Thermally conductive silicone resin composition
The thermally conductive silicone resin composition, combining liquid dimethylpolysiloxane, polydecene-ethylene-propylene copolymer, and varied inorganic particles, addresses the challenges of dripping and viscosity in silicone greases, offering high thermal conductivity and dischargeability for electronic component thermal management.
Patent Information
- Application Number
- PCT/JP2024/008950
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-31
AI Technical Summary
Thermally conductive silicone greases face issues with dripping and viscosity, requiring improved drop resistance and dischargeability while maintaining high thermal conductivity, especially as electronic components generate more heat and shrink in size.
A thermally conductive silicone resin composition comprising a matrix resin component based on liquid dimethylpolysiloxane and a mixed oil of polydecene and ethylene-propylene copolymer, combined with thermally conductive inorganic particles of varying sizes, which enhances thermal conductivity, reduces dripping, and improves dischargeability.
The composition achieves high thermal conductivity, reduced dripping, and excellent discharge properties, making it suitable for use between heat-generating and heat-radiating components in electronic devices, with improved stability and performance in cyclic temperature tests.
Smart Images

Figure JP2024008950_31102024_PF_FP_ABST
Abstract
Description
Thermally conductive silicone resin composition
[0001] The present invention relates to a thermally conductive silicone resin composition suitable for use between a heat-generating portion of an electric or electronic component and a heat sink.
[0002] In recent years, the performance of semiconductors such as CPUs has improved dramatically, resulting in a huge increase in the amount of heat generated. Heat sinks are therefore attached to heat-generating electronic components, and thermally conductive grease is used to improve adhesion between the heat sink and heat-generating components such as semiconductors. As devices become smaller, more powerful, and more highly integrated, thermally conductive greases are required to have high thermal conductivity as well as drop resistance.
[0003] Japanese Patent Application Laid-Open Publication No. 2018-104714 proposes a composition containing a thermally conductive filler, a polyorganosiloxane resin containing at least one polysiloxane having one curable functional group in the molecule, and a siloxane compound having an alkoxysilyl group and a linear siloxane structure. Japanese Patent Application Laid-Open Publication No. 2016-044213 proposes a thermally conductive silicone composition containing liquid silicone, a thermally conductive filler, and hydrophobic spherical silica microparticles, and having improved heat dissipation properties. Japanese Patent Application Laid-Open Publication No. 2004-131540 proposes a resin sheet containing an α-olefin copolymer containing two or more α-olefins having 2 to 12 carbon atoms and a thermally conductive filler. Japanese Patent Application Laid-Open Publication No. 2004-143195 proposes a resin sheet containing an α-olefin copolymer containing two or more α-olefins having 2 to 12 carbon atoms and a surface-treated thermally conductive filler. In Japanese Patent No. 7047199, the present inventors have proposed a thermally conductive grease in which a thermally conductive filler is blended with an ethylene-α-olefin copolymer.
[0004] The present invention provides a thermally conductive silicone resin composition comprising a matrix resin component (A) and thermally conductive inorganic particles (B), wherein the matrix resin component (A) contains, relative to 100 parts by mass of the matrix resin component (A), 70 to 99 parts by mass of a liquid dimethylpolysiloxane (A1) and 1 to 30 parts by mass of a mixed oil (A2) of polydecene and an ethylene-propylene copolymer, and the liquid dimethylpolysiloxane (A1) has a kinematic viscosity at 40°C of 50 to 10,000 mm 2 / s, and the mixed oil (A2) has a kinematic viscosity at 40°C of 1 to 1,000 mm 2 / s, and the thermally conductive silicone resin composition contains 400 to 3,000 parts by mass of the thermally conductive inorganic particles (B) per 100 parts by mass of the matrix resin component (A).
[0005] 1A-B are explanatory diagrams showing a method for measuring the thermal conductivity of a sample in one embodiment of the present invention. FIGS. 2A-D are schematic explanatory diagrams illustrating a drop test used in one embodiment of the present invention. FIG. 3 is a scanning electron microscope (SEM) photograph (magnification: 5000x) of amorphous alumina (B1) (D50 (median diameter) is 0.3 μm) used in one embodiment of the present invention. FIG. 4 is an SEM photograph (magnification: 2000x) of amorphous alumina (B1) (D50 (median diameter) is 2.3 μm) used in one embodiment of the present invention. FIG. 5 is an SEM photograph (magnification: 2000x) of amorphous aluminum nitride (B2) (D50 (median diameter) is 15 μm) used in one embodiment of the present invention. FIG. 6 is an SEM photograph (magnification: 100x) of spherical alumina (B3) (D50 (median diameter) is 105 μm) used in one embodiment of the present invention. Detailed Description of the Invention
[0006] However, the thermally conductive silicone grease of the above-mentioned prior art had the problem of dripping when held vertically. Also, greases that use ethylene-propylene copolymers to improve drop resistance have been reported, but these have the problem of higher viscosity than those that use silicone. Also, silicone greases that use a mixture of silicone and ethylene-propylene copolymers to improve drop resistance and have a relatively low viscosity have been reported, but a grease with even better ejection properties was desired.
[0007] In order to solve the above-mentioned problems of the prior art, the present invention provides a thermally conductive silicone resin composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability.
[0008] The present invention provides a thermally conductive silicone resin composition comprising a matrix resin component (A) and thermally conductive inorganic particles (B), wherein the matrix resin component (A) contains, relative to 100 parts by mass of the matrix resin component (A), 70 to 99 parts by mass of a liquid dimethylpolysiloxane (A1) and 1 to 30 parts by mass of a mixed oil (A2) of polydecene and an ethylene-propylene copolymer, and the liquid dimethylpolysiloxane (A1) has a kinematic viscosity at 40°C of 50 to 10,000 mm 2 / s, and the mixed oil (A2) has a kinematic viscosity at 40°C of 1 to 1,000 mm 2 / s, and the thermally conductive silicone resin composition contains 400 to 3,000 parts by mass of the thermally conductive inorganic particles (B) per 100 parts by mass of the matrix resin component (A).
[0009] By adopting the above-described configuration, the present invention can provide a thermally conductive silicone resin composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability. That is, by providing a thermally conductive silicone resin composition that includes, as the matrix resin component (A), a liquid dimethylpolysiloxane (A1) of a specific viscosity and a mixed oil (A2) of polydecene and an ethylene-propylene copolymer, and that contains 400 to 3,000 parts by mass of the thermally conductive inorganic particles (B) per 100 parts by mass of the matrix resin component (A), a thermally conductive silicone resin composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability can be provided.
[0010] The thermally conductive silicone resin composition of the present invention contains a matrix resin component (A) and thermally conductive inorganic particles (B).
[0011] <Matrix Resin Component (A)> The matrix resin component (A) contains 70 to 99 parts by mass of liquid dimethylpolysiloxane (A1) and 1 to 30 parts by mass of a mixed oil (A2) of polydecene and an ethylene-propylene copolymer, relative to 100 parts by mass of the matrix resin component (A).
[0012] (i) Liquid dimethylpolysiloxane (A1) The liquid dimethylpolysiloxane (A1) has a kinematic viscosity at 40°C of 50 to 10,000 mm 2 / s, preferably 60 to 9,000 mm 2 / s, and more preferably 70 to 8,000 mm 2 By using such a liquid dimethylpolysiloxane (A1), it is possible to obtain a thermally conductive silicone resin composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability.
[0013] The content of the liquid dimethylpolysiloxane (A1) is 70 to 99 parts by mass, preferably 71 to 98 parts by mass, and more preferably 72 to 98 parts by mass, per 100 parts by mass of the matrix resin component (A).
[0014] (ii) Mixed oil (A2) of polydecene and ethylene-propylene copolymer The kinematic viscosity of the mixed oil (A2) of polydecene and ethylene-propylene copolymer at 40°C is 1 to 1,000 mm 2 / s, preferably 5 to 900 mm 2 / s, and more preferably 10 to 800 mm 2 / s. By using such mixed oil (A2), it is possible to obtain a thermally conductive silicone resin composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability. The mixed oil (A2) of polydecene and ethylene-propylene copolymer is a hydrocarbon-based synthetic oil that does not contain polar groups, and is commercially available from Mitsui Chemicals, Inc. under the trade name "Lucant" HC-10. This mixed oil (A2) has a specific gravity of 0.83 (density of 0.83 g / cm 3 The inclusion of this mixed oil (A2) has the advantage of reducing the specific gravity of the thermally conductive silicone resin composition. Furthermore, the use of such a mixed oil (A2) makes it possible to obtain a thermally conductive silicone resin composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability.
[0015] The content of the mixed oil (A2) is 1 to 30 parts by mass, preferably 2 to 29 parts by mass, and more preferably 3 to 28 parts by mass, per 100 parts by mass of the matrix resin component (A).
[0016] The mixed oil (A2) preferably contains 30 to 99 mass% of polydecene and 1 to 70 mass% of an ethylene-propylene copolymer, more preferably 35 to 95 mass% of polydecene and 5 to 65 mass% of an ethylene-propylene copolymer, and even more preferably 40 to 90 mass% of polydecene and 10 to 60 mass% of an ethylene-propylene copolymer, relative to 100 mass% of the mixed oil (A2).
[0017] <Thermal Conductive Inorganic Particles (B)> The thermally conductive inorganic particles (B) preferably include thermally conductive inorganic particles (B1) having a median particle size (D50) of 0.01 to 10 μm, thermally conductive inorganic particles (B2) having a median particle size (D50) of more than 10 μm but not more than 80 μm, and thermally conductive inorganic particles (B3) having a median particle size (D50) of more than 80 μm but not more than 150 μm. By using thermally conductive inorganic particles (B) having such a configuration, the thermally conductive inorganic particles (B) can be packed in a state close to close-packed in the thermally conductive silicone resin composition, thereby increasing the thermal conductivity of the thermally conductive silicone resin composition. The median particle size is the D50 (median diameter) of the cumulative particle size distribution on a volume basis measured by laser diffraction light scattering. An example of an instrument for this measurement is the LA-950S2 laser diffraction / scattering particle size distribution analyzer manufactured by Horiba, Ltd.
[0018] The thermally conductive inorganic particles (B1) are preferably amorphous alumina because alumina is inexpensive. The thermally conductive inorganic particles (B2) are preferably at least one inorganic particle selected from the group consisting of alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, aluminum hydroxide, and silicon carbide. The thermally conductive inorganic particles (B2) are preferably amorphous in shape. The thermally conductive inorganic particles (B3) are preferably spherical alumina. When the proportion of spherical alumina added as the thermally conductive inorganic particles (B3) is high, the thermal conductivity of the thermally conductive silicone resin composition can be increased and costs can be reduced. When alumina is used as the thermally conductive inorganic particles (B), it is preferable to use a combination of so-called submicron particles (B1-1) having a D50 (median diameter) of 0.01 μm or more but less than 1 μm, small particles (B1-2) having a D50 (median diameter) of 1 μm or more but less than 10 μm, and large particles (B3) having a D50 (median diameter) of more than 80 μm but less than 150 μm. By using thermally conductive inorganic particles (B) of this configuration, the thermally conductive inorganic particles (B) can be closely packed in the thermally conductive silicone resin composition, thereby increasing the thermal conductivity of the thermally conductive silicone resin composition. Irregular shaped alumina is produced by pulverization or crushing, and commercially available products can be used. These thermally conductive inorganic particles (B1), (B2), and (B3) have high thermal conductivity.
[0019] The mass ratio of the thermally conductive inorganic particles (B1), (B2), and (B3) preferably satisfies the relationship (B2)≦(B1)≦(B3), because by satisfying this ratio, the thermally conductive inorganic particles can be packed in a state close to closest packing in the thermally conductive silicone resin composition, thereby increasing the thermal conductivity of the thermally conductive silicone resin composition.
[0020] The thermally conductive inorganic particles (B) preferably contain 100 to 1,000 parts by mass, more preferably 150 to 1,000 parts by mass, and even more preferably 300 to 850 parts by mass of the thermally conductive inorganic particles (B1) per 100 parts by mass of the matrix resin component (A). The thermally conductive inorganic particles (B) preferably contain 100 to 500 parts by mass, more preferably 150 to 500 parts by mass, and even more preferably 200 to 450 parts by mass of the thermally conductive inorganic particles (B2) per 100 parts by mass of the matrix resin component (A). The thermally conductive inorganic particles (B) preferably contain 300 to 1,400 parts by mass, more preferably 300 to 1,300 parts by mass, and even more preferably 500 to 1,200 parts by mass of the thermally conductive inorganic particles (B3) per 100 parts by mass of the matrix resin component (A). This makes it possible to obtain a thermally conductive silicone resin composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability. For the same reason, the thermally conductive inorganic particles (B) preferably contain 100 to 1,000 parts by mass of the thermally conductive inorganic particles (B1), 100 to 500 parts by mass of the thermally conductive inorganic particles (B2), and 300 to 1,400 parts by mass of the thermally conductive inorganic particles (B3) relative to 100 parts by mass of the matrix resin component (A), more preferably 150 to 1,000 parts by mass of the thermally conductive inorganic particles (B1), 150 to 500 parts by mass of the thermally conductive inorganic particles (B2), and 300 to 1,300 parts by mass of the thermally conductive inorganic particles (B3), and even more preferably 300 to 850 parts by mass of the thermally conductive inorganic particles (B1), 200 to 450 parts by mass of the thermally conductive inorganic particles (B2), and 500 to 1,200 parts by mass of the thermally conductive inorganic particles (B3).
[0021] The thermally conductive inorganic particles (B1) having a median particle size (D50) of 0.01 to 10 μm, the thermally conductive inorganic particles (B2) having a median particle size (D50) of more than 10 μm but not more than 80 μm, and the thermally conductive inorganic particles (B3) having a median particle size (D50) of more than 80 μm but not more than 150 μm may each contain two or more types of thermally conductive inorganic particles having different median particle sizes (D50). Use of thermally conductive inorganic particles (B) having such a configuration allows the thermally conductive inorganic particles (B) to be closely packed in the thermally conductive silicone resin composition, thereby increasing the thermal conductivity of the thermally conductive silicone resin composition. For example, the thermally conductive inorganic particles (B1) preferably contain two or more types of thermally conductive inorganic particles having different median particle sizes (D50). Specifically, the thermally conductive inorganic particles (B1) preferably include thermally conductive inorganic particles (B1-1) having a median particle size (D50) of 0.01 μm or more and less than 1 μm and thermally conductive inorganic particles (B1-2) having a median particle size (D50) of 1 μm or more and 10 μm or less, more preferably thermally conductive inorganic particles (B1-1) having a median particle size (D50) of 0.05 μm or more and less than 1 μm and thermally conductive inorganic particles (B1-2) having a median particle size (D50) of 1 μm or more and 8 μm or less, and even more preferably thermally conductive inorganic particles (B1-1) having a median particle size (D50) of 0.1 μm or more and less than 1 μm and thermally conductive inorganic particles (B1-2) having a median particle size (D50) of 1 μm or more and 5 μm or less. By using thermally conductive inorganic particles (B) having such a configuration, the thermally conductive inorganic particles (B) can be closest packed in the thermally conductive silicone resin composition, and as a result, the thermal conductivity of the thermally conductive silicone resin composition can be increased. When the thermally conductive inorganic particles (B1) contain the thermally conductive inorganic particles (B1-1) and the thermally conductive inorganic particles (B1-2), the thermally conductive inorganic particles (B1) preferably contain 50 to 400 parts by mass of the thermally conductive inorganic particles (B1-1) and 50 to 600 parts by mass of the thermally conductive inorganic particles (B1-2) relative to 100 parts by mass of the matrix resin component (A), more preferably contain 50 to 400 parts by mass of the thermally conductive inorganic particles (B1-1) and 100 to 600 parts by mass of the thermally conductive inorganic particles (B1-2), and even more preferably contain 100 to 350 parts by mass of the thermally conductive inorganic particles (B1-1) and 200 to 500 parts by mass of the thermally conductive inorganic particles (B1-2).By using thermally conductive inorganic particles (B) having such a configuration, the thermally conductive inorganic particles (B) can be closest packed in the thermally conductive silicone resin composition, and as a result, the thermal conductivity of the thermally conductive silicone resin composition can be increased.
[0022] A part or all of the thermally conductive inorganic particles (B1) having a median particle size (D50) of 0.01 to 10 μm are represented by the formula RaSi(OR′) 4-a (where R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1). The term "surface treatment" refers to pretreatment before mixing. Surface-treating the thermally conductive inorganic particles (B1) in advance not only facilitates the filling of the thermally conductive inorganic particles (B1) into the matrix resin component (A), but also prevents the adsorption of a curing catalyst (e.g., a platinum-based catalyst) onto the thermally conductive inorganic particles (B1), thereby preventing curing inhibition. This is useful for improving storage stability. Small particles having a D50 (median diameter) of 10 μm or less are particularly prone to adsorbing curing catalysts, so it is preferable to surface-treat thermally conductive inorganic particles having a D50 (median diameter) of 10 μm or less. The term "surface treatment" as used herein includes adsorption as well as covalent bonding. The surface-treated thermally conductive inorganic particles (B1) exhibit good mixability with the matrix resin component (A). The alkoxysilane is preferably added in an amount of 0.01 to 10 parts by mass per 100 parts by mass of the thermally conductive inorganic particles.
[0023] Examples of the alkoxysilane include octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, and dodecyltriethoxysilane. The alkoxysilanes can be used alone or in combination. As a surface treatment agent, an alkoxysilane and a siloxane having a silanol end may be used in combination.
[0024] The content of the thermally conductive inorganic particles (B) is 400 to 3,000 parts by mass, preferably 500 to 2,900 parts by mass, and more preferably 600 to 2,800 parts by mass, per 100 parts by mass of the matrix resin component (A).
[0025] <Thermal Conductive Silicone Resin Composition> The thermally conductive silicone resin composition is produced by mixing the matrix resin component (A), the thermally conductive inorganic particles (B), and, if necessary, other components.
[0026] The thermally conductive silicone resin composition may further contain a compound represented by the formula RaSi(OR') as a viscosity modifier. 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1), and the composition preferably contains 0.1 to 8 parts by mass of an alkoxysilane represented by the formula: (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1). This is because the dischargeability of the thermally conductive silicone resin composition is further improved by this.
[0027] Examples of the alkoxysilane include octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, and dodecyltriethoxysilane. The alkoxysilanes can be used alone or in combination. As a surface treatment agent, an alkoxysilane and a siloxane having a silanol end may be used in combination.
[0028] The thermal conductivity of the thermally conductive silicone resin composition is preferably 1.0 W / m K or more, more preferably 1.0 to 10 W / m K, and even more preferably 1.5 to 9 W / m K. Such a thermally conductive silicone resin composition is suitable as a heat sink, or TIM (Thermal Interface Material), between a heat-generating portion and a heat-dissipating portion of an electronic component or the like.
[0029] The thermally conductive silicone resin composition preferably has an absolute viscosity at 23°C measured with a Brookfield viscometer at a rotation speed of 5 rpm using a T-E spindle in the range of 1,000 to 20,000 Pa·s, more preferably 1,000 to 18,000 Pa·s, and even more preferably 1,000 to 15,000 Pa·s. Such a thermally conductive silicone resin composition has good dischargeability. Furthermore, such a thermally conductive silicone resin composition has excellent workability and is easily injected (dischargeable) or applied between a heat-generating portion and a heat-dissipating portion.
[0030] The thermally conductive silicone resin composition is preferably tested for a heat shock test in which 1.0 g of the composition is placed between two plates, the two plates compressing and sandwiching the composition so that the thickness of the layer made of the composition is 1.0 mm, the plates are placed in a heat shock tester with the main surfaces of the plates perpendicular to the ground, and the test is then repeated for 500 or 100 cycles, with the temperature being held at -40°C for 30 minutes, followed by heating, then holding at 125°C for 30 minutes, and then cooling to -40°C. In this test, the drop of the composition from the start of the test is preferably within 5 mm. This improves drop resistance and reduces dripping. It is even more preferable that the drop of the composition from the start of the test is within 5 mm in both the 500-cycle and 100-cycle heat shock tests.
[0031] The thermally conductive silicone resin composition is filled into a 30 mL syringe and discharged for 9 seconds at a discharge pressure of 0.5 MPa through a discharge hole diameter of 2.5 mm, and the discharge amount is preferably 2 to 10 g, more preferably 2 to 9 g, and even more preferably 2 to 8 g. This allows the thermally conductive silicone resin composition to have high drop resistance and good dischargeability while being less prone to dripping.
[0032] The thermally conductive silicone resin composition of the present invention can be used in the form of grease, putty, or liquid, but is preferably in the form of thermally conductive grease.When the thermally conductive silicone resin composition of the present invention is in the form of thermally conductive grease, the thermally conductive grease is suitable for filling a syringe and applying to a heat sink (TIM) between a heat-generating part and a heat-dissipating part of an electronic component or the like.
[0033] The thermally conductive silicone resin composition of the present invention is in an uncured or non-cured state, and therefore does not require a curing catalyst or curing agent, although these may be added in some cases.
[0034] The thermally conductive silicone resin composition of the present invention can contain other components as needed. For example, a heat resistance improver such as red iron oxide, titanium oxide, or cerium oxide, a flame retardant, or a flame retardant aid may be added to the thermally conductive silicone resin composition. Furthermore, an organic or inorganic particle pigment may be added to the thermally conductive silicone resin composition for the purpose of coloring or toning. An alkoxy group-containing silicone may be added to the thermally conductive silicone resin composition as a material added for the purpose of filler surface treatment, etc.
[0035] The thermally conductive silicone resin composition of the present invention can be filled into dispensers, bottles, cans, tubes, etc. to be made into commercial products.
[0036] The present invention includes the following aspects.
[0037] [Item 1] A thermally conductive silicone resin composition comprising a matrix resin component (A) and thermally conductive inorganic particles (B), wherein the matrix resin component (A) contains, per 100 parts by mass of the matrix resin component (A), 70 to 99 parts by mass of a liquid dimethylpolysiloxane (A1) and 1 to 30 parts by mass of a mixed oil (A2) of polydecene and an ethylene-propylene copolymer, and the liquid dimethylpolysiloxane (A1) has a kinematic viscosity at 40°C of 50 to 10,000 mm 2 / s, and the mixed oil (A2) has a kinematic viscosity at 40°C of 1 to 1,000 mm 2 / s, and the thermally conductive silicone resin composition contains 400 to 3,000 parts by mass of the thermally conductive inorganic particles (B) per 100 parts by mass of the matrix resin component (A).
[0038] [Item 2] The liquid dimethylpolysiloxane (A1) preferably has a kinematic viscosity at 40°C of 60 to 9,000 mm 2 / s, and more preferably 70 to 8,000 mm 2 Item 2. The thermally conductive silicone resin composition according to Item 1, wherein
[0039] [Item 3] The thermally conductive silicone resin composition according to Item 1 or 2, wherein the content of the liquid dimethylpolysiloxane (A1) is preferably 71 to 98 parts by mass, and more preferably 72 to 98 parts by mass, per 100 parts by mass of the matrix resin component (A).
[0040] [Item 4] The kinematic viscosity of the mixed oil (A2) at 40°C is preferably 5 to 900 mm 2 / s, and more preferably 10 to 800 mm 2 Item 4. The thermally conductive silicone resin composition according to any one of Items 1 to 3, wherein
[0041] [Item 5] The thermally conductive silicone resin composition according to any one of Items 1 to 4, wherein the content of the mixed oil (A2) is preferably 2 to 29 parts by mass, and more preferably 3 to 28 parts by mass, per 100 parts by mass of the matrix resin component (A).
[0042] [Item 6] The thermally conductive silicone resin composition according to any one of Items 1 to 5, preferably containing 30 to 99 mass% of polydecene and 1 to 70 mass% of an ethylene-propylene copolymer, more preferably 35 to 95 mass% of polydecene and 5 to 65 mass% of an ethylene-propylene copolymer, and even more preferably 40 to 90 mass% of polydecene and 10 to 60 mass% of an ethylene-propylene copolymer, relative to 100 mass% of the mixed oil (A2).
[0043] [Item 7] Further, the formula RaSi(OR′) 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1).
[0044] [Item 8] The thermally conductive silicone resin composition according to any one of Items 1 to 7, wherein the alkoxysilane is at least one selected from the group consisting of octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, and dodecyltriethoxysilane.
[0045] [Item 9] The thermally conductive silicone resin composition according to any one of Items 1 to 8, wherein the thermally conductive inorganic particles (B) comprise: thermally conductive inorganic particles (B1) having a median particle size (D50) of 0.01 to 10 μm; thermally conductive inorganic particles (B2) having a median particle size (D50) of more than 10 μm and not more than 80 μm; and thermally conductive inorganic particles (B3) having a median particle size (D50) of more than 80 μm and not more than 150 μm.
[0046] [Item 10] The thermally conductive silicone resin composition according to any one of Items 1 to 9, wherein the thermally conductive inorganic particles (B1) are preferably amorphous alumina.
[0047] [Item 11] The thermally conductive silicone resin composition according to any one of Items 1 to 10, wherein the thermally conductive inorganic particles (B2) are preferably at least one inorganic particle selected from the group consisting of alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, aluminum hydroxide, and silicon carbide, and more preferably amorphous aluminum nitride.
[0048] [Item 12] The thermally conductive silicone resin composition according to any one of Items 1 to 11, wherein the thermally conductive inorganic particles (B3) are preferably spherical alumina.
[0049] [Item 13] The thermally conductive silicone resin composition according to any one of Items 9 to 12, wherein the mass ratios of the thermally conductive inorganic particles (B1), (B2), and (B3) are expressed as (B2)≦(B1)≦(B3).
[0050] [Item 14] A part or all of the thermally conductive inorganic particles (B1) are represented by the formula RaSi(OR') 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1).
[0051] [Item 15] The thermally conductive silicone resin composition according to any one of Items 9 to 14, wherein the alkoxysilane is at least one selected from the group consisting of octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, and dodecyltriethoxysilane.
[0052] [Item 16] The thermally conductive silicone resin composition according to any one of Items 9 to 15, wherein the thermally conductive inorganic particles (B) contain preferably 100 to 1,000 parts by mass, more preferably 150 to 1,000 parts by mass, and even more preferably 300 to 850 parts by mass of the thermally conductive inorganic particles (B1) per 100 parts by mass of the matrix resin component (A).
[0053] [Item 17] The thermally conductive silicone resin composition according to any one of Items 9 to 16, wherein the thermally conductive inorganic particles (B) contain preferably 100 to 500 parts by mass, more preferably 150 to 500 parts by mass, and even more preferably 200 to 450 parts by mass of the thermally conductive inorganic particles (B2) per 100 parts by mass of the matrix resin component (A).
[0054] [Item 18] The thermally conductive silicone resin composition according to any one of Items 9 to 17, wherein the thermally conductive inorganic particles (B) contain preferably 300 to 1,400 parts by mass, more preferably 300 to 1,300 parts by mass, and even more preferably 500 to 1,200 parts by mass of the thermally conductive inorganic particles (B3) per 100 parts by mass of the matrix resin component (A).
[0055] [Item 19] The thermally conductive silicone resin composition according to any one of Items 9 to 18, wherein the thermally conductive inorganic particles (B1) preferably contain two or more types of thermally conductive inorganic particles having different median particle sizes (D50).
[0056] [Item 20] The thermally conductive inorganic particles (B1) preferably comprise thermally conductive inorganic particles (B1-1) having a median particle size (D50) of 0.01 μm or more and less than 1 μm and thermally conductive inorganic particles (B1-2) having a median particle size (D50) of 1 μm or more and 10 μm or less, more preferably thermally conductive inorganic particles (B1-1) having a median particle size (D50) of 0.05 μm or more and less than 1 μm and thermally conductive inorganic particles (B1-2) having a median particle size (D50) of 1 μm or more and 8 μm or less, and even more preferably thermally conductive inorganic particles (B1-1) having a median particle size (D50) of 0.1 μm or more and less than 1 μm and thermally conductive inorganic particles (B1-2) having a median particle size (D50) of 1 μm or more and 5 μm or less.
[0057] [Item 21] The thermally conductive silicone resin composition according to Item 20, wherein the thermally conductive inorganic particles (B1) preferably contain 50 to 400 parts by mass of the thermally conductive inorganic particles (B1-1) and 50 to 600 parts by mass of the thermally conductive inorganic particles (B1-2) relative to 100 parts by mass of the matrix resin component (A), more preferably contain 50 to 400 parts by mass of the thermally conductive inorganic particles (B1-1) and 100 to 600 parts by mass of the thermally conductive inorganic particles (B1-2), and even more preferably contain 100 to 350 parts by mass of the thermally conductive inorganic particles (B1-1) and 200 to 500 parts by mass of the thermally conductive inorganic particles (B1-2).
[0058] [Item 22] The thermally conductive silicone resin composition according to any one of Items 1 to 21, wherein the content of the thermally conductive inorganic particles (B) is preferably 500 to 2900 parts by mass, and more preferably 600 to 2800 parts by mass, per 100 parts by mass of the matrix resin component (A).
[0059] [Item 23] The thermally conductive silicone resin composition according to any one of Items 1 to 22, wherein the thermal conductivity is preferably 1.0 W / m K or more, more preferably 1.0 to 10 W / m K, and even more preferably 1.5 to 9 W / m K.
[0060] [Item 24] The thermally conductive silicone resin composition according to any one of Items 1 to 23, wherein the absolute viscosity at 23°C measured with a Brookfield viscometer is preferably in the range of 1,000 to 20,000 Pa s, more preferably 1,000 to 18,000 Pa s, and even more preferably 1,000 to 15,000 Pa s.
[0061] [Item 25] The thermally conductive silicone resin composition according to any one of Items 1 to 24, wherein 1.0 g of the thermally conductive silicone resin composition is placed between two plates, the two plates compress and sandwich the thermally conductive silicone resin composition so that the thickness of a layer made of the thermally conductive silicone resin composition is 1.0 mm, and the plates are placed in a heat shock tester so that the main surfaces of the plates are perpendicular to the ground. The heat shock test involves holding the composition at −40° C. for 30 minutes, followed by heating, and then holding the composition at 125° C. for 30 minutes, followed by cooling to −40° C., and performing this cycle for 500 or 100 cycles. In this heat shock test, the thermally conductive silicone resin composition falls within 5 mm from the start of the test, and preferably falls within 5 mm from the start of the heat shock test in both 500 and 100 cycles.
[0062] [Item 26] The thermally conductive silicone resin composition according to any one of Items 1 to 25, wherein the amount of the composition discharged when filled into a 30 mL syringe and discharged for 9 seconds at a discharge hole diameter of 2.5 mm and a discharge pressure of 0.5 MPa is preferably 2 to 10 g, more preferably 2 to 9 g, and even more preferably 2 to 8 g.
[0063] [Item 27] The thermally conductive silicone resin composition according to any one of Items 1 to 26, which is a thermally conductive grease.
[0064] [Item 28] The thermally conductive silicone resin composition according to any one of Items 1 to 27, in an uncured state or a cured state.
[0065] [Examples] The present invention will be described below using examples, but is not limited to these examples. Various parameters were measured by the following methods.
[0066] <Thermal Conductivity> The thermal conductivity of the thermally conductive silicone resin composition was measured using a hot disk (in accordance with ISO 22007-2:2008). As shown in FIG. 1A, this thermal conductivity measuring device 1 sandwiches a polyimide film sensor 2 between two samples 3a and 3b. A constant power is applied to the sensor 2, generating a constant amount of heat, and the thermal characteristics are analyzed from the temperature rise of the sensor 2. The sensor 2 has a 7 mm diameter tip 4 and, as shown in FIG. 1B, has a double spiral electrode structure, with an applied current electrode 5 and a resistance value electrode (temperature measurement electrode) 6 located at the bottom. The measurement sample can be obtained by rolling a degassed thermally conductive liquid composition to a thickness of 7 mm or more. The thermal conductivity is calculated using the following formula (Equation 1):
[0067]
[0068] <Absolute Viscosity of Thermally Conductive Silicone Resin Composition> The absolute viscosity of the thermally conductive silicone resin composition was measured using a Brookfield HBDV2T viscometer. The spindle used was a T-E spindle, and the absolute viscosity was measured at a rotation speed of 5 rpm and 23°C.
[0069] <Drop Test> Measurements were performed using the drop test shown in Figures 2A-D. 1.0 g of thermally conductive silicone resin composition 14 was applied to an aluminum plate 12 measuring 40 mm in length, 100 mm in width, and 5 mm in thickness (Figure 2A). A spacer 13 was interposed between the aluminum plate and a glass plate 11 measuring 40 mm in length, 100 mm in width, and 5 mm in thickness, and the thermally conductive silicone resin composition was compressed and sandwiched to a thickness of 1.0 mm (Figure 2B). In Figure 2B, 15 denotes the thermally conductive silicone resin composition compressed to a thickness of 1.0 mm. Next, the aluminum plate 12 and the glass plate 11 were placed in a heat cycle tester so that their main surfaces were perpendicular to the ground (Figure 2C). In Figure 2C, 16 denotes the test specimen before testing. In this state, a heat cycle test was performed in which the specimen was held at -40°C for 30 minutes, then heated to 125°C, held at 125°C for 30 minutes, and cooled to -40°C, with this cycle being repeated 100 times and 500 times. After 100 and 500 cycles, the specimen was removed and observed to see if the thermally conductive silicone resin composition 15 had fallen. 17 is the specimen after the test (Figure 2D), and 18 is the fall distance.
[0070] Evaluation criteria: A: The thermally conductive silicone resin composition fell a distance of 5 mm or less. B: The thermally conductive silicone resin composition fell a distance of more than 5 mm.
[0071] <Discharge Test> A 30 mL syringe PSY-30F manufactured by Musashi Engineering was filled with the thermally conductive silicone resin composition, and the amount discharged was measured when the composition was discharged for 9 seconds with a discharge hole diameter of 2.5 mm and a discharge pressure of 0.5 MPa.
[0072] (Examples 1 to 3, Comparative Examples 1 to 3) 1. Raw Material Components (1) Matrix Resin Component (A) Liquid dimethylpolysiloxane (A1): having a kinematic viscosity of 110 mm at 40°C 2 / s liquid dimethyl silicone oil, specific gravity 0.97 g / cm 3 , Dow Toray Industries, Inc., product name "SH200CV 110CS"; Polydecene and ethylene-propylene copolymer mixed oil (A2): kinematic viscosity at 40 ° C. 100 mm 2 / s, Mitsui Chemicals, Inc., product name "Lucant" HC-10 (polydecene content 50 to 80 mass%), specific gravity 0.83 g / cm 3 Ethylene-propylene copolymer oil: kinematic viscosity at 40°C of 200 mm 2 / s, Mitsui Chemicals, Inc., product name "Lucant" HC-20, specific gravity 0.83 g / cm 3
[0073] (2) Thermally conductive inorganic particles (B) Irregular shaped alumina (B1) (Fig. 3) with a median particle size of 0.3 µm (D50 = 0.3 µm): octyltrimethoxysilane pretreated product (2.4 g of octyltrimethoxysilane was adsorbed to 100 g of alumina), specific gravity 3.98 g / cm 3 Irregular shaped alumina (B1) (FIG. 4) with a median particle size of 2.3 μm (D50 = 2.3 μm): decyltrimethoxysilane pre-treated product (1.1 g of decyltrimethoxysilane was adsorbed to 100 g of alumina), specific gravity 3.98 g / cm 3 - Irregular shaped aluminum nitride (B2) (Fig. 5) with a central particle size of 15 μm (D50 = 15 μm) (no surface treatment), specific gravity 3.26 g / cm 3 Spherical alumina (B3) (Fig. 6) (no surface treatment) with a central particle size of 105 μm (D50 = 105 μm), specific gravity 3.98 g / cm 3 The blending amounts are shown in Table 1.
[0074] (3) Viscosity modifier (C) Decyltrimethoxysilane, specific gravity 0.90 g / cm 3 2. Mixing Method A thermally conductive silicone resin composition was produced by mixing the thermally conductive inorganic particles (B) and viscosity modifier with the matrix resin component (A) to obtain the composition shown in Table 1 below. The thermally conductive silicone resin composition obtained in this manner was evaluated. The composition and results are summarized in Table 1 below.
[0075]
[0076] The above results reveal the following: (1) Example 1 has better dischargeability than Comparative Example 2. (2) Example 2 has better dischargeability than Comparative Example 3 and does not fall even after 500 cycles of drop test. (3) Example 3, which contains a small amount of mixed oil (A2), also exhibits drop resistance. (4) Comparative Example 1, which does not contain mixed oil (A2), shows poor drop test results. (5) Comparative Example 2, which contains an ethylene-propylene copolymer oil instead of mixed oil (A2), shows good drop test results but poor dischargeability compared to Example 1. (6) Comparative Example 3, which contains a reduced amount of ethylene-propylene copolymer oil, shows poor drop test results. (7) Overall, it was confirmed that Examples 1 to 3 can provide thermally conductive silicone resin compositions that have high thermal conductivity, are relatively resistant to dripping, and have good dischargeability compared to Comparative Examples 1 to 3.
[0077] The thermally conductive silicone resin composition of the present invention is suitable for use between a heat-generating portion of an electric or electronic part and a heat sink.
[0078] DESCRIPTION OF SYMBOLS 1 Thermal conductivity measuring device 2 Sensors 3a, 3b Sample 4 Sensor tip 5 Electrode for applied current 6 Electrode for resistance value (electrode for temperature measurement) 11 Glass plate 12 Aluminum plate 13 Spacer 14 Thermally conductive silicone resin composition 15 Compressed thermally conductive silicone resin composition 16 Test piece before test 17 Test piece after test 18 Fall distance
Claims
1. A thermally conductive silicone resin composition comprising a matrix resin component (A) and thermally conductive inorganic particles (B), wherein the matrix resin component (A) comprises, per 100 parts by mass of the matrix resin component (A), 70 to 99 parts by mass of liquid dimethylpolysiloxane (A1) and 1 to 30 parts by mass of a mixed oil (A2) of polydecene and an ethylene-propylene copolymer, and the liquid dimethylpolysiloxane (A1) has a kinetic viscosity at 40°C of 50 to 10,000 mm 2 / s, and the mixed oil (A2) has a kinetic viscosity at 40° C. of 1 to 1,000 mm 2 / s, and the thermally conductive silicone resin composition contains 400 to 3,000 parts by mass of the thermally conductive inorganic particles (B) per 100 parts by mass of the matrix resin component (A).
2. The thermally conductive silicone resin composition according to claim 1, which contains 30 to 99 mass % of polydecene and 1 to 70 mass % of an ethylene-propylene copolymer relative to 100 mass % of the mixed oil (A2).
3. The thermally conductive resin composition further comprises a compound represented by the formula RaSi(OR') 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1).
4. The thermally conductive silicone resin composition according to any one of claims 1 to 3, wherein the thermally conductive inorganic particles (B) comprise: thermally conductive inorganic particles (B1) having a median particle size (D50) of 0.01 to 10 μm; thermally conductive inorganic particles (B2) having a median particle size (D50) of more than 10 μm and not more than 80 μm; and thermally conductive inorganic particles (B3) having a median particle size (D50) of more than 80 μm and not more than 150 μm.
5. The thermally conductive silicone resin composition according to claim 4, wherein the mass ratios of the thermally conductive inorganic particles (B1), (B2) and (B3) are expressed as (B2)≦(B1)≦(B3).
6. A part or all of the thermally conductive inorganic particles (B1) are represented by the formula RaSi(OR') 4-a(wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1).
7. The thermally conductive silicone resin composition according to any one of claims 1 to 6, wherein the thermal conductivity of the thermally conductive silicone resin composition is 1.0 W / m·K or more.
8. The thermally conductive silicone resin composition according to any one of claims 1 to 7, wherein the thermally conductive silicone resin composition has an absolute viscosity at 23°C measured with a B-type viscometer in the range of 1,000 to 20,000 Pa·s.
9. The thermally conductive silicone resin composition according to any one of claims 1 to 8, in which 1.0 g of the thermally conductive silicone resin composition is placed between two plates, the two plates compressively hold the thermally conductive silicone resin composition so that the thickness of a layer made of the thermally conductive silicone resin composition is 1.0 mm, and the plates are held in a heat shock tester so that the main surfaces of the plates are perpendicular to the ground. The heat shock test is then performed for 500 cycles, in which the thermally conductive silicone resin composition falls by 5 mm or less from the start of the test.
10. The thermally conductive silicone resin composition according to any one of claims 1 to 9, wherein the amount of the thermally conductive silicone resin composition discharged when filled into a 30 mL syringe and discharged for 9 seconds at a discharge pressure of 0.5 MPa and a discharge hole diameter of 2.5 mm is 2 to 10 g.
11. The thermally conductive silicone resin composition according to any one of claims 1 to 10, which is a thermally conductive grease.
12. The thermally conductive silicone resin composition according to any one of claims 1 to 11, wherein the thermally conductive silicone resin composition is in an uncured state or in a cured state.
Citation Information
Patent Citations
Organosilicone heat conducting adhesive for LED (light-emitting diode) packaging and preparation method thereof
CN107312493A
Anhydrous make-up article or dermatological composition containing combination of silicone oil and wax made of ethylene homopolymer or copolymer
JP1995252130A
Thermal conductor and its production
JP2000345042A
Heat conductive material and manufacture thereof
JP2000353771A
Heat conductive resin formation and its use
JP2002237554A