Multilayer ceramic capacitor

The multilayer ceramic capacitor addresses the issue of electrostrictive cracks by reducing voids in the dielectric layers at stress concentration points, improving mechanical strength and capacitance, and enhancing reliability and performance under high voltage and temperature conditions.

WO2024224920A1PCT designated stage expired Publication Date: 2024-10-31MURATA MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012176
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-03-27
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional multilayer ceramic capacitors experience cracks due to electrostriction when high voltage is applied, leading to reduced high-temperature load reliability and moisture resistance, as stress concentration occurs at the ends of the capacitor, making it difficult to screen for effective voltage without compromising screening efficiency.

Method used

The multilayer ceramic capacitor design incorporates a structure with a reduced amount of voids in the dielectric layers at the ends, where electrostrictive stress is concentrated, improving mechanical strength and dielectric constant, thereby reducing crack occurrence and enhancing capacitance.

Benefits of technology

This design effectively suppresses electrostrictive cracks at high voltages, improving the capacitor's reliability and capacitance by minimizing voids at stress concentration points, thus enhancing its performance under high-temperature and moisture conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012176_31102024_PF_FP_ABST
    Figure JP2024012176_31102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide a multilayer ceramic capacitor capable of suppressing occurrence of cracks generated inside a laminate due to electrostriction when a high voltage is applied. [Solution] A multilayer ceramic capacitor according to the present invention has: a laminate formed of an inner layer part that includes a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, that includes a first main surface and a second main surface facing each other in the height direction being the lamination direction of the plurality of dielectric layers, a first lateral surface and a second lateral surface facing each other in the width direction orthogonal to the height direction, and a first end surface and a second end surface facing each other in the length direction orthogonal to the height direction and the width direction, and that is obtained by alternately laminating the dielectric layers and the internal electrode layers, and an outer layer part disposed so as to sandwich the inner layer part from the first main surface side and the second main surface side; a first external electrode disposed on the first end surface; and a second external electrode disposed on the second end surface. The inner layer part is formed of inner dielectric layers among the plurality of dielectric layers disposed in the inner layer part. The inner dielectric layers contain voids. The inner dielectric layers have a width-direction center part-side dielectric layer disposed in a region of a center part in the width direction of the inner layer part, and a width-direction end part-side dielectric layer disposed in a region of an end part in the width direction of the inner layer part. The amount of voids contained in the width-direction end part-side dielectric layer is less than the amount of voids in the width-direction center part-side dielectric layer.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer ceramic capacitors

[0001] The present invention relates to a multilayer ceramic capacitor.

[0002] Conventionally, multilayer ceramic capacitors are constructed with a capacitor body made of a sintered ceramic body made of a dielectric such as barium titanate, and internal electrodes made of a noble metal material such as Ag or an Ag-Pd alloy or a base metal material such as Ni are disposed inside the capacitor body via ceramic layers (dielectric layers) so as to extend alternately from one end face to the other end face. The internal electrodes at one potential are electrically connected to an external electrode, and the internal electrodes at the other potential are electrically connected to an external electrode (see Patent Document 1).

[0003] The multilayer ceramic capacitor described in Patent Document 1 has internal electrodes made of a metal material and external electrodes made of a glass component and multiple metal components, including the same metal as the internal electrodes or a metal that can be alloyed with the internal electrodes, and is characterized in that the external electrodes are bonded to a wiring substrate via a conductive resin adhesive, and the area occupancy rate (porosity) of the metal components relative to the cross-sectional area of ​​the external electrodes is 60 to 95%. This allows the multilayer ceramic capacitor to be mounted on a wiring substrate inexpensively and with high reliability without using solder.

[0004] Japanese Patent Application Laid-Open No. 2001-237137

[0005] However, in multilayer ceramic capacitors with a general structure such as that described in Patent Document 1, electrostriction occurs when voltage is applied. Stress due to this electrostriction is concentrated at the ends of the effective portion in the length and width directions of the multilayer ceramic capacitor, and at a position halfway in the height direction. When a high voltage is applied, cracks occur starting from the aforementioned points of stress concentration. Although electrostrictive cracks are difficult to screen, they lead to deterioration in high-temperature load reliability and moisture resistance, and therefore pose a risk of becoming a problem in the market.

[0006] There are several methods to reduce cracks caused by electrostriction, but a typical countermeasure is to set the applied voltage during screening low so that electrostriction does not occur. If the voltage that generates electrostriction is low, the voltage required for screening cannot be applied, which reduces the screening effect.

[0007] SUMMARY OF THE INVENTION Therefore, a primary object of the present invention is to provide a multilayer ceramic capacitor that can suppress the occurrence of cracks inside the laminate due to electrostriction when a high voltage is applied.

[0008] The multilayer ceramic capacitor according to the present invention includes a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, and includes first and second main surfaces that face each other in a height direction, which is the lamination direction of the plurality of dielectric layers, first and second side surfaces that face each other in a width direction perpendicular to the height direction, and first and second end surfaces that face each other in a length direction perpendicular to the height direction and the width direction, and includes a laminate including inner layer portions formed by alternately laminating dielectric layers and internal electrode layers, and outer layer portions arranged to sandwich the inner layer portions from the first and second main surface sides; and and a second external electrode disposed on the second end face, wherein the inner layer portion is constituted by an inner dielectric layer among a plurality of dielectric layers disposed in the inner layer portion, the inner dielectric layer containing voids, the inner dielectric layer having a widthwise center side dielectric layer disposed in a widthwise center region of the inner layer portion, and a widthwise end side dielectric layer disposed in a widthwise end region of the inner layer portion, and the amount of voids contained in the widthwise end side dielectric layer is smaller than the amount of voids in the widthwise center side dielectric layer.

[0009] When voids exist in the dielectric layer, the mechanical strength is lower than in the region where the dielectric layer is filled with ceramic. Therefore, if voids exist in areas where electrostrictive stress is concentrated, electrostrictive cracks will occur in the dielectric layer, originating from the voids. Electrostriction is likely to occur at the widthwise ends of the dielectric layers present in the inner layer portion of the laminate. According to the multilayer ceramic capacitor of the present invention, the amount of voids near the widthwise ends of the dielectric layers present in the inner layer portion of the laminate, where electrostrictive stress is concentrated, is reduced compared to the widthwise center, thereby reducing the occurrence of electrostrictive cracks. Furthermore, reducing the amount of voids in the dielectric layers at the widthwise ends improves the sinterability of the ceramic, and the dielectric constant ε at the widthwise ends improves, thereby improving the capacitance.

[0010] According to the present invention, it is possible to provide a multilayer ceramic capacitor that can suppress the occurrence of cracks inside the laminate due to electrostriction when a high voltage is applied.

[0011] The above and other objects, features and advantages of the present invention will become more apparent from the following detailed description of the preferred embodiments of the present invention, which proceeds with reference to the accompanying drawings.

[0012] 1A and 1B are perspective views showing an example of a multilayer ceramic capacitor according to an embodiment of the present invention. A cross-sectional view taken along line II-II in FIG. 1. A cross-sectional view taken along line III-III in FIG. 1. (a) is a cross-sectional view schematically showing an internal dielectric layer taken along line II-II in FIG. 1, and (b) is a cross-sectional view schematically showing an internal dielectric layer taken along line III-III in FIG. 1. (a) is a cross-sectional view taken along line III-III in FIG. 1 showing a structure in which opposing electrode portions of internal electrode layers of a multilayer ceramic capacitor according to an embodiment of the present invention are divided into two. (b) is a cross-sectional view taken along line III-III in FIG. 1 showing a structure in which opposing electrode portions of internal electrode layers of a multilayer ceramic capacitor according to an embodiment of the present invention are divided into three. (c) is a cross-sectional view taken along line III-III in FIG. 1 showing a structure in which opposing electrode portions of internal electrode layers of a multilayer ceramic capacitor according to an embodiment of the present invention are divided into four.

[0013] 1. Multilayer Ceramic Capacitor A multilayer ceramic capacitor according to an embodiment of the present invention will be described.

[0014] Fig. 1 is an external perspective view showing an example of a multilayer ceramic capacitor according to an embodiment of the present invention. Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1. Fig. 3 is a cross-sectional view taken along line III-III in Fig. 1. Fig. 4(a) is a cross-sectional view schematically showing an internal dielectric layer taken along line II-II in Fig. 1, and Fig. 4(b) is a cross-sectional view schematically showing an internal dielectric layer taken along line III-III in Fig. 1.

[0015] As shown in FIGS. 1 to 3, the multilayer ceramic capacitor 10 includes a rectangular parallelepiped laminate 12 and external electrodes 30 disposed on both ends of the laminate 12 .

[0016] The laminate 12 has a plurality of stacked dielectric layers 14 and a plurality of internal electrode layers 20 stacked on the dielectric layers 14. The laminate 12 further has a first main surface 12a and a second main surface 12b facing in a height direction x, a first side surface 12c and a second side surface 12d facing in a width direction y perpendicular to the height direction x, and a first end surface 12e and a second end surface 12f facing in a length direction z perpendicular to the height direction x and the width direction y. The corners and ridges of the laminate 12 are rounded.

[0017] The corners refer to the intersections of three adjacent faces of the laminate 12, and the ridges refer to the intersections of two adjacent faces of the laminate 12. The term "rectangular parallelepiped" refers to any component having a first main surface 12a and a second main surface 12b, a first side surface 12c and a second side surface 12d, and a first end surface 12e and a second end surface 12f. Furthermore, unevenness may be formed on part or all of the first main surface 12a and the second main surface 12b, the first side surface 12c and the second side surface 12d, and the first end surface 12e and the second end surface 12f. The dielectric layers 14 and the internal electrode layers 20 are stacked in the height direction x.

[0018] As shown in Figures 2 and 3, the laminate 12 has an inner layer portion 16 formed by alternately stacking dielectric layers 14 and internal electrode layers 20 in a height direction x connecting the first main surface 12a and the second main surface 12b, a first outer layer portion 18a formed from a plurality of dielectric layers 14 located between the first main surface 12a and the internal electrode layer 20 located closest to the first main surface 12a, and a second outer layer portion 18b formed from a plurality of dielectric layers 14 located between the second main surface 12b and the internal electrode layer 20 located closest to the second main surface 12b.

[0019] The internal layer portion 16 is constituted by a plurality of internal dielectric layers 14a among the plurality of dielectric layers 14. That is, the internal layer portion 16 is arranged such that the plurality of internal electrode layers 20 face each other with the internal dielectric layers 14a interposed therebetween. Voids are contained inside the internal dielectric layers 14a.

[0020] As shown in Fig. 4(a), the internal dielectric layer 14a has a widthwise center side dielectric layer 14a1 arranged in a central region in the width direction y of the internal layer portion 16, and widthwise end side dielectric layers 14a2 arranged in end regions in the width direction y of the internal layer portion 16. The amount of voids contained in the widthwise end side dielectric layer 14a2 is smaller than the amount of voids contained in the widthwise center side dielectric layer 14a1. Note that the internal electrode layers 20 are not shown in Fig. 4(a).

[0021] It is preferable that the difference between the area occupancy of voids PCW in the WT cross section of the widthwise center side dielectric layer 14a1 and the area occupancy of voids PEW in the WT cross section of the widthwise end side dielectric layer 14a2 be 1.0% or more and 8.0% or less.

[0022] The regions WA in which the amount of voids in the widthwise end-side dielectric layers 14a2 is smaller than the amount of voids in the widthwise center-side dielectric layers 14a1 are located inward in the widthwise direction y from both ends in the widthwise direction y of the inner layer portion 16. The dimension w1 in the widthwise direction y of the region WA in which the amount of voids in the widthwise end-side dielectric layers 14a2 is smaller than the amount of voids in the widthwise center-side dielectric layers 14a1 is preferably 15% or less of the dimension w0 in the widthwise direction y of the inner layer portion 16.

[0023] 4(b), the internal dielectric layer 14a further includes a longitudinal center side dielectric layer 14a3 disposed in a central region in the longitudinal direction z of the internal layer portion 16, and a longitudinal end side dielectric layer 14a4 disposed in an end region in the longitudinal direction z of the internal layer portion 16. The amount of voids contained in the longitudinal end side dielectric layer 14a4 is preferably smaller than the amount of voids contained in the longitudinal center side dielectric layer 14a3. Note that the internal electrode layer 20 is not shown in FIG.

[0024] It is preferable that the difference between the area occupancy rate PCL of the voids in the LT cross section of the longitudinal center side dielectric layer 14a3 and the area occupancy rate PEL of the voids in the LT cross section of the longitudinal end side dielectric layer 14a4 be 4.0% or more and 8.0% or less.

[0025] The regions LA in which the amount of voids in the longitudinal end side dielectric layers 14a4 is smaller than the amount of voids in the longitudinal center side dielectric layers 14a3 are located in regions in the longitudinal direction z from both ends in the longitudinal direction z of the inner layer portion 16. The dimension l1 in the longitudinal direction z of the regions LA in which the amount of voids in the longitudinal end side dielectric layers 14a4 is smaller than the amount of voids in the longitudinal center side dielectric layers 14a3 is preferably 10% or less of the dimension l0 in the longitudinal direction z of the inner layer portion 16.

[0026] The voids are measured as follows: a cross-sectional image of the laminate 12 is obtained using a scanning electron microscope (SEM), and the ceramic filling portions and voids are binarized. The ratio of the area occupied by the voids to the total area of ​​the binarized image is then taken as the void ratio.

[0027] The first outer layer portion 18a is located on the first main surface 12a side of the laminate 12, and is an aggregate of a plurality of outer dielectric layers 14b which are a plurality of dielectric layers 14 located between the first main surface 12a and the internal electrode layer 20 closest to the first main surface 12a. The second outer layer portion 18b is located on the second main surface 12b side of the laminate 12, and is an aggregate of a plurality of outer dielectric layers 14b which are a plurality of dielectric layers 14 located between the second main surface 12b and the internal electrode layer 20 closest to the second main surface 12b. The region sandwiched between the first outer layer portion 18a and the second outer layer portion 18b is the inner layer portion 16.

[0028] The dimensions of the laminate 12 are not particularly limited, but it is preferable that the dimension in the length direction z is 0.95 mm or more and 3.1 mm or less, the dimension in the width direction y is 0.49 mm or more and 2.47 mm or less, and the dimension in the height direction x is 0.49 mm or more and 2.47 mm or less.

[0029] The dielectric layer 14 can be formed of, for example, a dielectric material. Examples of the dielectric material that can be used include dielectric ceramics containing, as a main component, BaTiO3, CaTiO3, SrTiO3, or CaZrO3. When the dielectric material is the main component, a secondary component such as a manganese compound, an iron compound, a chromium compound, a cobalt compound, or a nickel compound may be added in a smaller amount than the main component, depending on the desired characteristics of the laminate 12.

[0030] The thickness of the dielectric layer 14 after firing is preferably 0.5 μm or more and 10 μm or less.

[0031] The number of dielectric layers 14 to be stacked is preferably 50 or more and 1000 or less.

[0032] The first internal electrode layer 20a is disposed on the plurality of dielectric layers 14 and is located inside the laminate 12. The first internal electrode layer 20a has a first opposing electrode portion 22a facing the second internal electrode layer 20b and a first lead electrode portion 24a located on one end side of the first internal electrode layer 20a and extending from the first opposing electrode portion 22a to the first end face 12e of the laminate 12. The end of the first lead electrode portion 24a is extended to the surface of the first end face 12e and exposed from the laminate 12. In other words, the end of the first lead electrode portion 24a is not exposed on the first main surface 12a, the second main surface 12b, the second end face 12f, or the first side face 12c and the second side face 12d. Specifically, the end of the first internal electrode layer 20a is slightly recessed from the second end face 12f.

[0033] The shape of the first opposing electrode portion 22a of the first internal electrode layer 20a is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the first opposing electrode portion 22a may be tapered in plan view, with a slope increasing in either direction.

[0034] The shape of the first lead electrode portion 24a of the first internal electrode layer 20a is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the first lead electrode portion 24a may be tapered in plan view, with a slope increasing in either direction.

[0035] The width of the first opposing electrode portion 22a of the first internal electrode layer 20a and the width of the first extraction electrode portion 24a of the first internal electrode layer 20a may be formed to be the same width, or one of the widths may be formed to be narrower.

[0036] The second internal electrode layer 20b is disposed on the plurality of dielectric layers 14 and is located inside the laminate 12. The second internal electrode layer 20b has a second opposing electrode portion 22b facing the first internal electrode layer 20a and a second lead electrode portion 24b located on one end side of the second internal electrode layer 20b and extending from the second opposing electrode portion 22b to the second end face 12f of the laminate 12. The end of the second lead electrode portion 24b is extended to the surface of the second end face 12f and exposed from the laminate 12. In other words, the end of the first lead electrode portion 24a is not exposed on the first main surface 12a, the second main surface 12b, the first end face 12e, or the first side face 12c and the second side face 12d. Specifically, the end of the second internal electrode layer 20b is slightly recessed from the first end face 12e.

[0037] The shape of the second opposing electrode portion 22b of the second internal electrode layer 20b is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the second opposing electrode portion 22b may be tapered in plan view, with a slope increasing in either direction.

[0038] The shape of the second extraction electrode portion 24b of the second internal electrode layer 20b is not particularly limited, but is preferably rectangular in plan view. However, the corners in plan view may be rounded or may be formed obliquely in plan view (tapered). Alternatively, the second extraction electrode portion 24b may be tapered in plan view, with a slope increasing in either direction.

[0039] The width of the second opposing electrode portion 22b of the second internal electrode layer 20b and the width of the second extraction electrode portion 24b of the second internal electrode layer 20b may be formed to be the same width, or one of the widths may be formed to be narrower.

[0040] The laminate 12 includes side portions (hereinafter referred to as "W gaps") 26a of the laminate 12 formed between one ends of the first opposing electrode portion 22a and the second opposing electrode portion 22b in the width direction y and the first side surface 12c, and between the other ends of the first opposing electrode portion 22a and the second opposing electrode portion 22b in the width direction y and the second side surface 12d. Furthermore, the laminate 12 includes end portions (hereinafter referred to as "L gaps") 26b of the laminate 12 formed between an end of the first internal electrode layer 20a opposite to the first extraction electrode portion 24a and the second end surface 12f, and between an end of the second internal electrode layer 20b opposite to the second extraction electrode portion 24b and the first end surface 12e.

[0041] The internal electrode layers 20 can be made of an appropriate conductive material, such as a metal such as Ni, Cu, Ag, Pd, or Au, or an alloy containing at least one of these metals, such as an Ag-Pd alloy. The internal electrode layers 20 may further contain dielectric particles of the same composition as the ceramic contained in the dielectric layers 14.

[0042] The thickness of the internal electrode layer 20 is preferably 0.2 μm or more and 2.0 μm or less.

[0043] The total number of the first internal electrode layers 20a and the second internal electrode layers 20b is preferably 50 or more and 1000 or less.

[0044] As shown in FIG. 5, the laminate 12 shown in FIG. 1 may have, in addition to the first internal electrode layer 20a and the second internal electrode layer 20b, a floating internal electrode layer 20c that is not extended to either the first end face 12e or the second end face 12f. The floating internal electrode layer 20c may divide the opposing electrode portion 22 into multiple portions. For example, the opposing electrode portion 22 may have a two-part structure as shown in FIG. 5(a), a three-part structure as shown in FIG. 5(b), a four-part structure as shown in FIG. 5(c), or a structure with more than four parts. By dividing the opposing electrode portion 22 into multiple portions, multiple capacitor components are formed between the opposing first internal electrode layer 20a, the second internal electrode layer 20b, and the floating internal electrode layer 20c, and these capacitor components are connected in series. This reduces the voltage applied to each capacitor component, thereby increasing the withstand voltage of the multilayer ceramic capacitor 10.

[0045] Furthermore, like the first internal electrode layer 20a and the second internal electrode layer 20b, the floating internal electrode layer 20c can be made of an appropriate conductive material such as a metal such as Ni, Cu, Ag, Pd, or Au, or an alloy containing at least one of these metals, such as an Ag-Pd alloy.

[0046] As shown in FIGS. 1 to 3, external electrodes 30 are disposed on the first end face 12e side and the second end face 12f side of the laminate 12.

[0047] The external electrode 30 includes a base electrode layer 32 containing a metal component and glass, and a plating layer 34 disposed on the surface of the base electrode layer 32 .

[0048] The external electrode 30 includes a first external electrode 30a and a second external electrode 30b.

[0049] The first external electrode 30a is connected to the first internal electrode layer 20a and is disposed on at least the surface of the first end face 12e. The first external electrode 30a also extends from the first end face 12e of the laminate 12 and is disposed on part of the first main surface 12a, part of the second main surface 12b, and part of the first side surface 12c, and part of the second side surface 12d. In this case, the first external electrode 30a is electrically connected to the first extraction electrode portion 24a of the first internal electrode layer 20a.

[0050] The second external electrode 30b is connected to the second internal electrode layer 20b and is disposed on at least the surface of the second end face 12f. The second external electrode 30b also extends from the second end face 12f of the laminate 12 and is disposed on part of the first main surface 12a, part of the second main surface 12b, and part of the first side surface 12c, and part of the second side surface 12d. In this case, the second external electrode 30b is electrically connected to the second extraction electrode portion 24b of the second internal electrode layer 20b.

[0051] Within the laminate 12, capacitance is formed by the first opposing electrode portion 22a of the first internal electrode layer 20a and the second opposing electrode portion 22b of the second internal electrode layer 20b opposing each other via the dielectric layer 14. Therefore, capacitance can be obtained between the first external electrode 30a connected to the first internal electrode layer 20a and the second external electrode 30b connected to the second internal electrode layer 20b, and the characteristics of a capacitor are exhibited.

[0052] The base electrode layer 32 includes a first base electrode layer 32a and a second base electrode layer 32b.

[0053] The first base electrode layer 32a is connected to the first internal electrode layer 20a and is disposed on the surface of the first end face 12e. The first base electrode layer 32a also extends from the first end face 12e and is disposed on a part of the first main surface 12a, a part of the second main surface 12b, and a part of the first side surface 12c and a part of the second side surface 12d. In this case, the first base electrode layer 32a is electrically connected to the first extraction electrode portion 24a of the first internal electrode layer 20a.

[0054] The second base electrode layer 32b is connected to the second internal electrode layer 20b and is disposed on the surface of the second end face 12f. The second base electrode layer 32b also extends from the second end face 12f and is disposed on a part of the first main surface 12a, a part of the second main surface 12b, a part of the first side surface 12c, and a part of the second side surface 12d. In this case, the second base electrode layer 32b is electrically connected to the second extraction electrode portion 24b of the second internal electrode layer 20b.

[0055] The base electrode layer 32 includes at least one selected from a baked layer, a conductive resin layer, a thin film layer, and the like.

[0056] Hereinafter, each of the configurations when the base electrode layer 32 is the baked layer, the conductive resin layer, and the thin film layer will be described.

[0057] (In the case of a baking layer) The baking layer contains a metal component and glass. The metal component of the baking layer includes, for example, at least one selected from Cu, Ni, Ag, Pd, an Ag-Pd alloy, Au, etc. The baking layer is formed by applying a conductive paste containing glass and a metal to the laminate and baking it. The baking layer is formed by simultaneously baking a laminated chip having internal electrode layers 20 and dielectric layers 14 and the conductive paste applied to the laminated chip, but may also be baked after baking the laminated chip having internal electrode layers 20 and dielectric layers 14. The baking layer may be a multi-layered layer.

[0058] The thickness in the longitudinal direction z connecting the first end face 12e and the second end face 12f at the center in the height direction x of the first base electrode layer 32a located on the first end face 12e is preferably, for example, approximately 10 μm or more and 150 μm or less.

[0059] The thickness in the longitudinal direction z connecting the first end face 12e and the second end face 12f at the center in the height direction x of the second base electrode layer 32b located on the second end face 12f is preferably, for example, approximately 10 μm or more and 150 μm or less.

[0060] The thickness in the height direction x connecting the first main surface 12a and the second main surface 12b at the center of the length direction z connecting the first end face 12e and the second end face 12f of the first base electrode layer 32a located on part of the first main surface 12a and the second main surface 12b is preferably, for example, approximately 10 μm or more and 100 μm or less.

[0061] Furthermore, the thickness in the height direction x connecting the first main surface 12a and the second main surface 12b at the center of the length direction z connecting the first end face 12e and the second end face 12f of the second base electrode layer 32b located on part of the first main surface 12a and the second main surface 12b is preferably, for example, approximately 10 μm or more and 100 μm or less.

[0062] The thickness in the width direction y connecting the first side surface 12c and the second side surface 12d at the center of the length direction z connecting the first end face 12e and the second end face 12f of the first base electrode layer 32a located on part of the first side surface 12c and the second side surface 12d is preferably, for example, approximately 10 μm or more and 100 μm or less.

[0063] Furthermore, it is preferable that the thickness in the width direction y connecting the first side surface 12c and the second side surface 12d at the center of the length direction z connecting the first end face 12e and the second end face 12f of the second base electrode layer 32b located on part of the first side surface 12c and the second side surface 12d is, for example, approximately 10 μm or more and 100 μm or less.

[0064] (Conductive Resin Layer) The conductive resin layer has a first conductive resin layer and a second conductive resin layer.

[0065] The first conductive resin layer is preferably arranged as a first base electrode layer 32a so as to further cover other layers such as a baked layer, and the second conductive resin layer is preferably arranged as a second base electrode layer 32b so as to further cover other layers such as a baked layer.

[0066] Specifically, the first and second conductive resin layers, as the first and second base electrode layers 32a and 32b, are preferably disposed on other layers, such as baked layers, located on the first and second end faces 12e and 12f, and extend to the first and second main faces 12a and 12b and the first and second side faces 12c and 12d, respectively. However, the first and second conductive resin layers may be disposed only on the other layers, such as baked layers, located on the first and second end faces 12e and 12f.

[0067] The thickness of the first conductive resin layer and the second conductive resin layer is preferably, for example, about 10 μm or more and 200 μm or less.

[0068] The first conductive resin layer and the second conductive resin layer contain a thermosetting resin and a metal component.

[0069] Because the first conductive resin layer and the second conductive resin layer contain a thermosetting resin, they are more flexible than the base electrode layer 32 made of, for example, a plating film or a fired product of a conductive paste. Therefore, even if the multilayer ceramic capacitor 10 is subjected to a physical impact or an impact due to a thermal cycle, the conductive resin layer functions as a buffer layer and can prevent cracks in the multilayer ceramic capacitor 10.

[0070] Specific examples of the thermosetting resin include various known thermosetting resins such as epoxy resin, phenolic resin, urethane resin, silicone resin, polyimide resin, etc. Among these, epoxy resin is one of the most suitable resins because of its excellent heat resistance, moisture resistance, adhesion, etc.

[0071] The first conductive resin layer and the second conductive resin layer preferably contain a curing agent together with the thermosetting resin. When an epoxy resin is used as the base resin, various known compounds such as phenol-based, amine-based, acid anhydride-based, and imidazole-based compounds can be used as the curing agent for the epoxy resin.

[0072] The metal contained in the first conductive resin layer and the second conductive resin layer may be Ag, Cu, or an alloy thereof. Alternatively, a metal powder having an Ag-coated surface may be used. When using a metal powder having an Ag-coated surface, it is preferable to use Cu or Ni as the metal powder.

[0073] Alternatively, Cu that has been treated to prevent oxidation can also be used. The reason for using Ag-coated metal is that it allows the base metal to be inexpensive while maintaining the above-mentioned properties of Ag.

[0074] The metal contained in the first conductive resin layer and the second conductive resin layer is preferably contained in an amount of 35 vol % or more and 75 vol % or less with respect to the volume of the entire conductive resin.

[0075] The shape of the metal contained in the first conductive resin layer and the second conductive resin layer is not particularly limited, and the conductive filler may be spherical, flat, or the like.

[0076] The average particle size of the metal contained in the first conductive resin layer and the second conductive resin layer is not particularly limited. The average particle size of the conductive filler may be, for example, about 0.3 μm or more and 10 μm or less.

[0077] The metals contained in the first conductive resin layer and the second conductive resin layer are mainly responsible for the electrical conductivity of the conductive resin layers. Specifically, contact between the conductive fillers forms an electrical path inside the conductive resin layers.

[0078] The metal contained in the first conductive resin layer and the second conductive resin layer may be spherical, flat, or the like, but it is preferable to use a mixture of spherical metal powder and flat metal powder.

[0079] The conductive resin layer may be formed directly on the laminate without forming a baked layer.

[0080] Next, the first plating layer 34a and the second plating layer 34b, which are the plating layers 34 disposed on the base electrode layer 32, will be described with reference to FIGS. 2 and 3. FIG.

[0081] The first plating layer 34a and the second plating layer 34b contain at least one selected from, for example, Cu, Ni, Sn, Ag, Pd, an Ag--Pd alloy, Au, and the like.

[0082] The first plating layer 34a is disposed so as to completely cover the first base electrode layer 32a, and the second plating layer 34b is disposed so as to completely cover the second base electrode layer 32b.

[0083] The first plating layer 34a and the second plating layer 34b may be formed of multiple layers. In this case, the plating layer 34 preferably has a two-layer structure consisting of a lower plating layer (Ni plating layer) formed on the base electrode layer 32 by Ni plating and an upper plating layer (Sn plating layer) formed on the lower plating layer by Sn plating. That is, in this case, the first plating layer 34a has a first lower plating layer 36a and a first upper plating layer 38a located on the surface of the first lower plating layer 36a. Furthermore, the second plating layer 34b has a second lower plating layer 36b and a second upper plating layer 38b located on the surface of the second lower plating layer 36b.

[0084] The Ni-plated lower layer 36 is used to prevent the base electrode layer 32 from being eroded by solder when mounting the multilayer ceramic capacitor 10, and the Sn-plated upper layer 38 is used to improve the wettability of the solder when mounting the multilayer ceramic capacitor 10, thereby facilitating mounting. The thickness of each of the lower layer 36 and the upper layer 38 is preferably 1.0 μm or more and 15.0 μm or less.

[0085] The dimension in the length direction z of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 30a, and the second external electrode 30b is defined as dimension L, the dimension in the height direction x of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 30a, and the second external electrode 30b is defined as dimension T, and the dimension in the width direction y of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 30a, and the second external electrode 30b is defined as dimension W. The dimensions of the multilayer ceramic capacitor 10 are as follows: L in the length direction z is 1.0 mm to 3.2 mm, W in the width direction y is 0.5 mm to 2.5 mm, and T in the height direction x is 0.5 mm to 2.5 mm. The dimensions of the multilayer ceramic capacitor 10 can be measured using a microscope.

[0086] If voids exist in the dielectric layer 14, the mechanical strength is lower than that of the region filled with ceramic in the dielectric layer 14. Therefore, if voids exist in the area where electrostrictive stress is concentrated, electrostrictive cracks will occur in the dielectric layer 14, starting from the voids. Electrostriction is likely to occur at the ends in the width direction y of the dielectric layer 14 present in the inner layer portion 16 of the laminate 12.

[0087] 1, the amount of voids near the ends in the width direction y of the dielectric layers 14 present in the inner layer portion 16 of the laminate 12, where electrostrictive stress is concentrated, is made smaller than that in the center portion in the width direction y. Specifically, the amount of voids contained in the dielectric layers 14a2 near the width direction ends is smaller than the amount of voids contained in the dielectric layers 14a1 near the width direction center. This makes it possible to reduce the occurrence of electrostrictive cracks.

[0088] Furthermore, in the multilayer ceramic capacitor 10 shown in FIG. 1, the amount of voids contained in the width direction end side dielectric layers 14a2 is configured to be smaller than the amount of voids contained in the width direction center side dielectric layers 14a1. This improves the sinterability of the ceramic, and the dielectric constant ε of the width direction end side dielectric layers 14a2 is improved, thereby enabling the capacitance to be improved.

[0089] In addition, in the multilayer ceramic capacitor 10 shown in FIG. 1, when the difference between the area occupancy rate PCW of the voids in the WT cross section of the widthwise center side dielectric layer 14a1 and the area occupancy rate PEW of the voids in the WT cross section of the widthwise end side dielectric layer 14a2 is 1.0% or more and 8.0% or less, the occurrence of electrostrictive cracks can be further reduced.

[0090] Furthermore, in the multilayer ceramic capacitor 10 shown in FIG. 1, if the amount of voids contained in the longitudinal end side dielectric layer 14a4 is smaller than the amount of voids contained in the longitudinal center side dielectric layer 14a3, the effect of reducing the occurrence of electrostrictive cracks can be significantly achieved.

[0091] Furthermore, in the multilayer ceramic capacitor 10 shown in FIG. 1, when the difference between the area occupancy rate PCL of voids in the LT cross section of the longitudinal center side dielectric layer 14a3 and the area occupancy rate PEL of voids in the LT cross section of the longitudinal end side dielectric layer 14a4 is 4.0% or more and 8.0% or less, the effect of reducing the occurrence of electrostrictive cracks can be more significantly obtained.

[0092] 2. Method for Manufacturing a Multilayer Ceramic Capacitor Next, a method for manufacturing a multilayer ceramic capacitor will be described.

[0093] First, ceramic green sheets for the dielectric layers and conductive paste for the internal electrode layers are prepared. The ceramic green sheets and conductive paste for the internal electrode layers contain a binder and a solvent. The binder and solvent may be known.

[0094] Then, the conductive paste for the internal electrode layers is printed in a predetermined pattern on the ceramic green sheets for the dielectric layers by, for example, screen printing, gravure printing, etc. In this way, ceramic green sheets on which the patterns of the first internal electrode layers are formed and ceramic green sheets on which the patterns of the second internal electrode layers are formed are prepared.

[0095] (Process for Obtaining a Laminated Sheet) Subsequently, a predetermined number of ceramic green sheets for outer layers, on which the pattern of the internal electrode layer is not printed, are stacked to form a portion that will become the second outer layer portion on the second main surface side. Then, a ceramic green sheet on which the pattern of the first internal electrode layer is printed and a ceramic green sheet on which the pattern of the second internal electrode layer is printed are sequentially stacked on the portion that will become the second outer layer portion so as to form the structure of the present invention, to form a portion that will become the inner layer portion. A predetermined number of ceramic green sheets for outer layers, on which the pattern of the internal electrode layer is not printed, are stacked on this portion that will become the inner layer portion to form a portion that will become the first outer layer portion on the first main surface side. This completes the production of a laminated sheet.

[0096] (Step of Obtaining a Laminated Block) Next, the laminated sheet is pressed in the lamination direction by means of a hydrostatic press or the like to produce a laminated block.

[0097] (Step of Obtaining Laminated Chips) The laminated block is then cut to a predetermined size to obtain laminated chips. At this time, corners and ridges of the laminated chips may be rounded by barrel polishing or the like.

[0098] (Process for Obtaining a Laminate) Next, the laminated chip is fired to create a laminate. At this time, the heat distribution in the firing furnace during heat treatment is adjusted so that the heat amount at the center of the laminated chip in the width direction y is smaller than the heat amount at the ends of the laminated chip in the width direction y. This results in a higher ceramic filling rate at the ends of the laminate in the width direction y than at the center of the laminate in the width direction y, and the amount of voids at the ends of the laminate in the width direction y can be made smaller than the amount of voids at the center of the laminate in the width direction y. The firing temperature, although depending on the temperatures of the dielectric layers and internal electrode layers, is preferably 900°C or higher and 1400°C or lower.

[0099] Next, a conductive paste for the base electrode layer containing a metal component and a glass component is prepared.

[0100] (Step of forming external electrodes) The prepared conductive paste that will become the base electrode layer is applied to both end surfaces of the laminate to form the base electrode layer. The conductive paste can be applied to both end surfaces of the laminate by, for example, dipping or screen printing. The baking temperature at this time is preferably 700°C or higher and 900°C or lower.

[0101] Next, if necessary, plating is applied to the surface of the base electrode layer to form a plating layer. In this embodiment, two plating layers are formed on the surface of the base electrode layer. Specifically, a Ni plating layer and a Sn plating layer are formed on the base electrode layer. The Ni plating layer and the Sn plating layer are formed sequentially, for example, by barrel plating.

[0102] In the manner described above, the multilayer ceramic capacitor 10 according to the present embodiment is manufactured.

[0103] According to the method for manufacturing a multilayer ceramic capacitor of the present invention, the ceramic filling rate is higher at the ends of the laminate in the width direction y than at the center of the laminate in the width direction y, and the amount of voids at the ends of the laminate in the width direction y can be made smaller than the amount of voids at the center of the laminate in the width direction y. This makes it possible to obtain a multilayer ceramic capacitor that can reduce the rate of electrostrictive crack occurrence.

[0104] 3. Experimental Example Next, in order to confirm the effects of the multilayer ceramic capacitor according to the present invention described above, a multilayer ceramic capacitor sample was fabricated according to the manufacturing method described above as an experimental sample, and an experiment was conducted to confirm the presence or absence of cracks due to electrostriction.

[0105] (1) Specifications of Samples in Experimental Examples First, according to the above-described method for manufacturing a multilayer ceramic capacitor, samples of multilayer ceramic capacitors according to Examples 1 to 10 and a comparative example having the following specifications were fabricated.

[0106] (Specifications of the multilayer ceramic capacitor) Dimensions of the multilayer ceramic capacitor (design values): L x W x T = 1.6 mm x 0.8 mm x 0.8 mm Main ceramic material of the dielectric layer: BaTiO3 Capacitance: 22 μF Rated voltage: 16 V Material of the internal electrode layer: Ni Structure of the external electrode: Conductive metal (Cu) and glass component Film thickness at the center in the height direction of each of the first end face and the second end face of the external electrode: Approximately 90 μm Plating layer Two layers formed: Ni plating layer and Sn plating layer Ni plating layer thickness: Approximately 3 μm Sn plating layer thickness: Approximately 5 μm

[0107] (2) Evaluation Method for Crack Occurrence The electrostriction test of each sample multilayer ceramic capacitor was performed using a breakdown voltage measurement device. The detailed conditions for the breakdown voltage measurement device were a voltage boost of DC 150 V at a boost rate of 100 V / sec. For this evaluation, the presence or absence of cracks was observed using an ultrasonic flaw detector. Specifically, the sample multilayer ceramic capacitors were first aligned so that their main surfaces faced upward. Next, ultrasonic waves were irradiated onto the top surfaces of the aligned multilayer ceramic capacitors using an ultrasonic probe and scanned. The reflected waves of the ultrasonic waves were observed, and the presence or absence of cracks was confirmed by detecting the reflected waves that returned earlier than the bottom waves. Samples confirmed to have cracks were counted as electrostrictive defects, and the crack occurrence rate was calculated. For each example and comparative example, 100 samples were prepared, and the crack occurrence rate was measured. The crack occurrence rate was defined as the percentage of the number of cracks generated relative to the total number of measurements (100). The criteria for judging the crack occurrence rate were as follows: 0% or more and 10% or less: "◎", 11% or more and 30% or less: "◯", 31% or more and 50% or less: "△", and 51% or more and 100% or less: "×".

[0108] (3) Results Table 1 shows the crack occurrence rates of the dielectric layers of the laminates according to Examples 1 to 10 and the comparative example.

[0109]

[0110] According to Table 1, in each sample of Examples 1 to 10, the amount of voids contained in the dielectric layer on the widthwise end side was smaller than the amount of voids contained in the dielectric layer on the widthwise center side, and therefore, a good result of crack occurrence rate of 50% or less was obtained.

[0111] In addition, for each sample of Examples 2 to 6, the difference between the area occupancy rate PCW of the voids in the WT cross section of the dielectric layer on the widthwise center side and the area occupancy rate PEW of the voids in the WT cross section of the dielectric layer on the widthwise end side was 1.0% or more and 8.0% or less, so that the crack occurrence rate was 11% or more and 30% or less, which was a better result.

[0112] Furthermore, in each sample of Examples 8 to 10, the difference between the area occupancy rate PCL of voids in the LT cross section of the dielectric layer at the longitudinal center side and the area occupancy rate PEL of voids in the LT cross section of the dielectric layer at the longitudinal end side was 4.0% or more and 8.0% or less, so that the crack occurrence rate was 10% or less, and even better results were obtained.

[0113] On the other hand, in the sample according to the comparative example, the amount of voids contained in the dielectric layer at the widthwise end portion was the same as the amount of voids contained in the dielectric layer at the widthwise center portion, and therefore the crack occurrence rate was 66%.

[0114] From the above results, it has been suggested that in the present invention, the inner layer portion of the laminate is constituted by an inner dielectric layer, which contains voids, and the amount of voids contained in the dielectric layer on the widthwise end side arranged in the widthwise central region of the inner layer portion is smaller than the amount of voids contained in the dielectric layer on the widthwise central side. This makes it possible to reduce the amount of voids near the widthwise ends of the dielectric layers present in the inner layer portion of the laminate, which are locations where electrostrictive stress concentrates, compared to the amount of voids near the widthwise central portion, thereby reducing the occurrence of electrostrictive cracks.

[0115] As described above, the embodiment of the present invention has been disclosed in the above description, but the present invention is not limited to this.

[0116] In other words, various modifications can be made to the above-described embodiments in terms of mechanism, shape, material, quantity, position or arrangement, etc., without departing from the scope of the technical idea and purpose of the present invention, and these modifications are included in the present invention.

[0117] REFERENCE SIGNS LIST 10 Multilayer ceramic capacitor 12 Laminate 12a First main surface 12b Second main surface 12c First side surface 12d Second side surface 12e First end surface 12f Second end surface 14 Dielectric layer 14a Internal dielectric layer 14a1 Width direction center side dielectric layer 14a2 Width direction end side dielectric layer 14a3 Length direction center side dielectric layer 14a4 Length direction end side dielectric layer 14b External dielectric layer 16 Internal layer portion 18a First outer layer portion 18b Second outer layer portion 20 Internal electrode layer 20a First internal electrode layer 20b Second internal electrode layer 20c Floating internal electrode layer 22 Counter electrode portion 22a First counter electrode portion 22b Second counter electrode portion 24a First lead electrode portion 24b Second lead electrode portion 26a Side portion (W gap) 26b End portion (L gap) 30 External electrode 30a First external electrode 30b Second external electrode 32 Base electrode layer 32a First base electrode layer 32b Second base electrode layer 34 Plating layer 34a First plating layer 34b Second plating layer 36 Base plating layer 36a First base plating layer 36b Second base plating layer 38 Top plating layer 38a First top plating layer 38b Second top plating layer WA Region in which voids are arranged in the dielectric layer on the widthwise end side LA Region in which voids are arranged in the dielectric layer on the lengthwise end side x Height direction (stacking direction) y Width direction z Length direction

Claims

1. A laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate including a first main surface and a second main surface opposing each other in a height direction which is a lamination direction of the plurality of dielectric layers, a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the height direction and the width direction, the laminate including an inner layer portion in which the dielectric layers and the internal electrode layers are alternately laminated, and an outer layer portion arranged to sandwich the inner layer portion from the first main surface side and the second main surface side, a first external electrode arranged on the first end surface, and a second external electrode arranged on the second end surface, the inner layer portion being constituted by an inner dielectric layer of the plurality of dielectric layers arranged in the inner layer portion, the inner dielectric layer containing voids, the internal dielectric layer comprises a width direction center side dielectric layer arranged in a width direction center region of the inner layer portion, and a width direction end side dielectric layer arranged in a width direction end region of the inner layer portion, and an amount of the voids contained in the width direction end side dielectric layer is smaller than the amount of the voids in the width direction center side dielectric layer.

2. The multilayer ceramic capacitor of claim 1, wherein the difference between the area occupancy PCW of the void in the WT cross section of the dielectric layer at the width direction center and the area occupancy PEW of the void in the WT cross section of the dielectric layer at the width direction end is 1.0% or more and 8.0% or less.

Citation Information

Patent Citations

  • Laminated capacitor and external-electrode conductor paste therefor

    JP2001237137A

  • Laminated electronic component

    JP2022105470A

  • Multilayer ceramic capacitor and its manufacturing method