is sodium hypophosphite.
[0062] In one specific example, the inert gas is nitrogen.
[0063] In a specific example, the molar ratio of m-xylylenediamine to adipic acid is (102-104):100.
[0064] In a specific example, the amount of the nucleating agent is 2% to 3% of the total amount of m-xylylenediamine and adipic acid. More specifically, the amount of the nucleating agent is 2.5% of the total amount of m-xylylenediamine and adipic acid.
[0065] In a specific example, the weight of the catalyst is 0.05% to 0.15% of the total weight of m-xylenediamine, adipic acid, the catalyst and the nucleating agent. More specifically, the weight of the catalyst is 0.1% of the total weight of m-xylenediamine, adipic acid, the catalyst and the nucleating agent.
[0066] In a specific example, the weight of water is 25% to 35% of the total weight of the feed, more specifically, the weight of water is 30% of the total weight of the feed.
[0067] In a specific example, the conditions for solid phase adhesion include: a temperature of 220° C. to 280° C. and a vacuum degree of 45 Pa to 55 Pa. More specifically, the conditions for solid phase adhesion include: a temperature of 250° C. and a vacuum degree of 50 Pa.
[0068] In a specific example, the relative viscosity of PAMXD6 measured according to ASTM D 789-2006 is 2.4 to 2.9, including but not limited to 2.4, 2.5, 2.6, 2.7, 2.8 and 2.9.
[0069] In a specific example, in the mixture of PA6T / 6I and PAMXD6, the mass ratio of PA6T / 6I to PAMXD6 is (70-85.5):(14.5-30).
[0070] In a specific example, the aliphatic polyamide is PA66.
[0071] This application introduces polyamide PA66 into PA6T / 6I for an amide exchange reaction to slow the material's crystallization rate, thereby improving floating fibers. Furthermore, due to the high processing temperature of this system, exceeding 300°C, PA66 has a high melting point (265°C), making it suitable for this system. Furthermore, at the processing temperature of PA6T / 6I, PA66 has a fluidity far exceeding that of PA6T / 6I and MXD6, allowing it to accumulate in the cortex of the part during the "fountain" flow of injection molding, effectively masking "floating fibers."
[0072] In a specific example, the relative viscosity of PA66 measured according to ASTM D 789-2006 is 2.7 to 3.2. More specifically, the relative viscosity of PA66 is 2.7.
[0073] The present application also provides a method for preparing the above-mentioned semi-aromatic polyamide composition, comprising the following steps:
[0074] The components are mixed, then melted, pelletized, and extruded.
[0075] In a specific example, the extrusion is carried out in a twin-screw extruder, and the conditions of the twin-screw extruder include: a screw length-diameter ratio of 48:1, a barrel temperature of 260° C. to 340° C., and a screw speed of 200 rpm to 400 rpm.
[0076] The present application also provides applications of the semi-aromatic polyamide composition in the fields of automobiles, sports equipment, medical devices or aviation.
[0077] The semi-aromatic polyamide composition and its preparation method of the present application are further described in detail below with reference to specific examples. Unless otherwise specified, the raw materials used in the following examples are all commercially available products.
[0078] Semi-aromatic polyamide:
[0079] PA6T / 6I-1: 6T / 6I=70 / 30, relative viscosity 2.2, homemade;
[0080] PA6T / 6I-2: 6T / 6I=68 / 32, relative viscosity 2.2, homemade;
[0081] PA6T / 6I-3: 6T / 6I=72 / 28, relative viscosity 2.2, homemade;
[0082] PA6T / 6I-4: 6T / 6I=80 / 20, relative viscosity 2.1, homemade;
[0083] PA6T / 6I-5: 6T / 6I=60 / 40, relative viscosity 2.2, homemade;
[0084] The relative viscosity test is performed according to ASTM D 789-2006.
[0085] The above-mentioned PA6T / 6I homemade steps are as follows: add hexamethylenediamine, terephthalic acid and isophthalic acid monomers in a molar ratio of 102: (60-80): (20-40) in a pressure autoclave; then add benzoic acid, sodium hypophosphite (catalyst) and deionized water; the amount of benzoic acid substance is 2.5% of the total amount of hexamethylenediamine, terephthalic acid and isophthalic acid, the weight of sodium hypophosphite is 0.1% of the weight of other materials except deionized water, and the weight of deionized water is 30% of the total weight of the materials; vacuumize and fill with high-purity nitrogen as a protective The mixture was heated to 220° C. within 2 hours under stirring, the reaction mixture was stirred at 220° C. for 1 hour, and then the temperature of the reactants was raised to 230° C. under stirring; the reaction was continued at a constant temperature of 230° C. and a constant pressure of 2.2 MPa for 2 hours, and the pressure was kept constant by removing the formed water. After the reaction was completed, the prepolymer was discharged, and the prepolymer was vacuum-dried at 80° C. for 24 hours to obtain a prepolymer product. The prepolymer product was solid-phase thickened at 250° C. and a vacuum condition of 50 Pa for 10 hours to obtain PA6T / 6I with the corresponding structure.
[0086] PAMXD6: relative viscosity 2.4, homemade; relative viscosity test was conducted in accordance with ASTM D 789-2006.
[0087] The homemade steps of the above-mentioned PAMXD6 are as follows: m-xylenediamine and adipic acid monomers are added to a pressure autoclave in a molar ratio of (102-104):100; benzoic acid, sodium hypophosphite (catalyst) and deionized water are then added; the amount of benzoic acid is 2.5% of the total amount of m-xylenediamine and adipic acid, the weight of sodium hypophosphite is 0.1% of the weight of the other materials except deionized water, and the weight of deionized water is 30% of the total weight of the materials; vacuum is filled with high-purity nitrogen as a protective gas, and the mixture is stirred for 2 hours. The temperature was raised to 220° C., the reaction mixture was stirred at 220° C. for 1 hour, and then the temperature of the reactants was raised to 230° C. with stirring; the reaction was continued at a constant temperature of 230° C. and a constant pressure of 2.2 MPa for 2 hours, and the pressure was kept constant by removing the formed water. After the reaction was completed, the prepolymer was discharged and vacuum-dried at 80° C. for 24 hours to obtain a prepolymer product. The prepolymer product was solid-phase thickened at 250° C. and 50 Pa vacuum conditions for 10 hours to obtain PAMXD6 with the corresponding structure.
[0088] Carbon Fiber:
[0089] Carbon Fiber-1: STS40, PAN-based, single-filament diameter 7 μm, elastic modulus 240 GPa, Teijin Company;
[0090] Carbon Fiber-2: IMS60, PAN-based, single-filament diameter 5 μm, elastic modulus 290 GPa, Teijin Company;
[0091] Carbon Fiber-3: UMS40, PAN-based, single-filament diameter 5 μm, elastic modulus 390 GPa, Teijin Company;
[0092] Carbon fiber-4: PX35-65, PAN-based, single filament diameter 9 μm, elastic modulus 240 GPa, Zoltek;
[0093] Aliphatic polyamide:
[0094] PA66: relative viscosity 2.7, PA66 EPR27, China Pingmei Shenma Group;
[0095] dye:
[0096] Aniline black: Paliotol Black L0080, BASF, Germany.
[0097] Carbon black: M717, Cabot Corporation, USA.
[0098] The components were uniformly mixed according to the formulation amounts (mass percentages) of Examples 1 to 13 described in Table 1 and Comparative Examples 1 to 14 described in Table 2, and then added to a twin-screw extruder for melt granulation and extrusion to obtain a carbon fiber-reinforced semi-aromatic polyamide composition. The twin-screw extruder had a screw aspect ratio of 48:1, a barrel temperature of 260°C to 340°C, and a screw speed of 200 rpm to 400 rpm.
[0099] Table 1
[0100] Table 2 Note: “-” in the table means that the substance is not added.
[0101] Performance Testing
[0102] The semi-aromatic polyamide compositions prepared in Examples 1 to 13 and Comparative Examples 1 to 14 were subjected to performance tests, including elastic modulus and chromaticity value tests. The specific test methods are as follows:
[0103] (1) Elastic modulus: The carbon fiber reinforced semi-aromatic polyamide composition was heated and melted at 320°C to 340°C and injection molded into a tensile specimen. The tensile properties were tested in accordance with the international standard ISO 527-2019 at a tensile speed of 10 mm / min to obtain the elastic modulus.
[0104] (2) Chromaticity L: A carbon fiber-reinforced semi-aromatic polyamide composition was heated and melted at 320°C to 340°C, and injection molded into a 60 mm × 60 mm × 2 mm sample with a mold temperature of 130°C. The sample's chromaticity L was then measured using a colorimeter. This study found that when the surface of a part molded from a semi-aromatic polyamide composition exhibits apparent appearance defects such as "floating fibers" or "trapped air," the sample's chromaticity L increases significantly. Combined with visual evaluation, the following criteria can be used to evaluate the surface quality of the material.
[0105] Excellent: L value ≤ 28;
[0106] Good: 28<L value<33;
[0107] Difference: L value ≥ 33.
[0108] The test results of Examples 1 to 13 are shown in Table 3.
[0109] Table 3
[0110] The test results of Comparative Examples 1 to 14 are shown in Table 4.
[0111] Table 4
[0112] According to the test results in Table 3, the carbon fiber-reinforced semi-aromatic polyamide composite material prepared in this embodiment of the present application has an elastic modulus greater than or equal to 32 GPa, indicating excellent rigidity. Furthermore, the composite material has a chromaticity value L less than 33, and visually demonstrates a good surface appearance. This demonstrates that the semi-aromatic polyamide composition exhibits excellent surface properties.
[0113] As can be seen from Table 4, for the composite material without the addition of PA66 and aniline black (see Comparative Example 1), the surface effect of the material is poor. When the molar ratio of 6T to 6I is 80:20, which belongs to the PA6T / 6I resin not disclosed in this application (see Comparative Example 2), the rigidity of the material is poor and the surface effect is also poor. When the carbon fiber content used is lower than the range disclosed in this application (see Comparative Example 3), the rigidity of the material is poor. When the carbon fiber content used is higher than the range disclosed in this application (see Comparative Example 4), although the rigidity of the material is very good, the surface effect is poor. When a combination of PA6T / 6I and MXD6 ratios other than those disclosed in this application is used (see Comparative Examples 5 and 6), it is difficult for the material to simultaneously obtain good rigidity and surface effect. When carbon fibers other than those disclosed in this application are used (see Comparative Example 7), the rigidity of the material is poor. When using PA66 content outside the scope of this application (see Comparative Examples 8 and 9), the lower PA66 content makes it difficult to enrich the surface, resulting in poor surface effects. When using higher PA66 content, due to its low melting point, PA66 decomposes at current processing temperatures, resulting in poor surface effects. When using aniline black content outside the scope of this application (see Comparative Examples 10 and 11), lower amounts of aniline black make it difficult to achieve dyeing, resulting in poor surface effects. Higher amounts of aniline black easily decompose and produce more gas, trapping the material and also leading to poor surface effects. When the PA6T / 6I content and carbon fiber used in the composition are outside the scope of this application, the surface effects of the material are poor (see Comparative Example 12). Comparing Examples 8 and 13, it can be seen that when the PA6T / 6I content in the composition is outside the scope of this application, the material's rigidity is poor. Replacing aniline black with other soft materials, such as carbon black, can produce a "nucleation effect," accelerating the crystallization rate of the system and impairing the surface effects of the composite material (see Comparative Example 14).
[0114] Obviously, the above embodiments of the present application are merely examples for the purpose of clearly illustrating the present application, and are not intended to limit the embodiments of the present application. For those skilled in the art, other variations or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present application shall be included within the scope of protection of the claims of the present application.
[0115] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0116] The embodiments described above only express several implementation methods of the present application, which are convenient for understanding the technical solutions of the present application in a specific and detailed manner, but they cannot be understood as limiting the scope of protection of the patent application. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all fall within the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent application of this application shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A semi-aromatic polyamide composition, characterized in that In terms of mass percentage, it includes the following components: The semi-aromatic polyamide is a mixture of PA6T / 6I and PAMXD6; in the PA6T / 6I, the molar ratio of 6T to 6I is (68-72):(28-32); In the mixture of PA6T / 6I and PAMXD6, the mass ratio of PA6T / 6I to PAMXD6 is (70-92):(8-30); The single fiber diameter of the carbon fiber is 5 μm to 7 μm, and the elastic modulus e of the carbon fiber satisfies 240 GPa≤e≤380 GPa; The dye is aniline black; The aliphatic polyamide is PA66.
2. The semi-aromatic polyamide composition according to claim 1, characterized in that The PA6T / 6I is prepared by polymerizing raw materials including hexamethylenediamine, terephthalic acid, isophthalic acid, a catalyst and a nucleating agent at 210° C. to 240° C.
3. The semi-aromatic polyamide composition according to claim 1 or 2, characterized in that: The relative viscosity of the PA6T / 6I measured according to ASTM D 789-2006 is 2.2 to 2.7; and / or, The relative viscosity of the PAMXD6 measured according to ASTM D 789-2006 is 2.4-2.
9.
4. The semi-aromatic polyamide composition according to any one of claims 1 to 3, characterized in that The preparation of PAMXD6 comprises the following steps: Mix m-phenylenediamine, adipic acid, a catalyst, a nucleating agent and water in a pressure autoclave, evacuate, fill with inert gas, heat to 210°C-220°C, keep warm for 0.5h-1.5h, then heat to 230°C-240°C, keep at a constant temperature of 230°C-240°C and a constant pressure of 2.1MPa-2.3MPa for 1.5h-2.5h, discharge, dry and prepare a prepolymer product; solid phase thicken the prepolymer product for 8h-12h to prepare the PAMXD6.
5. The semi-aromatic polyamide composition according to any one of claims 1 to 4, characterized in that In the mixture of PA6T / 6I and PAMXD6, the mass ratio of PA6T / 6I to PAMXD6 is (70-85.5):(14.5-30).
6. The semi-aromatic polyamide composition according to any one of claims 1 to 5, characterized in that The relative viscosity of the PA66 measured according to ASTM D 789-2006 is 2.7-3.
2.
7. The semi-aromatic polyamide composition according to any one of claims 1 to 6, characterized in that The relative viscosity of the PA66 measured according to ASTM D 789-2006 is 2.
7.
8. A method for preparing a semi-aromatic polyamide composition according to any one of claims 1 to 7, characterized in that: The steps include: Mixing of components, melting, granulation, extrusion.
9. The method for preparing a semi-aromatic polyamide composition according to claim 8, characterized in that: The process is carried out in a twin-screw extruder, wherein the conditions of the twin-screw extruder include: a screw length-diameter ratio of 48:1, a barrel temperature of 260° C. to 340° C., and a screw speed of 200 rpm to 400 rpm.
10. Use of the semi-aromatic polyamide composition according to any one of claims 1 to 7 in the fields of automobiles, sports equipment, medical equipment or aviation.
Citation Information
Patent Citations
Flame-proofed polyamide molding materials and the use thereof
CN102618023A
Polyamide composition and molded article
CN110506079A
Semi-aromatic polyamide composition as well as preparation method and application thereof
CN116790116A
A semiaromatic polyamide and the preparation method thereof
WO2009079886A1
Semi-aromatic polyamide composition, preparation method therefor and use thereof
WO2022110677A1