Metal printing ink composition
The ink composition for metal printing, featuring a rosin-modified resin and polyoxyalkylene alkyl ether solvent, addresses the challenges of repellency and compatibility with water-based overprint varnishes by enhancing transfer properties and compatibility, ensuring effective printing with reduced solvent content.
Patent Information
- Application Number
- PCT/JP2024/009468
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-25
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-31
AI Technical Summary
Metal printing ink compositions face challenges with repellency and reduced quality of the coating film when using water-based overprint varnishes, and there is a trade-off between increasing oil length for better transferability and compatibility with aqueous overprint varnishes.
An ink composition for metal printing that includes a rosin-modified resin with a hydroxyl value of 10 mgKOH/g or more, along with a polyoxyalkylene alkyl ether solvent, and optionally hydrophilic silica particles, to enhance transfer properties and compatibility with water-based overprint varnishes without significantly increasing the oil length of the alkyd resin.
The ink composition achieves good transfer properties and suppresses repellency of water-based overprint varnishes, maintaining high transferability even with reduced solvent content, and supports the use of water-based overprint varnishes in a wet-on-wet application.
Smart Images

Figure JP2024009468_31102024_PF_FP_ABST
Abstract
Description
Metal printing ink composition
[0001] The present invention relates to an ink composition for metal printing.
[0002] For printing on the outer metal surfaces of metal materials, such as galvanized or tinned iron sheets, aluminum sheets, or metal cans made from these metal materials, metal printing ink compositions are used, the main vehicle components of which are binder resins such as alkyd resins, polyester resins, and epoxy resins, and organic solvents such as mineral oils or higher alcohols.
[0003] Furthermore, these printing surfaces are generally coated with an overprint varnish to improve the ink film's adhesion, bending resistance, impact resistance, abrasion resistance, etc. These overprint varnishes are commonly solvent-based varnishes that contain binder resins such as alkyd resins, polyester resins, acrylic resins, and epoxy resins, hardeners such as melamine resins and benzoguanamine resins, and organic solvents such as mineral oils and cellosolves.
[0004] When printing on the outer surface of a metal, ink is printed using an offset printing machine, dry offset printing machine, or the like, and then an overprint varnish is applied wet-on-wet onto the ink coating using a coater or the like, and then the varnish is baked at 150 to 280°C.
[0005] In recent years, due to concerns about air pollution caused by solvents and concerns about hygiene and safety in the printing environment, it has become common to use water-based overprint varnishes in place of the solvent-based overprint varnishes that have traditionally been used, even in the field of metal printing. However, when a water-based overprint varnish is applied to an ink film made from a conventional ink composition for metal printing, problems such as the repelling of the water-based overprint varnish or its penetration into the ink film occur, resulting in a significant decrease in the quality of the coating, such as gloss or adhesion. Therefore, ink compositions have been required to have excellent suitability for water-based overprint varnishes.
[0006] As methods for improving suitability for such aqueous overprint varnishes, for example, Patent Document 1 proposes the use of an alkylene glycol-based solvent having 4 to 8 carbon atoms, Patent Document 2 proposes the use of a polyoxyalkylene glycol-based solvent, Patent Document 3 proposes the use of a polyoxyalkylene alkyl ether-based organic solvent, and Patent Document 4 proposes the use of a polyoxyalkylene alkyl ester-based solvent. Although the organic solvents used in these ink compositions are effective in improving the suitability of the ink composition for aqueous overprint varnishes, there is still room for improvement in that the ink composition tends to have insufficient fluidity and tends to misting during printing.
[0007] When attempting to improve the fluidity of ink compositions for metal printing or misting during printing, one method is to use a solvent with low polarity, such as a high-boiling-point aromatic hydrocarbon, as described in the examples of Patent Document 5. However, in recent years, with the aim of further reducing the environmental load, aqueous overprint varnish products in which the solvent content has been reduced to the minimum have been on the market, and when such overprint varnishes are used, there is also the problem of cissing occurring with ink compositions that use solvents with low polarity.
[0008] Furthermore, in recent years, efforts have been made to increase printing speeds in metal printing in order to improve productivity. To accommodate these increased printing speeds, the transferability of ink compositions is important. Increasing the oil length of the alkyd resin contained in the ink composition is considered effective in ensuring the transferability of the ink composition. However, ink compositions containing alkyd resins with long oil lengths tend to be less compatible with the above-mentioned aqueous overprint varnish, which can easily cause the problem of cissing of the aqueous overprint varnish on the surface of the printed ink composition. In other words, there is a trade-off between increasing the oil length based on transferability and the coatability of the aqueous overprint varnish, which has been a technical challenge.
[0009] Japanese Patent Publication No. 5-75031 Japanese Patent Publication No. 5-40791 Japanese Patent Publication No. 5-40792 Japanese Patent Application Laid-Open No. 64-60670 Japanese Patent Application Laid-Open No. 2009-249435
[0010] The present invention has been made in view of the above circumstances, and aims to provide an ink composition for metal printing that can achieve good transferability during printing without excessively increasing the oil length of the alkyd resin.
[0011] As a result of extensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by using an ink composition containing, as at least a part of the resin contained in the ink composition, both a rosin-modified resin having a hydroxyl value of 10 mgKOH / g or more and a polyoxyalkylene alkyl ether solvent represented by the following general formula (1), and have thus completed the present invention. Specifically, the present invention provides the following.
[0012] (1) The present invention is an ink composition for metal printing comprising a color pigment, a resin, and a solvent, wherein at least a portion of the resin comprises a rosin-modified resin having a hydroxyl value of 10 mg KOH / g or more, and the solvent comprises at least one compound selected from the group consisting of compounds represented by the following general formula (1): (In the above general formula (1), each A is independently an alkylene group having 2 to 4 carbon atoms which may have a branch; R is an alkyl group having 1 to 13 carbon atoms which may have a branched and / or cyclic structure; and n is an integer of 2 to 8.)
[0013] (2) The present invention also provides the ink composition for metal printing according to (1), further comprising 1 to 8% by mass of hydrophilic silica particles.
[0014] (3) The present invention also provides the ink composition for metal printing according to item (1) or (2), wherein the rosin-modified resin has an acid value of 100 mg KOH / g or less.
[0015] (4) The present invention also provides an ink composition for metal printing according to any one of (1) to (3), characterized in that when 70 g of the rosin-modified resin is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130°C with stirring for 60 minutes, it gives a dissolved varnish having an n-hexane tolerance of more than 50 g / 5 g, as measured by the following procedure: After allowing the dissolved varnish to cool to room temperature, 5 g is placed in a beaker. While maintaining the liquid temperature in the beaker at 25°C, n-hexane is added to the dissolved varnish in the beaker in small amounts while stirring, and the mass (g) of n-hexane required until the liquid in the beaker begins to become cloudy is determined. The mass (g) of n-hexane thus determined is defined as the n-hexane tolerance (g / 5 g).
[0016] (5) The present invention also provides an ink composition for metal printing according to any one of (1) to (4), wherein the rosin-modified resin is a rosin ester resin.
[0017] According to the present invention, there is provided an ink composition for metal printing that can achieve good transferability during printing without excessively increasing the oil length of the alkyd resin.
[0018] An embodiment of the ink composition for metal printing of the present invention will be described below. Note that the present invention is not limited to the following embodiment, and can be practiced by making appropriate modifications within the scope of the present invention.
[0019] The ink composition of the present invention is for metal printing and is preferably applied to printing using a so-called dry offset printing method that uses a relief plate as the printing plate, or an offset printing method that uses a lithographic plate as the printing plate, but can also be applied to general printing methods commonly used in metal printing. Furthermore, the ink composition of the present invention can suppress cissing of an aqueous overprint varnish (OP varnish) even when the OP varnish is applied wet-on-wet immediately after printing with the ink composition. Therefore, it is not only preferably applied to two-piece can printing, which employs such printing and coating methods, but also to three-piece can printing. The ink composition of the present invention can maintain good transferability even in cases where a high pigment content is required, such as in a white ink composition. Furthermore, the ink composition of the present invention can achieve good transferability during printing without excessively increasing the oil length of the alkyd resin. Therefore, printing can be performed that achieves both suppressed cissing and good transferability during printing, even when an aqueous OP varnish with a reduced solvent content is applied wet-on-wet.
[0020] The ink composition of the present invention is an ink composition for metal printing comprising a color pigment, a resin, and a solvent, characterized in that at least a part of the resin contains a rosin-modified resin having a hydroxyl value of 10 mgKOH / g or more, and the solvent contains at least one compound selected from the group consisting of compounds represented by general formula (1). Each component will be described below.
[0021] [Resin] The ink composition of the present invention contains, at least in part, a rosin-modified resin having a hydroxyl value of 10 mg KOH / g or more. The ink composition of the present invention was completed based on the finding that the inclusion of such a rosin-modified resin with a high hydroxyl value improves the transferability of the ink composition during printing. At the same time, the inclusion of such a rosin-modified resin in the ink composition of the present invention is thought to increase the polarity of the composition itself, thereby increasing its affinity with aqueous OP varnishes, which also have a high polarity, and thereby suppressing repelling even when the ink composition is applied wet-on-wet.
[0022] Rosin-modified resins are resins prepared using rosin as one of the raw materials. Rosin contains a mixture of resin acids, such as abietic acid, palustric acid, isopimaric acid, and levopimaric acid. These resin acids contain hydrophilic, chemically active carboxyl groups, and some also contain conjugated double bonds. Therefore, various rosin-modified resins have been prepared by combining polyhydric alcohols and polybasic acids and subjecting them to condensation polymerization; adding resols, which are condensates of phenols, to the benzene rings contained in the rosin skeleton; or subjecting dienophiles such as maleic anhydride and maleic acid to a Diels-Alder reaction to add maleic acid or maleic anhydride skeletons. Various types of such rosin-modified resins are commercially available, and they can be obtained and used.
[0023] Examples of rosin-modified resins include rosin ester resins, maleated rosin, fumarated rosin resins, rosin-modified maleic acid resins, rosin-modified fumaric acid resins, rosin-modified phenolic resins, rosin-modified alkyd resins, rosin-modified polyester resins, etc. In the present invention, any of the rosin-modified resins may be used, but among these, rosin ester resins are preferably used.
[0024] The hydroxyl value of the rosin-modified resin is 10 mgKOH / g or more, preferably 15 mgKOH / g or more, and more preferably 20 mgKOH / g or more. The upper limit of the hydroxyl value of the rosin-modified resin is not particularly limited, but is, for example, about 200 mgKOH / g, preferably about 150 mgKOH / g, and more preferably about 100 mgKOH / g.
[0025] Furthermore, although not particularly limited, the acid value of the rosin-modified resin is preferably 100 mgKOH / g or less. Having an acid value of 100 mgKOH / g or less is preferable because it can achieve both suppression of repelling when the aqueous OP varnish is applied wet-on-wet and printability such as suppression of misting and smearing. The acid value of the rosin-modified resin is more preferably 80 mgKOH / g or less, and even more preferably 50 mgKOH / g or less.
[0026] The rosin-modified resin is used in the form of a varnish obtained by heating with a solvent described below to dissolve or disperse it. The rosin-modified resin may be used as a dissolved varnish in which it remains dissolved or dispersed in a solvent, or may be used in the form of a gelled varnish obtained by dissolving the resin in the varnish during preparation by adding a divalent or higher metal alkoxy compound as a gelling agent to the dissolved varnish. Among these, preparing a dissolved varnish from the rosin-modified resin and using it to prepare an ink composition is preferred, as it can improve the transferability of the ink composition during printing. Furthermore, preparing a gelled varnish from the rosin-modified resin and using it to prepare an ink composition can impart appropriate viscoelasticity to the ink composition, thereby improving flowability and reducing misting, and also forming a tougher cured coating.
[0027] The content of the rosin-modified resin in the ink composition is preferably 5 to 50 mass% relative to the total composition, more preferably 5 to 25 mass% relative to the total composition, and even more preferably 7 to 20 mass% relative to the total composition.
[0028] The ink composition of the present invention preferably contains an alkyd resin in addition to the rosin-modified resin. Alkyd resins are condensation polymers of polyhydric alcohols and polybasic acids, a type of polyester. They can also be prepared by condensation polymerization with animal and vegetable oils and / or their fatty acids. In this process, the animal and vegetable oils undergo transesterification with the polyhydric alcohol to form fatty acids, which are then incorporated into the alkyd resin structure. The proportion of fatty acids derived from animal and vegetable oils in an alkyd resin is referred to as the oil length, and the oil length of the alkyd resin used in the present invention is preferably 20 to 50% by mass. Oil-free alkyd resins, which do not contain fatty acid components from animal or vegetable oils, may also be used.
[0029] Various alkyd resins can be used in the present invention, but coconut oil-modified alkyd resins are preferred. The use of coconut oil-modified alkyd resins as the alkyd resin is preferred in that it improves the dispersion stability of the ink composition and also provides a high transparency and a good hue.
[0030] As such an alkyd resin, one prepared using phthalic acid (orthophthalic acid) as a polybasic acid and having a phthalic acid skeleton can be preferably used. The use of such an alkyd resin improves ink transferability and further increases the whiteness of white inks.
[0031] The content of the alkyd resin in the ink composition is preferably 10 to 40 mass % relative to the entire composition, more preferably 10 to 30 mass % relative to the entire composition, and even more preferably 15 to 25 mass %.
[0032] In addition to the rosin-modified resin or alkyd resin, the ink composition of the present invention can also contain resins conventionally used in preparing ink compositions for metal printing. That is, depending on the required performance, such as printability and coating properties, known resins compatible with the rosin-modified resin or alkyd resin can be used alone or in combination. Examples of such resins include polyester resins, petroleum resins, epoxy resins, ketone resins, amino resins, and benzoguanamine resins.
[0033] [Solvent] The ink composition of the present invention contains at least one solvent selected from the group consisting of compounds represented by the following general formula (1): Hereinafter, the at least one solvent selected from the group consisting of compounds represented by the following general formula (1) will also be referred to as a specific solvent.
[0034]
[0035] In the general formula (1), each A is independently determined and is an alkylene group having 2 to 4 carbon atoms, which may be branched. Examples of such an alkylene group include an ethylene group [—(CH 2 ) 2 -], propylene group [-CH 2 (CH 3 )-CH 2 - or -CH 2 CH 2 (CH 3 )-], trimethylene group [-(CH 2 ) 3 -], isopropylidene group [-C(CH 3 ) 2 -] and the like.
[0036] In the general formula (1), R is an alkyl group having 1 to 13 carbon atoms, which may have a branched and / or cyclic structure. This alkyl group may be not only an aliphatic group but also an alicyclic group. Examples of such an alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a hexyl group, a 2-ethylhexyl group, an octyl group, a decyl group, and a cyclohexyl group.
[0037] In the above general formula (1), n is an integer of 2 to 8. When n is 2 or more, it is possible to ensure a sufficient boiling point of the specific solvent to provide stability to the ink composition on a printing machine, which is preferable, and when n is 8 or less, it is possible to achieve a viscosity that is preferable as a solvent for the ink composition.
[0038] Examples of the compound represented by the general formula (1) include dipropylene glycol monomethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monooctyl ether, dipropylene glycol tridecyl ether, tripropylene glycol monobutyl ether, tripropylene glycol monodecyl ether, tetrapropylene glycol monohexyl ether, pentapropylene glycol monobutyl ether, and hexapropylene glycol monomethyl ether.
[0039] The content of the specific solvent in the ink composition of the present invention is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, of the entire composition. A content of the specific solvent of 5% by mass or more of the entire composition can enhance the compatibility of the rosin-modified resin in the ink composition and can effectively suppress repelling when an aqueous OP varnish is applied wet-on-wet after printing, which is preferable.
[0040] Here, the above-mentioned rosin-modified resin preferably provides a dissolved varnish with an n-hexane tolerance of greater than 50 g / 5 g when 70 g of the resin is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130°C by stirring for 60 minutes. Since measuring the n-tolerance is not particularly time-consuming, as described below, this selection process does not require excessive trial and error. By using a rosin-modified resin that satisfies these conditions, the compatibility of the rosin-modified resin in the ink composition can be improved, thereby further improving the transferability of the ink composition during printing. Furthermore, the above-mentioned tripropylene glycol monobutyl ether is an ether of tripropylene glycol and butanol formed by the polymerization of three molecules of propylene oxide, and is one of the specific solvents of the present invention.
[0041] Next, the method for measuring the n-hexane tolerance of a resin in the present invention will be described. First, 70 g of the rosin-modified resin to be measured is prepared and dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130°C by stirring for 60 minutes to prepare a dissolved varnish. After allowing the resulting dissolved varnish to cool to room temperature, 5 g is placed in a beaker. With the liquid temperature in the beaker maintained at 25°C, n-hexane is added to the dissolved varnish in the beaker in small amounts while stirring, and the mass (g) of n-hexane required until the liquid in the beaker begins to become cloudy is determined. The mass (g) of n-hexane thus determined is the n-hexane tolerance (g / 5 g). This measurement is so sensitive that adding just one drop of n-hexane to a solution immediately before clouding begins immediately initiates clouding, so measurement errors due to inconsistent judgment of clouding due to differences in the operator are not particularly problematic.
[0042] [Coloring Pigment] The coloring pigment is a component for imparting coloring power to the ink composition. Examples of the coloring pigment include, without particular limitation, organic and / or inorganic pigments that have conventionally been used in printing ink compositions.
[0043] Examples of such color pigments include yellow pigments such as Disazo Yellow (Pigment Yellow 12, Pigment Yellow 13, Pigment Yellow 17, Pigment Yellow 1) and Hansa Yellow; magenta pigments such as Brilliant Carmine 6B, Lake Red C, and Watching Red; cyan pigments such as Phthalocyanine Blue, Phthalocyanine Green, and Alkali Blue; black pigments such as carbon black; white pigments such as titanium oxide; and fluorescent pigments. Metal powder pigments for imparting metallic colors such as gold and silver to the ink composition are also considered to be color pigments in the present invention. Examples of such metal powder pigments include gold powder, bronze powder, aluminum paste prepared by processing aluminum powder into a paste, and mica powder.
[0044] The amount of color pigment added is, for example, about 5 to 50 mass % of the total ink composition, but is not particularly limited. When preparing a yellow ink composition using a yellow pigment, a magenta ink composition using a magenta pigment, a cyan ink composition using a cyan pigment, or a black ink composition using a black pigment, it is also possible to use a pigment of another color in combination or add an ink composition of another color as a complementary color.
[0045] [Other Components] The ink composition of the present invention may contain other components such as known curing agents, pigment dispersants, solvents other than the above-mentioned specific solvents, waxes, silica particles, stabilizers, etc., as needed.
[0046] As the curing agent, for example, an amino resin such as a melamine resin or a benzoguanamine resin can be used.
[0047] Examples of solvents other than the above-mentioned specific solvents include aliphatic hydrocarbons or alicyclic hydrocarbons having a boiling point range of about 230 to 400° C., aromatic hydrocarbons such as alkylbenzenes, and higher alcohols.
[0048] Silica particles are SiO 2These silica particles are commercially available as powders, and are readily available in various forms, including hydrophilic silica particles that have not been surface-treated or that have been hydrophilized, and hydrophobic silica particles that have been hydrophobized. Of these silica particles, hydrophilic silica particles are preferably used in the ink composition of the present invention. The use of hydrophilic silica particles is preferred because it can improve the transferability of the ink composition during printing and increase the fluidity of the ink composition. The content of silica particles in the ink composition is preferably 1 to 8% by mass, and more preferably 2 to 5% by mass.
[0049] The ink composition of the present invention can be prepared by mixing the components such as the color pigment, resin, and solvent including the specific solvent in a conventional manner using a roll mill, ball mill, bead mill, etc. The viscosity of the ink composition is, for example, 10 to 70 Pa s at 25°C as measured by a Raley viscometer, but is not particularly limited.
[0050] The metal for metal printing in the ink composition of the present invention is not particularly limited, but examples thereof include zinc-plated or tin-plated iron sheets, aluminum sheets, and metal cans made of these metal materials.
[0051] Furthermore, the aqueous OP varnish to be applied onto the printed ink composition can be any commonly used one, and specific examples include those that use an aqueous acrylic resin, aqueous polyester resin, aqueous alkyd resin, aqueous epoxy resin, or modified resins of two or more of these as a binder in combination with an amino resin as a curing agent.
[0052] When printing on the surface of a metal material using the ink composition and aqueous OP varnish, first, printing is carried out using the ink composition of the present invention using a dry offset printing machine, an offset printing machine, or the like, and then, while the ink composition is still in a wet-on-wet state, the aqueous OP varnish is overcoated using a coater or the like, and then baking is carried out at 150 to 280°C for several seconds to several minutes.
[0053] The ink composition of the present invention will be explained in more detail below by showing examples, but the present invention is not limited to the following examples in any way.
[0054] [Synthesis of Alkyd Resin] 5.98 parts by weight of neopentyl glycol, 8.53 parts by weight of pentaerythritol, 10.10 parts by weight of coconut oil fatty acid, 11.95 parts by weight of isophthalic acid, and 2.48 parts by weight of terephthalic acid were reacted at 220°C under a nitrogen atmosphere until the acid value of the mixture reached 7 mgKOH / g to perform the first-stage esterification. Then, 0.70 parts by weight of trimellitic anhydride was added and heated at 165°C under a nitrogen atmosphere for 30 minutes to perform the second-stage esterification. These esterification reactions were carried out according to conventional methods to obtain an alkyd resin with a weight-average molecular weight of 15,303 and a number-average molecular weight of 1,484. To this alkyd resin, 21.8 parts by weight of tripropylene glycol monobutyl ether (which corresponds to the above-mentioned specific solvent) and 2.0 parts by weight of triethanolamine were added to obtain an alkyd resin varnish.
[0055] [Preparation of Varnish 1] 61.6 parts by mass of rosin ester resin (hydroxyl value 40-50 mgKOH / g, acid value 10-20 mgKOH / g, weight-average molecular weight 744, number-average molecular weight 701) and 35.9 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, and 2.5 parts by mass of aluminum ethyl acetoacetate diisopropylate was added and heated at 130°C for 30 minutes to obtain Varnish 1. This Varnish 1 is a gelled varnish containing a rosin ester resin (hydroxyl value 40-50 mgKOH / g). The n-hexane tolerance of the rosin ester resin used to prepare Varnish 1 was determined using the procedure specified in the present invention and was found to be 50<g / 5g.
[0056] [Preparation of Varnish 2] 63.2 parts by mass of a rosin ester resin (hydroxyl value 20 to 30 mgKOH / g, acid value <10 mgKOH / g, weight average molecular weight 632, number average molecular weight 565) and 36.8 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, thereby obtaining Varnish 2. This Varnish 2 is a dissolved varnish containing a rosin ester resin (hydroxyl value 20 to 30 mgKOH / g). The n-hexane tolerance of the rosin ester resin used to prepare Varnish 2 was determined according to the procedure specified in the present invention and was found to be 50 < g / 5 g.
[0057] [Preparation of Varnish 3] 61.4 parts by mass of the same rosin ester resin (hydroxyl value 20 to 30 mgKOH / g, acid value <10 mgKOH / g, weight average molecular weight 632, number average molecular weight 565) used in the preparation of Varnish 2 above and 35.7 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, and then 2.9 parts by mass of aluminum ethyl acetoacetate diisopropylate was added and heated at 130°C for 30 minutes to obtain Varnish 3. Varnish 3 is a gelled varnish prepared using the same rosin ester used in the preparation of Varnish 2 above.
[0058] [Preparation of Varnish 4] 61.4 parts by mass of maleated rosin resin (hydroxyl value ≈ 0 mg KOH / g, acid value 220 mg KOH / g or less, weight average molecular weight 877, number average molecular weight 766) and 35.5 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, and 3.1 parts by mass of aluminum ethyl acetoacetate diisopropylate was added and heated at 130°C for 30 minutes to obtain Varnish 4. This Varnish 4 is a gelled varnish containing maleated rosin resin (hydroxyl value ≈ 0 mg KOH / g). The n-hexane tolerance of the maleated rosin resin used to prepare Varnish 4 was determined according to the procedure specified in the present invention and was found to be 4.9 g / 5 g.
[0059] [Examples 1 to 6, Comparative Example 1] Each ink composition of Examples 1 to 6 and Comparative Example 1 was prepared by mixing the components according to the formulation in Table 1 and kneading the resulting mixture in a three-roll mill. In Table 1, "white pigment" refers to titanium oxide, "hydrophobic silica" refers to surface-hydrophobically treated silica particles (manufactured by Nippon Aerosil Co., Ltd., product name Aerosil R972), "hydrophilic silica" refers to surface-untreated silica particles (manufactured by Tokuyama Corporation, product name Reolosil CP102), "clay" refers to organophilic bentonite (manufactured by BYK, product name CRAYTONE-APA), and "specific solvent" refers to tripropylene glycol monobutyl ether. In Table 1, the numerical values for each blend amount refer to parts by mass.
[0060] [Evaluation of Flowability] For each of the ink compositions of Examples 1 to 6 and Comparative Example 1, the slope measured at 25°C using a spreadmeter in accordance with JIS K5101-6-1:2004 is shown in the "Slope" column of Table 1. Note that a larger slope value means higher flowability of the ink composition.
[0061] [Transferability] The transferability of each of the ink compositions of Examples 1 to 6 and Comparative Example 1 was evaluated by the following procedure. First, 0.15 cc of the ink composition was spread on a blanket (Airtack FS, manufactured by Kinyosha Co., Ltd.) using a 4-section roll of an RI tester (manufactured by Akebono Seisakusho Co., Ltd.), and after leaving it for 10 or 20 minutes, an aluminum plate to be printed was attached to the spread blanket. When pressure was applied, the spread ink composition was visually evaluated to determine whether it was transferred to the aluminum plate and the extent of the transfer. The evaluation criteria were as follows, and the results are shown in the "Transferability Evaluation" column in Table 1. ○: Good transfer even after leaving it for 20 minutes △ to ○: Transfer was slightly insufficient when left for 20 minutes, but good transfer was achieved when left for 10 minutes △: No transfer was achieved when left for 20 minutes, but good transfer was achieved when left for 10 minutes ×: No transfer was achieved even when left for 10 minutes
[0062]
[0063] Comparing the ink compositions of Examples 1 to 6 with the ink composition of Comparative Example 1, it is clear that by using a combination of a rosin-modified resin having a specified hydroxyl value according to the present invention and a specific solvent, it is possible to improve the transferability of the ink composition without changing the oil length of the alkyd resin. Furthermore, comparing Example 1 with Example 2, it is clear that the ink composition using hydrophilic silica particles can maintain higher fluidity than the ink composition using hydrophobic silica particles.
Claims
1. An ink composition for metal printing comprising a color pigment, a resin and a solvent, wherein at least a portion of the resin comprises a rosin-modified resin having a hydroxyl value of 10 mg KOH / g or more, and the solvent comprises at least one compound selected from the group consisting of compounds represented by the following general formula (1): (In the above general formula (1), each A is independently an alkylene group having 2 to 4 carbon atoms which may have a branch, R is an alkyl group having 1 to 13 carbon atoms which may have a branched and / or cyclic structure, and n is an integer of 2 to 8.) 2. The ink composition for metal printing according to claim 1, further comprising 1 to 8% by mass of hydrophilic silica particles.
3. The ink composition for metal printing according to claim 1 or 2, wherein the acid value of the rosin-modified resin is 100 mg KOH / g or less.
4. The ink composition for metal printing according to any one of claims 1 to 3, characterized in that when 70 g of the rosin modified resin is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130°C by stirring for 60 minutes, it gives a dissolved varnish with an n-hexane tolerance of more than 50 g / 5 g, as measured by the following procedure: Procedure: After allowing the dissolved varnish to cool to room temperature, 5 g is placed in a beaker, and while maintaining the liquid temperature in the beaker at 25°C, n-hexane is added to the dissolved varnish in the beaker in small amounts while stirring, and the mass (g) of n-hexane required until the liquid in the beaker begins to become cloudy is determined. The mass (g) of n-hexane thus determined is the n-hexane tolerance (g / 5g).
5. The ink composition for metal printing according to any one of claims 1 to 4, wherein the rosin modified resin is a rosin ester resin.
Citation Information
Patent Citations
Printing ink for metal
JP1989060670A
Automatic register method for parts data base
JP1993040791A
Electronic card arranging book
JP1993040792A
Semiconductor device
JP1993075031A
Printing ink composition for seamless can
JP2009249435A
Cited By
Ink composition for printing on metal
WO2026220666A1