Composite coating and preparation method therefor, silicone rubber protective sleeve and insulator

By embedding hydrophobically modified four-needle zinc oxide powder and nano-metal oxide powder step by step on the surface of the composite insulator, a composite coating with a micro-nano structure is formed, which solves the aging problem of the composite insulator in a high-radiation and high-humidity environment. Its hydrophobicity and UV resistance are significantly improved, ensuring long-term stable operation.

WO2024222907A1PCT designated stage expired Publication Date: 2024-10-31DALI BUREAU OF ULTRA HIGH VOLTAGE TRANSMISSION CO CHINA SOUTHERN POWER GRID CO LTD

Patent Information

Application Number
PCT/CN2024/090176
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The macromolecular bonds of the silicone rubber material on the surface of composite insulators break under high radiation, high humidity, and high temperature difference environments, resulting in loss of hydrophobic properties, surface hardening and powdering, cracking and damage, and causing malignant electrical power such as pollution flashover, internal breakdown, and brittle fracture. Failure, the traditional anti-aging modification effect is not good.

Method used

A step-by-step embedding method is used to embed hydrophobically modified four-needle zinc oxide powder and nano-metal oxide powder on the surface of the liquid film, and the liquid film is completely solidified to form a composite coating with a micro-nano structure, using an inorganic UV shielding agent and hydrophobic modifiers to improve UV resistance and hydrophobic properties.

Benefits of technology

The long-term hydrophobicity and anti-ultraviolet stability of the composite coating is achieved, which significantly improves the anti-aging effect of the composite insulator, avoids mechanical damage to the substrate surface caused by the modification process, and enhances the bonding strength between the composite coating and the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024090176_31102024_PF_FP_ABST
    Figure CN2024090176_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a composite coating and a preparation method therefor, a silicone rubber protective sleeve and an insulator. The preparation method for the composite coating comprises the following steps: coating a substrate with an adhesive liquid, so as to obtain a liquid film; and first embedding a hydrophobically modified tetrapod-like zinc oxide powder into the surface of the liquid film, then embedding a hydrophobically modified nano metal oxide powder into the surface of the liquid film, and completely curing the liquid film, so as to obtain the composite coating, which has a micro-nano structure.
Need to check novelty before this filing date? Find Prior Art

Description

Composite coating and preparation method thereof, silicone rubber protective cover and insulator

[0001] Related applications

[0002] This application claims priority to Chinese patent application number 202310479747.9, filed on April 28, 2023, entitled “Composite coating and preparation method thereof, silicone rubber protective cover and insulator,” the entire text of which is hereby incorporated by reference. Technical Field

[0003] The present invention relates to the technical field of insulators, and in particular to a composite coating and a preparation method thereof, a silicone rubber protective sleeve and an insulator. Background Art

[0004] Insulators are insulating components installed between conductors of different potentials or between conductors and grounded structures, capable of withstanding voltage and mechanical stress. They play a vital role in overhead transmission lines. Depending on the insulating material used, insulators can be categorized as porcelain, glass, and composite. Composite insulators, consisting of a glass fiber resin core rod, a silicone rubber sheath, and sheds, exhibit excellent hydrophobicity and water migration properties, making them widely used in power systems.

[0005] During outdoor operation, composite insulators are not only subjected to long-term high electric fields but are also frequently exposed to environmental conditions such as high radiation, high temperature differences, and high humidity. This, particularly under strong ultraviolet radiation conditions at high altitudes, can easily cause the macromolecular bonds of the silicone rubber material on their surface to break, leading to aging phenomena such as loss of hydrophobicity, surface hardening and powdering, cracking and damage, and exposure of internal fillers. Furthermore, the loss of hydrophobicity can further induce corona aging and damp-heat aging on the silicone rubber surface, making composite insulators susceptible to serious power failures such as flashover, internal breakdown, and brittle fracture, seriously threatening the safe and reliable operation of the power grid. However, conventional technologies for anti-aging modification of silicone rubber materials are less than ideal, resulting in poor weather resistance of composite insulators.

[0006] Summary of the Invention

[0007] Based on this, according to various embodiments of the present application, a composite coating with excellent anti-aging effect and a preparation method thereof, a silicone rubber protective cover and an insulator are provided. The technical solution is:

[0008] In a first aspect, the present invention provides a method for preparing a composite coating, comprising the following steps:

[0009] Applying the adhesive liquid on the substrate to obtain a liquid film;

[0010] The hydrophobically modified tetrapod-shaped zinc oxide powder is first embedded in the surface of the liquid film, and then the hydrophobically modified nano metal oxide powder is embedded, and the liquid film is completely solidified to obtain a composite coating with a micro-nano structure.

[0011] In one embodiment, the nano metal oxide powder includes one or more of nano zinc oxide powder, nano titanium oxide powder, nano cerium oxide powder and nano iron oxide powder.

[0012] In one embodiment, the adhesive is a single-component room temperature vulcanized silicone rubber adhesive.

[0013] In one embodiment, embedding hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film comprises the following steps: after sprinkling the hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film, first curing at room temperature until the hydrophobically modified tetrapod-shaped zinc oxide powder is embedded and the liquid film is not completely cured; and removing the hydrophobically modified tetrapod-shaped zinc oxide powder that is not embedded on the surface of the liquid film.

[0014] In one embodiment, the conditions for completely curing the liquid film are: curing at 60° C. to 80° C. for 6 h to 8 h.

[0015] In one embodiment, the preparation method of the hydrophobically modified tetrapod-shaped zinc oxide powder and the hydrophobically modified nano metal oxide powder is a coupling modification method.

[0016] In one embodiment, the preparation method of hydrophobically modified tetrapod-shaped zinc oxide powder comprises the following steps:

[0017] Mixing tetrapod-shaped zinc oxide powder with ethanol and water to obtain a dispersion;

[0018] adding a silane coupling agent to the dispersion to obtain a mixed solution;

[0019] The pH of the mixed solution is adjusted to 7-9, stirred at 50-70° C. for 4-6 hours, and solid-liquid separation is performed to obtain hydrophobically modified tetrapod-shaped zinc oxide powder.

[0020] In one embodiment, the preparation method of hydrophobically modified nano metal oxide powder comprises the following steps:

[0021] mixing nano metal oxide powder with ethanol and water to obtain a dispersion;

[0022] adding a silane coupling agent to the dispersion to obtain a mixed solution;

[0023] The pH value of the mixed solution is adjusted to 7-9, stirred at 50-70° C. for 4-6 hours, and solid-liquid separation is performed to obtain hydrophobically modified nano-metal oxide powder.

[0024] In one embodiment, the preparation method of the hydrophobically modified tetrapod-shaped zinc oxide powder and the hydrophobically modified nano metal oxide powder meets one or more of the following conditions:

[0025] 1) The silane coupling agent is a perfluorinated silane coupling agent;

[0026] 2) The mass ratio of the silane coupling agent to the tetrapod-shaped zinc oxide powder or the nano metal oxide powder is (1-10):100;

[0027] 3) The concentration of the tetrapod-shaped zinc oxide powder or the nano metal oxide powder in the dispersion is 1 wt.% to 12 wt.%;

[0028] 4) The volume ratio of the ethanol to the water is (1-9):1.

[0029] In one embodiment, the composite coating satisfies one or more of the following conditions:

[0030] 1) The whisker length of the four-needle zinc oxide powder is 10 μm to 100 μm;

[0031] 2) The particle size of the nano metal oxide powder is ≤100 nm;

[0032] 3) The mass ratio of the tetrapod-shaped zinc oxide powder to the nano metal oxide powder is 1:(1-5);

[0033] 4) The thickness of the liquid film is 50 μm to 70 μm;

[0034] 5) The thickness of the composite coating is 80 μm to 100 μm.

[0035] In one embodiment, the adhesive liquid includes an adhesive and a diluent in a mass ratio of 1:(1-3).

[0036] In one embodiment, the substrate is one or more of a polymer substrate, a glass substrate, a ceramic substrate and a metal substrate.

[0037] In a second aspect, the present invention provides a composite coating, which is prepared using the above-mentioned method for preparing the composite coating.

[0038] In a third aspect, the present invention provides a silicone rubber protective cover comprising the composite coating described above.

[0039] A fourth aspect of the present invention provides an insulator comprising the silicone rubber protective sleeve described above.

[0040] The details of one or more embodiments of the present application are set forth in the description below, and other features, objects, and advantages of the application will become apparent from the description and from the claims thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the conventional technology, the following briefly introduces the drawings required for use in the embodiments or the conventional technology descriptions. Obviously, the drawings described below are merely embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the disclosed drawings without any creative work.

[0042] FIG1 is a SEM image of the composite coating prepared in Example 1;

[0043] FIG2 is a water contact angle test diagram of the composite coating prepared in Example 1;

[0044] FIG3 is a SEM image of the HTV silicone rubber in Comparative Example 1;

[0045] FIG4 is a water contact angle test diagram of the HTV silicone rubber in Example 1. DETAILED DESCRIPTION

[0046] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application.

[0048] the term

[0049] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0050] SEM: scanning electron microscope.

[0051] Contact angle: also known as the wetting angle, refers to the angle between the solid-liquid interface, the liquid interior and the gas-liquid interface at the junction of solid, liquid and gas.

[0052] Water contact angle: also known as water drop angle, is a type of contact angle, specifically referring to the contact angle formed by a water drop on a solid surface. It can be used to characterize the hydrophilicity and hydrophobicity of a solid surface. The larger the water contact angle, the stronger the hydrophobicity, and the smaller the water contact angle, the stronger the hydrophilicity.

[0053] Silicone rubber: refers to a rubber whose main chain is composed of alternating silicon and oxygen atoms, and the silicon atoms are usually connected to two organic groups. It can be divided into high-temperature vulcanized (HTV) silicone rubber and room-temperature vulcanized (RTV) silicone rubber according to the vulcanization mechanism. HTV rubber has outstanding electrical properties and stain resistance and hydrophobicity, and can be used to prepare shed protective covers for composite insulators.

[0054] The aging process of silicone rubber materials is usually the result of the combined effects of multiple factors such as moisture, heat, and ultraviolet rays. In traditional technologies, the anti-aging modification of silicone rubber often only focuses on one of these factors, such as hydrophobic modification or anti-ultraviolet modification.

[0055] The hydrophobic modification of silicone rubber materials is mainly achieved through laser etching or plasma fluorination on their surfaces. For example, there are reports of constructing a micro-nano composite layered structure on the surface of HTV silicone rubber using femtosecond laser etching technology, which increases the surface roughness and forms a fine papillary structure, thereby producing a stable superhydrophobic state on the surface of HTV silicone rubber. There are also reports of using CF4 radio frequency inductive and capacitive coupled plasmas to treat the surface of HTV silicone rubber, respectively, and hydrophobically modifying the silicone rubber surface through low-temperature plasma etching and fluorination. Although surface laser etching or plasma fluorination can improve the surface hydrophobicity of silicone rubber, these two treatment methods are not only complex in process, expensive in equipment, and difficult to achieve large-scale application, but also damage the silicone rubber surface itself during the treatment process, which can easily lead to the exposure of inorganic fillers inside the silicone rubber, thereby compromising its mechanical strength.

[0056] In terms of UV radiation aging resistance of silicone rubber, current research focuses on internal modification by adding additives or fillers with light-shielding and UV-absorbing properties to the silicone rubber matrix. For example, there are reports of adding nano-titanium dioxide particles to the silicone rubber matrix and preparing HTV silicone rubber composites through blending to improve its anti-aging ability under UV radiation; there are reports of preparing high-temperature vulcanized silicone rubber by adding three organic UV absorbers, UV-327, UV-531, and UVP-788, to silicone rubber to improve its UV aging resistance; there are reports of adding nano-cerium dioxide nanoparticles modified with the silane coupling agent KH151 to the RTV matrix through blending to improve the UV aging resistance of the RTV silicone rubber surface; there are reports of introducing nano-zinc oxide into the RTV matrix to prepare composite materials to improve its UV aging resistance. Although adding organic UV absorbers or inorganic UV shielding agents to the silicone rubber matrix can improve the silicone rubber's resistance to UV aging to a certain extent, organic UV absorbers have poor stability, are easy to migrate, and will weaken the mechanical strength of the matrix. Inorganic UV shielding agents are blended and dispersed inside the matrix, and have basically no effect on improving the hydrophobicity of the silicone rubber surface, and may even have the negative effect of reducing the hydrophobicity.

[0057] This shows that traditional technologies for anti-aging modification of silicone rubber materials involve either a single hydrophobic modification or a single UV resistance modification. Not only does this fail to organically combine hydrophobic and UV resistance, but optimizing one property can also lead to degradation of the other. Furthermore, the treatment process can easily damage the silicone rubber surface, making it impossible to enhance the weather resistance of silicone rubber through the synergistic effects of multiple factors. In summary, developing a simple, surface-damaging preparation method that simultaneously performs hydrophobic and UV resistance modifications to produce a composite coating with excellent anti-aging properties is crucial for achieving long-term, stable operation of composite insulators in environments characterized by high radiation, high humidity, and high temperature differences.

[0058] Based on this, the first aspect of the present invention provides a method for preparing a composite coating, comprising the following steps:

[0059] Applying the adhesive liquid on the substrate to obtain a liquid film;

[0060] The hydrophobically modified tetrapod-shaped zinc oxide powder is first embedded in the surface of the liquid film, and then the hydrophobically modified nano metal oxide powder is embedded, and the liquid film is completely solidified to obtain a composite coating with a micro-nano structure.

[0061] It can be understood that the method of first embedding the hydrophobically modified tetrapod-shaped zinc oxide powder and then embedding the hydrophobically modified nano-metal oxide powder on the surface of the liquid film is a step-by-step embedding method.

[0062] The present invention coats an adhesive liquid on the surface of a substrate to form a liquid film, then utilizes the uncured property of the liquid film to embed hydrophobically modified tetrapod-shaped zinc oxide powder and hydrophobically modified nano-metal oxide powder on the surface of the liquid film in steps, and completely cures the liquid film, thereby obtaining a composite coating with excellent anti-aging effect.

[0063] First, both the four-needle zinc oxide powder and the nano-metal oxide powder are inorganic ultraviolet shielding agents. After they are embedded in the liquid film surface step by step, the base material can obtain excellent anti-ultraviolet function through absorption, reflection and scattering. Secondly, the particles of the four-needle zinc oxide powder and the nano-metal oxide powder are relatively small, with a large specific surface area and a high surface energy, and thus exhibit strong hydrophilicity. They are hydrophobically modified before being embedded step by step, which can make them exhibit excellent hydrophobic properties and improve the surface hydrophobicity of the base material. Furthermore, since the four-needle zinc oxide powder is a micron-sized single crystal powder composed of a central body and four needle-shaped whiskers, the step-by-step embedding method can make the nano-metal oxide powder fill the large number of gaps between the four-needle zinc oxide powder whiskers, which can not only greatly enhance the ultraviolet shielding effect, but also form a micro-nano structure that imitates the lotus leaf papilla structure, so that the composite coating obtains a stable super-hydrophobic state.

[0064] Furthermore, the liquid film after step-by-step embedding is completely solidified to obtain an adhesive layer with strong adhesion, which can prevent the hydrophobically modified oxide powder from falling off, significantly improve the firmness of the bond between the composite coating and the substrate, and enable it to exhibit long-term hydrophobicity and stable UV resistance, thereby obtaining excellent anti-aging effects; in addition, the liquid film formed by the adhesive applied to the substrate can also avoid mechanical damage to the substrate surface caused by the modification treatment, greatly reducing the negative impact on the mechanical properties of the substrate.

[0065] In some embodiments, the nano metal oxide powder includes one or more of nano zinc oxide powder, nano titanium oxide powder, nano cerium oxide powder, and nano iron oxide powder.

[0066] Nanopowders of metal oxides such as zinc oxide, titanium dioxide, cerium oxide and iron oxide all have good UV shielding effects. They can block the invasion of ultraviolet rays through different effects such as scattering, reflection and absorption, thereby effectively improving the UV resistance of the composite coating.

[0067] In some preferred embodiments, the nano metal oxide powder is nano zinc oxide powder.

[0068] In some embodiments, the adhesive is a one-component room temperature vulcanized silicone rubber adhesive.

[0069] One-component RTV silicone rubber is an electrical anti-pollution flashover coating consisting of polydimethylsiloxane, a crosslinker, a catalyst, and a solvent. It exhibits excellent electrical properties and chemical inertness, is heat-neutral during curing, exhibits minimal shrinkage after curing, and exhibits excellent adhesion to various materials, particularly HTV silicone rubber. This allows the composite coating to remain firmly attached to the substrate surface for extended periods without detaching, resulting in long-term hydrophobicity and UV stability. Furthermore, one-component RTV silicone rubber cures by directly reacting with moisture in the air to form a thermosetting elastomer. This curing reaction can proceed slowly at room temperature or be accelerated by varying the ambient temperature and humidity. Compared to two-component or multi-component RTV silicone rubber, the curing reaction of one-component RTV silicone rubber is highly controllable and simpler to operate, facilitating the smooth implementation of subsequent step-by-step embedding.

[0070] In some preferred embodiments, the adhesive is a one-component PRTV silicone rubber adhesive.

[0071] One-component PRTV silicone rubber is a new type of electrical functional material. Compared with ordinary one-component RTV silicone rubber, it has stronger bonding ability, better hydrophobicity and better anti-fouling flashover effect, which can further enhance the comprehensive anti-aging ability of the composite coating.

[0072] In some embodiments, embedding hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film comprises the following steps: after sprinkling the hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film, first curing at room temperature until the hydrophobically modified tetrapod-shaped zinc oxide powder is embedded and the liquid film is not completely cured; and removing the hydrophobically modified tetrapod-shaped zinc oxide powder that is not embedded in the surface of the liquid film.

[0073] After sprinkling hydrophobically modified tetrapod-shaped zinc oxide powder onto the surface of the liquid film, the film is allowed to solidify for a period of time at room temperature. This allows some of the tetrapod-shaped zinc oxide powder's whiskers to become firmly embedded in the film surface, while the remaining tetrapod-shaped zinc oxide powder becomes loosely coated on the surface. This loose tetrapod-shaped zinc oxide powder is then immediately removed, exposing the spaces between the firmly bonded tetrapod-shaped zinc oxide powder whiskers. This facilitates the filling of the nano-metal oxide powder between these whiskers and its embedding into the liquid film surface.

[0074] In some more preferred embodiments, the first curing time is 10 min to 20 min.

[0075] In some preferred embodiments, embedding hydrophobically modified nano-metal oxide powder on the surface of the liquid film comprises the following steps: removing the hydrophobically modified tetrapod-shaped zinc oxide powder not embedded on the surface of the liquid film, and then performing a second solidification at room temperature, while the liquid film is not completely solidified; and sprinkling hydrophobically modified nano-metal oxide powder on the surface of the liquid film.

[0076] In some more preferred embodiments, the second curing time is 5 min to 10 min.

[0077] In some preferred embodiments, after the liquid film is completely solidified, the following step is included: removing the hydrophobically modified nano metal oxide powder that is not embedded in the surface of the liquid film.

[0078] In some embodiments, the conditions for completely curing the liquid film are: curing at 60° C. to 80° C. for 6 h to 8 h.

[0079] Single-component RTV silicone rubber requires at least 24 hours to fully cure at room temperature. Increasing the curing temperature can shorten the curing time and help enhance the depth and strength of the cure.

[0080] In some embodiments, the preparation method of the hydrophobically modified tetrapod-shaped zinc oxide powder and the hydrophobically modified nano metal oxide powder is a coupling modification method.

[0081] Methods for hydrophobic modification of inorganic materials include surfactants, polymer coating, and coupling modification. The surfactant method suffers from insufficient stability and easy loss of hydrophobicity, while the polymers commonly used in the polymer coating method are insufficiently hydrophobic and have poor UV resistance, making them unfavorable for hydrophobic modification of composite coatings. The coupling modification method utilizes a silane coupling agent to chemically react with the hydroxyl groups on the surface of inorganic particles, thereby introducing highly hydrophobic organic groups onto the surface of the inorganic particles and reducing their surface energy. This not only significantly improves the hydrophobic properties of the inorganic particles but also enhances their compatibility and dispersibility with the liquid film, thereby improving the embedding effect of the two inorganic UV shielding agents.

[0082] In some embodiments, the method for preparing hydrophobically modified tetrapod-shaped zinc oxide powder comprises the following steps:

[0083] Mixing tetrapod-shaped zinc oxide powder with ethanol and water to obtain a dispersion;

[0084] adding a silane coupling agent to the dispersion to obtain a mixed solution;

[0085] The pH value of the mixed solution is adjusted to 7-9, stirred at 50-70° C. for 4-6 hours, and solid-liquid separation is performed to obtain hydrophobically modified tetrapod-shaped zinc oxide powder or hydrophobically modified nano metal oxide powder.

[0086] In some embodiments, the method for preparing hydrophobically modified nano metal oxide powder comprises the following steps:

[0087] mixing nano metal oxide powder with ethanol and water to obtain a dispersion;

[0088] adding a silane coupling agent to the dispersion to obtain a mixed solution;

[0089] The pH value of the mixed solution is adjusted to 7-9, stirred at 50-70° C. for 4-6 hours, and solid-liquid separation is performed to obtain hydrophobically modified tetrapod-shaped zinc oxide powder or hydrophobically modified nano metal oxide powder.

[0090] In some preferred embodiments, adjusting the pH of the mixed solution comprises the following steps: adding one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate and aqueous ammonia to the mixed solution.

[0091] In some more preferred embodiments, the pH of the mixed solution is adjusted to 8.

[0092] In some embodiments, the preparation method of the hydrophobically modified tetrapod-shaped zinc oxide powder and the hydrophobically modified nano metal oxide powder satisfies one or more of the following conditions:

[0093] 1) The silane coupling agent is a perfluorinated silane coupling agent;

[0094] 2) The mass ratio of the silane coupling agent to the tetrapod-shaped zinc oxide powder or the nano metal oxide powder is (1-10):100;

[0095] 3) The concentration of the tetrapod-shaped zinc oxide powder or the nano metal oxide powder in the dispersion is 1 wt.% to 12 wt.%;

[0096] 4) The volume ratio of the ethanol to the water is (1-9):1.

[0097] Fluorine has the lowest surface energy, so using perfluorinated silane coupling agents to modify inorganic materials can achieve optimal hydrophobicity. By adjusting the various parameters of the coupling modification method, tetrapod-shaped zinc oxide powder or nano-metal oxide powder can achieve even better hydrophobicity.

[0098] In some preferred embodiments, the volume ratio of the ethanol to the water is 9:1.

[0099] In some embodiments, the composite coating satisfies one or more of the following conditions:

[0100] 1) The whisker length of the four-needle zinc oxide powder is 10 μm to 100 μm;

[0101] 2) The particle size of the nano metal oxide powder is ≤100 nm;

[0102] 3) The thickness of the liquid film is 50 μm to 70 μm;

[0103] 4) The thickness of the composite coating is 80 μm to 100 μm.

[0104] It can be understood that the particle size refers to the equivalent circular diameter of the particle, that is, the diameter of a circle equivalent to the plane projected area of ​​the particle.

[0105] By regulating the whisker length of the tetrapod-shaped zinc oxide powder and the particle size of the nano-metal oxide powder, it is beneficial to optimize the morphology of the micro-nanostructure and improve its hydrophobic properties. The thickness of the liquid film is greater than the whisker length of the tetrapod-shaped zinc oxide powder, which can form a stronger bond between the whiskers in the tetrapod-shaped zinc oxide powder and the liquid film and avoid mechanical damage to the substrate caused by the step-by-step embedding process. When the thickness of the composite coating is 80μm to 100μm, it will not fail to exhibit its hydrophobic and UV-resistant functions due to too low a thickness, nor will it be too thick, resulting in the oxide powder at the top of the composite coating having too low a bonding force with the substrate, making it easy to fall off or wear.

[0106] In some preferred embodiments, in the composite coating, the mass ratio of the hydrophobically modified tetrapod-shaped zinc oxide powder to the hydrophobically modified nano metal oxide powder is 1:(1-5).

[0107] The mass ratio of the hydrophobically modified tetrapod-shaped zinc oxide powder to the hydrophobically modified nano-metal oxide powder is controlled at 1: (1-5), so as to avoid the large difference in the feeding amount of the two and the inability to form an ideal micro-nano structure.

[0108] In some embodiments, the adhesive solution includes an adhesive and a diluent in a mass ratio of 1:(1-3).

[0109] In some preferred embodiments, the diluent includes one or more of ethyl acetate, acetone, n-hexane, dichloromethane, toluene, xylene, methanol, acetonitrile and silicone oil;

[0110] Diluents such as ethyl acetate, acetone, n-hexane, dichloromethane, toluene, xylene, methanol, acetonitrile and silicone oil can fully dissolve the one-component adhesive and adjust the viscosity and curing speed of the one-component adhesive to make it suitable for spraying and step-by-step embedding of inorganic materials.

[0111] In some more preferred embodiments, the diluent includes one or more of ethyl acetate, acetone, n-hexane and dichloromethane.

[0112] Diluents such as ethyl acetate, acetone, n-hexane and dichloromethane are less toxic, have less impact on the human body after volatilization, are highly safe, and will not cause environmental pollution.

[0113] In some embodiments, the substrate is one or more of a polymer substrate, a glass substrate, a ceramic substrate, and a metal substrate.

[0114] It can be understood that the polymer substrate includes one or more of an HTV silicone rubber substrate, an RTV silicone rubber substrate, a polyimide (PI) substrate, a polyethylene terephthalate (PET) substrate, a polycarbonate (PC) substrate, and a polymethyl methacrylate (PMMA) substrate; the glass substrate includes one or more of a quartz glass substrate, a soda glass substrate, a potassium glass substrate, an aluminum-magnesium glass substrate, a lead glass substrate, and a borosilicate glass substrate; the ceramic substrate includes one or more of an aluminum oxide substrate, a magnesium oxide substrate, a zirconium oxide substrate, and an electrical ceramic substrate; the metal substrate includes one or more of a copper substrate, an aluminum substrate, a stainless steel substrate, and a titanium alloy substrate.

[0115] The preparation method of the composite coating can select a suitable adhesive according to the material properties of the substrate, thereby forming a stable and strong bond between the substrate and the composite coating, thereby exhibiting long-term hydrophobicity and anti-ultraviolet stability, and has a wide range of applications.

[0116] In some preferred embodiments, the substrate is a high temperature vulcanized silicone rubber substrate.

[0117] When HTV silicone rubber is used as the base and one-component RTV silicone rubber adhesive is used as the adhesive, since the material properties are very similar, stronger adhesion can be obtained between the base and the composite coating, which is beneficial to improving the long-term hydrophobicity and UV resistance of the composite coating.

[0118] In a second aspect, the present invention provides a composite coating, which is prepared using the above-mentioned method for preparing the composite coating.

[0119] In a third aspect, the present invention provides a silicone rubber protective cover comprising the composite coating described above.

[0120] A fourth aspect of the present invention provides an insulator comprising the silicone rubber protective sleeve described above.

[0121] The present invention is further described in detail below with reference to specific embodiments.

[0122] Example 1

[0123] (1) Please refer to Table 1. After mixing 180 mL of ethanol and 10 mL of water, 5 g of tetrapod-shaped zinc oxide powder was added and ultrasonically dispersed for 30 minutes to obtain a dispersion. 0.1 g of perfluorooctyltrichlorosilane was added to the dispersion and stirred evenly to obtain a mixed solution. Sodium hydroxide was added to adjust the pH value of the mixed solution to 8, and then the mixture was heated to 50°C and reacted for 6 hours under continuous stirring. After centrifugation, the mixture was washed with deionized water and anhydrous ethanol three times each, and dried to obtain hydrophobically modified tetrapod-shaped zinc oxide powder.

[0124] (2) After mixing 180 mL of ethanol and 10 mL of water, 5 g of nano zinc oxide powder was added, and the nano zinc oxide powder was hydrophobically modified according to the method described in step (1) to obtain hydrophobically modified nano zinc oxide powder;

[0125] (3) Add 1 g of ethyl acetate to 1 g of one-component PRTV silicone rubber for dilution and stir for 10 min to obtain a uniformly mixed adhesive solution; pour the adhesive solution into the hopper of a pneumatic spray gun and spray it three times using the pneumatic spray gun to evenly coat the adhesive solution on the surface of the HTV silicone rubber, and preliminarily cure it at room temperature for 3 min to obtain a liquid film with a thickness of 60 μm;

[0126] (4) The hydrophobically modified tetrapod-shaped zinc oxide powder is evenly blown on the surface of the liquid film, and the first curing is carried out at room temperature for 10 minutes until the hydrophobically modified tetrapod-shaped zinc oxide powder is embedded. At this time, the liquid film is not completely cured; the loose hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film is blown away, and the second curing is carried out at room temperature for 5 minutes. At this time, the liquid film is not completely cured; the hydrophobically modified nano-zinc oxide powder is evenly blown on the surface of the liquid film, and cured at 60°C for 8 hours to completely cure the liquid film, and the loose hydrophobically modified nano-zinc oxide powder on the surface of the liquid film is blown away to obtain a composite coating with a micro-nano structure.

[0127] The microscopic morphology of the composite coating was observed and photographed using an SEM at a magnification of 5000, and the results are shown in FIG1 . Referring to GB / T30693-2014 Measurement of the contact angle of water with plastic films, the water contact angle of the composite coating was tested using a German Kruss DSA100 drop shape analyzer, and the results are shown in FIG2 . Referring to GB / T531.1-2008 Vulcanized rubber or thermoplastic rubber. Indentation hardness test method. Part 1: Shore hardness tester method (Shore hardness) , the hardness data of the composite coating was tested using a Shore A durometer, and the results are shown in Table 2 .

[0128] The composite coating was subjected to the following anti-aging test: under continuous UV radiation, the water contact angle and hardness of the composite coating were tested at regular intervals, and the results are shown in Table 3; wherein, the UV radiation conditions are as follows: the composite coating was irradiated for a long time using 6 UV lamps with a power of 40 W and a wavelength of 315 nm to 400 nm.

[0129] Example 2

[0130] (1) Please refer to Table 1. After mixing 180 mL of ethanol and 10 mL of water, add 10 g of tetrapod-shaped zinc oxide powder and ultrasonically disperse for 30 minutes to obtain a dispersion. Add 0.5 g of perfluorodecyltrimethoxysilane to the dispersion and stir evenly to obtain a mixed solution. Add sodium hydroxide to adjust the pH value of the mixed solution to 8, then heat it to 60°C and react for 5 hours under continuous stirring. After centrifugation, wash with deionized water and anhydrous ethanol three times each, and dry to obtain hydrophobically modified tetrapod-shaped zinc oxide powder.

[0131] (2) After mixing 180 mL of ethanol and 10 mL of water, 10 g of nano zinc oxide powder was added, and the nano zinc oxide powder was hydrophobically modified according to the method described in step (1) to obtain hydrophobically modified nano zinc oxide powder;

[0132] (3) Add 2 g of acetone to 1 g of one-component PRTV silicone rubber for dilution and stir for 10 min to obtain a uniformly mixed adhesive solution; pour the adhesive solution into the hopper of a pneumatic spray gun and spray it three times using the pneumatic spray gun to evenly coat the adhesive solution on the surface of the HTV silicone rubber, and cure it at room temperature for 4 min to obtain a liquid film with a thickness of 60 μm;

[0133] (4) The hydrophobically modified tetrapod-shaped zinc oxide powder is evenly blown on the surface of the liquid film, and the first curing is carried out at room temperature for 15 minutes until the hydrophobically modified tetrapod-shaped zinc oxide powder is embedded. At this time, the liquid film is not completely cured; the loose hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film is blown away, and the second curing is carried out at room temperature for 8 minutes. At this time, the liquid film is not completely cured; the hydrophobically modified nano-zinc oxide powder is evenly blown on the surface of the liquid film, and cured at 70°C for 7 hours to completely cure the liquid film, and the loose hydrophobically modified nano-zinc oxide powder on the surface of the liquid film is blown away to obtain a composite coating with a micro-nano structure.

[0134] The water contact angle and hardness data of the composite coating were tested according to the method described in Example 1. The results are shown in Table 2.

[0135] Example 3

[0136] (1) Please refer to Table 1. After mixing 180 mL of ethanol and 10 mL of water, add 20 g of tetrapod-shaped zinc oxide powder and ultrasonically disperse for 30 minutes to obtain a dispersion. Add 2 g of perfluorodecyltriethoxysilane to the dispersion and stir evenly to obtain a mixed solution. Add sodium hydroxide to adjust the pH value of the mixed solution to 8, then heat it to 70°C and react for 4 hours under continuous stirring. After centrifugation, wash it with deionized water and anhydrous ethanol three times each, and dry it to obtain hydrophobically modified tetrapod-shaped zinc oxide powder.

[0137] (2) After mixing 180 mL of ethanol and 10 mL of water, 20 g of nano zinc oxide powder was added, and the nano zinc oxide powder was hydrophobically modified according to the method described in step (1) to obtain hydrophobically modified nano zinc oxide powder;

[0138] (3) Add 3 g of n-hexane to 1 g of one-component PRTV silicone rubber for dilution and stir for 10 min to obtain a uniformly mixed adhesive solution; pour the adhesive solution into the hopper of a pneumatic spray gun and spray it three times using the pneumatic spray gun to evenly coat the adhesive solution on the surface of the HTV silicone rubber, and cure it at room temperature for 5 min to obtain a liquid film with a thickness of 60 μm;

[0139] (4) Sprinkle the hydrophobically modified tetrapod-shaped zinc oxide powder evenly on the surface of the liquid film, and perform a first curing at room temperature for 20 minutes until the hydrophobically modified tetrapod-shaped zinc oxide powder is embedded. At this time, the liquid film is not completely cured; blow away the loose hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film, and perform a second curing at room temperature for 10 minutes. At this time, the liquid film is not completely cured; sprinkle the hydrophobically modified nano-zinc oxide powder evenly on the surface of the liquid film, and cure it at 80°C for 6 hours to completely cure the liquid film. Blow away the loose hydrophobically modified nano-zinc oxide powder on the surface of the liquid film to obtain a composite coating with a micro-nano structure.

[0140] The water contact angle and hardness data of the composite coating were tested according to the method described in Example 1. The results are shown in Table 2.

[0141] Comparative Example 1

[0142] This comparative example served as a blank control group, meaning no composite coating was prepared on the HTV silicone rubber surface. The micromorphology of the HTV silicone rubber was observed and photographed using a SEM at a magnification of 5000, as shown in Figure 3. The water contact angle of the HTV silicone rubber was measured using the same method as described in Example 1, as shown in Figure 4. The hardness of the HTV silicone rubber was measured using the same method as described in Example 1, as shown in Table 2. The aging resistance of the HTV silicone rubber was also measured using the same method as described in Example 1, as shown in Table 3.

[0143] Table 1. Relevant parameters of raw materials in Examples 1 to 3 and Comparative Example 1

[0144] Table 2. Performance test results of the composite coatings in Examples 1 to 3 and Comparative Example 1

[0145] Table 3. Anti-aging test results of the composite coatings in Example 1 and Comparative Example 1

[0146] As shown in Figure 1, the composite coating in Example 1 possesses micro-nanostructures that mimic the papillae of a lotus leaf, while the HTV silicone rubber in Figure 3 has a smooth surface and lacks micro-nanostructures. Table 2 shows that the water contact angles of the composite coatings in Examples 1-3 reach 151.1°, while the water contact angle of the HTV silicone rubber in Comparative Example 1 is only 105.1°. This demonstrates that the composite coatings with micro-nanostructures significantly improve the hydrophobicity of the HTV silicone rubber substrate compared to the unmodified HTV silicone rubber.

[0147] As shown in Table 3, after 900 hours of UV irradiation, the water contact angle of the composite coating of Example 1 still remained at 140.2°, a relative decrease of only 7.21%, while the relative decrease of Comparative Example 1 reached 13.70%. This demonstrates that the composite coating of Example 1 not only has superior hydrophobicity, but also exhibits no significant degradation in hydrophobicity after prolonged UV irradiation, demonstrating excellent long-term hydrophobicity. Furthermore, after 900 hours of UV irradiation, the hardness of the composite coating of Example 1 increased from 68.5HA to 70.0HA, a relative increase of 2.19%, while the relative increase of Comparative Example 1 reached 9.30%, indicating that the hardness of the composite coating did not change significantly with the extension of UV aging time, and its UV resistance was more stable. Furthermore, the composite coating adhered firmly and was not easily detached, and the change in water contact angle after UV aging was minimal, further demonstrating that the composite coating has excellent UV resistance stability.

[0148] In summary, the composite coating with micro-nano structure can greatly improve the long-term hydrophobicity and UV stability of the substrate, thereby showing excellent anti-aging effect.

[0149] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0150] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.

Claims

1. A method for preparing a composite coating, characterized in that: The following steps are involved: Applying the adhesive liquid on the substrate to obtain a liquid film; The hydrophobically modified tetrapod-shaped zinc oxide powder is first embedded on the surface of the liquid film, and then the hydrophobically modified nano metal oxide powder is embedded, and the liquid film is completely solidified to obtain a composite coating with a micro-nano structure.

2. The method for preparing the composite coating according to claim 1, characterized in that: The nano metal oxide powder includes one or more of nano zinc oxide powder, nano titanium oxide powder, nano cerium oxide powder and nano iron oxide powder.

3. The method for preparing the composite coating according to claim 1, characterized in that: The adhesive is a single-component room temperature vulcanized silicone rubber adhesive.

4. The method for preparing the composite coating according to claim 3, characterized in that: Embedding hydrophobically modified tetrapod-shaped zinc oxide powder on the surface of the liquid film comprises the following steps: After the hydrophobically modified tetrapod-shaped zinc oxide powder is sprinkled on the surface of the liquid film, the liquid film is first cured at room temperature until the hydrophobically modified tetrapod-shaped zinc oxide powder is embedded and the liquid film is not completely cured; and removing the hydrophobically modified tetrapod-shaped zinc oxide powder that is not embedded in the surface of the liquid film.

5. The method for preparing the composite coating according to claim 3, characterized in that: The conditions for completely curing the liquid film are: curing at 60° C. to 80° C. for 6 h to 8 h.

6. The method for preparing a composite coating according to any one of claims 1 to 5, characterized in that: The preparation method of the hydrophobically modified tetrapod-shaped zinc oxide powder and the hydrophobically modified nano metal oxide powder is a coupling modification method.

7. The method for preparing the composite coating according to claim 6, characterized in that: The preparation method of hydrophobically modified tetrapod-shaped zinc oxide powder comprises the following steps: The tetrapod-shaped zinc oxide powder is mixed with ethanol and water to obtain a dispersion; adding a silane coupling agent to the dispersion to obtain a mixed solution; The pH value of the mixed solution is adjusted to 7-9, and the mixture is stirred at 50-70° C. for 4-6 hours, and the solid-liquid separation is performed to obtain hydrophobically modified tetrapod-shaped zinc oxide powder.

8. The method for preparing the composite coating according to claim 6, characterized in that: The preparation method of hydrophobically modified nano metal oxide powder comprises the following steps: Mixing nano metal oxide powder with ethanol and water to obtain a dispersion; adding a silane coupling agent to the dispersion to obtain a mixed solution; and adjusting the pH of the mixed solution to 7-9, stirring at 50-70° C. for 4-6 hours, and performing solid-liquid separation to obtain hydrophobically modified nano metal oxide powder.

9. The method for preparing the composite coating according to claim 7 or 8, characterized in that: The preparation method of the hydrophobically modified tetrapod-shaped zinc oxide powder and the hydrophobically modified nano metal oxide powder meets one or more of the following conditions: 1) The silane coupling agent is a perfluorinated silane coupling agent; 2) The mass ratio of the silane coupling agent to the tetrapod-shaped zinc oxide powder or the nano metal oxide powder is (1-10):100; 3) The concentration of the four-needle zinc oxide powder or the nano metal oxide powder in the dispersion is 1 wt.% to 12 wt.%; 4) The volume ratio of the ethanol to the water is (1-9):

1.

10. The method for preparing a composite coating according to any one of claims 1 to 5, characterized in that: The composite coating satisfies one or more of the following conditions: 1) The whisker length of the four-needle zinc oxide powder is 10 μm to 100 μm; 2) The particle size of the nano metal oxide powder is ≤100 nm; 3) The thickness of the liquid film is 50 μm to 70 μm; 4) The thickness of the composite coating is 80 μm to 100 μm.

11. The method for preparing a composite coating according to any one of claims 1 to 5, characterized in that: The adhesive liquid comprises an adhesive and a diluent in a mass ratio of 1:(1-3).

12. The method for preparing a composite coating according to any one of claims 1 to 5, characterized in that: The substrate is one or more of a polymer substrate, a glass substrate, a ceramic substrate and a metal substrate.

13. A composite coating, characterized in that: The composite coating is prepared by the preparation method of any one of claims 1 to 12.

14. A silicone rubber protective cover, characterized in that: Comprising the composite coating as claimed in claim 13.

15. An insulator, characterized in that: Comprising the silicone rubber protective cover as described in claim 14.

Citation Information

Patent Citations

  • Preparation method of super-hydrophobic surface of room temperature vulcanized silicone rubber

    CN104448374A

  • Preparation method of super-amphiphobic coating capable of being sprayed and lastingly resisting icing

    CN107022291A

  • Micro-nano composite super-hydrophobic wear-resistant coating layer and preparation method thereof

    CN113429867A

  • Composite coating and preparation method thereof, silicone rubber protective sleeve and insulator

    CN116426215A

  • Door-to-door sales bonus distribution method and bonus distribution system using the same

    KR102642543B1

Cited By

  • Electric porcelain insulator with wear-resistant hydrophobic structure and preparation method thereof

    CN120289210A

  • An electric porcelain insulator with a wear-resistant and hydrophobic structure and a preparation method thereof

    CN120289210B