Electrode catalyst and application thereof

Through the design of nanoparticle agglomeration structure and porous structure, the efficiency and cost problems of traditional catalysts in renewable energy are solved, and efficient and low-cost catalyst preparation and performance improvement are achieved.

WO2024222953A1PCT designated stage expired Publication Date: 2024-10-31SHANGHAI JUNA NEW MATERIAL TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/090387
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2024-04-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing catalysts still have room for improvement in terms of efficiency and cost in the utilization of renewable energy, especially in the field of hydrogen energy. The size and dispersion of traditional nanoparticles limit the performance of catalysts.

Method used

Adopting a nanoparticle agglomeration structure, including nanoparticles and protective layers, by controlling the size and dispersion of nanoparticles to reduce metal loading, using non-noble metal and conductive carrier nanoparticles to form high-entropy nanoparticle clusters and porous structures to improve the catalyst specific surface area and dispersion.

Benefits of technology

It achieves efficient and low-cost catalyst preparation, improves catalytic efficiency and material dispersion, is suitable for large-scale production, reduces the use of precious metals in electrode catalysts, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024090387_31102024_PF_FP_ABST
    Figure CN2024090387_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides an electrode catalyst, and an electrode and hydrogen electrolyzer which utilize the electrode catalyst. The electrode catalyst comprises: a nanoparticle agglomeration structure comprising nanoparticles, the size of the nanoparticle agglomeration structure being less than or equal to 65 nm, and the size of the nanoparticles being less than or equal to 10 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode catalyst and its application Technical Field

[0001] The present application belongs to the technical field of nanocatalyst structures, and specifically relates to an electrode catalyst and its application. Background Art

[0002] With the development of society, energy has gradually become a bottleneck restricting human progress, and environmental issues have become increasingly prominent. Therefore, the development of efficient, environmentally friendly renewable energy has become a key research topic for sustainable social and economic development. In recent years, renewable energy sources such as solar energy, wind energy, and hydrogen energy have been gradually developed. However, solar energy and wind energy are susceptible to environmental constraints, have low energy efficiency, and are difficult to transport. Hydrogen energy, with its high calorific value, easy storage and transportation, and environmentally friendly nature, has become one of the most promising energy sources of the 21st century.

[0003] However, the efficiency and cost of catalysts still need to be further improved.

[0004] Application Contents

[0005] In view of this, the purpose of the present application is to provide an electrode catalyst and an electrode and a hydrogen production electrolyzer using the same.

[0006] In various embodiments, the present application provides an electrode catalyst comprising:

[0007] Nanoparticle agglomerate structures, including nanoparticles;

[0008] The size of the nanoparticle agglomerate structure is less than or equal to 65 nm, and the size of the nanoparticles is less than or equal to 10 nm.

[0009] In various embodiments, an electrode for an electrochemical device is provided, comprising a substrate and the electrode catalyst described above.

[0010] In different embodiments, a hydrogen production electrolyzer is also provided, which includes the above-mentioned electrodes, namely electrode sheets or membrane electrodes. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] 1-4 are SEM images of nanoparticles and nanoparticle agglomerate structures in electrode catalysts of different embodiments.

[0012] FIG5 is a schematic diagram showing the microstructure of electrode catalysts in some embodiments of the present application.

[0013] FIG6 shows an SEM image of the electrode catalyst in some examples of the present application.

[0014] FIG7 is a schematic diagram showing the microstructure of electrode catalysts in some embodiments of the present application.

[0015] FIG8 shows a SEM image of the nanoparticles in the comparative example of the present application.

[0016] FIG9 is a schematic diagram showing the nanoparticles of the examples and comparative examples of the present application.

[0017] FIG10 shows an SEM image of a high entropy nanoparticle cluster in an embodiment of the present application.

[0018] FIG11 shows an SEM image of conventional nanoparticles in a comparative example of the present application.

[0019] 12-14 are scanning electron micrographs of electrode catalysts in different embodiments.

[0020] FIG15 shows a physical picture and performance curve of a membrane electrode prepared for electrode catalyst.

[0021] 16-19 show the special-shaped nanocatalysts in different embodiments.

[0022] 20-21 show scanning electron micrographs and X-ray energy spectrum diagrams of the heteromorphic nanocatalysts in different embodiments. DETAILED DESCRIPTION

[0023] The present application is further illustrated below through specific examples. However, it should be noted that the specific material ratios, process conditions and results described in the embodiments of the present application are only used to illustrate the present application and cannot be used to limit the scope of protection of the present application. Any equivalent changes or modifications made according to the spirit of the present application should be included in the scope of protection of the present application.

[0024] In some embodiments, the present application provides an electrode for an electrochemical device, such as an electrode sheet or a membrane electrode for electrolyzing water to produce oxygen. The electrode includes a substrate and an active material layer located on the substrate, wherein the active material layer includes a catalyst.

[0025] As shown in FIG1 , in some embodiments of the present application, the electrode catalyst may include a nanoparticle agglomerate structure 110, and the nanoparticle agglomerate structure 110 may be composed of agglomerates of nanoparticles 101. In an embodiment of the present application, the nanoparticle agglomerate structure of the electrode catalyst may be less than or equal to 65 nm, for example, 10 nm to 50 nm, or 30 nm to 50 nm, and the nanoparticles may be less than or equal to 10 nm, for example, 1 nm to 8 nm, or 1 nm to 6 nm. Furthermore, the nanoparticle agglomerate structure 110 also includes a protective layer P, which is formed between the nanoparticles. The material of the protective layer P may be, for example, selected from at least one of citrate, carboxymethyl cellulose, and polyacrylic acid, to coat at least a portion of the nanoparticles 101, control the size of the nanoparticles, limit agglomeration, and improve the dispersibility of the nanoparticles. It is worth noting that in the embodiments of the present application, alloy electrocatalytic materials with smaller nanoparticle size and excellent dispersibility can be prepared by efficient and rapid reduction.

[0026] In some embodiments, the electrode catalyst may include nanoparticles of different metals. Specifically, the electrode catalyst may include first metal nanoparticles 101 (e.g., the blue dots in FIG. 2 ) and second metal nanoparticles 102 (e.g., the green dots in FIG. 3 ), and the sizes of the first metal nanoparticles and the second metal nanoparticles may be less than or equal to 10 nm, for example, 1 nm to 8 nm, or even 1 nm to 6 nm. The second metal nanoparticles 102 may be dispersed between the first metal nanoparticles 101 and / or the nanoparticle agglomerate structures 110, and at least partially cover at least a portion of the first metal nanoparticles 101. In some embodiments, the first metal nanoparticles may agglomerate to form a first metal nanoparticle agglomerate structure 110 (as shown in FIG. 4 ), wherein the size of the first metal nanoparticle agglomerate structure is less than or equal to 65 nm, for example, 10 nm to 65 nm, or even 30 nm to 65 nm. The size of at least 50% of the nanoparticle agglomerate structures may be less than or equal to 50 nm, for example, the size of 50% to 80% of the nanoparticle agglomerate structures may be less than or equal to 50 nm.

[0027] In some embodiments, the nanoparticles of the electrode catalyst may further include non-precious metal nanoparticles 103, and the size of the non-precious metal nanoparticles may be less than or equal to 10 nm, for example, 1 nm to 8 nm, and for example, 1 nm to 6 nm. The material cost of the non-precious metal nanoparticles may be lower than the material cost of the first metal nanoparticles and / or the second metal nanoparticles. Therefore, by using non-precious metal nanoparticles, the material cost of the electrode catalyst can be reduced. Specifically, as shown in Figure 5, the first metal nanoparticles 101 and / or the second metal nanoparticles 102 can be agglomerated with the non-precious metal nanoparticles 103 to form a nanoparticle agglomerate structure to reduce the metal loading of the first metal nanoparticles 101 and / or the second metal nanoparticles 102, thereby reducing the material cost of the electrode catalyst. In the nanoparticle agglomerate structure, the metal loading of the first metal nanoparticles and / or the second metal nanoparticles may be less than or equal to 1 mg / cm 2 , for example 0.01 to 1 mg / cm 2 , for example 0.3~0.8mg / cm 2 .

[0028] For example, when used in hydrogen production electrolysis electrodes, the first metal nanoparticles can be metal nanoparticles of platinum or a platinum alloy, and the second metal nanoparticles can be metal nanoparticles of iridium or an iridium alloy. By controlling the size and structural composition of the nanoparticles and nanoparticle agglomerates, the metal loading of the first metal nanoparticles 101 and / or the second metal nanoparticles 102 can be reduced, thereby reducing the material cost of the electrode catalyst. The material of the non-noble metal nanoparticles can be a transition metal, such as at least one selected from titanium (Ti), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), osmium (Os), iridium (Ir), platinum (Pt), and gold (Au).

[0029] In some embodiments, as shown in FIG6 , the electrode catalyst may further include conductive carrier nanoparticles 104. The conductive carrier nanoparticles 104 may be formed in the nanoparticle agglomeration structure 110 or between the nanoparticles 101 and 102 to reduce the metal loading of the first metal nanoparticles 101 and / or the second metal nanoparticles 102 in the catalyst. The material cost of the conductive carrier nanoparticles 104 may be lower than the material cost of the first metal nanoparticles 101 and / or the second metal nanoparticles 102. Therefore, the use of the conductive carrier nanoparticles 104 may reduce the material cost of the electrode catalyst. The size of the conductive carrier nanoparticles 104 may be less than 100 nm, for example, less than or equal to 65 nm, or for example, between 30 nm and 65 nm. For example, the conductive carrier nanoparticles 104 may be carbon, nickel, or other metal conductive carrier nanoparticles.

[0030] In some embodiments, the electrode catalyst may further include a dispersion layer D, which may be formed between the nanoparticles to reduce the agglomeration of the nanoparticles and ensure the catalyst surface area of ​​the nanoparticles. For example, in FIG4 , the dispersion layer D may be formed between the second metal nanoparticles 102 to reduce the agglomeration of the second metal nanoparticles 102. The material of the dispersion layer may be selected from a mixture of one or more of (glycerol, citric acid (salt), carboxymethyl cellulose, sodium octadecyl sulfate, sodium lauryl sulfate, polyvinyl pyrrolidone, cetylpyridinium chloride (bromide), stearic acid, oleic acid, lauric acid, polyacrylic acid, etc.). However, not limited to this, in some embodiments, the second metal nanoparticles 102 may also aggregate to form a second metal nanoparticle agglomerate structure, wherein the size of the second metal nanoparticle agglomerate structure may be less than or equal to 50 nm, for example, 10 nm to 50 nm, or for example 30 nm to 50 nm.

[0031] In some embodiments, the second metal nanoparticles 102 may at least partially coat at least a portion of the surface of the nanoparticle agglomerate structure 110, as shown in, for example, Figures 2 to 4 and 7, and the nanoparticle agglomerate structure (i.e., the first nanoparticle agglomerate structure 110) may be composed of first metal nanoparticles and / or non-precious metal nanoparticles. When the material cost of the second metal nanoparticles is higher than the material cost of the first metal nanoparticles and the non-precious metal nanoparticles, the metal loading of the second metal nanoparticles in the catalyst may be reduced by coating the second metal nanoparticles on at least a portion of the surface of the nanoparticle agglomerate structure, thereby reducing the material cost of the electrode catalyst. In the electrode catalyst, the metal loading of the second metal nanoparticles may be less than or equal to 1 mg / cm 2 , for example 0.01 to 1 mg / cm 2 , for example 0.5~1mg / cm 2 .

[0032] The embodiments of the present application can control the size of nanoparticles, limit agglomeration, improve the dispersibility of nanoparticles, and can be reduced and prepared efficiently and quickly under a mild reaction environment with an electrocatalytic material having a smaller nanoparticle size and excellent dispersibility. For example, FIG. 1 shows an SEM image of the nanoparticles obtained in the embodiments of the present application, and FIG. 8 shows an SEM image of traditional nanoparticles. As can be seen from the comparison, the average particle size of the nanoparticles in FIG. 1 is about 5 nm, and the average particle size of the nanoparticles in FIG. 8 is about 50 nm, which shows that the method of the embodiments of the present application can control the size of nanoparticles and limit agglomeration. FIG. 9 shows a photograph of the nanoparticles (left) and traditional nanoparticles (right) after standing in an ethanol dispersion for 48 hours. As can be seen from FIG. 9, the embodiments of the present application can limit agglomeration and improve the dispersibility of nanoparticles. In general, the catalyst of the present application not only has a simple preparation process, but also has good catalytic efficiency and is suitable for large-scale production.

[0033] For example, a cathode electrode (electrode sheet or membrane electrode) in an electrolytic cell may include a nanoparticle agglomerate structure 110 formed by agglomeration of first metal nanoparticles 101 and non-noble metal nanoparticles 103. For another example, an anode electrode (electrode sheet or membrane electrode) in an electrolytic cell may include second metal nanoparticles 102, which may at least partially encapsulate the nanoparticle agglomerate structure 110.

[0034] In one embodiment, the nanoparticle agglomeration structure can be a high entropy nanoparticle cluster, and the high entropy nanoparticle cluster includes at least three metal elements. The nanoparticle agglomeration size of the high entropy nanoparticle cluster can be less than 50nm, as shown in Figure 10, for example, it can be less than or equal to 30nm, so that the nanocluster size can be controlled so that the active site is highly exposed, the mass transfer channel is sufficient, and the conductivity is high. Compared with the conventional nanoparticle agglomeration size greater than 100nm in the comparative example shown in Figure 11, the active site exposure of the high entropy nanoparticle cluster of the present application is higher and has higher conductivity. In some embodiments, the high entropy nanoparticle cluster can be spherical, flaky, linear, chain-like, irregular or other shape structures.

[0035] In one embodiment of the present application, the surface of the nanocatalyst structure or nanoparticle agglomerate structure may have multiple pores, with the pore size being less than 80 nm, for example, 1-80 nm, 5-60 nm. The nanocatalyst structure may be coral-shaped, spherical, sheet-like, linear, chain-like, irregularly shaped, or other shapes.

[0036] In one embodiment of the present application, the nanocatalyst structure or nanoparticle agglomerate structure may include a coral-like (e.g., dealloyed) nanowire array structure, wherein the nanowire array structure has a coral-like porous structure, and the size of the pores may be less than 80 nm. The length of the nanowire array is, for example, 10 μm to 1100 μm, and the diameter of the nanowire is, for example, 120 nm to 200 nm. In this embodiment, the electrode catalyst includes at least metal element A and element B, wherein element A is selected from at least one of transition metals such as Mn, Cr, Fe, Co, Ni, or Cu, and element B is selected from precious metals such as Ir. By forming a coral-like porous structure, the specific surface area of ​​the electrode catalyst is increased, thereby increasing the contact area with water under the same mass and improving the catalytic efficiency.

[0037] In one embodiment of the present application, the specific surface area of ​​the electrode catalyst may be greater than 10 m 2 / g, for example, 10 to 100 m 2 / g. This increases the electrochemical surface area of ​​the electrode catalyst, exposes more active sites, and provides numerous mass transfer channels, improving the catalytic performance of the electrode catalyst. Using the electrode catalyst to create a membrane electrode significantly reduces the amount of precious metals used in the catalyst layer, significantly reducing costs.

[0038] In another embodiment of the present application, the nanocatalyst structure or nanoparticle agglomerate structure may include a hollow spherical structure or a hollow chain structure, wherein the diameter of the hollow spherical structure is, for example, 3 nm to 25 nm. In the hollow chain structure, the length of the hollow chain is, for example, 10 μm to 1100 μm, and the diameter of the hollow spheres on the hollow chain is, for example, 0.5 μm to 1.5 μm. The electrode catalyst with a hollow structure has a regular shape and uniform size, which is conducive to the transmission of fluids.

[0039] In another embodiment of the present application, the electrode catalyst includes at least two of a transition metal, a lanthanide rare earth element and a platinum group noble metal element, wherein the transition metal includes, for example, at least one of Mn, Cr, Zr, Fe, Co, Ni, Cu, Zn, Mo or W, and the platinum group noble metal element includes at least one of Ru, Rh, Pd, Ag, Os, Ir, Pt or Au. In one embodiment of the present application, the electrocatalyst includes, for example, the following components in mass percentage: 70% transition metal, 30% lanthanide rare earth element and / or platinum group noble metal element, and the rest is oxygen. In one embodiment of the present application, the specific surface area of ​​the electrode catalyst is, for example, 15 to 25 m 2 By forming a hollow spherical electrode catalyst, the electrochemical specific surface area of ​​the electrode catalyst can be increased. At the same time, the hollow structure improves the mass transfer efficiency and strength of the catalyst, thereby improving the catalytic performance of the electrode catalyst.

[0040] In one embodiment of the present application, different metal precursor solutions can be selected to obtain electrode catalysts with different morphologies. For example, to obtain an electrode catalyst with a coral-like porous structure, the metal precursor solution includes at least one transition metal such as Mn, Cr, Fe, Co, Ni, or Cu, and a noble metal such as Ir. For example, to obtain an electrode catalyst with a hollow spherical structure or a hollow chain structure, the metal precursor solution includes at least two of a transition metal, a lanthanide rare earth element, and a platinum group noble metal element, wherein the transition metal includes, for example, at least one of Mn, Cr, Zr, Fe, Co, Ni, Cu, Zn, Mo, or W, and the platinum group noble metal element includes at least one of Ru, Rh, Pd, Ag, Os, Ir, Pt, or Au.

[0041] In one embodiment of the present application, nanocatalyst structures or nanoparticle agglomerate structures of different morphologies can be obtained by different morphology induction layers. In one embodiment of the present application, in order to obtain an electrode catalyst with a coral-like porous structure, a first inducer and a second inducer can be added in sequence. The first inducer includes a solvent such as a metal salt, a metal halide, a metal sulfate, and a metal nitrate, and the metal is selected from at least two of Mn, Cr, Fe, Co, Ni, Cu, Zn, and platinum group noble metal elements. The second inducer is selected from at least one of organic solvents such as methanol, ethanol, propanol, acetone, dimethylformamide, cyclohexane, ethyl acetate, and dimethyl sulfoxide. The (molar) ratio of the metal precursor solution, the first inducer, and the second inducer is, for example, 1:1 to 1:10.

[0042] In another embodiment of the present application, in order to obtain an electrode catalyst with a hollow spherical structure or a hollow chain structure, the organic inducer in the catalyst is, for example, selected from isophthalic acid esters, phthalates, 1,4-diazabicyclo[2.2.2]octane, triethylenediamine, 1,4-dimethylpiperazine, hexamethylenetetramine, pyromellitic acid, trimesic acid, 1,4-bis(1H-pyrazol-4-yl)benzene, 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetracarboxylic acid, 2,4,6-tris(4-pyridyl)-1,3 The organic inducing agent may be selected from at least one of: 1,5-triazine, tris(isobutylaminoethyl)amine, bis(3,5-dicarboxyphenyl)azo, biphenyldicarboxylic acid, 2,5-dihydroxyterephthalic acid, 2,6-naphthalene dicarboxylic acid, 1,4-phenylenedicarboxylic acid, 1,1,2,2-tetrakis(4-carboxyphenyl)ethylene, 1,3,5-tris(4-carboxyphenyl)benzene, 2-(diphenylphosphino)terephthalic acid, 2-amino-4-hydroxy-6-methylpyrimidine, 2-methylimidazole, 2-aminoterephthalic acid, terephthalic acid, fumaric acid, and trioctyl trimellitate. The molar concentration ratio of the organic inducing agent to the total metal ions in the metal precursor solution is, for example, 1:10,000 to 100:1.

[0043] In one embodiment of the present application, different metal precursor solutions and morphology inducing layers are selected according to the morphology or performance requirements of the electrode catalyst to be obtained, so as to achieve the production requirements of different morphologies.

[0044] In one embodiment of the present application, the intermediate is obtained by stirring at a preset temperature for a preset time, for example, the pH value of the mixed solution of the metal precursor solution and the morphology inducer is controlled to obtain solid intermediates with different morphologies.

[0045] In one embodiment of the present application, the electrode catalyst can obtain different morphologies by, under the conditions of a first inducer and a second inducer, obtaining a coral-like dealloyed nanowire array structure. In another specific embodiment of the present application, under the conditions of an organic inducer, a spherical or sphere-chain structure can be obtained.

[0046] In one embodiment of the present application, when forming pores in the intermediate, for example, acid washing or calcination treatment can be used to remove part of the metal, form pores on the catalyst surface, and obtain a porous electrode catalyst. The specific selection is based on the preset morphology of the electrode catalyst to be produced.

[0047] In another embodiment of the present application, when pores are formed in a spherical or ball-chain structure, for example, by adopting an acid wash treatment or a calcination treatment, a hollow structure can be obtained.

[0048] In this application, different metal precursor solutions and morphology-inducing layers are selected to achieve different morphology requirements. Based on the resulting morphology, different pore-forming methods are then selected to obtain nanocatalyst structures or nanoparticle agglomerates with multiple pores on their surfaces. By controlling the pore-forming time, the pore size is controlled to less than 80 nm to meet catalytic requirements.

[0049] As shown in Figure 12, the microscopic morphology of the electrode catalyst produced in this embodiment is characterized by a coral-like nanowire array structure forming a nanocatalyst structure. The nanowire array length ranges from 10 μm to 1100 μm, and the nanowire diameter ranges from 120 nm to 200 nm. Testing has shown that the electrode catalyst produced in this embodiment comprises 70% M, 20% N, and 10% oxygen, with a uniform distribution of elements, enhancing the consistency of the catalytic effect.

[0050] As shown in Figure 13, the microscopic morphology of the electrode catalyst can be: a hollow spherical structure, and the diameter of the hollow spherical structure is, for example, 3nm to 25nm. As shown in Figure 14, the microscopic morphology of the electrode catalyst can be: a hollow chain structure, and the length of the hollow chain is, for example, 10μm to 1100μm, and the diameter of the hollow sphere on the hollow chain is, for example, 0.5μm to 1.5μm.

[0051] Figure 15 shows a photo and performance curve of a membrane electrode fabricated using the electrode catalyst shown in Figure 12. Figure 15 demonstrates that the electrode catalyst is evenly distributed on the substrate, forming a high-quality membrane electrode. The voltage versus current density curve shows that the electrolysis voltage is 2.02 V at 2 A·cm⁻². This low voltage indicates that Ir usage can be reduced, lowering production costs.

[0052] In one embodiment of the present application, a special-shaped electrolytic water catalyst provided by the present application is used in an electrolytic water hydrogen production device. As shown in Figure 16, the special-shaped electrolytic water catalyst includes a special-shaped nanocatalyst structure 10 (or a nanoparticle agglomerate structure) and a morphology inducing layer 20. The morphology inducing layer 20 can be formed on a partial surface of the special-shaped nanocatalyst structure (nanoparticles or nanoparticle agglomerate structure). In one embodiment of the present application, the morphology inducing layer 20 is, for example, at least one layer. When the morphology inducing layer 20 is multi-layered, the multi-layer morphology inducing layer can be sequentially stacked on the special-shaped nanocatalyst structure. In one embodiment of the present application, the specific surface area of ​​the special-shaped electrolytic water catalyst is, for example, greater than or equal to 100m 2 / g, for example, 100 to 1000 m 2 / g. By forming heterogeneous nanocatalysts, the specific surface area of ​​the catalyst is larger, which increases the catalytic performance. At the same time, it can increase the porosity when forming the membrane electrode, reduce the bed pressure drop of the electrolyzer, facilitate water diffusion, and accelerate the catalytic efficiency. The heterogeneous catalyst also improves the processing performance during the formation of electrode sheets or membrane electrodes.

[0053] Referring to Figures 16 to 21, in one embodiment of the present application, the shape of the special-shaped electrolysis water catalyst is, for example, one or more combinations of polyhedral, needle-shaped, pointed prism-shaped, spherical, chain-shaped or fused spherical, and can be specifically controlled according to the manufacturing process. Wherein, when the shape of the special-shaped electrolysis water catalyst is different, the size of the special-shaped electrolysis water catalyst is different, specifically determined according to the morphology of the heterogeneous nanocatalyst formed. By forming a special-shaped electrolysis water catalyst of different shapes and sizes, when applied to the electrode (such as the electrode sheet or membrane electrode of an electrolyzer or battery) of an electrochemical device, an electrode sheet or membrane electrode with different catalytic abilities can be formed to meet the use under different environments or requirements.

[0054] In another embodiment of the present application, the special-shaped water electrolysis catalyst includes at least two of a transition metal, a lanthanide rare earth element, and a platinum group noble metal element, wherein the transition metal includes, for example, at least one of Mn, Cr, Zr, Fe, Co, Ni, Cu, Zn, Mo, or W, and the platinum group noble metal element includes at least one of Ru, Rh, Pd, Ag, Os, Ir, Pt, or Au.

[0055] In one embodiment of the present application, the material of the shaped nanocatalyst structure is at least one of a metal, an alloy, or a metal oxide, and the material of the morphology-inducing layer is at least one of a metal, an alloy, or a metal oxide. The material of the shaped nanocatalyst structure and the morphology-inducing layer can be the same or different, depending on the intended catalytic application (function). For example, a metal or alloy can be used in a cathode for hydrogen production, while a metal oxide can be used in an anode for oxygen production.

[0056] In one embodiment of the present application, in the metal precursor solution, the metal elements include at least two of transition metal elements, lanthanide rare earth elements and platinum group noble metal elements, wherein the transition metal elements include, for example, at least one of Mn, Cr, Zr, Fe, Co, Ni, Cu, Zn, Mo or W, and the platinum group noble metal elements include at least one of Ru, Rh, Pd, Ag, Os, Ir, Pt and Au, and the solvent of the metal precursor solution includes pure water, ultrapure water, deionized water or tap water. The metal elements come from water-soluble metal salts such as metal acid salts, metal halides, metal sulfates or metal nitrates. The metal salts are added to the solvent, for example, by ultrasonic stirring for 2 minutes to 5 minutes to obtain a metal precursor solution. In other embodiments, dissolution can also be performed by other means. In the metal precursor solution, the concentration of total metal ions is, for example, 0.01 to 1M.

[0057] In one embodiment of the present application, in order to obtain a shaped electrolytic water catalyst of different shapes, a morphology induction layer is used, and the material of the morphology induction layer is selected from, for example, isophthalic acid esters, phthalates, 1,4-diazabicyclo[2.2.2]octane, triethylenediamine, 1,4-dimethylpiperazine, hexamethylenetetramine, pyromellitic acid, trimesic acid, 1,4-bis(1H-pyrazol-4-yl)benzene, 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetracarboxylic acid, 2,4,6-tris(4-pyridyl)-1,3, At least one of 5-triazine, tris(isobutylaminoethyl)amine, bis(3,5-dicarboxyphenyl)azo, biphenyldicarboxylic acid, 2,5-dihydroxyterephthalic acid, 2,6-naphthalene dicarboxylic acid, 1,4-phenylenedicarboxylic acid, 1,1,2,2-tetrakis(4-carboxyphenyl)ethylene, 1,3,5-tris(4-carboxyphenyl)benzene, 2-(diphenylphosphino)terephthalic acid, 2-amino-4-hydroxy-6-methylpyrimidine, 2-methylimidazole, 2-aminoterephthalic acid, terephthalic acid, fumaric acid, and trioctyl trimellitate. The molar concentration ratio of the organic induction layer to the total metal ion concentration in the metal precursor solution is, for example, 1:10,000 to 100:1.

[0058] In one embodiment of the present application, different metal precursor solutions and morphology-inducing layers are selected based on the desired morphology or performance requirements of the desired shaped electrolytic water catalyst to achieve the desired morphology. Specifically, by controlling the reaction raw materials and reaction conditions, a shaped electrolytic water catalyst with the desired morphology can be obtained.

[0059] In one embodiment of the present application, to obtain a shaped electrolytic water catalyst having a multi-layer morphology-inducing layer, the morphology-inducing layer can be in situ grown on the shaped electrolytic water catalyst to obtain a shaped electrolytic water catalyst having a multi-layer morphology-inducing layer. The material of the multi-layer morphology-inducing layer can be exactly the same as the material of the shaped nanocatalyst structure, or it can be partially or completely different.

[0060] As can be seen from Figure 16, the microscopic morphology of the heterogeneous electrolytic water catalyst is, for example, a hexagonal heterogeneous electrolytic water catalyst, and the side length of the hexagon is, for example, 0.1μm to 1.5μm. As can be seen from Figure 17, the microscopic morphology of the heterogeneous electrolytic water catalyst is, for example, a needle-shaped heterogeneous electrolytic water catalyst, and the length of the nanocatalyst structure is, for example, 0.2μm to 5μm. As can be seen from Figure 18, the microscopic morphology of the heterogeneous electrolytic water catalyst is, for example, a pointed prism-shaped heterogeneous electrolytic water catalyst, and the length of the nanocatalyst structure is, for example, 0.01μm to 2μm. As can be seen from Figure 19, the microscopic morphology of the heterogeneous electrolytic water catalyst is, for example, a fused spherical heterogeneous electrolytic water catalyst, and the diameter of the sphere is, for example, 0.01μm to 0.5μm. That is, by selecting different metal precursors and morphology inducing layers, heterogeneous electrolytic water catalysts with different morphologies can be obtained.

[0061] As shown in Figure 20, the microscopic morphology of the heterogeneous electrolytic water catalyst is: a chain-like structure, with the chain length ranging from 8μm to 1000μm, for example, with only a portion of the length shown in the figure. Testing has shown that the heterogeneous nanocatalyst structure produced in this example comprises 50% transition metal, 45% noble metal, and 5% oxygen. The material of the morphology-inducing layer is the same as that of the heterogeneous nanocatalyst structure.

[0062] As shown in FIG21 , the heteromorphic nanocatalyst structure prepared in this embodiment includes 50% transition metal, 45% noble metal, and 5% oxygen. The material of the morphology inducing layer is the same as that of the heteromorphic nanocatalyst structure.

[0063] The present application also provides an electrochemical device, such as a water electrolysis device or a fuel cell, comprising the electrode catalyst as described above. The catalyst prepared in the present application has higher activity and better stability.

[0064] Therefore, the catalyst of the present application has a larger specific surface area, which enhances catalytic performance. Furthermore, when formed into electrodes for electrolytic cells, the porosity can be increased, reducing bed pressure drop, facilitating water diffusion and accelerating catalytic efficiency. By forming catalysts of different shapes and sizes, electrodes with varying catalytic capabilities can be formed to meet different environments or requirements.

[0065] In some embodiments, the electrode catalyst can be applied to a hydrogen production electrolysis unit or a hydrogen production electrolyzer, such as a proton exchange membrane (PEM) electrolyzer, an anion exchange membrane (AEM) electrolyzer, an alkaline solution electrolyzer, a solid oxide (SOEC) or other electrolyzer electrodes using catalyst electrodes. Specifically, the electrode catalyst of the present application can be formed on different substrates to form an electrode sheet or a membrane electrode. However, it is not limited thereto. In other embodiments, the electrode catalyst can also be applied to electrodes of other electrochemical devices, such as electrodes of fuel cells or other electrochemical electrolyzers.

[0066] The above embodiments are merely illustrative of the principles and effects of this application and are not intended to limit this application. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical concepts disclosed in this application shall be covered by the claims of this application.

Claims

1. An electrode catalyst comprising: Nanoparticle agglomerate structures, including nanoparticles; The size of the nanoparticle agglomeration structure is less than or equal to 65 nm, and the size of the nanoparticles is less than or equal to 10 nm. 2 . The electrode catalyst according to claim 1 , wherein the nanoparticle agglomeration structure further comprises a protective layer formed between the nanoparticles. 3 . The electrode catalyst according to claim 1 , wherein at least 50% of the nanoparticle agglomerate structures have a size of less than or equal to 50 nm. 4 . The electrode catalyst according to claim 1 , further comprising non-noble metal nanoparticles, wherein the nanoparticles are aggregated with the non-noble metal nanoparticles to form the nanoparticle aggregate structure.

5. The electrode catalyst according to claim 1, wherein the material of the non-precious metal nanoparticles may be a transition metal selected from at least one of titanium (Ti), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), osmium (Os), iridium (Ir), platinum (Pt), and gold (Au). 6 . The electrode catalyst according to claim 1 , further comprising conductive support nanoparticles formed between the nanoparticle agglomerated structures. 7 . The electrode catalyst according to claim 1 , further comprising a dispersion layer formed between the nanoparticles. The electrode catalyst according to claim 1 , wherein the nanoparticles are 1 nm to 8 nm. 9 . The electrode catalyst according to claim 1 , wherein the nanoparticles include first metal nanoparticles and second metal nanoparticles, and the first metal nanoparticles are aggregated to form the nanoparticle aggregate structure. 10 . The electrode catalyst according to claim 9 , further comprising a dispersion layer formed between the second metal nanoparticles.

11. The electrode catalyst according to claim 9, wherein the metal loading of the second metal nanoparticles in the electrode catalyst is less than or equal to 1 mg / cm 2 . 12 . The electrode catalyst according to claim 9 , wherein the second metal nanoparticles at least partially cover at least a portion of the surface of the nanoparticle agglomerate structure.

13. The electrode catalyst according to claim 9, wherein the metal loading of the first metal nanoparticles in the first nanoparticle agglomerate structure is less than or equal to 1 mg / cm 2 . 14 . The electrode catalyst according to claim 1 , further comprising conductive carrier nanoparticles, wherein the conductive carrier nanoparticles are formed in the nanoparticle agglomeration structure or between nanoparticles, and the size of the conductive carrier nanoparticles is less than 100 nm.

15. The electrode catalyst according to claim 1, wherein the nanoparticle agglomeration structure is a high entropy nanoparticle cluster. 16 . The electrode catalyst according to claim 1 , wherein the surface of the nanoparticle agglomeration structure has a plurality of holes, and the size of the holes is less than 80 nm.

17. The electrode catalyst according to claim 1, wherein the specific surface area of ​​the electrode catalyst is greater than 10 m 2 / g. 18 . The electrode catalyst according to claim 1 , further comprising a morphology inducing layer formed on a portion of the surface of the nanoparticles or the nanoparticle agglomerate structure.

19. An electrode for an electrochemical device, comprising: Substrate and electrode catalyst; Wherein the electrode catalyst comprises: Nanoparticle agglomerate structures, including nanoparticles; The size of the nanoparticle agglomeration structure is less than or equal to 65 nm, and the size of the nanoparticles is less than or equal to 10 nm.

20. A hydrogen production electrolyzer comprising the electrode according to claim 19.

Citation Information

Patent Citations

  • Graded dendritic PtCu electro-catalyst and preparation method thereof

    CN109174119A

  • Preparation method of PdCuFeCoNi high-entropy alloy nanoparticle catalyst applied to water electrolysis

    CN113774422A