Multilayer object having primer composition layer for debonding, and debonding method for multilayer object
The laminate structure with an ethylene vinyl alcohol resin release primer layer effectively addresses the challenge of maintaining gas barrier properties and separating layers for recycling, ensuring efficient recycling and reuse.
Patent Information
- Application Number
- PCT/JP2024/004712
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-02-13
- Publication Date
- 2024-10-31
AI Technical Summary
Existing methods for removing plastic laminate layers fail to maintain excellent gas barrier properties under high temperature and high humidity conditions, and are inefficient in separating printed layers from resin base layers for recycling.
A laminate structure comprising a resin base layer, a release primer layer made of ethylene vinyl alcohol resin with a specific ethylene content and saponification degree, and a printing layer, where the release primer layer is formed using a desorption primer composition containing ethylene vinyl alcohol resin, allowing for easy detachment using a desorption liquid.
The laminate achieves excellent gas barrier properties and enables easy separation of the resin base layer from the printing layer, facilitating recycling and reuse while maintaining adhesion and barrier properties.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Laminate having a removal primer composition layer and method for removing the laminate
[0001] The present invention relates to a laminate having a removal primer composition layer, and a method for removing the laminate.
[0002] Packaging materials using various plastic films are used for foods, confectioneries, household goods, pet food, etc., from the viewpoints of design, economy, content protection, transportability, etc. Furthermore, many packaging materials are subjected to gravure printing or flexographic printing with the intention of imparting designs and messages that appeal to consumers. To obtain these packaging materials, as-printed printing is performed on the surface of the base film of the packaging material, or printing is performed in which an adhesive or anchor agent is applied as needed to the printed surface of the base film of the packaging material and the base film is laminated. In printing for lamination, a color ink composition and a white ink composition are sequentially printed on various base films such as polyester, nylon, and aluminum foil, and then a polyethylene film, a polypropylene film, or the like for heat sealing is laminated on the printed layer of the white ink composition by dry lamination using an adhesive or extrusion lamination using an anchor coating agent (see Patent Document 1).
[0003] In recent years, packaging, plastic bottles, and other plastic products made from plastic film have been discarded or dumped into the ocean as waste, causing environmental pollution problems. These plastic products decompose in seawater, turning into submicron-sized fragments (microplastics), which then float in the seawater. When these plastics are ingested by marine organisms such as fish, they become concentrated in their bodies. This raises concerns about the health of seabirds and humans who consume these marine organisms as food. To address this issue, various efforts to reduce microplastics have been proposed, including a recycling method for removing the plastic substrate from a laminate coated with a printing ink composition. Methods for removing the plastic substrate from a laminate have been proposed, including a release ink composition (see, for example, Patent Document 2), a release adhesive (see, for example, Patent Document 3), a release anchor coating agent (see, for example, Patent Documents 4 to 6), and a release liquid (see, for example, Patent Document 7).
[0004] However, these methods have the problem of insufficient barrier properties. Furthermore, it has been proposed to provide a resin layer containing polyvinyl alcohol (hereinafter sometimes referred to as PVA) as a release layer (for example, Patent Document 8). However, when a resin layer containing polyvinyl alcohol is provided as a release layer, there is a problem that the gas barrier properties are reduced under high temperature and high humidity conditions.
[0005] Japanese Patent Publication No. 5-97959 Japanese Patent No. 6631964 Japanese Patent No. 6642688 Japanese Patent No. 6388131 Japanese Patent Publication No. 2020-175620 Japanese Patent Publication No. 2023-50125 Japanese Patent No. 6690806 International Publication No. 2021 / 090690
[0006] The present invention aims to provide a gas barrier film that is excellent in gas barrier properties under high temperature and humidity conditions, and that allows a printed layer to be separated and released from a resin substrate layer with a release liquid after use.
[0007] The present inventors have found that the above problems can be solved by providing the following laminate and laminate detachment method, and have thus achieved the present invention. 1. A laminate comprising a resin substrate layer, a detachment primer layer containing an ethylene vinyl alcohol resin, and a printed layer laminated in this order. 2. The laminate according to 1, wherein the content of ethylene units in all monomers constituting the ethylene vinyl alcohol resin is 1 to 35 mol %. 3. The laminate according to 1 or 2, wherein the ethylene vinyl alcohol resin has a degree of saponification of 90% or more. 4. The solids coating amount of the detachment primer layer is 0.1 to 2.0 g / m 2 5. The laminate according to any one of 1 to 3, which has an anchor coat layer between the resin substrate layer and the detachment primer layer. 6. A method for detaching a resin substrate layer, comprising the steps of immersing the laminate according to any one of 1 to 5 in a detachment liquid, and recovering the resin substrate layer.
[0008] According to the present invention, the laminate has excellent barrier properties under high temperature and high humidity conditions, and the resin substrate layer can be easily removed from the printed layer with a release liquid, which results in the advantageous effect that the printed layer can be recovered separately from the other layers, and the resin substrate layer can be reused.
[0009] The present invention relates to a laminate comprising a resin substrate layer, a detachment primer layer containing an ethylene vinyl alcohol-based resin (hereinafter sometimes referred to as a "detachment primer layer"), and a printed layer laminated in this order. The detachment primer composition for forming the detachment primer layer is a detachment primer composition containing an ethylene vinyl alcohol-based resin (EVOH), and the laminate comprises a layer made of such a detachment primer composition. The laminate of the present invention may comprise a detachment primer layer and a printed layer formed on the entire surface of the resin substrate layer on the side on which the detachment primer layer is formed, or may comprise a detachment primer layer and a printed layer formed on a portion of the surface of the resin substrate layer on the side on which the detachment primer layer is formed.
[0010] [Resin Substrate Layer] The resin substrate layer in the present invention may consist of one layer or multiple layers. It may be a resin film formed by laminating a resin to a paper substrate. A laminate having a thermoplastic resin layer and a polyethylene-based resin layer may or may not be employed. Examples of such a resin substrate layer include a resin substrate layer capable of being printed on its front surface and a resin substrate layer capable of being printed on its back surface. Examples of resin substrate layers include resin films such as polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene (PE) and polypropylene (PP), and polyamides such as nylon; the above-mentioned resin films having a metal layer such as aluminum; the above-mentioned resin films having a transparent vapor-deposited layer; shrinkable polypropylene films (particularly shrinkable surface-untreated polypropylene films); shrinkable polyvinyl chloride films; and shrinkable polyethylene phthalate films and other shrinkable resin films.
[0011] The surface of the resin substrate layer on which the detachable primer composition layer is to be formed can be subjected to a surface treatment in advance. Examples of such surface treatments include plasma treatment, corona discharge treatment, formation of an anchor coating agent layer, and formation of an adhesive layer, and other surface treatments for improving the adhesion between the resin substrate layer surface and the detachable primer composition layer. Furthermore, after forming a printing ink composition layer on the resin substrate layer via the detachable primer composition layer, a sealant layer may be formed on the printing layer by dry lamination using an adhesive or extrusion lamination using an anchor coating agent.
[0012] [Removal Primer Layer] The removal primer layer in the present invention is a layer provided between the resin substrate layer and the printed layer. Furthermore, when reusing a printed matter after use, the removal primer layer is used to separate the resin substrate layer from the printed layer formed thereon, and to remove the printed layer from the resin substrate layer. A removal primer composition containing an ethylene vinyl alcohol-based resin for forming the removal primer layer will be described below.
[0013] <Release Primer Composition Containing Ethylene-Vinyl Alcohol Resin> The laminate of the present invention has a layer composed of a release primer composition containing an ethylene-vinyl alcohol resin (ethylene-vinyl alcohol (EVOH) resin). (Ethylene-vinyl alcohol resin) Ethylene-vinyl alcohol resins are obtained by saponifying an ethylene-vinyl acetate copolymer and have the properties of excellent moisture barrier properties and high transparency. Furthermore, ethylene-vinyl alcohol resins may contain copolymerized units of vinyl acetate and its saponified products, as well as copolymerized units derived from ethylene, and other copolymerizable monomer units. Furthermore, ethylene-vinyl alcohol resins have copolymerized units derived from ethylene and units derived from a vinyl alcohol structure as copolymerization components. The ethylene content is calculated by dividing the number of moles of ethylene by the total number of moles of all copolymerization components, with ethylene constituting the ethylene-vinyl alcohol resin as one copolymerizable component and another component having an unsaturated double bond as the other copolymerization component. The ethylene content of the ethylene-vinyl alcohol resin is preferably 1 mol% or more, more preferably 4 mol% or more. Furthermore, it is preferably 35 mol% or less, more preferably 30 mol% or less. If the ethylene content is less than 1 mol%, the gas barrier properties at high temperatures and high humidity tend to decrease, and if the ethylene content is more than 35 mol%, the viscosity tends to increase. The ethylene vinyl alcohol resin preferably has a degree of saponification of 95% or more, more preferably 96% or more. If the degree of saponification is less than 95%, the gas barrier properties and oil resistance may decrease. The release primer composition can be obtained by adding the ethylene vinyl alcohol resin to a mixed solvent of lower alcohols as needed, stirring and dissolving the resin.
[0014] The release primer composition can contain an inorganic layered compound to the extent that adhesion to adjacent layers, such as the surface of the resin substrate layer or the printed layer, is not impaired. Examples of inorganic layered compounds that can be used include those that swell and cleave in a dispersion medium. Examples include the kaolinite group, which has a 1:1 phyllosilicate structure; the antigorite group, which belongs to the jamonite group; the smectite group, which is determined by the number of interlayer cations; the vermiculite group, which is a hydrous silicate mineral; and the mica group. Specific examples of inorganic layered compounds include kaolinite, dickite, nacrite, halloysite, antigorite, chrysotile, pyrophyllite, montmorillonite, beidellite, hectorite, saponite, sauconite, stevensite, tetrasilylic mica, sodium taeniolite, muscovite, margarite, talc, vermiculite, phlogopite, xanthophyllite, and chlorite, whether natural or synthetic. Scaly silica and the like can also be used. These may be used alone or in combination of two or more. Among these, montmorillonite is preferred from the viewpoint of coatability and gas barrier properties when used in a barrier coating agent.
[0015] The dispersion medium contained in the detachable primer composition can be either an aqueous dispersion medium or an organic dispersion medium. The aqueous dispersion medium may be water alone, or a dispersion medium obtained by mixing water with a water-miscible organic solvent such as alcohols such as methanol, ethanol, and propanol, polyhydric alcohols such as ethylene glycol and propylene glycol, and their alkyl ether derivatives, esters such as ethyl formate, methyl acetate, and ethyl acetate, or ketones such as acetone. From the viewpoint of maintaining an appropriate solids content, it is preferable to use a mixture containing 50 to 95% by mass of water and 5 to 50% by mass of at least one lower alcohol having 2 to 4 carbon atoms, selected from ethyl alcohol, propyl alcohol, and butyl alcohol. The amount of the detachable primer layer is such that the solids coating amount is 0.1 to 2 g / m. 2 The preferred range is a solid coating amount of 0.1 g / m 2 If the amount is less than 2 g / m, the releasing property tends to decrease. 2If the amount is larger, the adhesiveness tends to decrease.
[0016] [Printed Layer] In the present invention, the printed layer printed with the printing ink composition is not particularly limited and may be a known type. Examples include printed layers printed with lithographic offset printing inks using a plate, gravure printing inks, flexographic printing inks, and inkjet printing inks not using a plate. Gravure printing inks and flexographic printing inks are the most common printing inks used for food packaging films, which may become plastic waste, including food packaging. In recent years, active energy ray-curable inkjet printing ink compositions, active energy ray-curable flexographic printing ink compositions, and active energy ray-curable offset printing ink compositions have also come into use for environmental reasons and to accommodate small-lot production. Here, gravure printing inks, active energy ray-curable inkjet printing ink compositions, and active energy ray-curable offset printing ink compositions will be used as examples. Note that an anchor coating agent layer and / or an adhesive layer may be formed on the surface of the release primer composition layer formed on the resin substrate layer before forming the printed layer. Alternatively, after forming an anchor coating agent layer and / or an adhesive layer on the surface of a resin substrate layer, a release primer composition layer may be formed on these layers, and a print layer may be further formed on top of that.
[0017] <Gravure Printing Ink Composition> The printing ink composition for gravure printing ink (surface printing, shrink printing, reverse printing gravure printing ink) contains a binder resin, a colorant, a solvent such as an organic solvent or an aqueous medium, additives, etc. Examples of binder resins include cellulose-based resins such as soluble nitrocellulose, (biomass) urethane resins, (biomass) polyamide resins, vinyl chloride / vinyl acetate copolymers, rosin-based resins and modified products thereof, ketone resins, cellulose-based resins, (biomass) polyester resins, and (meth)acrylic resins, and these can be used in appropriate combinations. Among these, cellulose-based resins, (biomass) urethane resins, (biomass) polyamide resins, (meth)acrylic resins, vinyl chloride / vinyl acetate copolymers, etc. can be used in appropriate combinations.
[0018] Examples of colorants include organic and inorganic pigments and dyes commonly used in gravure inks. Examples of organic pigments include azo, phthalocyanine, anthraquinone, perylene, perinone, quinacridone, thioindigo, dioxazine, isoindolinone, quinophthalone, azomethine azo, dictylopyrrolopyrrole, and isoindoline pigments. Examples of inorganic pigments include carbon black, titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, silica, red iron oxide, aluminum, and mica. Examples of other pigments include glitter pigments (Metashine; Nippon Sheet Glass Co., Ltd.) made of glass flakes or aggregate flakes as a base material coated with a metal or metal oxide. As the solvent, organic solvents such as aromatic organic solvents, ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester solvents such as ethyl acetate, n-propyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate, and alcohol solvents such as n-propanol, isopropanol, n-butanol, and propylene glycol monomethyl ether can be used. In recent years, the use of ester solvents and alcohol solvents has become preferable from an environmental perspective. Usable additives include extender pigments, pigment dispersants, leveling agents, antifoaming agents, waxes, plasticizers, antiblocking agents, infrared absorbers, ultraviolet absorbers, fragrances, and flame retardants. In addition, some inks further contain crosslinking agents or chelating agents to crosslink the printing ink layer itself and increase its hardness.
[0019] <Actinic Energy Ray-Curable Inkjet Printing Ink Composition> Conventionally used active energy ray-curable inkjet printing ink compositions can be used. The active energy ray-curable inkjet printing ink composition contains a color pigment, a hydroxyl group-containing photopolymerizable compound, and, if necessary, an initiator, a pigment dispersant, and additives. For example, a composition containing a colorant such as those described in WO 2023 / 276290, a hydroxyl group-containing monofunctional (meth)acrylate, a polyfunctional monomer having an ether bond, an amine-modified oligomer, and, if necessary, a polymerization initiator, a sensitizer, a pigment dispersant, and additives can be used.
[0020] <Active energy ray-curable offset printing ink composition> Conventionally used active energy ray-curable offset printing ink compositions can be used. The active energy ray-curable offset printing ink composition contains a color pigment, a hydroxyl group-containing photopolymerizable compound, and, as necessary, an initiator, a pigment dispersant, additives, etc. For example, active energy ray-curable offset printing ink compositions such as those described in JP-A-2018-127541, JP-A-2015-168730, JP-A-2021-195502, JP-A-2020-33465, and JP-A-2018-21138 can be used.
[0021] [Anchor Coat Layer] The laminate may or may not have an anchor coat layer between the resin substrate layer and the detachable primer layer to improve adhesion. As the anchor coat agent for forming the anchor coat layer, urethane-based, isocyanate-based, polyethyleneimine-based, or other anchor coat agents can be used.
[0022] [Method for Producing a Laminate Having a Removal Primer Layer] The laminate of the present invention can be obtained by applying an anchor coating agent to a resin substrate layer, if necessary, to form an anchor coating layer, then applying a detachment primer composition containing an ethylene vinyl alcohol resin to form a detachment primer layer, and then printing or printing each of the printing ink compositions using various printers, inkjet printing devices, etc. After forming the printing layer, a sealant layer can also be formed by dry lamination or extrusion lamination to obtain a laminate.
[0023] [Method for Removing a Laminate Having a Removable Primer Layer] A laminate having a removable primer layer is separated into a resin substrate layer and a printed layer, and the printed layer is removed from the laminate having a removable primer layer. To achieve this, a process can be employed in which the laminate is cut into small pieces by any means, and the pieces are immersed in an alkaline aqueous solution containing a basic compound such as sodium hydroxide or potassium hydroxide, which serves as a release liquid, and stirred as necessary. The concentration of sodium hydroxide or potassium hydroxide used here is preferably 0.5 to 15.0% by mass, more preferably 1.0% by mass or more, and even more preferably 1.5% by mass or more. Furthermore, when treating waste liquid after use, a concentration of 5.0% by mass or less is preferred, and even more preferably 3.0% by mass or less is preferred. The release liquid used for release may be at room temperature (approximately 25°C) or heated to 25 to 90°C. The immersion time is preferably 1 minute to 12 hours, more preferably 1 hour or less, even more preferably 30 minutes or less, and most preferably 10 minutes or less. At the same time, it is preferable to treat the fragmented laminate with a sufficiently large amount of release liquid, 100 to 1,000,000 times the weight of the fragmented laminate, for smooth release. After the immersion in release liquid step, a step of recovering the resin substrate layer and the printed layer is provided. If the resin substrate layer of the laminate is, for example, polyester, this release method allows the ink layer to be removed in the release liquid, and the separated polyester can be washed with water and dried to obtain a recycled polyester substrate. The recycled polyester substrate can also be recycled into pellets using an extruder for reuse.
[0024] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass."
[0025] <Resin substrate layer> The following three types were used as the resin substrate layer (excluding shrink films): OPP: biaxially oriented polypropylene film P-2161#25 (Toyobo Co., Ltd.) PET: polyethylene terephthalate film E-5102#12 (Toyobo Co., Ltd.) NY: nylon film ONY-15#12 (Unitika Ltd.) PE: polyethylene film 25 μm thick corona-treated L-LDPE film (linear low-density polyethylene, Mitsui Chemicals Tohcello Co., Ltd.) <Anchor coating agent> Takelac A-3210 / Takelac A-3072 diluted with ethyl acetate to a solids content of 7%
[0026] [Removal Primer Composition] <Removal Primer Composition 1> Five parts by mass of an ethylene-vinyl alcohol copolymer (product name: Soarnol V2504NB (ethylene content: 25 mol%)) was added to 95 parts by mass of a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol, and the mixture was stirred and dissolved at 80°C to obtain a removal primer composition 1 having a solids content of 5% by mass.
[0027] <Removal Primer Composition 2> 7 parts by mass of an ethylene-vinyl alcohol copolymer (product name: Soarnol V2504NB (ethylene content: 25 mol%)) was added to 93 parts by mass of a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol, and the mixture was stirred and dissolved at 80°C, to obtain a removal primer composition 2 having a solids content of 7% by mass.
[0028] <Removal Primer Composition 3> 10 parts by mass of an ethylene-vinyl alcohol copolymer (product name: EXCEVAL HR-3010 (ethylene content: 4.5 mol%)) was added to 90 parts by mass of purified water, stirred and dissolved at 95°C, and diluted with a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol, to obtain a removal primer composition 3 having a solids content of 5% by mass.
[0029] <Removal Primer Composition 4> Five parts by mass of an ethylene-vinyl alcohol copolymer (product name: Soarnol DC3212 (ethylene content: 32 mol%)) was added to 95 parts by mass of a mixed solvent containing 30% by mass of purified water and 70% by mass of isopropyl alcohol, and the mixture was stirred and dissolved at 80°C to obtain a removal primer composition 4 having a solids content of 5% by mass.
[0030] <Release Primer Composition 5> 5 parts by mass of montmorillonite (trade name: Kunipia F, Kunimine Industries Co., Ltd.), an inorganic layered compound, was added to 95 parts by mass of purified water with stirring, and the mixture was thoroughly dispersed at a pressure of 50 MPa using a high-pressure disperser to obtain an inorganic layered compound dispersion with a solids content of 5% by mass. Next, 15 parts by mass of the inorganic layered compound dispersion was added to 85 parts by mass of release primer composition 1 while stirring at high speed, and the mixture was further dispersed at a pressure of 50 MPa using a high-pressure disperser and filtered using a 255-mesh filter to obtain release primer composition 5 with a solids content of 5% by mass (ethylene-vinyl alcohol copolymer resin / inorganic layered compound=85 / 15 (solids mass ratio)).
[0031] <Removal Primer Composition of Comparative Example 1> 2 parts by mass of polyethyleneimine (Epomin P-1000 (Nippon Shokubai Co., Ltd.) (amine value 18 mmol / g)) was added to 98 parts by mass of a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol, and the mixture was stirred and dissolved to obtain a removal primer composition of Comparative Example 1 having a solids content of 2% by mass.
[0032] <Removal Primer Composition of Comparative Example 2> 5 parts by mass of Poval 5-98 (Kuraray Co., Ltd.) was added to 95 parts by mass of a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol and stirred to obtain a removal primer composition of Comparative Example 2 having a solids content of 5% by mass.
[0033] <Preparation of Resin Substrate Layer with Removal Primer Composition Layer Formed> Removal primer compositions 1, 3, and 4 were applied to a resin substrate with a dry coating amount of 0.1 g / m using a bar coater. 2 The surface of the anchor coating agent layer of the resin substrate layer was coated with a bar coater so that the dry coating amount was 1.0 g / m 2 The release primer composition 5 was applied to the surface of the substrate with a bar coater so that the dry coating amount of the anchor coating agent was 0.1 g / m. 2 The surface of the anchor coating agent layer of the resin substrate layer was coated with a bar coater so that the dry coating amount was 0.5 g / m 2 The release primer composition 2 was applied to the surface of the substrate with a bar coater so that the dry coating amount of the anchor coating agent was 0.1 g / m. 2The surface of the anchor coating agent layer of the resin substrate layer was coated with a bar coater so that the dry coating amount was 1.4 g / m 2 The release primer composition of Comparative Example 1 was applied to the surface of the substrate with a bar coater in a dry coating amount of 0.1 g / m. 2 The surface of the anchor coating agent layer of the resin substrate layer was coated with a bar coater so that the dry coating amount was 0.2 g / m 2 The release primer composition of Comparative Example 2 was applied to the surface of the substrate with a bar coater in a dry coating amount of 0.1 g / m. 2 The surface of the anchor coating agent layer of the resin substrate layer was coated with a bar coater so that the dry coating amount was 1.0 g / m 2 The coating was applied so that the
[0034] <Printing Ink Composition for Surface Printing> As the printing ink composition for surface printing, for example, Sapyria-N Indigo 800 YZ RE-1 (manufactured by Sakata Inx Corporation) can be used, but the composition is not limited to this.
[0035] (Printing with surface printing ink composition) An anchor coating agent was applied to each of the four resin substrate layers using a bar coater in a dry coating amount of 0.1 g / m 2 The above-mentioned detachment primer compositions 1 to 5 of each Example and detachment primer compositions 1 and 2 of the Comparative Examples (a total of seven detachment primer compositions) were applied using a bar coater to the coated surface so that the surface had been coated with a coating such that the detachment primer composition layer was formed, yielding a total of 28 samples. The surface printing ink composition was diluted with a mixed solvent (ethyl acetate / propyl acetate / IPA (isopropyl alcohol) = 50 / 25 / 25) to a dilution of 16 seconds using a Rigo Zahn Cup No. 3. This diluted surface printing ink composition was printed on the detachment primer composition layer of each sample using a bar coater and dried to obtain a printed product (laminate) of each surface printing ink composition. Each surface printing ink composition printed product (laminate) was shredded into small pieces approximately 15 mm MD x 25 mm TD to obtain samples for printing layer peeling tests.
[0036] <UV-curable inkjet printing ink composition> The UV-curable inkjet printing ink composition may be prepared as described below, but is not limited to this composition. (Preparation of UV-curable inkjet printing ink composition) P.B. 2.6 parts by mass of 15:4, 1.04% by mass of Solsperse S56000 (manufactured by Lubrizol Japan Corporation), 30.00 parts by mass of amine-modified acrylate oligomer (manufactured by Sartomer, CN371NS), 4.50% by mass of 1,6-hexanediol diacrylate, 7.96 parts by mass of neopentyl glycol PO-modified diacrylate, 7.00 parts by mass of dipropylene glycol diacrylate, 5.00 parts by mass of ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate, 3.00 parts by mass of bis(2,4,6-trimethylbenzoyl)phenoxyphosphine oxide (IGM Resins B.V.), (2-carboxymethoxythioxanthone)-(polytetramethylene glycol 250) diester (IGM Resins B.V.) A UV-curable inkjet printing ink composition was prepared containing 2.50 parts by mass of a quinone polymerization inhibitor (UV22, manufactured by BASF), 0.40 parts by mass of a quinone polymerization inhibitor (UV22, manufactured by BASF), and 0.20 parts by mass of a silicone surface conditioner (BYK-377, manufactured by BYK-Chemie).
[0037] (Printing with UV-curable inkjet printing ink composition) An anchor coating agent was applied to each of the four resin substrate layers using a bar coater in a dry coating amount of 0.1 g / m 2 Each of the above-mentioned detachment primer compositions 1 to 5 and Comparative Examples 1 and 2 (a total of seven detachment primer compositions) was applied using a bar coater to the coated surface so that a detachment primer composition layer was formed, to obtain a total of 28 samples. The above-mentioned UV-curable inkjet printing ink composition was printed on each of the detachment primer composition layers of the samples using a bar coater, and the samples were printed using a UV-LED light lamp manufactured by Phoseon Technologies, Inc., at a distance of 2 cm between the lamp and the ink coated surface, with an integrated UV light dose of 180 mJ / cm. 2This UV-curable inkjet printing ink composition print (laminate) was shredded into small pieces of approximately 15 mm MD x 25 mm TD to obtain samples for printing layer peeling tests.
[0038] <EB (electron beam) curable offset printing ink composition> The EB (electron beam) curable offset printing ink composition may be prepared as follows, but is not limited to this composition. (Preparation of EB curable offset printing ink composition) 22.7 parts by mass of PB15:3, 40.0 parts by mass of polyester acrylate oligomer CN704 (Sartomer), 36.2 parts by mass of 6EO-modified TMPTA (6EO-modified trimethylolpropane triacrylate), 0.1 part by mass of methylhydroquinone, and 1.0 part by mass of dimethyl silicone oil TSF-451-5M (Momentive) were blended and mixed with stirring to obtain an EB-curable offset printing ink composition.
[0039] (Printing with EB (electron beam) curable offset printing ink composition) An anchor coating agent was applied to each of the four resin substrate layers using a bar coater in a dry coating amount of 0.1 g / m 2 The above-mentioned detachment primer compositions 1 to 5 of each Example and detachment primer compositions 1 and 2 of the Comparative Examples (a total of seven detachment primer compositions) were applied using a bar coater to the coated surface, which had been coated so that the detachment primer composition layer was formed, to obtain a total of 28 samples. 0.1 cc of each of the above EB-curable offset printing ink compositions was transferred onto each of the detachment primer composition layers of the samples using a simple color developer (RI Tester, manufactured by Toyoei Seiko Co., Ltd.). The compositions were then irradiated with electron beams at a conveyor speed of 10 m / min using an electron beam curing device (EC90, manufactured by Iwasaki Electric Co., Ltd.) (accelerating voltage 90 kV, exposure dose 30 kGy) to completely cure the composition, thereby obtaining a printed product (laminate). Each of the EB-curable offset printing ink composition printed products (laminates) was shredded into small pieces approximately 15 mm MD x 25 mm TD to obtain samples for printing layer peeling tests.
[0040] <UV (ultraviolet) curable offset printing ink composition> The UV (ultraviolet) curable offset printing ink composition may be prepared as follows, but is not limited to this composition. (Preparation of UV-curable offset printing ink composition) 50.0 parts by mass of rosin-modified maleic acid resin (Halima M-453, manufactured by Harima Chemicals Co., Ltd.), 41.0 parts by mass of trimethylolpropane (6EO) triacrylate, 2.0 parts by mass of dimethyl silicone oil (KF-96H-100,000cs), 5.0 parts by mass of 2-methyl-1(4-methylthiophenyl)-2-morpholinopropan-1-one, and 4.4'-bis(diethylamino)benzophenone were blended and mixed with stirring to obtain a UV-curable offset printing ink composition.
[0041] (Printing with UV-curable offset printing ink composition) An anchor coating agent was applied to each of the four resin substrate layers using a bar coater in a dry coating amount of 0.1 g / m 2 The above-mentioned detachment primer compositions 1 to 5 of each Example and detachment primer compositions 1 and 2 of the Comparative Examples (a total of seven detachment primer compositions) were applied using a bar coater to the coated surface so that a detachment primer composition layer was formed, obtaining a total of 28 samples. 0.1 cc of each of the above UV-curable offset printing ink compositions was transferred onto each detachment primer composition layer of the samples using a simple color developer (RI Tester, manufactured by Toyoei Seiko Co., Ltd.), and the ink was then applied using a UV-LED light lamp manufactured by Phoseon Technologies, Inc., at a distance of 2 cm from the lamp to the ink-coated surface, with an integrated UV light dose of 180 mJ / cm. 2 The printed matter (laminate) of each UV-curable offset printing ink composition was shredded into small pieces of approximately 15 mm MD x 25 mm TD to obtain samples for the print layer peeling test.
[0042] <Shrinkable Printing Ink Composition> As the shrinkable printing ink composition, for example, XBT-7018 N Indigo 800 (manufactured by Sakata Inx Corporation) can be used, but the composition is not limited to this.
[0043] (Printing with Shrink Printing Ink Composition) The above anchor coating agent was applied to a crystallizable shrinkable PET (polyethylene terephthalate) film with a bar coater in a dry coating amount of 0.1 g / m 2 After coating and drying so that the thickness of the detachable primer composition layer was 15 mm, the detachable primer composition 1 was coated and dried using a bar coater. The shrinkable printing ink composition was then printed on the detachable primer composition layer using a bar coater, dried, and cured to obtain a printed matter (laminate). This shrinkable printing ink composition printed matter (laminate) was shredded into small pieces measuring approximately 15 mm MD x 25 mm TD to obtain samples for printing layer peeling tests.
[0044] <Evaluation of Ink Release Properties> (Releasing Solution Composed of an Alkaline Aqueous Solution) 2.0 parts by mass of sodium hydroxide was added to 98.0 parts by mass of water, and the mixture was stirred and dissolved to obtain a releasing solution composed of an alkaline aqueous solution. (Releasing) The releasing solution composed of the alkaline aqueous solution was placed in an HDPE (high-density polyethylene) container and heated to 70°C in a hot water bath. After that, each of the printed layer peeling test samples was placed in the respective releasing solutions and stirred for 30 minutes using a stainless steel stirring blade with a blade diameter of 25 mm. After stirring, the HDPE (high-density polyethylene) container was removed from the hot water bath and allowed to stand at room temperature for 5 minutes. The releasing solution and each film piece, such as the resin substrate layer, were separated using a stainless steel mesh with a mesh opening of approximately 2 mm. (Rinsing) After release, each film piece was transferred to another HDPE container with a volume of 200 cc, and 100 g of water was added. Stirring was continued for 5 minutes using a stainless steel stirring blade with a blade diameter of 25 mm. After leaving the film pieces to stand for 5 minutes, the film pieces were separated from the water using a stainless steel mesh. After drying, the ink peelability from the film pieces was visually evaluated.
[0045] <Evaluation criteria> (Ink releasability) ○: Ink film completely peeled off from the film as film pieces ×: Not peeled
[0046] (Tape Adhesion Strength (Each Printed Material Immediately After Printing and Drying)) Cellophane tape was applied to the printed surface of each of the obtained printed materials, and then quickly peeled off to evaluate the degree of peeling of the printed coating, according to the following evaluation criteria. (Evaluation Criteria) ◯: Less than 5% of the area of the printed coating peeled off from the film. Δ: 5% or more but less than 30% of the area of the printed coating peeled off from the film. ×: 30% or more of the area of the printed coating peeled off from the film.
[0047] (Barrier properties) Oxygen transmission rate (OTR value) was measured using an oxygen transmission rate measuring device (manufactured by Mocon, product name: OX-TRAN1 / 50) in accordance with JIS K7126 B method. The measurement was carried out at 20°C in an atmosphere of 65% RH. ◯: OTR value is 10 or less, ×: OTR value is more than 10
[0048] The test results are shown in Table 1 below. "No detachable primer composition applied" is an example in which an anchor coating agent layer and a detachable primer layer were not formed, and the other examples are examples in which an anchor coating agent was applied, and then detachable primer compositions 1 to 5 or the detachable primer composition of Comparative Example 1 or 2 were applied. The same effect was obtained regardless of the resin substrate layer, printing method, or type of printing ink, so these requirements are summarized in Table 1 below.
[0049]
[0050] The above examples are examples in which an anchor coat layer is formed, but even if an anchor coat layer is not formed, the printed layer has sufficient adhesion immediately after printing, etc. Table 1 above shows that by using the detachable primer composition of the present invention to form a detachable primer layer of the present invention, both detachability and barrier properties are good, regardless of the presence or absence of a resin substrate layer or an anchor coat layer, or differences in printing ink composition or printing method.
[0051] Next, the case where a reverse printing ink composition is used will be described. When a layer made of a reverse printing ink composition is used as the printing layer, the resulting laminate has a resin substrate layer, an anchor coat layer, a detachable primer layer, a printing layer, and a sealant layer. <Detachable primer composition> The same composition as described above was used.
[0052] <Reverse Printing Ink Composition> As the reverse printing ink composition, for example, Bellflora® Indigo 800MK (manufactured by Sakata Inx Corporation) can be used, but the composition is not limited to this.
[0053] (Printing with reverse printing ink composition) An anchor coating agent was applied to each of the four resin substrate layers using a bar coater in a dry coating amount of 0.1 g / m 2 The above-mentioned detachment primer compositions 1 to 5 of each Example and detachment primer compositions 1 and 2 of the Comparative Examples (a total of seven detachment primer compositions) were applied using a bar coater to the coated surface so as to form a detachment primer composition layer, obtaining a total of 28 samples. A mixed solvent (ethyl acetate / propyl acetate / IPA (isopropyl alcohol) = 50 / 25 / 25) was added to the above-mentioned reverse printing ink composition, and the diluted reverse printing ink composition was diluted to 16 seconds using a Rigosha Zahn Cup No. 3. The diluted reverse printing ink composition was printed using a bar coater on each detachment primer composition layer of the samples, and dried to obtain a printed layer.
[0054] (Dry Lamination) RXC-22#60 (unstretched propylene film (Mitsui Chemicals Tohcello Inc.)) and T.U.X™: linear low-density polyethylene (Mitsui Chemicals Tohcello Inc.) were each coated with an adhesive (Takelac A-515 / Takelac A-50, solids content 30% by mass when the resin substrate layer was PET, NY, or PE) (Takelac A-969V / Takelac A-5 (solids content 30% by mass when the resin substrate layer was OPP) using a bar coater, and then manually attached to each printed layer to form laminates.
[0055] (Extrusion Lamination) An AC agent (Takelac A-3210 / Takelac A-3072, solid content 7% by mass) was applied onto each printed matter (printed layer), and then molten polyethylene Sumikathene L705 (Sumitomo Chemical Co., Ltd.) was laminated using an extrusion laminator to prepare each laminate.
[0056] <Evaluation of ink release properties> The printed matter of each laminate was shredded into small pieces of approximately 15 mm MD x 25 mm TD to obtain samples for print layer peeling tests. Evaluation was carried out in the same manner as described above. <Evaluation criteria> (Ink release properties) ○: The ink coating completely peeled off from the resin substrate layer as coating pieces ×: No peeling The results are shown in Table 2.
[0057] <Evaluation of tape adhesive strength (for each printed matter immediately after printing and drying) and barrier properties> Evaluations were carried out in the same manner as described above. The results are shown in Table 2.
[0058] (Laminate strength) Each laminate was cut into a width of 15 mm, and the T-peel strength was measured using a peel tester manufactured by Yasuda Seiki Seisakusho Co., Ltd. (Evaluation criteria) When the resin substrate layer is OPP: ◯: Peel strength is 1.2 N / 15 mm or more; △: Peel strength is 0.7 N / 15 mm or more but less than 1.2 N / 15 mm; ×: Peel strength is less than 0.7 N / 15 mm When the resin substrate layer is PET, NY, or PE: ◯: Peel strength is 5 N / 15 mm or more; △: Peel strength is 3 N / 15 mm or more but less than 5 N / 15 mm; ×: Peel strength is less than 3 N / 15 mm
[0059] The test results are shown in Table 2. "No detachable primer composition applied" is an example in which an anchor coating agent and a detachable primer layer were not formed. Other examples are examples in which an anchor coat was applied, and then detachable primer compositions 1 to 5 or the detachable primer composition of Comparative Example 1 or 2 were applied. The same effect was obtained regardless of the type of resin substrate layer, printing method, printed ink layer, adhesive layer, and sealant layer, so these requirements are summarized and shown in Table 2 below.
[0060]
[0061] Although the above example is an example in which an anchor coat layer is formed, even if an anchor coat layer is not formed, adhesion is maintained immediately after printing, etc., and no particular problems arise. Table 2 above shows that by using the detachable primer composition of the present invention to form a detachable primer layer of the present invention, regardless of differences in resin substrate layer, printing ink composition, or printing method, detachability, barrier properties, adhesion immediately after printing, and laminate strength are all good.
Claims
1. A laminate comprising a resin substrate layer, a removable primer layer containing an ethylene vinyl alcohol resin, and a printed layer, laminated in this order.
2. The laminate according to claim 1, wherein the content of ethylene units in all monomers constituting the ethylene-vinyl alcohol resin is 1 to 35 mol %.
3. The laminate according to claim 1 or 2, wherein the saponification degree of the ethylene-vinyl alcohol-based resin is 90% or more.
4. The solid coating amount of the removable primer layer is 0.1 to 2.0 g / m 2 3. The laminate according to claim 1 or 2, 5. The laminate according to claim 1 or 2, which has an anchor coat layer between the resin substrate layer and the removable primer layer.
6. A method for removing a resin substrate layer, comprising the steps of immersing the laminate according to claim 1 or 2 in a removing liquid, and recovering the resin substrate layer.
Citation Information
Patent Citations
Resin for printing ink
JP1993097959A
Active energy ray-curable ink composition for offset printing and production method of printed matter using the same
JP2015168730A
Curing method of ultraviolet-curable offset ink, and printed matter printed by using the curing method
JP2018021138A
Ink composition for active energy ray-curable off set printing, and printing method to non-absorptive medium using the same
JP2018127541A
Active energy ray-curable composition, active energy ray-curable ink, and printed matter
JP2020033465A