Method for producing thermoplastic resin composition

By adding a high-temperature carbonate to PC/ABS alloys to neutralize magnesium and calcium ions, the method enhances the moist heat properties and appearance of thermoplastic resin compositions, addressing the issues of hydrolysis-induced deterioration.

WO2024224626A1PCT designated stage expired Publication Date: 2024-10-31MITSUBISHI ELECTRIC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/016932
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Thermoplastic resin compositions, particularly PC/ABS alloys, suffer from poor moist heat properties and appearance defects due to hydrolysis accelerated by moisture and heat, leading to deterioration in their performance and recyclability.

Method used

Incorporating a carbonate with a decomposition temperature of 200°C or higher, free from Group 1 and Group 2 elements, in specific amounts into the PC/ABS alloy to capture magnesium and calcium ions, thereby preventing alkaline environments and enhancing moist heat properties.

Benefits of technology

The method produces thermoplastic resin compositions with improved moist heat resistance and reduced appearance defects, maintaining performance and enabling better recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023016932_31102024_PF_FP_ABST
    Figure JP2023016932_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for producing a thermoplastic resin composition, the method comprising a step for mixing a polycarbonate / ABS alloy containing a first polycarbonate resin and a first ABS resin with a carbonate, wherein the first ABS resin is obtained by emulsion polymerization, the carbonate does not contain a group 1 element of the periodic table and a group 2 element of the periodic table, the carbonate has a decomposition temperature of 200°C or higher, and the content of the carbonate is more than 0.1 parts by mass and less than 6.0 parts by mass with respect to 100 parts by mass of the polycarbonate / ABS alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing thermoplastic resin composition

[0001] The present disclosure relates to a method for producing a thermoplastic resin composition.

[0002] Polycarbonate (PC) resin, a thermoplastic resin, is used for housings and parts of various products, such as machines, automobiles, home appliances, and office automation equipment. Furthermore, by blending other thermoplastic resins and additives with PC resin to impart functionality and flame retardancy, highly functionalized PC resin compositions are used in many applications. In particular, PC / styrene resin compositions, which are alloys of PC resin and styrene-based resins, such as ABS resin, which is a copolymer of acrylonitrile, butadiene, and styrene, are widely used in the above applications due to their low cost and improved moldability, impact resistance, and other properties of PC resin.

[0003] In many cases, the ABS resin used in a PC / ABS resin composition, which is a representative example of a PC / styrene-based resin composition, is an ABS resin produced by emulsion polymerization from the viewpoint of cost. However, Non-Patent Document 1 discloses that an ABS resin produced by bulk polymerization has better moist heat properties than an ABS resin produced by emulsion polymerization. Thus, in order to reduce costs, it is preferable to use an ABS resin produced by emulsion polymerization as the ABS resin used in a PC / ABS resin composition, but this has the disadvantage of being inferior in moist heat properties.

[0004] In recent years, environmental concerns have led to calls for efforts to recycle resins. However, there is a problem in that used thermoplastic resin compositions generally deteriorate the longer they are used, resulting in a decrease in their properties.

[0005] Patent Document 1 (JP 2002-60610 A) discloses that phosphite compounds, phosphonite compounds, and the like are blended into PC resins as antioxidants to improve thermal stability, that these compounds are more susceptible to hydrolysis by heat and moisture than PC resins and generate acid components upon hydrolysis, and that the acid components accelerate the hydrolysis of the PC resin, causing deterioration of the moist heat properties of the PC resin. Patent Document 1 also discloses a method of deactivating adverse components such as the acid components by adsorbing or coordinating them to the surface of a compound selected from metal carbonates, metal silicates, and specific metal oxides.

[0006] Japanese Patent Application Laid-Open No. 2002-60610

[0007] Molding Volume 30 Issue 4 p.155-157 2018

[0008] However, the hydrolysis mechanism of the PC resin described in Patent Document 1 has not been fully elucidated, and there is still room for improvement in the deterioration of the hygrothermal properties of the PC resin. Furthermore, when using used resin, the deterioration of the hygrothermal properties may cause a deterioration in the appearance of the molded product.

[0009] The present disclosure has been made to solve the above-mentioned problems, and aims to provide a method for producing a thermoplastic resin composition that has excellent moist heat properties and reduced appearance defects.

[0010] The present inventors have conducted extensive research to solve the above problems and have found that removing magnesium and calcium contained in a thermoplastic resin composition by reacting them with carbonate ions makes it possible to obtain a thermoplastic resin composition that has excellent moist heat properties and reduced appearance defects.The present disclosure relates to a method for producing a thermoplastic resin composition.

[0011] 1. A method for producing a thermoplastic resin composition, comprising: mixing a polycarbonate / ABS alloy containing a first polycarbonate resin and a first ABS resin; and a carbonate; wherein the first ABS resin is obtained by emulsion polymerization; the carbonate does not contain an element of Group 1 or Group 2 of the periodic table; the carbonate has a decomposition temperature of 200°C or higher; and the content of the carbonate is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the polycarbonate / ABS alloy.

[0012] 1. A method for producing a thermoplastic resin composition, comprising: mixing a polycarbonate / ABS alloy containing a first polycarbonate resin and a first ABS resin with at least one resin selected from the group consisting of a second polycarbonate resin and a second ABS resin; and a carbonate; wherein the first ABS resin and the second ABS resin are obtained by emulsion polymerization; the carbonate does not contain an element of Group 1 or Group 2 of the Periodic Table; the carbonate has a decomposition temperature of 200°C or higher; and the content of the carbonate is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the polycarbonate / ABS alloy and the at least one resin selected from the group consisting of the second polycarbonate resin and the second ABS resin.

[0013] A method for producing a thermoplastic resin composition, comprising: a step of mixing a second polycarbonate resin, a second ABS resin, and the carbonate; wherein the second ABS resin is obtained by emulsion polymerization; the carbonate does not contain an element of Group 1 or Group 2 of the periodic table; the carbonate has a decomposition temperature of 200°C or higher; and the content of the carbonate is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the total of the second polycarbonate resin and the second ABS resin.

[0014] According to the present disclosure, it is possible to provide a method for producing a thermoplastic resin composition that has excellent wet heat properties and reduced appearance defects.

[0015] FIG. 1 is a diagram illustrating the mechanism of trapping magnesium ions and calcium ions in a polycarbonate / ABS alloy.

[0016] Hereinafter, embodiments of the present disclosure will be described.

[0017] Embodiment 1. <Method for Producing a Thermoplastic Resin Composition> The method for producing a thermoplastic resin composition according to this embodiment includes mixing a polycarbonate / ABS alloy (PC / ABS alloy) containing a first PC resin and a first ABS resin with a carbonate. The first ABS resin is obtained by emulsion polymerization. The carbonate does not contain Group 1 or Group 2 elements of the periodic table and has a decomposition temperature of 200°C or higher. The carbonate content is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the PC / ABS alloy. In this embodiment, the first PC resin will be referred to simply as "PC resin," and the first ABS resin will be referred to simply as "ABS resin."

[0018] In the mixing step, the PC / ABS alloy and the carbonate are mixed together. At this time, other components such as additives may be added.

[0019] In this step, the PC / ABS alloy and the carbonate are used in the form of, for example, flakes, pellets, powder, or granules.

[0020] The mixing method is not particularly limited. For example, physical mixing such as melt kneading, solvent cast blending, latex blending, polymer complexing, etc. is possible. Mixing is preferably melt kneading.

[0021] In the mixing step, a mixing device such as a tumbler, a Henschel mixer (registered trademark), a rotary mixer, a super mixer, a ribbon tumbler, or a V blender can be used. The materials are mixed uniformly in advance using such a mixing device to prepare a mixture. It is preferable to further melt-knead the mixture and finally form it into pellets.

[0022] For melt-kneading and pelletization, a single-screw, multi-screw, tandem or other extrusion kneader can be used. Alternatively, a Banbury mixer, roller, co-kneader, blast mill, Prabender blotograph or the like may be used. The extrusion kneader or the like may be operated batchwise or continuously.

[0023] Alternatively, the mixture may be prepared by mixing the PC / ABS alloy and the carbonate without melt-kneading, and the mixture may be fed to a molding machine and melt-kneaded in the heating barrel of the molding machine. That is, mold blending may be performed.

[0024] The thermoplastic resin composition produced by the production method of this embodiment can be processed into a molded product by a conventionally known molding method, such as injection molding.

[0025] <Polycarbonate / ABS Alloy> The PC / ABS alloy of this embodiment is a mixture (polymer alloy) of a PC resin and an ABS resin. The PC / ABS alloy may be produced by using a compatibilizer or by block polymerization or graft polymerization, or a commercially available product may be used.

[0026] The PC / ABS alloy may be a PC / ABS alloy recovered from used products or the like (hereinafter referred to as a "used PC / ABS alloy"), or may be a PC / ABS alloy that has not yet been used (hereinafter referred to as a "virgin PC / ABS alloy").

[0027] The PC / ABS alloy may be a mixture of used PC / ABS alloy and virgin PC / ABS alloy. The mixing ratio of used PC / ABS alloy and virgin PC / ABS alloy is not particularly limited. However, from the viewpoint of resource efficiency, it is preferable that the content of used PC / ABS alloy is high.

[0028] (Polycarbonate Resin) The PC resin is not particularly limited, and various types can be used. For example, an aromatic polycarbonate produced by a solution method (interfacial polycondensation method) or a melting method (ester exchange method) of a dihydric phenol and a carbonate precursor can be used. That is, a polycarbonate produced by reacting a dihydric phenol with phosgene by an interfacial polycondensation method, a dihydric phenol with diphenyl carbonate, or the like by an ester exchange method, or the like, may be used. In addition, a commercially available PC resin may be used.

[0029] Examples of dihydric phenols include various types, such as 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 4,4'-dihydroxydiphenyl, bis(4-hydroxyphenyl)cycloalkane, bis(4-hydroxyphenyl)oxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)ketone, and halogen-substituted derivatives thereof. Other examples include hydroquinone, resorcinol, and catechol. These may be used alone or in combination of two or more. Among these, bis(hydroxyphenyl)alkanes are preferred, and bisphenol A is more preferred.

[0030] The carbonate precursor may be a carbonyl halide, a carbonyl ester, a haloformate, or the like, and specifically may be phosgene, a dihaloformate of a dihydric phenol, diphenyl carbonate, dimethyl carbonate, diethyl carbonate, or the like.

[0031] The PC resin may be PC resin recovered from used products, etc. (hereinafter referred to as "used PC resin"), or may be PC resin that has not yet been used (hereinafter referred to as "unused PC resin").

[0032] The PC resin may be a mixture of used PC resin and virgin PC resin. The mixing ratio of the used PC resin and the virgin PC resin is not particularly limited. However, from the viewpoint of resource efficiency, it is preferable that the content of the used PC resin is higher than the content of the virgin PC resin.

[0033] The content of PC resin in the PC / ABS alloy is 45% by mass or more and 90% by mass or less. Since PC resin has better heat resistance and flame retardancy than ABS resin, it is preferable that the content of PC resin is greater than that of ABS resin. However, if the content of PC resin in the PC / ABS alloy exceeds 90% by mass, the fluidity during molding may decrease, i.e., moldability may decrease. The content of PC resin in the PC / ABS alloy may be 50% by mass or more, 55% by mass or more, or 60% by mass or more. The content of PC resin in the PC / ABS alloy may be 85% by mass or less, 80% by mass or less, or 75% by mass or less.

[0034] <<ABS Resin>> ABS resin is a copolymer of acrylonitrile, butadiene, and styrene. Molded products of ABS resin have excellent surface gloss and impact strength. Therefore, ABS resin is widely used in home appliances, office automation equipment, etc. In the present embodiment, the composition ratio of acrylonitrile, butadiene, and styrene in the ABS resin is not particularly limited.

[0035] The ABS resin may be an ABS resin recovered from used products (hereinafter referred to as "used ABS resin"), or an ABS resin that has not yet been used (hereinafter referred to as "virgin ABS resin").

[0036] The ABS resin may be a mixture of used ABS resin and virgin ABS resin. The mixing ratio of the used ABS resin and the virgin ABS resin is not particularly limited. However, from the viewpoint of resource efficiency, it is preferable that the content of the used ABS resin is higher than the content of the virgin ABS resin.

[0037] The content of ABS resin contained in the PC / ABS alloy is 5% by mass or more and 50% by mass or less. If the content of ABS resin contained in the PC / ABS alloy exceeds 50% by mass, there is a risk of a decrease in heat resistance and flame retardancy. The content of ABS resin contained in the PC / ABS alloy may be 10% by mass or more, 15% by mass or more, or 20% by mass or more. The content of ABS resin contained in the PC / ABS alloy may be 45% by mass or less, 40% by mass or less, or 35% by mass or less.

[0038] The ABS resin in this example was obtained by emulsion polymerization. The ABS resin may be produced by a known emulsion polymerization method, or a commercially available emulsion polymerized product may be used.

[0039] The method for producing ABS resin by emulsion polymerization is generally as follows: In the presence of an emulsifier, butadiene is emulsion polymerized with a water-soluble polymerization initiator to obtain a polymer latex. Acrylonitrile and styrene are polymerized in the presence of the resulting polymer latex and emulsifier to obtain an ABS-type polymer latex. A coagulant is added to the resulting ABS-type polymer latex to separate the polymer, which is then washed and dried to produce ABS.

[0040] The emulsifier, water-soluble polymerization initiator, and coagulant used may be any of those known in the art. Examples of emulsifiers include higher fatty acid soaps and rosin acid soaps. Examples of water-soluble polymerization initiators include potassium peroxodisulfate and α-cumyl hydroperoxide. Examples of coagulants include inorganic acids and metal salts.

[0041] Here, the emulsifier is usually not completely removed by washing, and some of it remains in the resulting ABS resin. While thorough washing of the resulting ABS resin beforehand is also conceivable, even thorough washing with water or an organic solvent such as methanol does not easily remove the emulsifier incorporated into the ABS resin. Among such emulsifier-derived residues, Group 1 and Group 2 elements of the periodic table react with moisture in the air to generate hydroxide ions, creating an alkaline environment that is thought to accelerate hydrolysis of the PC resin and deteriorate its moist-heat properties.

[0042] The inventors analyzed used and unused PC / ABS alloys using inductively coupled plasma atomic emission spectroscopy (ICP-AES) and confirmed that each PC / ABS alloy contained 0.01% by mass of sodium (Na), magnesium (Mg), and calcium (Ca) as Group 1 and Group 2 elements of the periodic table, respectively. After extensive research, the inventors discovered that while it is difficult to capture Na ions, Mg ions and Ca ions react with sulfate ions and carbonate ions to form precipitates in water, making them less reactive with water. Therefore, by incorporating sulfate ions and carbonate ions into the resin, it is possible to prevent an alkaline environment (see Figure 1). The used and unused PC / ABS alloys used were commercially available.

[0043] Furthermore, the solubilities in water at room temperature are 2.1 mol / L for magnesium sulfate and 0.018 mol / L for calcium sulfate, while those for magnesium carbonate are 0.0012 mol / L and 0.00015 mol / L for calcium carbonate. Thus, for Mg ions and Ca ions, the solubility of carbonates in water is lower than that of sulfates. Therefore, in this embodiment, mixing a carbonate, as described below, is considered to be significantly more effective in preventing an alkaline environment. However, because carbonates decompose by releasing carbon dioxide when heated, it is preferable to mix a carbonate with a high decomposition temperature.

[0044] (Additives) The PC / ABS alloy may contain additives such as oil-absorbing inorganic compounds, flow control agents, plasticizers, mold release agents, antioxidants, flame retardants, flame retardant assistants, metal deactivators, dyes, pigments, antistatic agents, etc. These additives may be contained in the PC / ABS alloy either alone or in combination of two or more.

[0045] The oil-absorbing inorganic compound is not particularly limited, and examples thereof include aluminum oxides such as alumina and boehmite, calcium silicate, kaolinite, and calcium carbonate.

[0046] The flow adjuster is not particularly limited, and examples thereof include hydrocarbons such as liquid paraffin, paraffin wax, and synthetic polyethylene wax; fatty acids such as stearic acid, palmitic acid, and oleic acid; higher alcohols such as stearyl alcohol, cetyl alcohol, and oleyl alcohol; fatty acid amides such as stearic acid amide, oleic acid amide, erucic acid amide, methylene bisstearic acid amide, and ethylene bisstearic acid amide; metal soaps such as magnesium stearate, calcium stearate, and zinc stearate; and esters such as stearic acid monoglyceride, stearyl stearate, and hydrogenated oil.

[0047] The plasticizer is not particularly limited, and examples thereof include polyethylene glycol, polyamide oligomer, ethylene bisstearamide, phthalate ester, adipate ester, polystyrene oligomer, polyethylene wax, silicone oil, and mineral oil.

[0048] The release agent is not particularly limited, and examples thereof include polyethylene wax, silicone oil, long-chain carboxylic acid, and metal salt of long-chain carboxylic acid.

[0049] The antioxidant is not particularly limited, and examples thereof include phosphoric acid antioxidants such as tris(2,4-di-t-butylphenyl)phosphite and tetrakis(2,4-di-t-butylphenyl)[1,1-biphenyl]-4,4′-diylbisphosphonite, sulfur-based antioxidants such as dilauryl-3,3′-thiodipropionate and dioctadecyl-3,3′-thiodipropionate, and hindered phenol-based antioxidants such as tetrakis[methylene-3-(3′,5′-di-t-butyl-4′-hydroxyphenyl)propionate]methane and stearyl β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate.

[0050] The flame retardant is not particularly limited. In the present embodiment, conventionally known flame retardants can be used. Examples include phosphorus-based flame retardants such as bisphenol A bis(diphenyl phosphate), tricresyl phosphate, triphenyl phosphate, and tris-3-chloropropyl phosphate; bromine-based flame retardants such as 2,2-bis[4-(2,3-dibromopropoxyl)-3,5-dibromophenyl]propane, bis(3,5-dibromo-4-dibromopropyloxyphenyl)sulfone, ethylene bispentabromobenzene, and hexabromocyclododecane; silicone-based flame retardants; and hydroxide-based flame retardants such as magnesium hydroxide and aluminum hydroxide.

[0051] To enhance the flame retardancy of the flame retardant, a flame retardant aid may be used in combination. The flame retardant aid is not particularly limited. Examples of the flame retardant aid include an additive obtained by acrylic modification of polytetrafluoroethylene and antimony compounds such as antimony trioxide.

[0052] The metal deactivator is not particularly limited, and examples thereof include 2',3-bis[[3-[3,5-di-t-butyl-4-hydroxyphenyl]propionyl]]propionohydrazide, decamethylenedicarboxylic acid disalicyloylhydrazide, and the like.

[0053] The content of each additive contained in the PC / ABS alloy is, for example, 0% by mass or more and 20% by mass or less. The content of each additive contained in the PC / ABS alloy may be 2% by mass or more, 5% by mass or more, 7% by mass or more, 17% by mass or less, 15% by mass or less, or 13% by mass or less.

[0054] (Used Resin) At least one of the PC resin, ABS resin, and PC / ABS alloy is preferably used, i.e., at least one is preferably used PC resin, used ABS resin, or used PC / ABS alloy. Also, at least one of the PC resin, ABS resin, and PC / ABS alloy preferably includes used resin, i.e., at least one is preferably a mixture of used PC resin and virgin PC resin, a mixture of used ABS resin and virgin ABS resin, or a mixture of used PC / ABS alloy and virgin PC / ABS alloy. This is from the viewpoint of resource efficiency.

[0055] However, when a used PC / ABS alloy, a used PC resin, or a used ABS resin is used, various properties of the thermoplastic resin composition, such as mechanical properties and moist heat properties, may be reduced. Therefore, when at least one of the PC / ABS alloy, the PC resin, and the ABS resin is used, it is preferable to add at least one of a virgin PC / ABS alloy, a virgin PC resin, and a virgin ABS resin, from the viewpoint of improving various properties of the thermoplastic resin composition.

[0056] <<Carbonate>> The carbonate contained in the thermoplastic resin composition of the present embodiment does not contain an element of Group 1 or Group 2 of the periodic table. If the carbonate contains an element of Group 1 or Group 2 of the periodic table, it will react with moisture in the air to generate hydroxide ions, as described above, creating an alkaline environment, which may accelerate hydrolysis of the PC resin and deteriorate the moist heat properties.

[0057] The carbonate has a decomposition temperature of 200°C or higher. Here, the term "decomposition temperature" in the present embodiment refers to a temperature at which a carbonate undergoes a decomposition reaction into two or more compounds when heated at a certain temperature or temperature range. The decomposition temperature is measured, for example, by thermal analysis such as differential scanning calorimetry (DSC), and is the temperature at which endothermic or exothermic heat begins to be generated when heated from room temperature at a certain heating rate in a nitrogen gas atmosphere. If the decomposition temperature is lower than 200°C, the viscosity of the thermoplastic resin composition increases, which may result in insufficient mixing. From the viewpoint of fluidity (moldability) during molding, the decomposition temperature is preferably 220°C or higher, more preferably 240°C or higher. Furthermore, if the decomposition temperature is too high, the physical properties of the thermoplastic resin composition after molding may be reduced. Therefore, the decomposition temperature is, for example, 300°C or lower, preferably 280°C or lower, and more preferably 260°C or lower.

[0058] Examples of carbonates in the present embodiment include cobalt carbonate (decomposition temperature: 280° C.), manganese carbonate (decomposition temperature: 200° C.), cadmium carbonate (decomposition temperature: 357° C.), iron carbonate (decomposition temperature: 200° C.), silver carbonate (decomposition temperature: 210° C.), etc. Among these, cobalt carbonate is preferred because it has an optimum decomposition temperature.

[0059] The content of carbonate in the thermoplastic resin composition of this embodiment is more than 0.1 parts by mass and less than 6.0 parts by mass relative to 100 parts by mass of the PC / ABS alloy. If the content of carbonate is 0.1 parts by mass or less, the moist heat properties may not be sufficiently improved. If the content of carbonate is 6.0 parts by mass or more, the carbonate may bleed out, resulting in poor appearance. The content of carbonate is preferably 0.5 parts by mass or more and 5.0 parts by mass or less.

[0060] Others The thermoplastic resin composition of the present embodiment may contain additives such as oil-absorbing inorganic compounds, flow control agents, plasticizers, mold release agents, antioxidants, flame retardants, flame retardant assistants, metal deactivators, dyes, pigments, and antistatic agents, as long as the additives do not impair the object of the present embodiment. These additives may be contained in the thermoplastic resin composition alone or in combination of two or more. Details of each additive are as described above.

[0061] The content of each additive in the thermoplastic resin composition of this embodiment is, for example, 0 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the PC / ABS alloy. The content of each additive in the thermoplastic resin composition may be 2 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, 17 parts by mass or less, 15 parts by mass or less, or 13 parts by mass or less.

[0062] Embodiment 2. A method for producing a thermoplastic resin composition according to this embodiment includes mixing a PC / ABS alloy containing a first PC resin and a first ABS resin, at least one resin selected from the group consisting of a second PC resin and a second ABS resin, and a carbonate. The first ABS resin and the second ABS resin are obtained by emulsion polymerization. The carbonate does not contain Group 1 or Group 2 elements of the periodic table and has a decomposition temperature of 200°C or higher. The carbonate content is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the PC / ABS alloy and at least one resin selected from the group consisting of the second PC resin and the second ABS resin.

[0063] This embodiment will be described below, but explanations that overlap with those of the first embodiment will be omitted. For convenience of description, the PC resin contained in the PC / ABS alloy is referred to as the first PC resin and distinguished from the second PC resin, but the first PC resin and the second PC resin may be the same or different. Similarly, for convenience of description, the ABS resin contained in the PC / ABS alloy is referred to as the first ABS resin and distinguished from the second ABS resin, but the first ABS resin and the second ABS resin may be the same or different. With regard to the second PC resin and the second ABS resin, the descriptions of the first PC resin and the first ABS resin in the first embodiment will be referenced except for the following explanation.

[0064] In this embodiment, the resins used are a PC / ABS alloy containing a first PC resin and a first ABS resin, and at least one resin selected from the group consisting of a second PC resin and a second ABS resin.

[0065] The total content of the first PC resin and the second PC resin (hereinafter, the total of the first PC resin and the second PC resin is also referred to as "total PC resin") relative to the total of the PC / ABS alloy and at least one resin selected from the group consisting of the second PC resin and the second ABS resin is 45% by mass or more and 90% by mass or less. Because PC resin has better heat resistance and flame retardancy than ABS resin, it is preferable that the PC resin content be higher than ABS resin. However, if the total PC resin content relative to the total of the PC / ABS alloy and at least one resin selected from the group consisting of the second PC resin and the second ABS resin exceeds 90% by mass, fluidity during molding, i.e., moldability, may be reduced. The total PC resin content relative to the total of the PC / ABS alloy and at least one resin selected from the group consisting of the second PC resin and the second ABS resin, may be 50% by mass or more, 55% by mass or more, or 60% by mass or more. The content of all PC resins relative to the total of the PC / ABS alloy and the at least one resin selected from the group consisting of the second PC resin and the second ABS resin may be 85% by mass or less, 80% by mass or less, or 75% by mass or less.

[0066] The total content of the first ABS resin and the second ABS resin (hereinafter, the total of the first ABS resin and the second ABS resin is also referred to as "total ABS resin") relative to the total of the PC / ABS alloy and at least one type selected from the group consisting of the second PC resin and the second ABS resin is 5% by mass or more and 50% by mass or less. If the total content of the ABS resin relative to the total of the PC / ABS alloy and at least one type selected from the group consisting of the second PC resin and the second ABS resin exceeds 50% by mass, heat resistance and flame retardancy may be reduced. The total content of the ABS resin relative to the total of the PC / ABS alloy and at least one type selected from the group consisting of the second PC resin and the second ABS resin may be 10% by mass or more, 15% by mass or more, or 20% by mass or more. The content of all ABS resins relative to the total of the PC / ABS alloy and the at least one resin selected from the group consisting of the second PC resin and the second ABS resin may be 45% by mass or less, 40% by mass or less, or 35% by mass or less.

[0067] In this embodiment, the carbonate content is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the total of the PC / ABS alloy and at least one resin selected from the group consisting of the second PC resin and the second ABS resin. If the carbonate content is 0.1 parts by mass or less, the moist heat properties may not be sufficiently improved. If the carbonate content is 6.0 parts by mass or more, the carbonate may bleed out, resulting in poor appearance. The carbonate content is preferably 0.5 parts by mass or more and 5.0 parts by mass or less.

[0068] The content of each additive in the thermoplastic resin composition of this embodiment is, for example, 0 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total of the PC / ABS alloy and the at least one resin selected from the group consisting of the second PC resin and the second ABS resin. The content of each additive in the thermoplastic resin composition may be 2 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, 17 parts by mass or less, 15 parts by mass or less, or 13 parts by mass or less.

[0069] At least one of the first PC resin, the second PC resin, the first ABS resin, the second PC resin, and the PC / ABS alloy is preferably used, i.e., at least one is a used PC resin, a used ABS resin, or a used PC / ABS alloy. Also, at least one of the first PC resin, the second PC resin, the first ABS resin, the second PC resin, and the PC / ABS alloy preferably includes a used resin, i.e., at least one is a mixture of used PC resin and virgin PC resin, a mixture of used ABS resin and virgin ABS resin, or a mixture of used PC / ABS alloy and virgin PC / ABS alloy, from the viewpoint of resource efficiency.

[0070] Embodiment 3. A method for producing a thermoplastic resin composition according to this embodiment includes mixing a second PC resin, a second ABS resin, and a carbonate. The second ABS resin is obtained by emulsion polymerization. The carbonate does not contain any Group 1 or Group 2 elements of the periodic table and has a decomposition temperature of 200°C or higher. The carbonate content is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the second PC resin and the second ABS resin combined.

[0071] The present embodiment will be described below, but explanations that overlap with the first and second embodiments will be omitted.

[0072] In this embodiment, the resins used are a second PC resin and a second ABS resin, i.e., a PC / ABS alloy is not used.

[0073] The content of the second PC resin relative to the total of the second PC resin and the second ABS resin is 45% by mass or more and 90% by mass or less. Because PC resin has better heat resistance and flame retardancy than ABS resin, a high PC resin content is preferable. However, if the content of the second PC resin relative to the total of the second PC resin and the second ABS resin exceeds 90% by mass, fluidity during molding, i.e., moldability, may decrease. The content of the second PC resin relative to the total of the second PC resin and the second ABS resin may be 50% by mass or more, 55% by mass or more, or 60% by mass or more. The content of the second PC resin relative to the total of the second PC resin and the second ABS resin may be 85% by mass or less, 80% by mass or less, or 75% by mass or less.

[0074] The content of the second ABS resin relative to the total of the second PC resin and the second ABS resin is 5% by mass or more and 50% by mass or less. If the content of the second ABS resin relative to the total of the second PC resin and the second ABS resin exceeds 50% by mass, heat resistance and flame retardancy may be reduced. The content of the second ABS resin relative to the total of the second PC resin and the second ABS resin may be 10% by mass or more, 15% by mass or more, or 20% by mass or more. The content of the second ABS resin relative to the total of the second PC resin and the second ABS resin may be 45% by mass or less, 40% by mass or less, or 35% by mass or less.

[0075] In this embodiment, the carbonate content is more than 0.1 parts by mass and less than 6.0 parts by mass, relative to 100 parts by mass of the total of the second PC resin and the second ABS resin. If the carbonate content is 0.1 parts by mass or less, the moist heat properties may not be sufficiently improved. If the carbonate content is 6.0 parts by mass or more, the carbonate may bleed out, resulting in poor appearance. The carbonate content is preferably 0.5 parts by mass or more and 5.0 parts by mass or less.

[0076] The content of each additive in the thermoplastic resin composition of this embodiment is, for example, 0 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total of the second PC resin and the second ABS resin. The content of each additive in the thermoplastic resin composition may be 2 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, 17 parts by mass or less, 15 parts by mass or less, or 13 parts by mass or less.

[0077] At least one of the second PC resin and the second ABS resin is preferably used, i.e., at least one is a used PC resin or a used ABS resin. Also, at least one of the second PC resin and the second ABS resin preferably includes a used resin, i.e., at least one is a mixture of used PC resin and virgin PC resin, or a mixture of used ABS resin and virgin ABS resin, from the viewpoint of resource efficiency.

[0078] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples.

[0079] Test Example 1 In Test Example 1, the following test was conducted to compare used PC / ABS alloys with virgin PC / ABS alloys. The used PC / ABS alloys were sorted and recovered from used home appliances, and the virgin PC / ABS alloys were commercially available PC / ABS alloys. The ABS resin contained in each PC / ABS alloy was confirmed to be obtained by emulsion polymerization by examining the particle shape using an electron microscope.

[0080] (Measurement) The components and contents contained in the used PC / ABS alloy and the unused PC / ABS alloy were measured by thermogravimetric analysis (TGA), gas chromatography mass spectrometry (GC-MS) and ICP-AES.

[0081] As a sample, 10 mg of each PC / ABS alloy was weighed out and measured using a TGA device (STA7200, manufactured by Hitachi High-Tech Science Corporation) in the temperature range of 30°C to 1000°C at a temperature increase rate of 10°C / min.

[0082] As a sample, 0.5 mg of each PC / ABS alloy was weighed out, immersed in 20 mL of tetrahydrofuran, heated to 50 ° C, and stirred until the pellet shape disappeared. The stirred mixture was added to 80 mL of ethanol, and measured using a GC-MS device (JEOL Ltd., Jms-Q1000GCK9 Ultra Quad GC / MS) at a heating temperature of 340 ° C for 24 minutes.

[0083] As samples, 150 mg of each PC / ABS alloy was weighed out, various acids were added, the samples were sealed, and the samples were dissolved in a microwave pretreatment device. The insoluble matter was then filtered off. The filtrate was transferred to a measuring flask and the volume was adjusted (Test Solution A). The insoluble matter was transferred to a platinum dish together with the filter paper, incinerated using a burner, and then acid was added again to dissolve the matter by heating. After cooling, the sample was transferred to a measuring flask and the volume was adjusted (Test Solution B). Test Solutions A and B obtained above were each used as ICP measurement solutions and measured using an ICP-AES device (Hitachi High-Tech Science Corporation, SPS-3100).

[0084] Measurements revealed that the used PC / ABS alloy contained 59% by mass of PC resin, 26% by mass of ABS resin, 13% by mass of bisphenol A bis(diphenyl phosphate), a phosphate ester-based flame retardant, and 2% by mass of inorganic substances and other impurities. The inorganic substances included 0.01% by mass of Na, 0.01% by mass of Mg, 0.01% by mass of Ca, 0.3% by mass of silicon (Si), 0.3% by mass of titanium (Ti), 0.06% by mass of aluminum (Al), 0.04% by mass of iron (Fe), and 0.03% by mass of tin (Sb). Meanwhile, the unused PC / ABS alloy contained 70% by mass of PC resin, 16% by mass of ABS resin, 11% by mass of bisphenol A bis(diphenyl phosphate), a phosphate ester-based flame retardant, and 3% by mass of inorganic substances and other impurities. The inorganic substances contained 0.01 mass% of Na, 0.01 mass% of Mg, 0.01 mass% of Ca, 0.3 mass% of Si, and 0.1 mass% of Ti. Note that the unused PC / ABS alloy did not contain Al, Fe, or Sb.

[0085] (Bending Test) Each PC / ABS alloy was molded into an ISO dumbbell type A test piece using an injection molding machine under conditions of a molding temperature of 240°C and a mold temperature of 60°C. The bending strength of each test piece was measured by a bending test. The bending test was performed according to a method in accordance with JIS K 7171. Specifically, each test piece was exposed to a humid heat environment of 65°C and 85% relative humidity for 1,340 hours, and then measured at a test speed of 2 mm / min using a universal testing machine (AG-X20KN, manufactured by Shimadzu Corporation). Each test piece was subjected to the test until its strength became less than 75% of its pre-exposure strength.

[0086] As a result of the bending test, it took 2500 hours for the virgin PC / ABS alloy to reach the above-mentioned strength, while it took 1200 hours for the used PC / ABS alloy. Thus, it was confirmed that the moist heat properties of the used PC / ABS alloy were significantly deteriorated compared to the moist heat properties of the virgin PC / ABS alloy.

[0087] (Melt Flow Rate Test) The melt flow rate (MFR) of each PC / ABS alloy was measured by an MFR test. The MFR test was performed according to JIS K 7210. Specifically, the measurement was performed using a melt flow indexer (Melt Indexer TP-401, manufactured by Tester Sangyo Co., Ltd.) under conditions of a temperature of 260°C and a load of 2.16 kgf. The larger the MFR value, the greater the fluidity of the resin, but the lower the molecular weight of the PC, which is thought to be the cause of deterioration of the PC / ABS alloy.

[0088] The MFR test results showed that the virgin PC / ABS alloy had a melt flow rate of 20 g / 10 min, while the used PC / ABS alloy had a melt flow rate of over 70 g / 10 min. Thus, it was confirmed that the fluidity of the used PC / ABS alloy was significantly higher than that of the virgin PC / ABS alloy. This is thought to be due to the progress of hydrolysis of the PC resin caused by aging.

[0089] Furthermore, when the weight-average molecular weight of each PC / ABS alloy was measured by gel permeation chromatography (GPC), the unused PC / ABS alloy had a molecular weight of 47,000, while the used PC / ABS alloy had a molecular weight of 40,000. Because the physical properties of PC / ABS alloys depend on the molecular weight of the PC, it is thought that the smaller the weight-average molecular weight, the more hydrolysis of the PC resin progressed, resulting in a decrease in physical properties due to moist heat degradation.

[0090] Test Example 2 In Test Example 2, a thermoplastic resin composition containing the used PC / ABS alloy etc. used in Test Example 1 was produced, and its moist heat properties were evaluated.

[0091] Example 1 The same used PC / ABS alloy as in Test Example 1 and cobalt carbonate (manufactured by Thermo Scientific) were prepared. These materials were mixed in the volumes shown in Table 1, and the resulting mixture was fed into a kneader and melted while being heated at 240°C. Then, an ISO dumbbell test piece Type A (hereinafter simply referred to as "test piece") was molded using an injection molding machine under conditions of a molding temperature of 240°C and a mold temperature of 60°C.

[0092] Examples 2 and 3 Test pieces were molded under the same conditions as in Example 1, except that the amount of cobalt carbonate added was changed to the mass shown in Table 1.

[0093] (Examples 4 to 6) In addition to the same used PC / ABS alloy as in Test Example 1 and the above cobalt carbonate, virgin PC resin (Makrolon, manufactured by Covestro) was prepared. These materials were mixed in the volumes shown in Table 1. The resulting mixture was heated and melted and injection molded under the same conditions as in Example 1 to form each test specimen.

[0094] Examples 7 to 9: Used ABS resin was prepared in addition to the cobalt carbonate and the virgin PC resin. These materials were mixed in the volumes shown in Table 1. The resulting mixture was heated and melted and injection-molded under the same conditions as in Example 1 to form test specimens. The used ABS resin was obtained by separating low-density polypropylene and high-density engineering plastics from a mixed plastics mixture obtained by crushing used large home appliances using wet sorting, followed by separating the PS resin using electrostatic sorting. The used ABS resin was confirmed to have been obtained by emulsion polymerization using the same method as in Test Example 1.

[0095] Comparative Example 1 The above-mentioned used PC / ABS alloy was prepared, and a test piece was molded under the same conditions as in Example 1, except that cobalt carbonate was not mixed.

[0096] Comparative Examples 2 and 3 Test pieces were molded under the same conditions as in Example 1, except that the amount of cobalt carbonate added was changed to the mass shown in Table 1.

[0097] (Evaluation Method) Evaluation was carried out by the following method.

[0098] [Appearance] Each test piece was visually inspected to see if the added cobalt carbonate had bled out. The results are shown in Table 1. The cases where no bleed-out had occurred were marked "A," and the cases where bleed-out had occurred were marked "B."

[0099] [Bending Test] The bending strength of each test piece was measured by a bending test. The bending test was performed according to JIS K 7171. Specifically, each test piece was exposed for 1,340 hours in a humid and hot environment at a temperature of 65°C and a relative humidity of 85%, and the bending strength at yield was measured at a test speed of 2 mm / min using the same universal testing machine as in Test Example 1. The bending strength retention rate after exposure relative to the bending strength before exposure (bending strength retention rate) was calculated. The results are shown in Table 1. For each test piece, a bending strength retention rate of 75% or more was assigned an "A" rating, and a bending strength retention rate of less than 75% was assigned a "B" rating.

[0100] [Overall Evaluation] A comprehensive evaluation was made based on the above-mentioned evaluations of appearance and bending test. When both were "A", the sample was rated "A", and when at least one of the appearance and bending test was "B", the sample was rated "B".

[0101]

[0102] (Results) From Table 1, it was confirmed that the thermoplastic resin compositions according to the examples were rated "A" in the appearance and bending test, and were excellent in appearance and wet heat properties.

[0103] On the other hand, the thermoplastic resin composition according to the comparative example was rated "B" in either the appearance or the bending test, and it was confirmed that either the appearance or the moist heat properties were poor.

[0104] Comparative Examples 1 and 2 had poor bending strength. This is thought to be because the moist heat properties were not improved due to the absence of cobalt carbonate or the small amount of cobalt carbonate added. Comparative Example 3 had poor appearance. This is thought to be because the amount of cobalt carbonate added was too large.

[0105] The embodiments and examples disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present disclosure is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims.

Claims

1. A method for producing a thermoplastic resin composition, comprising the step of mixing a polycarbonate / ABS alloy containing a first polycarbonate resin and a first ABS resin with a carbonate, wherein the first ABS resin is obtained by emulsion polymerization, the carbonate does not contain an element of Group 1 or Group 2 of the Periodic Table, the carbonate has a decomposition temperature of 200°C or higher, and the content of the carbonate is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the polycarbonate / ABS alloy.

2. The method for producing a thermoplastic resin composition according to claim 1, wherein at least one of the first polycarbonate resin, the first ABS resin and the polycarbonate / ABS alloy is or includes a used material.

3. A method for producing a thermoplastic resin composition, comprising the step of mixing a polycarbonate / ABS alloy containing a first polycarbonate resin and a first ABS resin, at least one selected from the group consisting of a second polycarbonate resin and a second ABS resin, and a carbonate, wherein the first ABS resin and the second ABS resin are obtained by emulsion polymerization, the carbonate does not contain an element of Group 1 of the Periodic Table or an element of Group 2 of the Periodic Table, the carbonate has a decomposition temperature of 200°C or higher, and the content of the carbonate is more than 0.1 parts by mass and less than 6.0 parts by mass per 100 parts by mass of the polycarbonate / ABS alloy and the at least one selected from the group consisting of the second polycarbonate resin and the second ABS resin.

4. The method for producing a thermoplastic resin composition according to claim 3, wherein at least one of the first polycarbonate resin, the second polycarbonate resin, the first ABS resin, the second ABS resin and the polycarbonate / ABS alloy is or includes a used resin.

5. A method for producing a thermoplastic resin composition, comprising a step of mixing a second polycarbonate resin, a second ABS resin, and the carbonate, wherein the second ABS resin is obtained by emulsion polymerization, the carbonate does not contain an element of Group 1 or Group 2 of the periodic table, the carbonate has a decomposition temperature of 200°C or higher, and the content of the carbonate is more than 0.1 part by mass and less than 6.0 parts by mass per 100 parts by mass of the total of the second polycarbonate resin and the second ABS resin.

6. The method for producing a thermoplastic resin composition according to claim 5, wherein at least one of the second polycarbonate resin and the second ABS resin is or includes a used resin.

7. A method for producing a thermoplastic resin composition described in any one of claims 1 to 6, wherein the carbonate is at least one selected from the group consisting of cobalt carbonate, manganese carbonate, cadmium carbonate, iron carbonate and silver carbonate.

Citation Information

Patent Citations

  • Polycarbonate composition and preparation method thereof

    CN104877329A

  • Thermoplastic resin composition

    JP1979040846A

  • Polycarbonate-based resin composition, product, resin for forming housing, method for using polycarbonate-based resin composition as resin for forming housing, and method for producing polycarbonate-based resin composition