Method for producing a semiconductor wafer, and semiconductor wafer
The method of using mechanical and ion beam/laser beam thinning with iterative checks and chemical-mechanical polishing addresses the challenge of producing uniform semiconductor wafers, ensuring precise and damage-free thickness adjustment and high-quality crystalline thin films.
Patent Information
- Application Number
- PCT/EP2024/061215
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Existing methods for producing semiconductor wafers often result in damaged or inhomogeneous single-crystalline thin films on amorphous materials, leading to issues with uniformity and precision in thickness adjustment.
A method involving a coating wafer attached to a carrier wafer, where the initial thickness is reduced mechanically and then finely adjusted using ion beams or laser beams based on thickness maps, with iterative checks and chemical-mechanical polishing to achieve precise and uniform thinning, minimizing damage to the crystalline layer.
This method allows for precise adjustment of the semiconductor wafer thickness with low risk of damage, achieving high uniformity and quality of the crystalline thin films, enabling efficient production of semiconductor wafers with improved layer homogeneity and reduced light conduction losses in waveguides.
Smart Images

Figure EP2024061215_31102024_PF_FP_ABST
Abstract
Description
[0001] METHOD FOR PRODUCING A SEMICONDUCTOR WAFER AND SEMICONDUCTOR WAFER
[0002] The invention relates to a method for producing a semiconductor wafer and to a semiconductor wafer.
[0003] US 2023 / 0039295 A1 discloses a method for manufacturing an image sensor, in which a receiver substrate and a donor substrate are bonded together. The donor substrate is partially stripped to transfer a semiconductor layer of the donor substrate to the receiver substrate. Subsequently, the transferred monocrystalline semiconductor layer is subjected to finishing processing, which comprises thinning the transferred monocrystalline semiconductor layer by sacrificial oxidation, followed by chemical etching and smoothing the transferred monocrystalline semiconductor layer by at least one rapid annealing step.
[0004] A method for processing and manufacturing semiconductor components is known from CN 115697016 A. Lithium niobate is bonded to a silicon substrate at low temperature, followed by a thinning and polishing process.
[0005] Furthermore, a semiconductor substrate is known from US 2014 / 0367691 A1.
[0006] The object of the present invention is to provide a solution by means of which the production of damaged or inhomogeneous, single-crystalline thin films on amorphous materials can be avoided during the production of a semiconductor wafer.
[0007] This object is achieved according to the invention by the subject matter of the independent claims. Further possible embodiments of the invention are specified in the subclaims, the description, and the drawings. Features, advantages, and possible embodiments presented in the description for one of the subject matter of the independent claims are to be regarded at least analogously as features, advantages, and possible embodiments of the respective subject matter of the other independent claims, as well as any possible combination of the subject matter of the independent claims, optionally in conjunction with one or more of the subclaims.
[0008] The invention relates to a method for producing a semiconductor wafer. In microelectronics, photovoltaics, and microsystem technology, wafers are circular or square discs. They are manufactured from monocrystalline or polycrystalline semiconductor blanks, so-called ingots, and typically serve as a substrate and thus base plate for electronic components, including integrated circuits and thus chips, micromechanical components, or photoelectric coatings.
[0009] The method for producing the semiconductor wafer comprises the method steps a) to d) described below, which must be carried out consecutively. In the first method step a), a coating wafer is placed on a carrier wafer and attached to this carrier wafer. In a second method step b), an initial thickness of the coating wafer is reduced to a first processing thickness by means of a first mechanical removal process. Mechanical methods for material removal are used for the first mechanical removal process. During this first mechanical removal process, the coating wafer's thickness can be reduced by grinding and / or polishing. In a third method step c), the thickness of the coating wafer resulting from the first removal process is determined in the form of a thickness map over its entire base area adjacent to the carrier wafer.This checks how the thickness of the coating wafer behaves across the entire base area. The thickness map thus stores the thickness of the coating wafer at each point on the base area. In particular, the thickness is perpendicular to the base area.
[0010] The method further provides that, in a fourth method step d), the thickness of the coating wafer is further reduced in a second ablation process using an ion beam and / or a laser beam, wherein the areas to be ablated and the portions of the coating wafer's thickness to be ablated are selected depending on the created thickness map. This means that, depending on the created thickness map and thus depending on the distribution of the coating wafer's thickness across its base area, it is selected in which areas of the coating wafer which portion of the coating wafer's thickness is to be reduced during the second ablation process.This enables the coating wafer to be reduced in thickness in a targeted and thus locally defined manner during the second removal process, enabling particularly good uniformity of the coating wafer's thickness across the base area of the coating wafer. The method thus involves a rough reduction of the coating wafer's thickness using the first mechanical removal process, followed by a fine adjustment of the thickness across the entire base area of the coating wafer in the second removal process. This allows the risk of damage to the thin film of the coating wafer, particularly the monocrystalline film, to be kept particularly low.
[0011] In other words, the method provides for two wafers, in this case the coating wafer and the carrier wafer, which in particular have an identical size. The coating wafer only comprises material intended to provide the crystalline thin film in the semiconductor wafer. The carrier wafer serves as the carrier for the coating wafer and can have an amorphous dielectric, such as silicon dioxide, as its uppermost layer. Alternatively, the coating wafer can be coated with an amorphous dielectric and applied to the carrier wafer with this coating. In the method, the coating wafer is connected to the carrier wafer. The coating wafer is thinned by means of a mechanical thinning technique during the first removal process to a thickness which is greater than the final desired thin film for the coating wafer over its entire base area.The thickness of the remaining coating wafer material is mapped across the entire coating wafer. The carrier wafer, with the remaining coating wafer material on its upper surface, undergoes selective etching during the second removal process. This process enables the thickness of the coating wafer on the carrier wafer to be precisely adjusted with minimal damage for the thin film to be produced. The thickness of the coating wafer can be removed with particular precision using the ion beam or laser beam.
[0012] In a possible further development of the invention, it is provided that after the second removal process, the thickness of the coating wafer over the base area is determined in the form of a further thickness map and, depending on the further thickness map, the coating wafer is subjected to a further second removal process or is not subjected to a further second removal process. In other words, the creation of the thickness map and the reduction of the thickness of the coating wafer in the second removal process are repeated alternately until the thickness of the coating wafer over its entire base area lies within predetermined tolerance limits for the thickness of the coating wafer. Thus, the thickness of the coating wafer is checked several times and the thickness of the coating wafer is reduced during the second removal process.The thickness of the coating wafer on the carrier wafer can thus be adjusted iteratively with great precision. This minimizes the risk of damage when adjusting the thickness of the coating wafer. Furthermore, the actual thickness of the coating wafer can be adjusted very closely to a specified target thickness for the coating wafer across its entire surface area.
[0013] In a further possible embodiment of the invention, it is provided that after carrying out the last, second removal process, an outer surface of the coating wafer opposite the base surface is polished. By polishing the coating wafer, a variance in the thickness of the coating wafer above the base surface is reduced. This means that the surface of the coating wafer is leveled. Differences in thickness between different regions of the coating wafer are thus reduced. This subsequent polishing process helps to smooth and thus homogenize the uppermost layers of the coating wafer, which were attacked by the second removal process (e.g. by means of an ion beam or laser beam). In this way, even the finest chippings that have arisen in the upper boundary layer as a result of the ion beam or laser beam process can be removed.
[0014] In a further possible embodiment of the invention, it is provided that after performing the first removal process and before performing the second removal process, the outer surface of the coating wafer opposite the base surface is polished. In other words, the polishing process can already take place after the first removal process. This allows the surface of the coating wafer to be leveled after the first removal process, which is particularly carried out as a mechanical removal process (such as grinding or polishing).
[0015] In this context, it may be particularly necessary for the outer surface to be polished using chemical-mechanical polishing. Chemical-mechanical polishing, also known as chemical-mechanical planarization, is a polishing process used in wafer processing to evenly remove thin layers. For the production of microelectronic circuits, among other things, thin layers are applied to a very flat and smooth wafer in several steps and then structured. After several layers, severe unevenness can arise, which can lead to the tearing off of a higher layer and thus make multilayer systems difficult to implement. This problem becomes more pronounced with increasing circuit complexity, since multiple metallization levels are required for component wiring. Chemical-mechanical polishing smooths out unevenness in the coating wafer.This allows additional layers to be applied to the coating wafer with particular precision, while the risk of a higher layer being torn off can be kept particularly low.
[0016] Chemical-mechanical polishing offers the further advantage that waveguides subsequently incorporated into the coating wafer have a very smooth top surface. The top surface here refers to the area facing away from the carrier wafer. By keeping the top and side surfaces as smooth as possible, losses during light transmission in the waveguide are reduced, which has a positive effect on waveguiding efficiency.
[0017] In a further possible embodiment of the invention, the thickness map is determined using ellipsometry or reflection spectrometry. Spectroscopic ellipsometry is an optical examination method for measuring the thickness of thin films. Ellipsometry determines the change in the polarization state of light upon reflection or transmission from a sample. Reflection spectroscopy is understood to be the investigation of the spectral composition of radiation reflected from surfaces in relation to its angle-dependent intensity and the composition of the incident primary radiation. Creating the thickness map using ellipsometry or reflection spectrometry enables a particularly precise determination of the thickness of the coating wafer across all areas of the base surface of the coating wafer.
[0018] In a further possible embodiment of the invention, it is provided that an average thickness of the coating wafer across its base area is set to a maximum of 3000 nanometers, preferably a maximum of 1200 nanometers, in particular a maximum of 600 nanometers, by means of the second removal process. This means that the average thickness of the coating wafer is to be reduced during the second removal process such that the thickness of the coating wafer in the semiconductor wafer is on average a maximum of 3000 nanometers, preferably a maximum of 1200 nanometers, particularly preferably a maximum of 600 nanometers. Thus, both relatively thick and particularly thin layers can be formed on the carrier wafer using the coating wafer.
[0019] In a further possible embodiment of the invention, a lithium niobate wafer is applied as a coating wafer to a silicon dioxide layer of a silicon carrier wafer as the carrier wafer. The lithium niobate of the lithium niobate wafer thus forms the crystalline thin-film on the carrier wafer. The silicon carrier wafer containing the silicon dioxide layer is used as the carrier wafer. Lithium niobate exhibits a wide transparency range, high electro-optical and non-linear optical coefficients, very high electromechanical coupling coefficients, and high chemical and mechanical stability.
[0020] In a further possible embodiment of the invention, it is provided that in the second removal process the thickness of the coating wafer is reduced by means of ion beam etching with a focused ion beam, which is also referred to as ion thinning or focused ion beam electric etching (FIBE), by means of grayscale lithography combined with ion beam etching, which is also referred to as grayscale lithography combined with ion beam etching (IBE), or by means of laser ablation. In unfocused ion beam etching, which is also referred to as ion beam etching (IBE), a broad beam of positively charged ions is directed onto a substrate and material is removed from the substrate surface by ion bombardment. Laser ablation, also called laser evaporation, is ablation by pulsed laser radiation. The laser radiation used here with a high power density leads to rapid heating and the formation of a plasma on the surface.This exceeding of the plasma threshold is used to distinguish it from laser desorption, which does not produce plasma. Grayscale lithography was developed with the goal of achieving a desired thickness topography. A photolithography concept can be followed here, which involves the production of binary structures, i.e. structures consisting of removed and unchanged regions. The surface topography is adjusted by varying the dose of ion radiation. A variable dose of ion irradiation can be achieved via multiple irradiation or grayscale masks. With multiple irradiation, depending on the desired structure, either a mask is moved step by step or several binary masks with different shading are used. Each irradiation step can have a different irradiation dose. Grayscale masks have regions with different transmittances.These transmittances are implemented via a layer of a partially absorbing material, the thickness of which is varied in the range of complete absorption and transmission for the ion radiation.
[0021] In one specific embodiment, a photoresist is applied to the top of the wafer, and the wafer is exposed to different intensities in different regions. After development, a photoresist thickness remains that varies according to the different exposure levels. The wafer is then placed in an IBE process, which removes the photoresist layer. The thinner areas of the photoresist last less long as a protective layer compared to thicker photoresist layers. This means that the layer of the wafer beneath the thinner photoresist comes into contact with the ion beam sooner than the layer beneath the thicker photoresist. If the wafer is processed in the IBE process for a while until all of the photoresist has been removed, the profile of the photoresist thickness is transferred to the thickness of the layer of the wafer beneath the photoresist.
[0022] The described methods enable a particularly precise delimitation of the respective areas of the coating wafer whose thickness is to be reduced during the second removal process, as well as a particularly precise reduction of the thickness in the respective delimited areas.
[0023] In a further possible embodiment of the invention, it is provided that the coating wafer is attached to the carrier wafer by means of a metallic bonding technique, a van der Waals bonding technique, a polymer layer, or an anodic bonding technique. The respective bonding techniques described enable particularly secure holding of the coating wafer to the carrier wafer. The invention further relates to a semiconductor wafer produced using a method as already described in connection with the method according to the invention for producing a semiconductor wafer.
[0024] Further features of the invention can be derived from the following description of the figures and from the drawings. The features and combinations of features mentioned above in the description, as well as the features and combinations of features shown below in the description of the figures and / or in the figures alone, can be used not only in the respective combinations specified, but also in other combinations or on their own, without departing from the scope of the invention.
[0025] The drawings show (not to scale) in:
[0026] Fig. 1 is a process diagram for a method for producing a semiconductor wafer; and
[0027] Fig. 2a-2b a schematic side view of a semiconductor wafer in different stages of a manufacturing process.
[0028] Fig. 1 shows a process diagram for a method for producing a semiconductor wafer. This method comprises several process steps a) to e) to be carried out successively. In a first process step a), a coating wafer 1, which in this case is a lithium niobate wafer (LiNbOa), is placed on a carrier wafer 2 and attached to the carrier wafer 2. The carrier wafer 2 in this case is a silicon carrier wafer 4 (Si) coated with a silicon dioxide layer 3 (SiCh). In this case, the lithium niobate wafer is applied to the silicon dioxide layer 3 of the silicon carrier wafer 4. The lithium niobate wafer is attached to the carrier wafer 2 by means of a metallic bonding technique, a van der Waals bonding technique, a polymer layer, or an anodic bonding technique.
[0029] In a second method step b) of the method, an initial thickness of the lithium niobate wafer is reduced to a first processing thickness by means of a mechanical first removal process. The thickness of the lithium niobate wafer can be removed by means of a conventional first removal process, which includes grinding and / or polishing.
[0030] In a third method step c) of the method, the thickness of the lithium niobate wafer resulting from the first removal process is determined over its entire base area adjacent to the carrier wafer 2 in the form of a thickness map. The thickness map is determined using ellipsometry or reflection spectrometry. Following the determination of the thickness map, in a fourth method step d) of the method, the thickness of the lithium niobate wafer is further reduced in a second removal process using an ion beam and / or a laser beam. The areas to be removed and the portions of the thickness of the lithium niobate wafer to be removed are selected depending on the thickness map created. During the second removal process, the thickness of the lithium niobate wafer is reduced using ion beam etching with a focused ion beam and / or grayscale lithography in combination with ion beam etching or laser ablation.
[0031] After the second removal process, the thickness of the coating wafer 1 above the base area can be checked by creating another thickness map. This thickness map can also be determined using ellipsometry or reflection spectrometry. If necessary, the third method step c) is carried out again, in which the thickness of the lithium niobate wafer is determined in the form of the another thickness map. If it is determined from the determined another thickness map that the thickness of the lithium niobate wafer lies within specified tolerance limits over the entire base area, then no further second removal process is carried out. If, however, it is determined that the thickness of the lithium niobate wafer lies outside the specified tolerance limits at least in one area above the base area, then the lithium niobate wafer is subjected to another second removal process.Following this additional second removal process, the thickness of the lithium niobate wafer can be checked again by creating a thickness map. In particular, the thickness check and the respective second removal processes can be repeated until it is determined that the thickness of the lithium niobate wafer lies within the specified tolerance limits across its entire base area. After the final second removal process, a fifth process step e) can be performed, in which an outer surface opposite the base area of the lithium niobate wafer is polished. In this process, the outer surface of the lithium niobate wafer is leveled using chemical-mechanical polishing.Within the scope of the method, it is provided in particular that an average thickness of the lithium niobate wafer over its entire base area is set to a maximum of 3000 nanometers, preferably a maximum of 1200 nanometers, in particular a maximum of 600 nanometers, by means of the at least one second removal process.
[0032] Fig. 2a shows the semiconductor wafer in an unprocessed state of the coating wafer 1. The coating wafer 1 is merely attached to the carrier wafer 2, without any reduction in thickness of the coating wafer 1 having taken place. Fig. 2b shows the finished semiconductor wafer. This shows a waveguide 5 arranged on the coating wafer 1, which is produced on a surface of the semiconductor wafer by subsequent etching or mechanical processing or mechanical removal of the surrounding surface. The waveguide 5 is an inhomogeneous medium which, due to its physical properties, bundles a wave so that it is guided therein as a traveling wave. This waveguide 5 has a ceiling surface 6 and side surfaces 7 that slope laterally away from the ceiling surface 6.The ceiling surface 6 and the side surfaces 7 are designed to be as smooth as possible, whereby losses in the light transmission in the waveguide 5 can be reduced, which has a positive effect on waveguiding efficiency.
[0033] Through the respective measurements and the spatially selective etching of the lithium niobate wafer, the thin film of the semiconductor wafer is reduced in thickness with nanometer precision without damaging the thin film, in this case the lithium niobate.
[0034] The process involves producing a semiconductor wafer with a 400-nanometer-thick layer of lithium niobate on a five-micrometer-thick layer of silicon dioxide on a 500-micrometer-thick silicon carrier wafer 4. In this case, the lithium niobate wafer is attached to the carrier wafer 2 by hot-melt bonding, whereby the lithium niobate wafer is held to the carrier wafer 2 via van der Waals forces. The bond between the lithium niobate wafer and the carrier wafer 2 can be annealed at elevated temperatures to increase the strength of the bond. The topmost layer of the semiconductor wafer, and thus the lithium niobate wafer, is then reduced in thickness by mechanical grinding. Any roughness resulting from this mechanical grinding can be smoothed by final polishing using chemical-mechanical polishing.This process allows the lithium niobate layer remaining on the lithium niobate wafer to be reduced to a thickness of 3000 nanometers, preferably a maximum of 1200 nanometers, and in particular to a maximum of 600 nanometers across the entire surface area. A thickness variation of five to ten micrometers across the entire surface area of the lithium niobate wafer, and thus, for example, with a 600 nanometer thickness of the lithium niobate wafer, between 5.6 and 10.6 micrometers can occur. The topography of the resulting thickness of the lithium niobate wafer is recorded using reflective spectrometry with spatial resolution in the millimeter range, with the resolution of the layer thickness measurement being in the nanometer range.Based on this thickness map, the thickness of the lithium niobate layer on the carrier wafer 2 is planarized and homogenized by placing the adjacent wafers in a focused ion beam etching system, and reducing the thickness of the lithium niobate wafer using a focused ion beam. After the second removal process, the thickness of the lithium niobate wafer can be determined again, and a second iteration of focused ion beam etching can be performed depending on the thickness measurement results. This iteration of measuring the thickness of the lithium niobate wafer and ion beam etching is repeated until the specified specifications for the semiconductor wafer and the thin film of lithium niobate on the carrier wafer 2 are achieved.As an alternative to the mechanical initial removal process, the initial thickness of the lithium niobate wafer could be reduced using a so-called crystal ion slicing process.
[0035] The described process has the advantage that the crystalline thin film of lithium niobate is of particularly high quality because it is not penetrated by ions. Furthermore, the thickness of the thin film of lithium niobate can be controlled down to the nanometer range within the process. Furthermore, the thickness of the lithium niobate layer can be made particularly homogeneous. The conventional method of crystal ion slicing for reducing the thickness of a coating wafer 1 to a predetermined target thickness without further post-processing is technically inferior to the described process, relying on the interplay of implanted ions, the material itself, voltage buildup, and temperature.
[0036] Overall, the invention shows how thin films can be produced on insulators by selective etching.
[0037] 1 coating wafer
[0038] 2 Carrier wafer 3 Silicon dioxide layer
[0039] 4 silicon carrier wafers
[0040] 5 waveguides
[0041] 6 Ceiling surface
[0042] 7 Side surface a) to d) respective process steps
Claims
PATENT CLAIMS 1. Method for producing a semiconductor wafer, in which a) a coating wafer (1) is placed on a carrier wafer (2) and fastened to the carrier wafer (2), b) an initial thickness of the coating wafer (1) is reduced to a first processing thickness by means of a first mechanical removal process, c) the thickness of the coating wafer (1) resulting after the first removal process is determined in the form of a thickness map over its entire base area lying against the carrier wafer (2), d) the thickness of the coating wafer (1) is further reduced in a second removal process by means of an ion beam and / or a laser beam, wherein regions to be removed and portions of the thickness of the coating wafer (1) to be removed are selected depending on the thickness map created.
2. Method according to claim 1, characterized in that after the second removal process, the thickness of the coating wafer (1) over the base area is determined in the form of a further thickness map and, depending on the further thickness map, the coating wafer (1) is subjected to a further second removal process or not.
3. Method according to claim 1 or 2, characterized in that e) after carrying out the last second removal process, an outer surface of the coating wafer (1) opposite the base surface is polished.
4. Method according to one of the preceding claims, characterized in that after carrying out the first removal process and before carrying out the second removal process, the outer surface of the coating wafer (1) opposite the base surface is polished.
5. Method according to claim 3 or 4, characterized in that the outer surface is polished by means of chemical-mechanical polishing.
6. Method according to one of the preceding claims, characterized in that the thickness map is determined by means of ellipsometry or reflection spectrometry.
7. Method according to one of the preceding claims, characterized in that an average thickness of the coating wafer (1) over its base area is set to a maximum of 3000 nm, preferably a maximum of 1200 nm, in particular a maximum of 600 nm by means of the second removal process.
8. Method according to one of the preceding claims, characterized in that a lithium niobate wafer is applied as coating wafer (1) to a silicon dioxide layer (3) of a silicon carrier wafer (4) as carrier wafer (2).
9. Method according to one of the preceding claims, characterized in that in the second removal process the thickness of the coating wafer (1) is reduced by means of ion beam etching, grayscale lithography in combination with ion beam etching or laser ablation.
10. Method according to one of the preceding claims, characterized in that the coating wafer (1) is attached to the carrier wafer (2) by means of a metallic bonding technique or by means of a van der Waals bonding technique or by means of a polymer layer or by means of an anodic bonding technique.
11. A semiconductor wafer produced by a method according to any one of the preceding claims.
Citation Information
Patent Citations
Semiconductor substrate, thin film transistor, semiconductor circuit, liquid crystal display apparatus, electroluminescent apparatus, semiconductor substrate manufacturing method, and semiconductor substrate manufacturing apparatus
US20140367691A1
Method for manufacturing an image sensor
US20230039295A1
Interdigital piezoelectric vibration sensor based on d15 and d22 and preparation method thereof
CN115697016A
Method for making uniform the thickness of a Si single crystal thin film
US5213657A
SOI substrate fabrication
US5344524A