Preparation method for electronic-grade ammonium fluoride

By adopting preheating reaction and ion exchange purification combined with ethanol drip purification in the preparation of ammonium fluoride, the problems of low purity of ammonium fluoride product and low preparation efficiency were solved, and electronic-grade fluorination with a purity of 99.9% was efficiently prepared. ammonium, simplifying the process and reducing energy consumption.

WO2024222873A1PCT designated stage expired Publication Date: 2024-10-31FUJIAN TIANFU ELECTRONIC MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/090080
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing ammonium fluoride preparation process has low product purity and low preparation and purification process efficiency, making it difficult to efficiently prepare electronic-grade ammonium fluoride.

Method used

Preheated hydrogen fluoride solution is reacted with ammonia water or ammonia gas, the pH value is controlled to ≤5.0, and high-purity ammonium fluoride is directly produced through two steps of ion exchange purification and ethanol drip purification, simplifying the synthesis path and improving preparation efficiency.

Benefits of technology

The preparation of 99.9% ultra-high purity ammonium fluoride is achieved, which significantly improves the preparation efficiency, eliminates multiple recrystallization processes, and greatly saves energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to the field of chemical synthesis, and in particular to a preparation method for electronic-grade ammonium fluoride. The method comprises: (1) reacting a preheated hydrogen fluoride solution with 0.8-1.0 Eq of ammonia water or ammonia gas, and supplementing hydrogen fluoride in the reaction process to control the pH value to be less than or equal to 5.0 to obtain a crude product solution; and (2) carrying out ion exchange purification and ethanol dripping purification on the crude product solution to obtain electronic-grade ammonium fluoride. According to the present invention, existing ammonium fluoride preparation processes are simplified and then are combined with a unique two-step purification method, so that the preparation effect of ammonium fluoride can be improved, and electronic-grade ammonium fluoride having the purity of 99.9% is directly prepared; and in the preparation method, multiple recrystallization processes required by a traditional preparation method are omitted, thereby greatly improving preparation efficiency, and remarkably reducing energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

A preparation method of electronic grade ammonium fluoride Technical Field

[0001] The invention belongs to the field of chemical synthesis, and in particular relates to a method for preparing electronic-grade ammonium fluoride. Background Art

[0002] Ammonium fluoride is a white crystal with the molecular formula NH₄F. It is highly deliquescent and decomposes into ammonia and hydrogen fluoride when heated or exposed to hot water. It can corrode glass. Traditional methods for preparing ammonium fluoride include liquid-phase and gas-liquid two-phase methods.

[0003] The liquid-phase preparation method typically involves neutralizing hydrofluoric acid with ammonia followed by concentration and crystallization. This method is relatively inefficient and cannot guarantee complete reaction. Therefore, to promote the forward reaction, an excess of hydrogen fluoride is often used. Similarly, the gas-liquid two-phase contact method also requires a slight excess of hydrogen fluoride. However, the use of excessive hydrogen fluoride results in a very limited purity of the product.

[0004] This is because in the obtained product, ammonium fluoride mainly forms ammonium fluoride through NH-F hydrogen bond, and the effect of this hydrogen bond causes to exist a certain amount of hydrogen fluoride impurity that is inevitable, almost difficult to remove in the common product, and it may exist with forms such as ammonium bifluoride.And the ammonium fluoride of electronic grade usually needs at least 99.9% ultra-high purity, and adopts conventional recrystallization method, industrially can not realize purification preparation in large quantities, on a large scale.To this, developing a kind of method that can directly and continuously produce electronic grade ammonium fluoride is very important. Technical issues

[0005] In order to solve the problems that the ammonium fluoride product obtained by the existing ammonium fluoride preparation process has low purity, the existing preparation and purification process has low efficiency and limited effect, and it is difficult to efficiently prepare electronic-grade ammonium fluoride, the present invention provides a method for preparing electronic-grade ammonium fluoride.

[0006] The objects of the present invention are:

[0007] 1. It can directly produce electronic grade ammonium fluoride with a purity of up to 99.9%;

[0008] Second, the preparation efficiency is improved, and continuous production and preparation can be achieved. Technical Solutions

[0009] To achieve the above objectives, the present invention adopts the following technical solutions.

[0010] A method for preparing electronic-grade ammonium fluoride, comprising:

[0011] (1) Preheated hydrogen fluoride solution is reacted with 0.8 to 1.0 Eq of ammonia water or ammonia gas, and hydrogen fluoride is added during the reaction process to control the pH value to ≤5.0 to obtain a crude product liquid;

[0012] (2) The crude product solution is purified by ion exchange and ethanol dropwise purification to obtain electronic grade ammonium fluoride.

[0013] The present invention first simplifies the synthesis route of ammonium fluoride and controls the excess of hydrogen fluoride. Compared with traditional liquid-phase and / or gas-liquid two-phase preparation methods, the present invention simplifies the crystallization process and can directly perform the subsequent two-step purification treatment on the crude product liquid to obtain ultra-high-purity electronic-grade ammonium fluoride.

[0014] As a preference,

[0015] The hydrogen fluoride solution used in step (1) is a hydrogen fluoride aqueous solution with a concentration of 10 to 50 wt%.

[0016] The above-mentioned concentration of hydrogen fluoride aqueous solution is a commonly used solution concentration for industrial production of ammonium fluoride and has a relatively stable production and synthesis effect.

[0017] As a preference,

[0018] The ammonia content in the ammonia water or ammonia gas used in the step (1) is calculated based on the hydrogen fluoride contained in the hydrogen fluoride solution used, and the ammonia content is controlled to be 0.8 to 1.0 Eq.

[0019] The present invention controls the amount of hydrogen fluoride to be slightly excessive to ensure that the subsequent impurity components are mainly hydrogen fluoride. The Eq is the equivalent required for the theoretical reaction, such as 1 mol of hydrogen fluoride, corresponding to 1 Eq of ammonia is 1 mol of ammonia, and the same applies to the following.

[0020] As a preference,

[0021] The ion exchange purification in step (2) comprises:

[0022] The electrolytic cell is divided into a cathode region and an anode region by a cation exchange membrane, the crude product solution obtained in step (1) is used as the cathode region electrolyte, a carbon electrode is used as the cathode electrode, an aqueous sodium hydroxide and / or potassium hydroxide solution is used as the anode region electrolyte, and a copper electrode is used as the anode electrode. After electrolysis, the cathode region electrolyte is recovered, excess anhydrous ethanol is added to dissolve ammonium fluoride, and the ammonium fluoride is removed by dehydration with an inert desiccant, and then filtered to remove solid impurities, and purified ammonium fluoride is obtained by crystallization.

[0023] The ion exchange purification used in the present invention is a directional ion exchange, so that the hydrogen fluoride in the crude ammonium fluoride liquid is fully transformed. In the specific process, in the anode area, sodium hydroxide aqueous solution and / or potassium hydroxide aqueous solution are used. In the actual industrial production process, a saturated solution can be directly used or sodium hydroxide and / or potassium hydroxide with a hydrogen fluoride content of at least 1.5 Eq in the crude liquid can be used to prepare an aqueous solution according to the crude liquid characterization results. During the electrolysis process, the copper electrode loses electrons and oxidizes into the sodium hydroxide or potassium hydroxide aqueous solution and forms a complex precipitation to avoid copper ions entering the cathode area to cause loss of ammonium ions. During the electrolysis process, the hydrogen ions in the cathode area are reduced to hydrogen gas. To maintain the electrical neutrality of the electrolysis system, the sodium ions and / or potassium ions in the anode area are exchanged and enter the cathode area. After the electrolysis process is completed, the components in the cathode area electrolyte recovered are converted into ammonium fluoride and sodium fluoride and / or potassium fluoride, and instead of the traditional multiple recrystallization method to remove hydrogen fluoride, the present invention uses solubility difference to directly separate sodium fluoride and potassium fluoride. In anhydrous ethanol, ammonium fluoride still maintains a certain solubility, but sodium fluoride and potassium fluoride are insoluble. Moreover, since the fluorine content in the solution increases after the ammonium fluoride dissolves, it actually further limits the solubility of sodium fluoride and potassium fluoride. Therefore, after dehydration and drying, the present invention uses a special recrystallization method to directly, effectively and thoroughly remove excess fluoride impurities, thereby obtaining a purified ammonium fluoride product with a purity of more than 99.6 wt%. The recovery rate of ammonium fluoride is close to 100%, and no ammonium fluoride loss occurs.

[0024] As a preference,

[0025] During the electrolysis process, the starting voltage was controlled to be 1.23 V and the ending voltage was controlled to be 1.32-1.34 V.

[0026] During the constant current electrolysis process, the electrolysis potential changes as the solution systems in the anode and cathode regions change. In actual production and preparation, once the voltage reaches the above-mentioned cut-off voltage, it can be generally determined that the hydrogen fluoride in the cathode electrolyte has been completely reacted. Further increasing the cut-off voltage will not further improve the preparation effect, but will instead lead to increased energy consumption.

[0027] As a preference,

[0028] After the cathode electrolyte is recovered, the cathode electrolyte is mixed with anhydrous ethanol having a volume of at least 48 times the volume of the cathode electrolyte.

[0029] A large amount of anhydrous ethanol is used to ensure that ammonium fluoride in the cathode electrolyte can be effectively recovered, so as to improve the yield of the product.

[0030] As a preference,

[0031] The inert desiccant is calcium oxide;

[0032] The amount of calcium oxide used is controlled so that its loose volume is at least 0.8 times the recovered cathode electrolyte.

[0033] The present invention uses excess calcium oxide to remove residual water in the cathode electrolyte because water and anhydrous ethanol are miscible and the presence of water will affect the impurity content in the final product.

[0034] As a preference,

[0035] The ethanol dropwise purification in step (2) comprises:

[0036] The product obtained by ion exchange purification is slowly dissolved in anhydrous ethanol until the purified ammonium fluoride product no longer dissolves, and then the solid matter is removed by solid-liquid separation. The anhydrous ethanol solution of ammonium fluoride is crystallized again to obtain electronic grade ammonium fluoride.

[0037] The purified product is subjected to further dropwise purification to further remove a very small amount of residual impurities, thereby further improving the purity of the ammonium fluoride product. Beneficial effects

[0038] The beneficial effects of the present invention are:

[0039] (1) The present invention combines the existing ammonium fluoride preparation process with a simplified process and combines it with a unique two-step purification method to improve the preparation effect of ammonium fluoride and directly produce electronic grade ammonium fluoride with a purity of 99.9%;

[0040] (2) The preparation method eliminates the multiple recrystallization processes required by traditional preparation methods, greatly improving the preparation efficiency and significantly saving energy consumption. Modes for Carrying Out the Invention

[0041] The present invention is further described in detail below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only a portion of the embodiments of the present invention, rather than all of the embodiments. Therefore, all other embodiments derived by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0042] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0043] Example 1: A method for preparing electronic grade ammonium fluoride, comprising:

[0044] (1) A hydrogen fluoride solution (20 wt%) preheated to 85 °C was used as the liquid phase reactant. 0.8 Eq of ammonia was introduced into the hydrogen fluoride solution for reaction. During the reaction, an equal concentration (20 wt%) of hydrogen fluoride was added to dynamically control the pH value of the reaction system to 4.0-5.0 to obtain a crude liquid.

[0045] (2) An electrolytic cell is provided, which is divided into a cathode region and an anode region by a cation exchange membrane N2050WX (Nafion ion exchange membrane), a carbon electrode is provided in the cathode region, a saturated sodium hydroxide aqueous solution is provided in the anode region as the anode region electrolyte, and a copper electrode is used as the anode electrode. The sodium hydroxide equivalent in the saturated sodium hydroxide aqueous solution used is about 2.7 Eq. The crude product liquid obtained in step (1) is placed in the cathode region as the cathode region electrolyte, and electrolysis is performed by power supply, and the starting voltage is controlled to be 1.23 V and the ending voltage is controlled to be 1.32 V. After the electrolysis is completed, the cathode region electrolyte obtained is recovered and mixed with 48 times the volume of anhydrous ethanol, and then industrial quicklime with a loose volume of 0.8 times the cathode region electrolyte is added to remove water and dry. After filtering to remove the precipitate, the precipitate is evaporated at low pressure at 20 ° C and the anhydrous ethanol is recovered, and the crystallized product is recovered to obtain the purified ammonium fluoride product, and at least 50 Slowly add anhydrous ethanol to dissolve kg of purified ammonium fluoride product, and control the addition rate of anhydrous ethanol to add 15 mL of anhydrous ethanol per minute per gram of purified ammonium fluoride product. After the purified ammonium fluoride product no longer dissolves within 2 consecutive minutes, vacuum filtration is performed to separate and remove insoluble matter. The anhydrous ethanol solution of ammonium fluoride is placed at 20°C and evaporated under low pressure. After recovering the anhydrous ethanol, the crystalline product is recovered to obtain an electronic grade ammonium fluoride product.

[0046] The maximum theoretical yield is calculated based on the amount of ammonia used, the purity and ammonium fluoride content of the electronic-grade ammonium fluoride product are characterized, the actual yield is calculated, and the yield of ammonium fluoride is calculated based on the maximum theoretical yield and the actual yield.

[0047] The specific calculation formula of recovery rate is: recovery rate = (actual yield / maximum theoretical yield) × 100%;

[0048] Through characterization and calculation, the purity of the purified ammonium fluoride product obtained in this example is 99.9%, and the calculated yield is 98.1%.

[0049] Example 2: A method for preparing electronic grade ammonium fluoride, comprising:

[0050] (1) A hydrogen fluoride solution (50 wt%) preheated to 85 °C was used as the liquid phase reactant. 1.0 Eq of ammonia was introduced into the hydrogen fluoride solution for reaction. During the reaction, an equal concentration (50 wt%) of hydrogen fluoride was added to dynamically control the pH value of the reaction system to 4.0-5.0 to obtain a crude liquid.

[0051] (2) An electrolytic cell is provided, which is divided into a cathode region and an anode region by a cation exchange membrane N2050WX (Nafion ion exchange membrane), a carbon electrode is provided in the cathode region, a saturated sodium hydroxide aqueous solution is provided in the anode region as the anode region electrolyte, and a copper electrode is used as the anode electrode. The sodium hydroxide equivalent in the saturated sodium hydroxide aqueous solution used is about 2.7 Eq. The crude product liquid obtained in step (1) is placed in the cathode region as the cathode region electrolyte, and electrolysis is performed by power supply, and the starting voltage is controlled to be 1.23 V and the ending voltage is controlled to be 1.32 V. After the electrolysis is completed, the cathode region electrolyte obtained is recovered and mixed with 48 times the volume of anhydrous ethanol, and then industrial quicklime with a loose volume of 0.8 times the cathode region electrolyte is added to remove water and dry. After filtering to remove the precipitate, the precipitate is evaporated at low pressure at 20 ° C and the anhydrous ethanol is recovered, and the crystallized product is recovered to obtain the purified ammonium fluoride product, and at least 50 Slowly add anhydrous ethanol to dissolve kg of purified ammonium fluoride product, and control the addition rate of anhydrous ethanol to add 15 mL of anhydrous ethanol per minute per gram of purified ammonium fluoride product. After the purified ammonium fluoride product no longer dissolves within 2 consecutive minutes, vacuum filtration is performed to separate and remove insoluble matter. The anhydrous ethanol solution of ammonium fluoride is placed at 20°C and evaporated under low pressure. After recovering the anhydrous ethanol, the crystalline product is recovered to obtain an electronic grade ammonium fluoride product.

[0052] The maximum theoretical yield is calculated based on the amount of ammonia used, the purity and ammonium fluoride content of the electronic-grade ammonium fluoride product are characterized, the actual yield is calculated, and the yield of ammonium fluoride is calculated based on the maximum theoretical yield and the actual yield.

[0053] The specific calculation formula of recovery rate is: recovery rate = (actual yield / maximum theoretical yield) × 100%;

[0054] Through characterization and calculation, the purity of the purified ammonium fluoride product obtained in this example is 99.9%, and the calculated yield is 96.2%.

[0055] Example 3: A method for preparing electronic grade ammonium fluoride, comprising:

[0056] (1) A hydrogen fluoride solution (20 wt%) preheated to 85 °C was used as the liquid phase reactant. 0.8 Eq of ammonia was introduced into the hydrogen fluoride solution for reaction. During the reaction, an equal concentration (20 wt%) of hydrogen fluoride was added to dynamically control the pH value of the reaction system to 4.0-5.0 to obtain a crude liquid.

[0057] (2) An electrolytic cell is provided, which is divided into a cathode region and an anode region by a cation exchange membrane N2050WX (Nafion ion exchange membrane), a carbon electrode is provided in the cathode region, a saturated potassium hydroxide aqueous solution is provided in the anode region as the anode region electrolyte, and a copper electrode is used as the anode electrode. The potassium hydroxide equivalent in the saturated potassium hydroxide aqueous solution used is about 2.9 Eq. The crude product liquid obtained in step (1) is placed in the cathode region as the cathode region electrolyte, and electrolysis is performed by power supply, and the starting voltage is controlled to be 1.23 V and the ending voltage is controlled to be 1.32 V. After the electrolysis is completed, the cathode region electrolyte is recovered and mixed with 48 times the volume of anhydrous ethanol, and then industrial quicklime with a loose volume of 0.8 times the cathode region electrolyte is added to remove water and dry. After filtering to remove the precipitate, the precipitate is evaporated at low pressure at 20 ° C and the anhydrous ethanol is recovered, and the crystallized product is recovered to obtain the purified ammonium fluoride product, and at least 50 Slowly add anhydrous ethanol to dissolve kg of purified ammonium fluoride product, and control the addition rate of anhydrous ethanol to add 15 mL of anhydrous ethanol per minute per gram of purified ammonium fluoride product. After the purified ammonium fluoride product no longer dissolves within 2 consecutive minutes, vacuum filtration is performed to separate and remove insoluble matter. The anhydrous ethanol solution of ammonium fluoride is placed at 20°C and evaporated under low pressure. After recovering the anhydrous ethanol, the crystalline product is recovered to obtain an electronic grade ammonium fluoride product.

[0058] The maximum theoretical yield is calculated based on the amount of ammonia used, the purity and ammonium fluoride content of the electronic-grade ammonium fluoride product are characterized, the actual yield is calculated, and the yield of ammonium fluoride is calculated based on the maximum theoretical yield and the actual yield.

[0059] The specific calculation formula of recovery rate is: recovery rate = (actual yield / maximum theoretical yield) × 100%;

[0060] Through characterization and calculation, the purity of the purified ammonium fluoride product obtained in this example is 99.9%, and the calculated yield is 97.9%.

[0061] Example 4: A method for preparing electronic grade ammonium fluoride, comprising:

[0062] (1) A hydrogen fluoride solution (20 wt%) preheated to 85 °C was used as the liquid phase reactant. 0.8 Eq of ammonia was introduced into the hydrogen fluoride solution for reaction. During the reaction, an equal concentration (20 wt%) of hydrogen fluoride was added to dynamically control the pH value of the reaction system to 4.0-5.0 to obtain a crude liquid.

[0063] (2) An electrolytic cell is provided, which is divided into a cathode region and an anode region by a cation exchange membrane N2050WX (Nafion ion exchange membrane), a carbon electrode is provided in the cathode region, a saturated sodium hydroxide aqueous solution is provided in the anode region as the anode region electrolyte, and a copper electrode is used as the anode electrode. The sodium hydroxide equivalent in the saturated sodium hydroxide aqueous solution used is about 2.7 Eq. The crude product liquid obtained in step (1) is placed in the cathode region as the cathode region electrolyte, and electrolysis is performed by power supply, and the starting voltage is controlled to be 1.23 V and the ending voltage is controlled to be 1.34 V. After the electrolysis is completed, the cathode region electrolyte is recovered and mixed with 48 times the volume of anhydrous ethanol, and then industrial quicklime with a loose volume of 0.8 times the cathode region electrolyte is added to remove water and dry. After filtering to remove the precipitate, the precipitate is evaporated at low pressure at 20 ° C and the anhydrous ethanol is recovered, and the crystallized product is recovered to obtain the purified ammonium fluoride product, and at least 50 Slowly add anhydrous ethanol to dissolve kg of purified ammonium fluoride product, and control the addition rate of anhydrous ethanol to add 15 mL of anhydrous ethanol per minute per gram of purified ammonium fluoride product. After the purified ammonium fluoride product no longer dissolves within 2 consecutive minutes, vacuum filtration is performed to separate and remove insoluble matter. The anhydrous ethanol solution of ammonium fluoride is placed at 20°C and evaporated under low pressure. After recovering the anhydrous ethanol, the crystalline product is recovered to obtain an electronic grade ammonium fluoride product.

[0064] The maximum theoretical yield is calculated based on the amount of ammonia used, the purity and ammonium fluoride content of the electronic-grade ammonium fluoride product are characterized, the actual yield is calculated, and the yield of ammonium fluoride is calculated based on the maximum theoretical yield and the actual yield.

[0065] The specific calculation formula of recovery rate is: recovery rate = (actual yield / maximum theoretical yield) × 100%;

[0066] Through characterization and calculation, the purity of the purified ammonium fluoride product obtained in this example is 99.9%, and the calculated yield is 98.2%.

[0067] Comparative Example 1: A method for preparing electronic grade ammonium fluoride, comprising:

[0068] (1) A hydrogen fluoride solution (20 wt%) preheated to 85 °C was used as the liquid phase reactant. 0.8 Eq of ammonia was introduced into the hydrogen fluoride solution for reaction. During the reaction, an equal concentration (20 wt%) of hydrogen fluoride was added to dynamically control the pH value of the reaction system to 4.0-5.0 to obtain a crude liquid.

[0069] (2) An electrolytic cell is provided, which is divided into a cathode region and an anode region by a cation exchange membrane N2050WX (Nafion ion exchange membrane), a carbon electrode is provided in the cathode region, a saturated sodium hydroxide aqueous solution is provided in the anode region as the anode region electrolyte, and a copper electrode is used as the anode electrode. The sodium hydroxide equivalent in the saturated sodium hydroxide aqueous solution used is about 2.7 Eq. The crude product liquid obtained in step (1) is placed in the cathode region as the cathode region electrolyte, and electrolysis is performed by power supply, and the starting voltage is controlled to be 1.23 V and the ending voltage is controlled to be 1.30 V. After the electrolysis is completed, the cathode region electrolyte obtained is recovered and mixed with 48 times the volume of anhydrous ethanol, and then industrial quicklime with a loose volume of 0.8 times the cathode region electrolyte is added to remove water and dry. After filtering to remove the precipitate, the precipitate is evaporated at low pressure at 20 ° C and the anhydrous ethanol is recovered, and the crystallized product is recovered to obtain the purified ammonium fluoride product, and at least 50 Slowly add anhydrous ethanol to dissolve kg of purified ammonium fluoride product, and control the addition rate of anhydrous ethanol to add 15 mL of anhydrous ethanol per minute per gram of purified ammonium fluoride product. After the purified ammonium fluoride product no longer dissolves within 2 consecutive minutes, vacuum filtration is performed to separate and remove insoluble matter. The anhydrous ethanol solution of ammonium fluoride is placed at 20°C and evaporated under low pressure. After the anhydrous ethanol is recovered, the crystalline product is recovered to obtain an electronic grade ammonium fluoride product.

[0070] The maximum theoretical yield is calculated based on the amount of ammonia used, the purity and ammonium fluoride content of the electronic-grade ammonium fluoride product are characterized, the actual yield is calculated, and the yield of ammonium fluoride is calculated based on the maximum theoretical yield and the actual yield.

[0071] The specific calculation formula of recovery rate is: recovery rate = (actual yield / maximum theoretical yield) × 100%;

[0072] Through characterization and calculation, the purity of the purified ammonium fluoride product obtained in this example is 99.6%, and the calculated yield is 97.8%.

[0073] It can be seen that lowering the threshold potential used to determine the electrolysis process will lead to a significant decrease in the purity of the ammonium fluoride product. Product characterization also revealed that this is due to incomplete removal of hydrogen fluoride. Increasing the termination voltage to 1.35 V can also produce ammonium fluoride with a purity of 99.9%, but the energy consumption is increased by approximately 12% and 9% compared to the termination voltages of 1.32 V and 1.34 V, respectively.

[0074] Comparative Example 2: Preparation of ammonium fluoride using existing process:

[0075] (1) A hydrogen fluoride solution (20 wt%) preheated to 85 °C was used as the liquid phase reactant. 0.8 Eq of ammonia was introduced into the hydrogen fluoride solution for reaction. During the reaction, an equal concentration (20 wt%) of hydrogen fluoride was added to dynamically control the pH value of the reaction system to 4.0-5.0 to obtain a crude product liquid. The crude product liquid was cooled to 22 °C and allowed to stand for crystallization. When the crystals no longer increased, the solid-liquid separation was performed to separate the crystals. The obtained crystals were crude product crystals.

[0076] (2) The crude crystals were dissolved in excess deionized water and placed at a constant temperature of 22°C for 2 h for conventional recrystallization. After a total of five recrystallizations, the purity of the product was characterized.

[0077] Characterization results showed that the product had a purity of approximately 97.8%. The same yield calculation as in Example 1 showed a yield of only approximately 90.2%. This indicates that the present invention significantly improves product purity, yield, efficiency, and energy consumption compared to existing processes for preparing ammonium fluoride.

Claims

1. A method for preparing electronic grade ammonium fluoride, characterized in that: The method comprises: (1) reacting a preheated hydrogen fluoride solution with 0.8 to 1.0 Eq of ammonia water or ammonia gas, supplementing hydrogen fluoride during the reaction to control the pH value to ≤5.0, to obtain a crude product liquid; (2) The crude product solution is subjected to ion exchange purification and ethanol drop purification to obtain electronic grade ammonium fluoride.

2. The method for preparing electronic grade ammonium fluoride according to claim 1, wherein: The hydrogen fluoride solution used in step (1) is a hydrogen fluoride aqueous solution with a concentration of 10 to 50 wt%.

3. The method for preparing electronic grade ammonium fluoride according to claim 1, wherein: The ammonia content in the ammonia water or ammonia gas used in the step (1) is calculated based on the hydrogen fluoride contained in the hydrogen fluoride solution used, and the ammonia content is controlled to be 0.8 to 1.0 Eq.

4. The method for preparing electronic grade ammonium fluoride according to claim 1, wherein: The ion exchange purification in step (2) comprises: The electrolytic cell is divided into a cathode region and an anode region by a cation exchange membrane, the crude product solution obtained in step (1) is used as the cathode region electrolyte, the carbon electrode is used as the cathode electrode, the sodium hydroxide and / or potassium hydroxide aqueous solution is used as the anode region electrolyte, and the copper electrode is used as the anode electrode. After electrolysis, the cathode region electrolyte is recovered, excess anhydrous ethanol is added to dissolve the ammonium fluoride, and the water is removed by an inert desiccant, and then the solid impurities are removed by filtration to obtain purified ammonium fluoride by crystallization.

5. The method for preparing electronic grade ammonium fluoride according to claim 4, wherein: During the electrolysis process, the starting voltage is controlled to be 1.23 V and the ending voltage is controlled to be 1.32-1.34 V.

6. The method for preparing electronic grade ammonium fluoride according to claim 4, characterized in that: After the cathode electrolyte is recovered, the cathode electrolyte is mixed with anhydrous ethanol having a volume at least 48 times that of the cathode electrolyte.

7. The method for preparing electronic grade ammonium fluoride according to claim 4, characterized in that: The inert desiccant is calcium oxide; The amount of calcium oxide used is controlled so that its loose volume is at least 0.8 times of the recovered cathode electrolyte.

8. A method for preparing electronic grade ammonium fluoride according to claim 1 or 4, characterized in that, The ethanol dropwise purification in step (2) comprises: Slowly add anhydrous ethanol to dissolve the product obtained by ion exchange purification until the purified ammonium fluoride product no longer dissolves, then separate the solid and remove the solid matter, and crystallize the anhydrous ethanol solution of ammonium fluoride again to obtain electronic grade ammonium fluoride.

Citation Information

Patent Citations

  • Preparation method of etching and cleaning grade ammonium fluoride

    CN110615447A

  • Method for refining and purifying etching waste liquid

    CN113045089A

  • Production management control system for ammonium fluoride production and control method thereof

    CN115453990A

  • Method for purifying ammonium fluoride crude product

    CN117165960A

  • Preparation method of electronic-grade ammonium fluoride

    CN117165961A